Quick-drying, high build, anti-sagging composition, coating, two-component package and coating method
By using a composition of hyperbranched polymer and a covalent bonded surfactant, combined with melamine and gas forming agent, the problem of existing coatings being susceptible to weather during application and drying is solved, and rapid water resistance is achieved, Touching the dry film reduces cost and improves performance.
Patent Information
- Application Number
- CN201880073494.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-04
- Filing Date
- 2018-11-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2038-11-13
AI Technical Summary
Existing expansion, vibration-absorbing and insulation coatings are susceptible to weather conditions during application and drying, resulting in a degradation of quality and difficulty in quickly forming water-resistant, finger-drying films, increasing labor and energy costs.
Using a composition including a polymeric binder, a coagulant and an additive, the polymeric binder is a hyperbranched polymer or a covalently bonded surfactant, the coagulant is a micronized pentaerythritol derivative, the additive is melamine, a carbon source and The gas-forming agent is arranged to form a non-sag, water-resistant coating within 30 seconds.
It realizes the formation of water-resistant and finger-drying coatings in a short time, reducing labor and energy costs, and improving the water resistance and fire-resistance, vibration-resistance and isolation properties of the coatings.
Smart Images

Figure BDA0002489697780000161 
Figure BDA0002489697780000171 
Figure BDA0002489697780000191
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Patent Application No. 62 / 585,804 filed on November 14, 2017 and U.S. Patent Application No. 62 / 680,321 filed on June 4, 2018, the contents of which are incorporated herein in their entirety. Technical Field
[0003] The present technology generally relates to expansion, vibration damping (ie, sound deadening) and insulation compositions and / or coatings, and methods of making and using the same. Background Art
[0004] Intumescent coatings are commonly used to protect substrates (e.g., commercial and residential structures) from the effects of fire and to extend the time until the substrate reaches a critical failure temperature. Intumescent agents / materials are substances that expand when exposed to heat to produce insulating foam or "charcoal". Heat can be generated by any type of fire conditions including cellulose, hydrocarbons and / or jetfire conditions. The thermal conductivity of charcoal is low, and the volume is many times that of the original coating. Volume expansion and charring protect any underlying substrate because charcoal acts as a poor thermal conductor and thus reduces the heating rate experienced by the substrate. Therefore, charcoal extends the time before the substrate loses its integrity and the building / structure collapses, thereby allowing additional time for safe evacuation. Therefore, intumescent coatings are used in passive fire protection and are applied to substrates as flame retardant coatings to improve fire resistance. Such coatings are suitable for use in many construction applications, such as providing a flame retardant barrier in steel and / or concrete structures.
[0005] To reduce noise generated by vibrations (e.g., in vehicles, electrical equipment, and machinery), sound-deadening materials are applied to the vibrating area to effectively dissipate the vibration energy. Applying glue or asphalt pads to the vibrating surface can dissipate some of the vibration energy, but this method is labor intensive and expensive in application because complex shapes must be produced to cover critical areas. Epoxy or PVC-based vibration-damping coatings are also used, but these are expensive and contain volatile organic compounds that can create hazards when the coating is applied.
[0006] Insulation materials are applied to cavities, ducts, and structures. Typically, insulation materials are applied for thermal insulation. Fiberglass insulation has been widely accepted for use in residential and light commercial construction. Fiberglass insulation products are made in a variety of configurations; however, in many applications, this insulation technology does reach its optimal thermal performance due to air infiltration, which can also allow water to condense. To overcome this drawback, spray-applied polyurethane foam insulation materials have been developed. However, similar to vibration damping coatings, these materials are generally expensive and contain volatile organic compounds that can create hazards when the coating is applied.
[0007] The formation of expansion, damping and insulation coatings on external surfaces and / or vertical surfaces also poses many challenges. It is worth noting that the coatings on external surfaces are usually kept exposed to the elements during application and drying. As a result, weather conditions during coating application and drying can affect the quality of the external coating. For example, rainfall during and / or after coating application can remove some or all of the coating, resulting in coating failure. By shortening the setting time of the coating, examples of coating failure (such as those due to unexpected rainfall) can be minimized. In addition, due to film rupture after curing, the expansion, damping and insulation coatings used previously cannot usually be applied in a single coating form to achieve the required film thickness, and therefore such coatings are often applied in a multi-coat form, resulting in increased labor costs. In some applications, external methods that accelerate the curing of these coatings, such as dryers, are used to accelerate the curing process, resulting in increased energy costs. It is necessary to obtain expansion, damping and insulation coatings that quickly form a film that is dry to the touch and water-resistant after application without sagging and thick slurry. Summary of the invention
[0008] The present technology provides a composition, which includes: a first composition, which includes a polymeric binder, the polymeric binder includes a hyperbranched polymer or a polymer containing a covalently bonded surfactant, a second composition, which includes a coagulant; and an additive, which includes an expander, a vibration damper, an insulating agent or a combination of two or more thereof; wherein the additive is present in the first composition, the second composition, or the first composition and the second composition; the expander includes an acid source, a carbon source and a gas forming agent; the vibration damper includes a first filler; the insulating agent includes a second filler; and the first composition and the second composition are configured to form a coating within 30 seconds of application to a substrate, and the coating is non-sag, water-resistant and dry to the touch. The composition is suitable for deposition onto a substrate that requires improved fire resistance, vibration damping or insulation. In some embodiments, the substrate can be a substrate used in the construction industry to provide passive fire protection / fire resistance; the substrate can be a vibration area of a vehicle, electrical equipment or machinery that requires vibration energy damping; the substrate can be a residential or commercial building, vehicle or aircraft that requires insulation (including thermal insulation).
[0009] In some embodiments, the hyperbranched polymer may include a reaction product of an acid-functional resin and an epoxy resin; wherein the hyperbranched polymer comprises carboxyl groups, hydroxyl groups, amino groups, urea groups, acetoacetoxy groups, diacetone groups, or any combination of two or more thereof. In some embodiments, the acid-functional resin may be a partially neutralized acid-functional resin; wherein the partially neutralized acid-functional resin is the reaction product of an acid-functional resin and at least a functionalized amine.
[0010] In certain embodiments, the polymer comprising the covalently bonded surfactant comprises one or more polymerized monomers, which include acrylic acid, methacrylic acid, alkyl acrylate, alkyl methacrylate, acrylonitrile, styrene, vinyl-containing monomers or any two or more combinations thereof. Surfactant can be an anionic surfactant. In certain embodiments, surfactant can include sulfate radical. Before being covalently bonded to polymer, surfactant can include allyl or vinyl. In certain embodiments, surfactant can include polyoxyalkyl (e.g., polyethylene oxide or polypropylene oxide). In certain embodiments, surfactant can include aromatic radical, such as phenyl.
[0011] The present technology also provides a method for forming a composition, a coating, a 2-pack coating kit including the composition, and a method of producing the coating. DETAILED DESCRIPTION
[0012] Various embodiments are described below. It should be noted that the specific embodiments are not intended to be exhaustive descriptions or limitations on the broader aspects discussed herein. An aspect described in conjunction with a specific embodiment is not necessarily limited to that embodiment and can be practiced with any other one or more embodiments.
[0013] As used herein, "about" will be understood by one of ordinary skill in the art and will vary to some extent depending on the context in which it is used. If a term is used that is not clear to one of ordinary skill in the art, then "about" will mean up to plus or minus 10% of the particular term, given the context in which it is used.
[0014] Unless otherwise indicated herein or clearly contradictory to the context, the use of the terms "a / an" and "said" and similar references in the context of describing elements (especially in the context of the following claims) should be interpreted as covering the singular and the plural. Unless otherwise indicated herein, the recitation of the range of values herein is intended only to serve as a shorthand method of individually referring to each individual value belonging to the range, and each individual value is incorporated into this specification as if it were individually described herein. Unless otherwise indicated herein or clearly contradictory to the context, all methods described herein can be performed in any suitable order. Unless otherwise stated, the use of any and all examples or exemplary language (such as "such as") provided herein is intended only to better illustrate the embodiments and does not limit the scope of the claims. The language in the specification should not be understood to indicate that any unclaimed element is essential. 。
[0015] In general, "substituted" refers to one or more hydrogen atom bonds contained in an alkyl, alkenyl, alkynyl, aryl or ether group (e.g., alkyl) as defined below, replaced by non-hydrogen or non-carbon atom bonds. Substituted groups also include groups in which one or more bonds to carbon or hydrogen atoms are replaced by one or more bonds to heteroatoms (including double bonds or triple bonds). Therefore, unless otherwise stated, a substituted group will be substituted by one or more substituents. In some embodiments, a substituted group is substituted by 1, 2, 3, 4, 5 or 6 substituents. Examples of substituents include: halogen (i.e., F, Cl, Br, and I); hydroxy; alkoxy, alkenyloxy, alkynyloxy, aryloxy, aralkyloxy, heterocyclyloxy, and heterocyclylalkoxy; carbonyl (oxo); carboxyl; ester; carbamate; oxime; hydroxylamine; alkoxyamine; aralkyloxyamine; thiol; sulfide; sulfoxide; sulfone; sulfonyl; sulfonamide; amine; N-oxide; hydrazine; hydrazide; hydrazone; azide; amide; urea; amidine; guanidine; enamine; imide; isocyanate; isothiocyanate; cyanate; thiocyanate; imine; nitro; nitrile (i.e., CN); and the like.
[0016] As used herein, "alkyl" includes straight and branched chain alkyl groups having 1 to about 20 carbon atoms, and typically 1 to 12 carbons, or in some embodiments, 1 to 8 carbon atoms. As used herein, "alkyl" includes cycloalkyl groups as defined below. Alkyl groups may be substituted or unsubstituted. Examples of straight chain alkyl groups include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, and n-octyl. Examples of branched chain alkyl groups include, but are not limited to, isopropyl, sec-butyl, tert-butyl, neopentyl, and isopentyl. Representative substituted alkyl groups may be substituted one or more times, for example, by amino, sulfenyl, hydroxyl, cyano, alkoxy, and / or halogen groups (such as F, Cl, Br, and I groups). As used herein, the term haloalkyl group is an alkyl group having one or more halogen groups. In certain embodiments, haloalkyl refers to a perhaloalkyl group.
[0017] Cycloalkyl is a cyclic alkyl, such as but not limited to cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl. In certain embodiments, cycloalkyl has 3 to 8 ring members, and in other embodiments, the range of ring carbon atoms is 3 to 5, 6 or 7. Cycloalkyl can be substituted or unsubstituted. Cycloalkyl further includes polycyclic cycloalkyl such as but not limited to norbornyl, adamantyl, bornyl, camphenyl, isocamphenyl and carenyl and fused rings such as but not limited to decahydronaphthyl etc. Cycloalkyl also includes the ring substituted by straight or branched alkyl as defined above. Representative substituted cycloalkyl groups may be monosubstituted or substituted more than once, such as, but not limited to, 2,2-; 2,3-; 2,4-; 2,5-; or 2,6-disubstituted cyclohexyl or mono-, di-, or tri-substituted norbornyl or cycloheptyl, which may be substituted, for example, with alkyl, alkoxy, amino, thiol, hydroxy, cyano, and / or halo.
[0018] Alkenyl is a straight chain, branched or cyclic alkyl group having 2 to about 20 carbon atoms and further including at least one double bond. In some embodiments, the alkenyl group has 1 to 12 carbons, or typically 1 to 8 carbon atoms. The alkenyl group may be substituted or unsubstituted. Alkenyl groups include, for example, ethenyl, propenyl, 2-butenyl, 3-butenyl, isobutenyl, cyclohexenyl, cyclopentenyl, cyclohexadienyl, butadienyl, pentadienyl and hexadienyl, etc. Alkenyl groups may be substituted similarly to alkyl groups. Divalent alkenyl groups, i.e., alkenyl groups having two points of attachment, include, but are not limited to, CH-CH=CH 2 、C=CH 2 or C=CHCH 3 .
[0019] As used herein, "aryl" or "aromatic" groups are cyclic aromatic hydrocarbons that do not contain heteroatoms. Aryl groups include monocyclic, bicyclic, and polycyclic systems. Thus, aryl groups include, but are not limited to, phenyl, azulenyl, cycloheptatrienyl, biphenylene, dicyclopentadienylphenylene, fluorenyl, phenanthrenyl, triphenylene, pyrenyl, naphthyl, chrysene, biphenyl, anthracenyl, indenyl, indanyl, pentalenyl, and naphthyl. In some embodiments, aryl groups contain 6-14 carbon atoms in the ring portion of the group, and in other embodiments contain 6 to 12 or even 6-10 carbon atoms. The phrase "aryl" includes groups containing fused rings, such as fused aromatic-aliphatic ring systems (e.g., indanyl, tetrahydronaphthyl, etc.). Aryl groups may be substituted or unsubstituted.
[0020] As used herein, the term "hyperbranched polymer" refers to a polymer having a main polymer chain and at least two branching points along the main polymer chain, which itself may also have additional branching points.
[0021] As used herein, the term "microgel" refers to a dispersion of polymer particles that are internally crosslinked without any significant amount of crosslinking in the continuous phase to provide a dispersion with lower viscosity and higher solids content. Typically, a microgel forms a continuous network after film formation.
[0022] As used herein, "anti-sag", "anti-sagging" or "no sag" refers to the ability of a composition to be applied to a vertical surface of a substrate at a dry film thickness ranging from about 1 mil to about 1000 mils without the coating sagging.
[0023] As used herein, the term "fast drying" refers to the ability of a coating to be touched within 30 seconds after application to a substrate surface of the composition without any transfer of the coating to the touched object.
[0024] As used herein, the terms "crosslinking" and "curing" refer to the toughening or hardening of the composition by reactive crosslinking of the components of the composition. In some embodiments, the composition can form a fully cured coating in less than 48, less than 36, less than 24, less than 12 hours, less than 10 hours, less than 8 hours, less than 6 hours, or less than 4 hours.
[0025] As used herein, "heat" refers to a type of energy transfer in which energy flows from a warmer substance or object to a cooler substance or object. Energy transfer as heat can occur through direct contact, a barrier that is impermeable to the substance (e.g., conduction), radiation, an intermediate fluid, or through a combination of two or more.
[0026] As used herein, an "intumescent coating" is a coating that expands due to heat exposure, thereby increasing volume and decreasing density. Typically, the intumescent coating can provide fire protection to the coated substrate and the structure to which the substrate is attached. Typically, the fire protection is passive fire protection.
[0027] As used herein, the term "flame retardant" is a material that inhibits or delays the spread of fire by inhibiting chemical reactions in a flame or by forming a protective layer on the surface of a substrate. The flame retardant can be mixed with the substrate material (such mixtures can be referred to as "additive flame retardants"), or chemically combined with the substrate material (such compounds can be referred to as "reactive flame retardants").
[0028] As used herein, the term "vibration dampening coating" is a coating that dampens mechanical vibrations of an article that includes a source of mechanical vibration. A vibration dampening coating may be provided using a liquid applied sound dampening ("LASD") composition.
[0029] As used herein, the term "barrier coating" is a coating that insulates a residential or commercial building, vehicle, or aircraft. In some embodiments, the coating can provide thermal and / or moisture insulation. Barrier coatings can be applied to any area that requires insulation. For example, barrier coatings can be applied to wall spaces in residential and commercial buildings.
[0030] The present technology provides a composition including a first composition and a second composition, which is configured to form a coating within 30 seconds of application after sequential or simultaneous application to a substrate, and the coating is non-sagging, water-resistant and dry to the touch. The composition includes a first composition, which includes a polymeric binder; a second composition, which includes a coagulant; and an additive, which is present in the first composition and / or the second composition. The coating provides fire resistance and / or flame retardancy, vibration damping and / or insulation.
[0031] In one aspect, the present technology provides a composition comprising: a first composition comprising a polymeric binder comprising a hyperbranched polymer or a polymer comprising a covalently bonded surfactant, a second composition comprising a coagulant; and additives comprising a swelling agent, a dampening agent, an isolating agent or a combination of two or more thereof; wherein the additive is present in the first composition, the second composition, or the first composition and the second composition; the swelling agent comprises an acid source, a carbon source, and a gas forming agent; the dampening agent comprises a first filler; the isolating agent comprises a second filler; and the first composition and the second composition are configured to form a coating within 30 seconds of being applied to a substrate, and the coating is non-sag, water-resistant, and dry to the touch.
[0032] In some embodiments, the dry film thickness of the coating is from about 5 μm to about 5 cm. In some embodiments, the dry film thickness of the coating is from about 100 μm to about 4 cm, from about 120 μm to about 3 cm, from about 140 μm to about 2.5 cm, from about 150 μm to about 2 cm, or from about 200 μm to about 1.5 cm. One or more layers of the composition can be applied to a substrate. In some embodiments, the composition can be applied to a substrate as a single layer or as part of a multilayer system. In some aspects, the composition can be applied on top of a primer or applied as a primer itself. In some embodiments, the composition can form a top coat.
[0033] In some embodiments, the acid source may include melamine phosphate, magnesium phosphate, boric acid and ammonium polyphosphate, polyphosphoric acid or any combination of two or more thereof. In some embodiments, the acid source may be present in about 5% to about 40% by weight based on the total weight of the composition. In some embodiments, the acid source may be present in about 15% to about 40% by weight, about 15% to about 35% by weight, about 15% to about 30% by weight or about 15% to about 25% by weight based on the total weight of the composition.
[0034] The carbon source may be a compound, salt, complex or composition that can be generated or decomposed or expanded into carbon at high temperature. In some embodiments, the carbon source may include a mono- or poly-substituted long chain hydrocarbon. For example, the carbon source may include a mono- or poly-substituted C 4 -C 20 A hydrocarbon chain comprising a mono- or poly-substituted C 5 -C 12 The hydrocarbon chain may be branched or straight, saturated or unsaturated, acyclic or cyclic. Preferred substituents include hydroxyl and / or alkoxy. In some embodiments, the carbon source may include C 4 -C 20 Alcohols, polyol compounds, polyhydroxylated C 4 -C 20 In certain embodiments, the carbon source may include pentaerythritol, dipentaerythritol, tripentaerythritol, starch, polyol compound, sugar, expanded graphite, cellulose acetate or any two or more thereof. ...
[0035] Gas forming agent can include melamine, melamine derivatives, nitrogen-containing derivatives, phosphorus-containing derivatives or any two or more combinations thereof. In certain embodiments, melamine derivatives can be salts. In certain embodiments, gas forming agent can include melamine, melamine cyanurate, melamine borate, melamine phosphate, tri-(hydroxyethyl) isocyanurate, melamine polyphosphate, chlorinated paraffin or any two or more combinations thereof. In certain embodiments, based on the gross weight of the composition, the gas forming agent can exist in about 1 wt % to about 40 wt %. In certain embodiments, based on the gross weight of the composition, the gas forming agent can exist in about 5 wt % to about 40 wt %, about 5 wt % to about 35 wt %, about 5 wt % to about 30 wt %, about 5 wt % to about 25 wt % or about 5 wt % to about 20 wt %.
[0036] The first filler may include mineral fillers, polymeric plastic fillers or a combination thereof. In certain embodiments, mineral fillers may include alkaline earth carbonate. In certain embodiments, mineral fillers may include: calcium carbonate (e.g., ground or precipitated), mica, diatomaceous earth, zeolite, graphite, kaolin, clay (e.g., calcined, peeled or constructed), glass flakes, illite (hillite), kaolinite (caolinite), titanium dioxide, calcium silicate, aluminum silicate, magnesium silicate, wollastonite, zinc oxide, iron oxide, magnesium carbonate, amorphous silicon dioxide, zinc hydroxide, aluminum oxide, aluminum hydroxide, talc, satin white (satin white), barium sulfate, calcium sulfate or a combination of two or more thereof. In certain embodiments, polymeric plastic fillers are non-agglomerated (at least at use temperature). In certain embodiments, polymeric plastic fillers may include solid beads, porous, porous, adhesive-coated, filled or a combination of two or more thereof. In certain embodiments, the first filler may include the recycled alkaline earth carbonate provided in PCT / US2017 / 063570 (incorporated herein). In some embodiments, the first filler may include spent calcium carbonate.
[0037] In some embodiments, the first filler may be present in about 15% to about 80% by weight. Based on the total weight of the composition, this may include, but is not limited to, about 20% to about 70% by weight; about 25% to about 70% by weight; about 40% to about 70% by weight; or about 50% to about 65% by weight.
[0038] The composition can exhibit sound dampening properties, such as measured by a composite loss tangent of about 0.13 to about 0.40, including about 0.15 to about 0.35, about 0.20 to about 0.30, or about 0.30 to about 0.40, at a frequency of 200 Hz and at a temperature of about 20° C. to about 30° C.
[0039] The second filler may include balsa wood, calcium silicate, cellulose, chalk, cork board, regranulated cork, cotton, raw cotton, diatomaceous earth, felt insulation, glass fiber, foam glass, glass wool, felt, kapok insulation, magnesium oxide insulation, mineral wool insulation, paper, peat, foamed plastic, polypropylene, polyethylene, polyurethane, rock wool, wool, silica aerogel, slag wool, polystyrene, vermiculite, wax, perlite, rice husk, hollow glass ball, hollow ceramic ball, alumina-silica fiber, alumina-silica-zirconia fiber, polycrystalline mullite fiber, calcium aluminosilicate fiber, alumina fiber, mineral fiber or a combination of two or more thereof. In some embodiments, the second filler may include ceramic fiber, such as alumina-silica fiber, alumina-silica-zirconia fiber, polycrystalline mullite fiber, calcium aluminosilicate fiber, alumina fiber and mineral fiber. In some embodiments, the second filler may include glass, such as glass fiber, foam glass, glass wool, hollow glass ball or hollow ceramic ball. In some embodiments, the second filler may include hollow glass spheres.
[0040] In some embodiments, the second filler can be present at about 15% to about 80% by weight. Based on the total weight of the composition, this can include, but is not limited to, about 15% to about 70% by weight; about 15% to about 65% by weight; about 15% to about 50% by weight; or about 20% to about 40% by weight.
[0041] The composition can exhibit a thermal conductivity of about 0.020 N / mK to about 0.065 N / mK, including about 0.040 N / mK to about 0.062 N / mK or about 0.053 N / mK to about 0.059 N / mK, as measured according to ASTM C-518.
[0042] In some embodiments, the composition may further include a soundproofing material and an aqueous composition that can be sprayed or otherwise applied to a construction substrate to provide improved soundproofing properties. For example, the soundproofing material can be used in building and construction applications where it is necessary to eliminate impact and / or airborne noise, such as in doors, roofs, walls, floors, and ceilings. Specific uses may include incorporating the soundproofing material into gypsum underlayment systems, such as floor / ceiling assemblies in multi-family or commercial buildings.
[0043] In some embodiments, the sound insulation material includes an acrylic polymer polymerization product of a molten resin mixture, the molten resin mixture including at least one acrylic monomer, a polymerization initiator, which is present in a molar ratio of the polymerization initiator to the at least one acrylic monomer of about 0.0005:1 to about 0.06:1; and 0 to about 25 weight percent of a reaction solvent, based on the weight of the acrylic monomer, wherein the acrylic polymer polymerization product includes unreacted acrylic monomer and an acrylic polymer product.
[0044] In some embodiments, at least one acrylic monomer may include an acrylic monomer as described in any embodiment herein. In some embodiments, at least one acrylic monomer includes but is not limited to acrylic acid, methacrylic acid, chloroacrylic acid, ethylacrylic acid, crotonic acid, itaconic acid, sorbic acid, cinnamic acid, citraconic acid, mesaconic acid, maleic acid, fumaric acid, sodium 2-sulfoethyl acrylate, sodium N-(1,1-dimethyl-2-sulfoethyl) acrylamide or 3-acrylamido-3-methylbutyric acid, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2,3-hydroxypropyl acrylate, 2,3-hydroxypropyl methacrylate, 2,4-hydroxybutyl acrylate, 2,4-hydroxybutyl methacrylate, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, sec-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, Isobornyl acrylate, n-hexyl acrylate, 2-ethylbutyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-decyl acrylate, methylcyclohexyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, methyl methacrylate, ethyl methacrylate, 2-hydroxyethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isopropyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, isopentyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, 2-ethylbutyl methacrylate, methylcyclohexyl methacrylate, cinnamyl methacrylate, crotonyl methacrylate, cyclohexyl methacrylate, cyclopentyl methacrylate, 2-ethoxyethyl methacrylate, isobornyl methacrylate.
[0045] In certain embodiments, at least one acrylic monomer further includes at least one latent crosslinking monomer. As used herein, "latent crosslinking ability" refers to the ability of one or more types of functional groups on the polymer backbone to further react and form covalent bonds when applying and evaporating water from the acrylic polymer polymer product. Such latent crosslinking monomers include, but are not limited to, monomers with reactive ketone groups, such as diacetone acrylamide (DAAM), diacetone methacrylamide, acetoacetic acid vinyl ester, acrolein and methacrolein. In certain embodiments, the molten resin mixture may further include one or more styrene monomers. Suitable styrene monomers may include, but are not limited to, styrene, alpha-methyl styrene, ethyl styrene, isopropyl styrene and tert-butyl styrene.
[0046] In certain embodiments, when the polymer backbone of the acrylic polymer polymer product including polymerization latent cross-linking monomers, the acrylic polymer may further include a cross-linking agent. Suitable cross-linking agents may include but are not limited to polyamines, polyhydrazides, hydrazides (e.g., adipic acid dihydrazides) or mixtures of two or more thereof. In certain embodiments, the cross-linking agent for reacting with the latent cross-linking monomer functional groups can achieve the necessary amount of the desired degree of cure (i.e., cross-linking) to exist. For example, the cross-linking agent can provide at least about 0.1 equivalents of each equivalent of latent cross-linking functional groups to exist. In certain embodiments, the cross-linking agent can provide about 0.2 to about 2.0 equivalents of each equivalent of latent cross-linking functional groups to exist. In certain embodiments, the cross-linking agent can provide about 0.4 to about 1.2 equivalents of each equivalent of latent cross-linking functional groups to exist. In certain embodiments, the cross-linking agent can provide about 0.4 to about 1.0 equivalents of each equivalent of latent cross-linking functional groups to exist.
[0047] In some embodiments, the polymerization initiator may include a compound that thermally decomposes into free radicals in a primary reaction, but this is not a critical factor. In some embodiments, the polymerization initiator may exhibit a suitable half-life decomposition temperature suitable for the selected reaction temperature and residence time. In some embodiments, the polymerization initiator may be a thermal initiator. Suitable polymerization initiators may include, but are not limited to, 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), tert-butyl perbenzoate, tert-amyl peroxy-2-ethylhexyl carbonate, 1,1-bis(tert-amyl peroxy)cyclohexane, tert-amyl peroxy-2-ethylhexanoate, tert-amyl peroxyacetate, tert-butyl peroxyacetate, tert-butyl peroxybenzoate (TBPB), 2,5-di-(tert-butyl peroxy)-2,5-dimethylhexane, di-tert-amyl peroxide (DTAP), di-tert-butyl peroxide (DTBP), lauryl peroxide, dilauryl peroxide (DLP), succinic acid peroxide; or benzoyl peroxide. The polymerization initiator may be present in a molar ratio of the polymerization monomer to the at least one acrylic monomer of about 0.0005: 1 to about 0.06: 1. Suitable molar ratios include, but are not limited to, about 0.0005: 1, about 0.0006: 1, about 0.0007: 1, about 0.0008: 1, about 0.0009: 1, about 0.001: 1, about 0.002: 1, about 0.003: 1, about 0.004: 1, about 0.005: 1, about 0.006: 1, about 0.007: 1, about 0.008: 1, about 0.009: 1, about 0.01: 1, about 0.02: 1, about 0.03: 1, about 0.04: 1, about 0.05: 1, about 0.06: 1, or any range including and / or between any two of the above values.
[0048] In certain embodiments, the molten reaction mixture includes a reaction solvent. Suitable reaction solvents include, but are not limited to, water, acetone or other water-compatible solvents. The suitable amount of the reaction solvent present may include, but is not limited to, 0 wt %, about 1 wt %, about 2 wt %, about 3 wt %, about 4 wt %, about 5 wt %, about 6 wt %, about 7 wt %, about 8 wt %, about 9 wt %, about 10 wt %, about 11 wt %, about 12 wt %, about 13 wt %, about 14 wt %, about 15 wt %, about 16 wt %, about 17 wt %, about 18 wt %, about 19 wt %, about 20 wt %, about 21 wt %, about 22 wt %, about 23 wt %, about 24 wt %, about 25 wt % (based on the weight of acrylic acid monomer) or any including any two values and / or the scope between any two values.
[0049] In some embodiments, the polydispersity ratio of the acrylic polymer polymerization product may be less than about 3. For example, the polydispersity ratio of the acrylic polymer polymerization product may be less than about 3.0, about 2.9, about 2.8, about 2.7, about 2.6, about 2.5, about 2.4, about 2.3, about 2.2, about 2.1, about 2.0, about 1.9, about 1.8, about 1.7, about 1.6, about 1.5, about 1.4, about 1.3, about 1.2, about 1.1, about 1.0, about 0.9, about 0.8, about 0.7, about 0.6, about 0.5, or any range including and / or between any two of the foregoing values.
[0050] In some embodiments, the number average molecular weight (M) of the acrylic acid polymer polymerization product is n ) is about 1000 g / mol to about 10,000 g / mol. Suitable number average molecular weight (M n) may include, but are not limited to, about 1000 g / mol, about 1200 g / mol, about 1400 g / mol, about 1600 g / mol, about 1800 g / mol, about 2000 g / mol, about 2200 g / mol, about 2400 g / mol, about 2600 g / mol, about 2800 g / mol, about 3000 g / mol, about 3200 g / mol, about 3400 g / mol, about 3600 g / mol, about 3800 g / mol, about 4000 g / mol, about 4200 g / mol, about 4400 g / mol, about 4600 g / mol, about 4800 g / mol, about 5000 g / mol, about 5200 g / mol, about 5400 g / mol, about 5600 g / mol, In some embodiments, the acrylic acid polymer has an M of about 500 g / mol, about 6000 g / mol, about 6200 g / mol, about 6400 g / mol, about 6600 g / mol, about 6800 g / mol, about 7000 g / mol, about 7200 g / mol, about 7400 g / mol, about 7600 g / mol, about 7800 g / mol, about 8000 g / mol, about 8200 g / mol, about 8400 g / mol, about 8600 g / mol, about 8800 g / mol, about 9000 g / mol, about 9200 g / mol, about 9400 g / mol, about 9600 g / mol, about 9800 g / mol, about 10,000 g / mol, or any range including any two of the above values and / or between any two of the above values. In some embodiments, the M of the acrylic acid polymer polymerized product is about 5000 g / mol, about 5100 g / mol, about 5200 g / mol, about 5400 g / mol, about 5500 g / mol n From about 1000 g / mol to about 2500 g / mol, from about 1000 g / mol to about 3500 g / mol, from about 1000 g / mol to about 5000 g / mol, from about 1000 g / mol to about 7500 g / mol, or from about 1000 g / mol to about 10,000 g / mol.
[0051] In some embodiments, the polymerization of the sound insulation material includes a continuous bulk polymerization process, which includes: charging a molten resin mixture as described in any embodiment herein into a continuous mixing reactor zone; maintaining a flow rate of the molten resin mixture through the reaction zone; and maintaining the molten resin mixture at an elevated temperature in the range of about 180°C to about 270°C.
[0052] In certain embodiments, the residence time that flow rate provides the molten resin mixture filled in reaction zone is about 1 to about 30min.Suitable residence time includes but is not limited to about 1min, about 2min, about 3min, about 4min, about 5min, about 6min, about 7min, about 8min, about 9min, about 10min, about 11min, about 12min, about 13min, about 14min, about 15min, about 16min, about 17min, about 18min, about 19min, about 20min, about 21min, about 22min, about 23min, about 24min, about 25min, about 26min, about 27min, about 28min, about 29min, about 30min or any including above-mentioned any two values and / or the scope between above-mentioned any two values.In certain embodiments, flow rate can be suitable for maintaining the predetermined level of reaction mixture in reaction zone.
[0053] In some embodiments, the method includes maintaining the molten resin mixture at an elevated temperature of about 180°C to about 270°C. Suitable temperatures include, but are not limited to, about 180°C, about 190°C, about 200°C, about 210°C, about 220°C, about 230°C, about 240°C, about 250°C, about 260°C, about 270°C, or any range including any two of the above values and / or between any two of the above values. In some embodiments, the elevated temperature may be sufficient to provide an accelerated conversion to an acrylic polymer polymer product. For example, the elevated temperature is sufficient to provide an accelerated conversion to an acrylic polymer product, wherein the acrylic polymer product is a polymer product that is easily processable, uniform, and concentrated.
[0054] In some embodiments, the sound-deadening material may be prepared via a high temperature continuous polymerization process as described in US Pat. Nos. 4,546,160, 4,414,370, or 4,529,787, each of which is incorporated herein by reference.
[0055] In some embodiments, the composition may exhibit sound attenuation properties, including, but not limited to, a minimum Impact Insulation Class (IIC) rating of about 50, as measured according to ASTM E989, and / or a minimum Impact Insulation Class field rating of 45, as measured according to ASTM 1007. For example, the composition may exhibit sound attenuation properties as described herein when applied to a floor and / or ceiling assembly. In some embodiments, the composition may be applied to a floor and / or ceiling assembly and may exhibit an IIC rating of about 45 or greater. In some embodiments, the composition may be applied to a floor and / or ceiling assembly and may exhibit an IIC rating of about 35 to about 55.
[0056] In some embodiments, the coagulant may include dialkylaminoalkyl (meth)acrylate polymers, hexose polymers, montmorillonite clay, chitosan, poly[oxyalkylene (dialkylimino) alkylene] polymers, epihalohydrin / dialkylamine polymers, polydiallyldialkylammonium halide polymers, polyepiamines, electrolytes containing dialkylamine epihalohydrin, halides containing dialkylamine-epihalohydrin-alkylenediamine polymers, dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate methyl chloride quaternary ammonium salt, dimethylaminoethyl methacrylate methyl sulfate quaternary ammonium salt, dimethylaminoethyl methacrylate methyl chloride quaternary ammonium salt, acrylamidopropyl trimethylammonium chloride, aluminum chlorohydrate, sulfuric acid Aluminum, zinc chloride, ferric chloride, calcium chloride, magnesium hydroxide, calcium propionate, calcium polyphosphate, potassium tripolyphosphate, zinc ammonium bicarbonate, zinc ammonium nitrate, zinc ammonium acetate, sodium chloride, potassium chloride, potassium bromide, sodium sulfate, magnesium sulfate, copper sulfate, zinc sulfate, ferrous sulfate, ferrous sulfate, magnesium chloride, magnesium carbonate, alum, monocalcium phosphate, monomagnesium phosphate, monozinc phosphate, calcium pantothenate, glycine calcium salt, alanine calcium salt, serine calcium salt, threonine calcium salt, methionine calcium salt, phenylalanine calcium salt, calcium aspartate, sodium oxalate, calcium acetate, magnesium acetate, calcium pantothenate, glycine calcium salt, alanine calcium salt, serine calcium salt, threonine calcium salt, methionine calcium salt, phenylalanine calcium salt, calcium aspartate, polyphosphoric acid or any two or more thereof. In some embodiments, the coagulant may be present in about 0.01 wt % to about 20 wt % based on the total weight of the first composition. In some embodiments, the coagulant may be present at about 0.1% to about 20% by weight, about 1% to about 15% by weight, about 1% to about 10% by weight, about 1% to about 5% by weight, or about 0.1% to about 5% by weight, based on the total weight of the first composition. In some embodiments, the coagulant may be present at about 0.01% to about 20% by weight, based on the total weight of the second composition. In some embodiments, the coagulant may be present at about 0.1% to about 20% by weight, about 1% to about 15% by weight, about 1% to about 10% by weight, about 1% to about 5% by weight, or about 0.1% to about 5% by weight, based on the total weight of the second composition. In some embodiments, the coagulant may be present at about 0.01% to about 20% by weight, based on the total weight of the second composition. In some embodiments, the coagulant may be present at about 0.1 wt % to about 20 wt %, about 1 wt % to about 15 wt %, about 1 wt % to about 10 wt %, about 1 wt % to about 5 wt %, or about 0.1 wt % to about 5 wt %, based on the total weight of the second composition.
[0057] In some embodiments, the hyperbranched polymer may include the reaction product of an acid-functional resin and an epoxy resin; wherein the hyperbranched polymer comprises carboxyl, hydroxyl, amino, urea, acetoacetoxy, diacetone, or any combination of two or more thereof. In some embodiments, the hyperbranched polymer comprises one or more hydroxyl groups.
[0058] In some embodiments, the acid functional resin can be a partially neutralized acid functional resin; wherein the partially neutralized acid functional resin is the reaction product of an acid functional resin and at least a functionalized amine. In some embodiments, the acid groups on the acid functional resin are at least partially neutralized before the acid groups on the acid functional resin are bonded to the epoxy resin. In some embodiments, at least about 5 mol% of the acid groups on the acid functional resin are neutralized. In some embodiments, up to about 95 mol% of the acid groups on the acid functional resin are bonded to the epoxy resin.
[0059] The acid-functional resin may include an acid-functional acrylic resin, a styrene-acrylic resin, a non-acrylic functional resin, a mixed acrylic functional resin, an acid-functional polyester, an acid-functional polyamide, an acid-functional wax, or a mixed copolymer thereof. The mixed resin includes a copolymer (e.g., a block copolymer) comprising two or more covalently bonded homopolymers or copolymers. In some embodiments, the acid-functional resin may include one or more polymerized monomers selected from the group consisting of: 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2,3-hydroxypropyl acrylate, 2,3-hydroxypropyl methacrylate, 2,4-hydroxybutyl acrylate, 2,4-hydroxybutyl methacrylate, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, sec-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, isobornyl acrylate, n-hexyl acrylate, 2-ethylbutyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, acrylate n-Decanyl methacrylate, methylcyclohexyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, methyl methacrylate, ethyl methacrylate, 2-hydroxyethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isopropyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, isopentyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, 2-ethylbutyl methacrylate, methylcyclohexyl methacrylate, cinnamyl methacrylate, crotonyl methacrylate, cyclohexyl methacrylate, cyclopentyl methacrylate, 2-ethoxyethyl methacrylate and isobornyl methacrylate.
[0060] In some embodiments, epoxy resin may have multiple epoxy groups. In some embodiments, epoxy resin may include polyepoxy-functional polymers, monoepoxide-functional polymers or combinations thereof. The epoxy equivalent of polyepoxy-functional polymers may be from about 100Eq. / kg to about 1000Eq. / kg. Polyepoxy-functional polymers include diglycidyl ester polymers, glycidyl amine polymers, cyclohexanedimethanol diglycidyl ether polymers, polyoxypropylene diglycidyl ether polymers, bisphenol A diglycidyl ether polymers, bisphenol F diglycidyl ether polymers or any two or more thereof. Monoepoxy-functional polymers may include glycidyl ether polymers, glycidyl ester polymers, glycidyl amine polymers, glycidyl ester polymers or any two or more thereof. In some embodiments, monoepoxy-functional polymers may include glycidyl methacrylate, glycidyl ester of neodecanoic acid, biphenol A monoglycidyl ether, 2-ethylhexyl glycidyl ether or any two or more thereof. The monoepoxy-functional polymer may include one or more hydroxyl groups.
[0061] In some embodiments, the functionalized amine includes a hydroxyl group, a cyano group, a carboxyl group, a nitro group, a heteroaryl group, or any combination of two or more thereof. The functionalized amine may include a compound represented by Formula IA, Formula IIA, Formula IIIA, or any mixture of two or more thereof:
[0062]
[0063] Where: R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 and R 11 are independently hydrogen or C 1 -C 6 Alkyl; R 12 , R 13 , R 14 , R 15 , R 16 and R 17 are each independently hydrogen, hydroxyl, halogen, carboxyl, amide, ester, thiol, alkylthio, guanidine or C 1 -C 6 Alkyl, C 3 -C 10 Cycloalkyl, C 3 -C 10 Heterocycloalkyl, C 5 -C 12Aryl or C 5 -C 12 heteroaryl; l and p are each independently 0, 1, 2, 3, 4 or 5; and m and n are each independently 1, 2, 3, 4 or 5. In some embodiments, the functionalized amine comprises ethanolamine, triethanolamine, 3-amino-1-propanol, amino-2-propanol, 4-amino-1-butanol, 3-amino-1-butanol, 2-amino-1-butanol, 5-amino-1-pentanol, methyldiethanolamine, dimethylethanolamine or any two or more thereof. In some embodiments, the functionalized amine comprises ethanolamine, triethanolamine, methyldiethanolamine, dimethylethanolamine or any two or more thereof.
[0064] In some embodiments, the acid-functional resin comprises the polymerization product of a mixture of monomers comprising a styrenic monomer and a monomer of formula V, maleic anhydride, itaconic acid, an ester of itaconic acid, or a mixture of any two or more thereof; wherein:
[0065]
[0066] R 20 is hydrogen or CH 3 ; and R 19 is hydrogen, alkyl, cycloalkyl, aryl or alkaryl. In some embodiments, R 19 Can be C 1 -C 20 Alkyl, C 3 -C 20 Cycloalkyl, C 5 -C 12 Aryl or C 5 -C 20 Alkyl.
[0067] In some embodiments, the number average molecular weight (M) of the acid-functional resin is n ) is about 1000 g / mol to about 100,000 g / mol. In some embodiments, the number average molecular weight (M) of the acid-functional resin is about 1000 g / mol to about 100,000 g / mol. n ) is about 1000 g / mol to about 10,000 g / mol. In some embodiments, the number average molecular weight (M) of the acid-functional resin is about 1000 g / mol to about 10,000 g / mol. n ) is about 2500 g / mol until the gel point of the acid-functional resin. In some embodiments, the weight average molecular weight (M) of the acid-functional resin is about 2500 g / mol. w ) is from about 2000 g / mol to about 1,000,000 g / mol.
[0068] In some embodiments, the hyperbranched polymer has an acid value of about 15 mg KOH / g to about 300 mg KOH / g. In some embodiments, the hyperbranched polymer has an acid value of about 20 mg KOH / g to about 250 mg KOH / g. In some embodiments, the hyperbranched polymer has a hydroxyl number of about 1 mg KOH / g to about 300 mg KOH / g. In some embodiments, the hyperbranched polymer has a hydroxyl number of about 10 mg KOH / g to about 250 mg KOH / g.
[0069] In some embodiments, the hyperbranched polymer can be a microgel.
[0070] In some embodiments, the hyperbranched polymer may be any hyperbranched polymer disclosed in U.S. Pat. No. 7,887,626, RE 44,931, or PCT / US2017 / 057214, each of which is incorporated herein by reference.
[0071] In some embodiments, the polymer comprising a covalently bonded surfactant comprises one or more polymerized monomers comprising acrylic acid, methacrylic acid, an alkyl acrylate, an alkyl methacrylate, acrylonitrile, styrene, a vinyl-containing monomer, or a combination of any two or more thereof. In some embodiments, the one or more polymerized monomers comprise acrylic acid, methacrylic acid, acrylic acid C 1 -C 4 Alkyl ester, methacrylate C 1 -C 4 Alkyl ester, acrylic acid C 1 -C 4 Hydroxyalkyl ester, methacrylate C 1 -C 4 In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer. In some embodiments, the polymer comprising a covalently bonded surfactant may be a copolymer.
[0072] The covalently bonded surfactant may include an anionic surfactant. In some embodiments, the anionic surfactant may include a sulfate group, a sulfonate group, a carboxylate group, or a phosphate group. In some embodiments, the anionic surfactant may include a sulfate group.
[0073] Before being covalently bonded to the polymer, the surfactant may include an allyl or vinyl group. In some embodiments, the surfactant may include a polyoxyalkyl group (e.g., polyethylene oxide or polypropylene oxide). In some embodiments, the surfactant may include an aromatic group. In some embodiments, the aromatic group may be a phenyl group.
[0074] In some embodiments, the covalently bonded surfactant may include a compound represented by Formula IB, Formula IIB, or a mixture thereof prior to covalent bonding to the polymer:
[0075]
[0076] Where: R 21 and R 27 Each is independently a sulfate; R 20 is hydrogen or methyl; R 22 , R 23 , R 24 , R 25 and R 26 are independently hydrogen or C 1 -C 6 Alkyl; R 28 , R 29 , R 30 , R 31 and R 32 are independently hydrogen, C 1 -C 6 Alkyl or C 2 -C 6 alkenyl, provided that R 28 , R 29 , R 30 , R 31 and R 32 At least one of them is C 2 -C 6 and q and r are each independently 5-30. In some embodiments, R 21 and R 27 Each can be SO independently 2 O - X + , where X + for Na + or NH 4 + In some embodiments, R 22 , R 23 , R 24 , R 25 and R 26 can be independently hydrogen or branched C 1 -C 6 In some embodiments, R 22 , R23 , R 25 and R 26 Each is hydrogen and R 24 In some embodiments, R 28 , R 29 , R 30 , R 31 and R 32 Each is hydrogen or C 2 -C 4 In some embodiments, q and r are each independently 5-15. In some embodiments, q and r are each independently 15-25. Other suitable surfactants that can be covalently bonded to the polymer include those disclosed in U.S. Published Patent Application No. 2001 / 0020064 and Journal of Applied Polymer Science, Vol. 109, 2275-2282 (2008), which are incorporated herein by reference.
[0077] In some embodiments, the number average molecular weight (M) of the polymer including the covalently bonded surfactant is n ) is about 10,000 g / mol to about 200,000 g / mol. In some embodiments, the number average molecular weight (M) of the polymer is n ) is about 50,000 g / mol to about 150,000 g / mol. In some embodiments, the weight average molecular weight (M) of the polymer is w ) is about 50,000 g / mol to about 1,000,000 g / mol. In some embodiments, the weight average molecular weight (M) of the polymer is about 1,000,000 g / mol to about 1,000,000 g / mol. w ) is from about 100,000 g / mol to about 500,000 g / mol.
[0078] In some embodiments, the polymeric binder is present in an amount of about 5 wt % to about 60 wt % based on the total weight of the first composition. In some embodiments, the polymeric binder is present in an amount of about 5 wt % to about 50 wt %, about 5 wt % to about 40 wt %, about 5 wt % to about 30 wt %, or about 5 wt % to about 25 wt %, based on the total weight of the first composition.
[0079] The composition may also contain a mineral filler, which may be selected from energy dissipative fillers such as aluminum hydroxide, magnesium hydroxide, calcium carbonate or mixtures thereof, providing an additional contribution to flame retardancy. Talc, clay, silica, silicates, carbonates and sulfates may also be used. Mixtures of the foregoing fillers are also contemplated.
[0080] The clay may be a clay mineral (i.e., a natural unmodified clay), such as bentonite, laponite or montmorillonite; a synthetic clay (e.g., a synthetic layered clay), such as hydrotalcite, fluoromica or laponite; an organoclay (e.g., a clay mineral as defined herein or a synthetic clay modified by an organic material), or a mixture thereof. In another embodiment, the clay is a nanocomposite-forming clay (e.g., in a polymer dispersant).
[0081] In another embodiment, the clay is an organoclay. The organoclay present in the composition is typically a clay mineral that has been physically or (preferably) chemically modified (e.g., at the surface) by an organic modifier. For example, a hydrophilic clay can be chemically modified to be organophilic by an organic modifier. The organic modifier can be present on either or both of the surface and the interlayer space.
[0082] In another embodiment, the organic modifier is an alkyl or alkylammonium ions (e.g. tetraalkylammonium or tetraalkyl In another embodiment, the organic modifier is an optionally hydrogenated mono- or di-tallow alkyl or alkylammonium ions.
[0083] In another embodiment, the clay is an organically modified montmorillonite (e.g., hexadecyl tributyl In another embodiment, the clay is a synthetic hydrotalcite LDH (available from Sud Chemie, Germany). In another embodiment, the clay is a nanoclay such as Cloisite (available from Southern Clay Products) or an organically modified sodium-coesite. In another embodiment, the organically modified sodium-coesite is coesite 6A, coesite 25A, coesite 30B, coesite 15A, coesite 10A, coesite 30B, coesite 15A, coesite 10A, or coesite 10A. In another embodiment, the clay is a mixture of sodium-coesite and one or more of the group consisting of coesite 30B, coesite 15A, and coesite 10A.
[0084] The effective amount of clay present in the composition is 0.0 to 6.0 weight percent. In another embodiment, the effective amount of clay present in the composition is about 0.2 weight percent to about 5.0 weight percent. In another embodiment, the effective amount of clay present in the composition is about 0.25 to about 2 weight percent. In another embodiment, the effective amount of clay present in the composition is about 0.75 to about 1.5 weight percent. In another embodiment, the effective amount of clay present in the composition is about 0.5 to about 1.25 weight percent.
[0085] The coating composition may further comprise an inorganic char enhancer. The inorganic char enhancer may be selected from the group consisting of mineral wool fibers, glass flakes, aluminosilicates (eg potassium sodium silicate alumina, such as nepheline syenite) or ceramic materials (eg ceramic pigments).
[0086] The inorganic coking enhancer is present in an amount of about 0 to about 9 weight percent. In another embodiment, the inorganic coking enhancer is present in an amount of about 0.5 to about 9 weight percent. In another embodiment, the inorganic coking enhancer is present in an amount of about 1 to about 9 weight percent. In another embodiment, the inorganic coking enhancer is present in an amount of about 2 to about 8 weight percent.
[0087] In another embodiment, the composition may further include a flame retardant selected from the group consisting of: a mineral, an organophosphorus compound, and a reaction product of 2,4-bis[(1-cyclohexyloxy-2,2,6,6-piperidin-4-yl)butylamino]-6-chloro-s-triazine and N,N'-bis(3-aminopropyl)ethylenediamine).
[0088] In another embodiment, the composition may include additional flame retardant minerals selected from the group consisting of aluminum hydroxide, magnesium hydroxide, volcanite and hydromagnesite, various hydrates, red phosphorus, boron compounds, and borates.
[0089] In another embodiment, the composition includes an additional flame retardant organophosphorus compound selected from the group consisting of triphenyl phosphate, resorcinol bis(diphenyl phosphate), bisphenol A diphenyl phosphate, tricresyl phosphate, dimethyl methyl phosphate, diethyl aluminum phosphite, tris(2,3-dibromopropyl) phosphate (tribromide), tris(1,3-dichloro-2-propyl) phosphate, and tetrakis(2-chloroethyl)dichloroisopentyl diphosphate.
[0090] The additional flame retardant is present in an amount of about 0 to 9 weight percent. In another embodiment, the additional flame retardant is present in an amount of about 0.5 to 9 weight percent. In another embodiment, the additional flame retardant is present in an amount of about 1 to 9 weight percent. In another embodiment, the additional flame retardant is present in an amount of about 2 to 8 weight percent.
[0091] In some aspects, the composition may further include a fibrous material suitable for strengthening. Such fibrous materials may include organic, glass or mineral. The fibrous material may be present in the composition in any suitable amount. In some aspects, based on the total solid weight of the composition, the composition may include about 0.5 to 10 % by weight or about 1 to 8 % by weight of the fibrous material. The fibrous material may be present in the composition measuring any suitable length. In some aspects, the length of the fibrous material is at most 1000 microns.
[0092] The composition contains an additive or a combination of additives. Suitable additives will be well known to those skilled in the art. Examples of suitable additives include, but are not limited to, the following: plasticizers; pigments; defoamers; thixotropic agents; biocides; fragrances; fillers; adhesives; expanders and fire retardants; buffers; dispersants; surfactants; degassing agents; surface contrast additives; hydrophobic agents; wetting additives; rheological agents; anti-cratering additives; radiation curing additives; anti-corrosion additives; pH adjusters; anti-graffiti additives or combinations thereof.
[0093] Suitable rheology modifiers (rheological agents) will be well known to those skilled in the art. Suitable examples of rheology modifiers include, but are not limited to, the following: fumed silica; bentonite; castor oil and its derivatives; micronized amide waxes or combinations thereof. In certain aspects, the rheology modifier (when present) may be used in the composition in an amount of at least 0.01 wt % based on the total solids weight of the composition.
[0094] The composition may be a clear coating or a color coating with one or more pigments (e.g., titanium dioxide). The coating comprising the composition may include other typical coating additives such as dispersants, pigments, extenders and fillers, rheology modifiers, solvents and / or wetting agents. Suitable pigments will be well known to those skilled in the art. Suitable pigments may be, for example, titanium dioxide and / or carbon black. The pigment (when present) may be used in the composition in any suitable amount. In some aspects, the pigment (when present) may be used in the composition in an amount of up to about 40% by weight, such as up to about 30% by weight, or even up to about 15% by weight, based on the total solid weight of the composition. In some aspects, the pigment may be present in an amount between 3 and 20% by weight, such as 5 to 15% by weight. A plasticizer may optionally be added to the composition to increase flexibility. Suitable plasticizers will be well known to those skilled in the art. Suitable plasticizers include, but are not limited to, the following: aromatic alcohols, such as benzyl alcohol and nonylphenol; phosphates, such as isopropylated triaryl phosphates or combinations thereof. The plasticizer (when present) may be present in an amount of about 1 to 10 wt % based on the total solid weight of the composition. Suitably, the composition may comprise a pigment volume concentration of between 30 and 80 wt %, such as between 40 and 70 wt %, such as between 45 and 70 wt %. "Pigment volume concentration" refers to the volume of the solid content in the total composition.
[0095] The composition generally includes water. In some embodiments, the composition may include an organic solvent. Organic solvents include, but are not limited to, glycol ethers, such as alkylene glycol alkyl ethers (e.g., ethylene glycol monobutyl ether). The composition generally has a relatively low viscosity to facilitate easy application, and no pipeline heater is required during application at ambient temperature. In some embodiments, water may be present in an amount of about 5% by weight to about 60% by weight, based on the total weight of the composition. In some embodiments, water may be present in an amount of about 8% by weight to about 50% by weight or about 10% by weight to about 40% by weight, based on the total weight of the composition. In some embodiments, the viscosity of the composition at 20°C and a shear rate of 1.5s is between 20,000 and 140,000mPa / s. In some embodiments, the viscosity of the composition at 20°C and a shear rate of 1.5s may be about 25,000 to 125,000mPa / s, suitably about 30,000 to 110,000mPa / s, such as about 35,000 to 95,000mPa / s. In some embodiments, the viscosity of the composition at 20° C. and a shear rate of 1.5 s may be about 40,000 to 95,000 mPa / s. Methods for measuring viscosity will be well known to those skilled in the art. Suitably, viscosity is measured according to ASTM D2196-10 (“Standard Test Method for Rheological Properties of Non-Newtonian Materials Using a Rotational (Brookfield Type) Viscometer”) using a Brookfield RV spindle s7 at 6 rpm and a shear rate of 1.5 s. In some embodiments, when spraying the coating, the viscosity may be reduced by adding water (depending on the application parameters of the spraying equipment).
[0096] In some embodiments, the composition comprising the expansion agent can expand at a temperature of 300°C or less, suitably 250°C or less, or even 200°C or less. In some embodiments, when heated according to the EN 1363-1 (ISO 834) flame test, the composition expands at least 10 times (1000%) or at least 20 times (2000%) its original thickness in less than 20 minutes. After 10 minutes of this test, the temperature in the furnace was about 678°C, and after 30 minutes, it was about 842°C.
[0097] The present technology provides a method for forming a coating, the method comprising: applying a first composition as described herein to the surface of a substrate; applying a second composition as described herein to the surface of the substrate; and allowing the first composition and the second composition to crosslink within 30 seconds to form a coating; wherein the coating is non-sag, water-resistant and dry to the touch.
[0098] The present technology also provides a method for forming a coating, the method comprising: co-applying a first composition and a second composition as described herein to a surface of a substrate; and allowing the first composition and the second composition to crosslink for 30 seconds to form a coating; wherein the coating is non-sag, water-resistant, and dry to the touch. In some embodiments, co-application comprises co-spraying the first composition and the second composition simultaneously to the surface of the substrate.
[0099] In some embodiments, the surface of the substrate is a vertical surface. The composition can be applied to any suitable substrate. Examples of suitable substrates include, but are not limited to, steel, aluminum, wood, and / or concrete; structural units such as drywall; beams; hollow beams; porous beams; columns and hollow columns. In some embodiments, the substrate is steel, aluminum, and / or concrete. In some embodiments, the substrate is steel. Various steel substrates may include cold rolling, hot rolling, cold stretching (cold surface treatment), etc. In some embodiments, the substrate is aluminum. In some embodiments, the substrate is wood and / or drywall. The substrate for the insulation and / or vibration reduction coating may further include plastic.
[0100] The present technology provides a 2-pack coating kit comprising a first package containing a first composition described herein, and a second package containing a second composition described herein.
[0101] The present technology also provides a method of producing a composition as described herein, the method comprising: forming a polymeric binder; forming a first composition; and forming a second composition.
[0102] The polymeric binders disclosed herein can be formed using methods known to those of ordinary skill in the art, including those disclosed in U.S. Pat. Nos. 7,887,626, RE 44,931, PCT / US2017 / 057214, U.S. Published Patent Application No. 2001 / 0020064, and Journal of Applied Polymer Science, Vol. 109, 2275-2282 (2008) (each of which is incorporated herein by reference).
[0103] Thus, the present technology, generally described, will be more readily understood by reference to the following examples, which are provided by way of illustration and are not intended to be limiting of the present technology.
[0104] Examples
[0105] The compositions of the various trade name components used below are as follows:
[0106] PX 4585 is a water-based dispersant of an acrylic block copolymer made by controlled free radical polymerization (CFRP), available from BASF;
[0107] Ti-Pure TM R-900 is a rutile titanium dioxide pigment available from Chemours Company;
[0108] ST 2438 is a 100% active defoamer compound combining a highly branched star polymer with a high-end organo-siloxane, available from BASF;
[0109] 200 is hydrophilic fumed silica, which has 200m 2 / g specific surface area, available from Evonik Corporation;
[0110] Melamine can be purchased from Sigma-Aldrich;
[0111] APP 422 is a product based on ammonium polyphosphate. The crystal modification is phase II and is available from Clariant.
[0112] 4750 is an all-acrylic resin dispersion, 50 wt% solids, VOC=<0.2, Brookfield viscosity=<500 cps, available from BASF;
[0113] 200 is melamine polyphosphate, which is a salt of melamine and polyphosphoric acid and is available from BASF;
[0114] MP is melamine phosphate, which is a salt of melamine and phosphoric acid, available from BASF;
[0115] Rheovis 1235 is a nonionic associative HEUR thickener available from BASF;
[0116] PM40 is a micronized pentaerythritol derivative available from Perstorp;
[0117] Butyl Cellosolve TM (Butyl Cellosolve TM) is 2-butoxyethanol, available from The Dow Chemical Company;
[0118] ST 2446 is a defoamer compound combining hyperbranched star polymer technology with high-end organo-siloxane, available from BASF;
[0119] Glass Bubbles K37 are lightweight hollow glass microspheres with a density of 0.37 g / cc and a crush strength of 3,000 psi, available from 3M; and
[0120] Glass Bubbles XLD3000 are hollow glass spheres with a typical density of 0.23 g / cc and an isostatic crush strength of 3,000 psi, available from 3M.
[0121] For the purpose of calculating the PVC of an intumescent composition, melamine is used on the resin side of the equation.
[0122] Example 1. Polymeric Binder Synthesis - Polymer including a covalently bonded surfactant. In a one liter resin kettle equipped with a stirrer, nitrogen inlet, thermometer, and addition port, water (154 g), 1-poly(ethylene oxide) 20 -2-vinyl-4-nonylphenyl ether ammonium sulfate (Montello, 1.98 g, 20 wt% active in water) and sodium cetylstearyl sulfate (0.6 g, Aldrich Chemical Company). The solution was degassed with argon for 10 minutes. The solution was heated to 85°C with stirring. In a separate reactor, water (66 g), sodium cetylstearyl sulfate (2.4 g), styrene (27.8 g, Aldrich Chemical Company), methyl methacrylate (70.2 g, Aldrich Chemical Company), 1-poly(ethylene oxide) 20-2-vinyl-4-nonylphenyl ether ammonium sulfate (Montello, 9.69 g, 20 wt % active in water), butyl acrylate (72 g, Aldrich Chemical Co.), methacrylic acid (5.4 g, Aldrich Chemical Co.), hydroxyethyl methacrylate (4.5 g, Aldrich Chemical Co.), and isooctyl 3-mercaptopropionate (0.09 g, Aldrich Chemical Co.) were combined to produce a stable emulsion. The emulsion and initiator feed (ammonium persulfate, 0.39 g of a 20 wt % aqueous solution) were added simultaneously to the resin kettle solution over a period of 2 hours with good stirring while maintaining 85°C. Ammonia or another base may be added during or at the completion of the feed to maintain the pH at 7.5-8.5. After the feed is complete, isoascorbic acid and tert-butyl hydroperoxide dissolved in water are fed to the reactor over a period of about 20 minutes. After a short hold period, the reactor was cooled, pH = 9, viscosity 150-950 cps (Brookfield #2LV, 30 rpm, 60 seconds), 45 wt% resin solids. The resulting polymer had the following properties: M n =72,350;M w =340,988,M z =988,068, as determined by gel permeation chromatography; T g =37.0°C as determined by differential scanning calorimetry, and having a reactive surface covalently attached thereto.
[0123] Example 2. Polymeric Binder Synthesis - Hyperbranched Polymers. A three-necked round-bottom flask was charged with a latex (400 g) prepared from 20% styrene, 35% 2-ethylhexyl acrylate, 33.3% butyl methacrylate, 1.67% isooctyl mercaptopropionate and 10% methacrylic acid. 14% NH 4 The latex was neutralized with 1% hydroxyethyl ether (4.34 g, Aldrich Chemical Co.). The neutralized latex was then heated to 85°C and a diepoxide (diglycidyl ether of cyclohexanedimethanol, 5.45 g, Aldrich Chemical Co.) was added over 30 minutes. After the diepoxide addition, the solution was held at 85°C for 30 minutes, followed by the addition of a monofunctional epoxide (alkyl C 12 -C 14 Glycidyl ether, 11.48 g, Aldrich Chemical Company). The temperature was then raised to 87°C and held for 150 minutes to produce a modified latex having a hyperbranched polymer structure. The modified latex was then cooled and filtered to yield a material having 39.5% solids, a pH of 7.95, and a viscosity of 6 cps, as measured using a Brookfield viscometer with a #2 spindle at 50 rpm. The resulting hyperbranched polymer had the following properties: n =31,966; M w =337,943,Mz = 1,018,561, as determined by gel permeation chromatography; and T g = 36.8°C as determined by differential scanning calorimetry.
[0124] Example 3. Polymeric Binder Synthesis - Hyperbranched Polymers. Random copolymers were synthesized from the following monomers according to the high temperature continuous polymerization method described in U.S. Pat. Nos. 5,461,60; 4,414,370; and 4,529,787: acrylic acid (100 g, Aldrich Chemical Company), butyl acrylate (140 g, Aldrich Chemical Company), methyl methacrylate (490 g, Aldrich Chemical Company), styrene (270 g, Aldrich Chemical Company); a solid polymer having about 99% solids by weight was obtained. The resulting polymer had the following properties: M n =5,126;M w = 15,853 (measured by GPC using polystyrene standards for calibration); T g 75°C (measured by DSC-midpoint value; ramp rate 10°C / min), theoretical acid value (mg KOH / g)=78, theoretical hydroxyl number (mg KOH / g)=0.
[0125] An aqueous dispersion of the polymer was prepared as follows: The polymer as described above (653.71 g), water (733.9 g), methyldiethanolamine (22.77 g, Aldrich Chemical Company) and diethanolamine (10.13 g, Aldrich Chemical Company) were added to a reaction vessel. The mixture was heated to 88-92° C. and kept under stirring until all the polymer was dispersed in the water (approximately 3-4 hours). Bisphenol F diglycidyl ether (29.22 g, Aldrich Chemical Company) was added to the polymer dispersion and the mixture was kept at 88-92° C. for 2 hours. C was then added. 12 -C 14 Monoglycidyl ether (33.8 g, Aldrich Chemical Company) was added and the temperature was maintained for another 3 hours. After the reaction with the glycidyl ether compound, more base may be added to adjust pH, hydroxyl number, etc. The resulting polymer has the following properties: M n =188,591;M w =341,273,M z =998,195, as determined by gel permeation chromatography; T g =36.7°C, 43-45 wt% solids as determined by differential scanning calorimetry, pH = 7.8-8.3, hydroxyl number (mg KOH / g) = 70.
[0126] Comparative Example 1: Intumescent composition and coating thereof In a high speed disperser with a 2:1 blade, water (71 g) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (5 g), Ti-Pure R-900 (30 g), FoamStar 2438 (1.5 g), Aerosil 200 (5 g), melamine (37.5 g), Exolit APP422 (110 g), Charmor PM40 (45 g), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Acronal 4750 (45% solids, 156 g) and Rheovis PU 1235 (5 g dissolved in 10 g butyl cellosolve) were added over 2-3 minutes. Water (40 g) and butyl cellosolve (10 g) were added and stirring was continued for 5 minutes. The solid percentage was 58.8% and the PVC was about 50%. This high PVC formulation using a low Tg resin (15°C) was coated onto a cold rolled steel (CRS) panel using a drawdown bar with varying wet film thicknesses (WFT, 50-250 mils) and cured for 7 days at 22°C. Some cracking was observed in the cured coating. The expansion properties of the panels were tested using a muffle furnace (1000°F for 10 min). There was a slight increase in char thickness as the coating thickness increased, however, the increase in char thickness was not significant.
[0127]
[0128] Example 4. Intumescent composition and coating thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (71 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Rheovis 1235 (5 grams), Ti-Pure R-900 (30 grams), FoamStar 2438 (1.5 grams), Aerosil 200 (5 grams), melamine (37.5 grams), Exolit APP 422 (110 grams), Charmor PM40 (45 grams), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Example 1 (45% solids, 156 grams) and Rheovis PU 1235 (5 grams dissolved in 10 grams of butyl cellosolve) were added over 2-3 minutes. Water (40 grams) and butyl cellosolve (10 grams) were added and stirring was continued for 5 minutes. The solid percentage was 58.8% and the PVC was about 50%. The viscosity measured at 22°C using a Brookfield viscometer using spindle #3 and 20 rpm was 4115 cP. This high PVC formulation without a coagulant was applied to cold rolled steel (CRS) panels with different wet film thicknesses (WFT, 50-250 mils) using a drawdown bar and cured for 7 days at 22°C. After seven days, some cracks were observed in the cured coating. The expansion properties of the panels were tested using a muffle furnace (1000°F for 10 min). Compared to Comparative Example 1, as the coating thickness increased, there was an increase in scorch thickness and an increase in char thickness.
[0129]
[0130] Example 5. Intumescent composition and coating thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (71 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (5.5 grams), Ti-Pure R-900 (30 grams), FoamStar 2438 (1.7 grams), Aerosil 200 (5 grams), melamine (37.5 grams), Exolit APP 422 (110 grams), Charmor PM40 (45 grams), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Example 1 (45% solids, 156 grams) was added over 2-3 minutes. Water (40 grams) and butyl cellosolve (21 grams) were added and stirring was continued for 5 minutes. The solids percentage was 58.3% and the PVC was about 50%. The viscosity was 85 cP measured using a Brookfield viscometer using spindle #3 and 20 rpm at 22°C. This high PVC formulation with a coagulant (3 wt% aluminum sulfate in water, 30 g) mixed during spraying was sprayed onto cold rolled steel (CRS) panels with varying wet film thicknesses (WFT, 50 mils). The coatings dried to the touch in less than 30 seconds with no coating or coating transfer.
[0131] Example 6. Intumescent composition and coating thereof - Example 3 polymer. In a high speed disperser with a 2:1 blade, water (71 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (5 grams), Ti-Pure R-900 (30 grams), FoamStar 2438 (1.5 grams), Aerosil 200 (5 grams), melamine (37.5 grams), Exolit APP 422 (110 grams), Charmor PM40 (45 grams), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Example 3 (45% solids, 156 grams) and Rheovis PU 1235 (5 grams dissolved in 10 grams of butyl cellosolve) were added over 2-3 minutes. Water (40 grams) and butyl cellosolve (10 grams) were now added and stirring was continued for 5 minutes. The solid percentage was 58.7% and the PVC was about 50%. The viscosity was about 4000-5000 cP. This high PVC formulation without a coagulant was applied to cold rolled steel (CRS) panels with different wet film thicknesses (DFT, 50 and 100 mils) using a drawdown bar, cured for 7 days at room temperature, and dried to the touch within 24 hours. The expansion properties of the panels were tested using a muffle furnace (1000°F for 10 min). Compared to Comparative Example 1, as the coating thickness increased, there was an increase in scorch thickness and an increase in char thickness.
[0132] Example 7. Intumescent composition and coating thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (71 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (5 grams), Ti-Pure R-900 (30 grams), FoamStar 2438 (1.5 grams), Aerosil 200 (5 grams), melamine (27.3 grams), Melapur 200 (53 grams), Exolit APP 422 (80.5 grams), Charmor PM40 (33 grams), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Example 1 (45% solids, 156 grams) and Rheovis PU1235 (5 grams dissolved in 10 grams of butyl cellosolve) were added over 2-3 minutes. Water (40 grams) and butyl cellosolve (10 grams) were added and stirring was continued for 5 minutes. The solid percentage was 58.3% and the PVC was about 50%. The viscosity was about 4000-5000 cP as measured using a Brookfield DVII viscometer using spindle #3 and 20 rpm at 22C. This high PVC formulation without a coagulant was sprayed onto cold rolled steel (CRS) panels with different wet film thicknesses (DFT 50 and 100 mils), cured for 7 days at RT, and dried to the touch within 24 hours. The panels were tested for their expansion properties using a muffle furnace (1000°F for 10 min). As the coating thickness increased, there was an increase in char thickness and an increase in char thickness compared to Comparative Example 1.
[0133] Example 8. Intumescent composition and coating thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (71 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (5 grams), Ti-Pure R-900 (30 grams), FoamStar 2438 (1.5 grams), Aerosil 200 (5 grams), melamine (27.3 grams), Melapur 200 (26.5 grams), Melapur MP (26.5 grams), Exolit APP 422 (80.5 grams), Charmor PM40 (33 grams), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Example 1 (45% solids, 156 grams) and Rheovis PU 1235 (5 grams dissolved in 10 grams of butyl cellosolve) were added over 2-3 minutes. Water (40 grams) and butyl cellosolve (10 grams) were added and stirring was continued for 5 minutes. The percent solids was 58.8% and the PVC was about 50. The viscosity was about 5000 cP as measured using a Brookfield DVII viscometer using spindle #3 and 20 rpm at 22C.
[0134] Example 9. Intumescent composition and coating thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (71 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (5 grams), Ti-Pure R-900 (30 grams), FoamStar 2438 (1.5 grams), Aerosil 200 (5 grams), melamine (27.3 grams), Melapur MP (53 grams), Exolit APP 422 (80.5 grams), Charmor PM40 (33 grams), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Example 1 (45% solids, 156 grams) and Rheovis PU1235 (5 grams dissolved in 10 grams of butyl cellosolve) were added over 2-3 minutes. Water (40 grams) and butyl cellosolve (10 grams) were added and stirring was continued for 5 minutes. The percent solids was 58.8% and the PVC was about 50%. The viscosity was about 5000 cP as measured using a Brookfield DVII viscometer using spindle #3 and 20 rpm at 22°C.
[0135] Example 10. Barrier compositions and coatings thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (8.4 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (8.5 grams), FoamStar ST 2446 (1.0 grams), and K37 glass spheres (32.8 grams). Stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Resin Example 1 (45% solids, 45.6 grams) was added over 2-3 minutes. Ethylene glycol monobutyl ether (Eastman EB, 5.7 grams) was added and stirring was continued for 5 minutes. The solids percentage was 55.6% and the PVC was 79.7%.
[0136] Example 11. Barrier compositions and coatings thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (8.4 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: FoamStar ST2446 (1.0 grams) and K37 glass balls (32.8 grams). Stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while Resin Example 1 (45% solids, 45.6 grams) was added over 2-3 minutes. Ethylene glycol monobutyl ether (Eastman EB, 5.7 grams) was added and stirring was continued for 5 minutes. The solids percentage was 55.6% and the PVC was 78.9%.
[0137] Example 12. Barrier compositions and coatings thereof - Example 1 polymer. In a high speed disperser with a 2:1 blade, water (400 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: K37 glass balls (75 grams) and XLD 3000 glass balls (75 grams). Stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while adding Resin Example 1 (45% solids, 150 grams) over 2-3 minutes. Ethylene glycol monobutyl ether (Eastman EB, 18 grams) was added and stirring was continued for 5 minutes. The solids percentage was 29.8% and the PVC was 89.8%.
[0138] The resulting composition was sprayed onto three polycarbonate sheets (Marklon, Bayer). After 30 seconds, the coated sheets had no material transfer when touched. After 4 hours at ambient temperature, the sheets had a DFT of 2-3 mm by curing. The sheets were slightly different as follows:
[0139] Plate 1: as with some spots;
[0140] Plate 2: Slightly sanded to make the surface smooth;
[0141] Panel 3: Panel 2 was placed in an environmental chamber at 100°F, 80% relative humidity for 18 hours; water absorption was negligible.
[0142] Using the procedure described above, two comparative example panels were also prepared from:
[0143] Comparative Example 2: Heat-Flex Thermal Insulation Coating is a multi-purpose insulating water-soluble acrylic coating engineered to optimize thermal properties, provide personnel burn protection and process insulation, available from Sherwin Williams.
[0144] Comparative Example 3: Industrial-DTI is a composite ceramic and silica based waterborne acrylic barrier coating that provides an insulation barrier, protects personnel and stops all corrosion in one application, available from Mascoat.
[0145] The thermal conductivity of all the panels prepared above was measured according to ASTM C-518. The results are listed in Table 1.
[0146] Table 1: Thermal conductivity
[0147] <![CDATA[ Examples ]]> <![CDATA[ Thermal conductivity (N / mK) ]]> Comparative Example 2 0.097 Comparative Example 3 0.0698 Plate 1 0.057 Plate 2 0.054 Plate 3 0.055
[0148] The results demonstrate that the barrier compositions of the present invention can provide coatings with better barrier properties than commercial barrier compositions, as judged by lower thermal conductivity measurements.
[0149] Examples 10-12 were sprayed onto panels. All spray coated panels showed no cracking, no shrinkage from the panel edges, and no delamination after post spray exposure after 72 hours at ambient temperature.
[0150] Example 13: Polymer resin synthesized via a continuous high temperature polymerization process (soundproofing material). Soundproofing materials suitable for the technology of the present invention can be prepared via addition polymerization in a uniform or non-uniform medium. Table 2 summarizes the acrylic polymer polymerization products prepared by a continuous free radical polymerization process according to the technology of the present invention and at relatively high temperatures. The polymerization is carried out in a homogeneous environment. The high reaction temperature allows low molecular weights to be achieved without the use of chain transfer agents. After the polymerization step, the resin is subjected to a devolatilizer to remove unreacted monomers and process solvents.
[0151] Table 2: Polymer resins synthesized via a continuous polymerization process
[0152] polymer Polymer composition (wt%) Tg(℃) Mn(kDa) Mw(kDa) PDI Example 13 50MMA / 30Sty / 10AA / 10DAAM 85 3.3 8.1 2.6
[0153] MMA = methyl methacrylate; Sty = styrene; AA-acrylic acid; DAAM = diacetone acrylamide; wt = weight
[0154] The acid functional polymer described above is dispersed in water by neutralizing a portion of the acid group with a base under stirring and heating. As described in Table 3, the dispersion of Example 13 with 43% by weight solids is prepared by adding the polymer (518.6 grams) of Example 13, deionized water (668 grams) and ammonia (13.4 grams, 29% by weight activity) to a reaction vessel equipped with a condenser and an overhead stirrer. This mixture is heated to 88-92°C and maintained for 4 hours under stirring. The reaction mixture is cooled to 50-55°C, and 0.75 equivalents of adipic acid dihydrazide (relative to the keto group of DAAM present in the resin) are added to promote self-crosslinking during curing; afterwards, the reaction mixture is cooled to room temperature and filtered.
[0155] Table 3: Aqueous resin dispersions made from synthetic polymeric resins via a continuous polymerization process
[0156]
[0157] Visc. = viscosity, d = diameter
[0158] Example 14. Intumescent composition and coating thereof - Example 13 polymer. In a high speed disperser with a 2:1 blade, water (71 grams) was added and stirring was set at 2000 rpm. The following materials were added in the order listed: Dispex 4585 (5 grams), Ti-Pure R-900 (30 grams), FoamStar 2438 (1.5 grams), Aerosil 200 (5 grams), melamine (35 grams), Exolit APP 422 (124 grams), Charmor PM40 (35 grams), and stirring was continued for 15 minutes. The stirring rate was reduced to 1500 rpm while adding Example 13 dispersion (159 grams) and Rheovis PU 1235 (5 grams dissolved in 10 grams of butyl cellosolve) over 2-3 minutes. Water (40 grams), Butyl Carbitol (10 grams) and Butyl Cellosolve (27.65 grams) were now added and stirring continued for 5 minutes. The solids percentage was 57.4%. This formulation was sprayed onto a cold rolled steel (CRS) panel having a fully cured epoxy primer using a 2K Pleth Assembly spray gun system using an approximate ratio of 10:1 by weight of the formulation described above to catalyst. The catalyst was a 15 wt % aluminum sulfate solution in water.
[0159] Comparative Examples 4A and 4B: Avicor 2456 is a self-crosslinking terpolymer emulsion of vinyl acetate / versatile carbonic acid / acrylic acid having the following properties: solids = 50 wt%, Tg = 19°C, minimum film formation temperature = 11°C, and a particle size of 175 nm, which is commercially available from Celanese. According to the procedure of Example 14, an aqueous intumescent formulation was prepared. Due to extremely slow curing and severe sagging, this formulation may not be sprayed at a wet film thickness greater than 10 mils. In order to obtain a wet film thickness greater than 10 mils, a cold rolled steel (CRS) plate with a fully cured epoxy primer was placed on a laboratory bench surface and the coating formulation was applied to the desired thickness via a pipette. The wet coating film was cured at 23°C and 50% relative humidity for about 72 hours. The expansion properties of the plate were tested using a muffle furnace (1000°F for 10 min). The increase in char was measured by the average expansion factor relative to the uncharred plate.
[0160] Table 4: Swelling data of comparative resins with (4A) and without (4B) catalyst
[0161]
[0162] Wet film thicknesses of up to 150 mils were obtained by spraying the coating formulations of Example 14 and Comparative Examples 4A and 4B continuously. The wet coating films were cured for about 72 hours at 23°C and 50% relative humidity. The expansion properties of the panels were tested using a muffle furnace (1000°F for 10 min). The char increase relative to the uncharred panel was measured by the average expansion factor, which was calculated by dividing the film char height in inches by the uncharred dry film thickness in inches (Table 5).
[0163] These results clearly show that the intumescent formulations of the present invention produce increased char heights (in terms of average expansion factor) at lower film thicknesses. This char will protect the substrate during a fire or other high temperature event, and the higher char height will provide improved fire protection.
[0164] These results further indicate that the catalyst has little effect on the average expansion factor of this comparative resin.
[0165] Table 5: Comparative expansion data of resins of the present invention
[0166]
[0167] WFT = wet film thickness; DFT = dry film thickness
[0168] While certain embodiments have been illustrated and described, it will be appreciated that changes and modifications may be made therein in accordance with the knowledge of those skilled in the art without departing from the technology in its broader aspects as defined in the following claims.
[0169] The embodiments illustratively described herein may be appropriately practiced in the absence of any element or elements, limitation or limitations not specifically disclosed herein. Thus, for example, the terms "comprising," "including," "containing," and the like should be read broadly and not restrictively. In addition, the terms and expressions used herein have been used as terms of description and not of limitation, and it is not intended that such terms and expressions be used to exclude any equivalents of the features shown and described, or portions thereof, but it should be recognized that various modifications may be made within the scope of the claimed technology. In addition, the phrase "consisting essentially of" will be understood to include those elements specifically described and those additional elements that do not significantly affect the basic and novel features of the claimed technology. The phrase "consisting of" excludes any element not described.
[0170] The present disclosure is not limited to the specific embodiments described in this application. As will be apparent to those skilled in the art, many modifications and variations can be made without departing from its spirit and scope. In addition to those listed herein, functionally equivalent methods and compositions within the scope of the present disclosure are apparent to those skilled in the art based on the foregoing description. Such modifications and variations are also intended to fall within the scope of the appended claims. The present disclosure is limited only by the terms of the appended claims and the full scope of equivalents authorized by such claims. It should be understood that the present disclosure is not limited to the specific methods, reagents, compound compositions or biological systems that may vary of course. It should also be understood that the terms used herein are only for the purpose of describing specific embodiments and are not intended to be restrictive.
[0171] In addition, where features or aspects of the disclosure are described in terms of Markush groups, those skilled in the art will recognize that the disclosure is also thereby described in terms of any individual member or subgroup of members of the Markush group.
[0172] As will be understood by those skilled in the art, for any and all purposes, particularly with respect to providing a written description, all ranges disclosed herein also encompass any and all possible subranges and combinations of subranges thereof. Any listed range can be easily identified as fully described, and the same range can be decomposed into at least equal halves, thirds, quarters, fifths, tenths, etc. As a non-limiting example, each range discussed herein can be easily decomposed into a lower third, a middle third, and an upper third, etc. As will be understood by those skilled in the art, all language such as "at most," "at least," "greater than," "less than," etc. includes the narrated number and refers to a range, which can then be decomposed into subranges, as discussed above. Finally, as will be understood by those skilled in the art, a range includes each individual member.
[0173] All publications, patent applications, issued patents, and other documents mentioned in this specification are incorporated herein by reference as if each individual publication, patent application, issued patent, or other document was specifically and individually indicated to be incorporated herein by reference in its entirety. Definitions contained in the text incorporated by reference are excluded to the extent they conflict with definitions in this disclosure.
[0174] Other embodiments are set forth in the dependent claims.
Claims
1. A coating composition comprising: - a first composition comprising a polymeric binder present in an amount of 5% to 50% by weight, based on the total weight of the first composition, the polymeric binder comprising a polymer comprising a covalently bonded surfactant, wherein the covalently bonded surfactant comprises an anionic surfactant comprising a sulfate group, a sulfonate group or a carboxylate group, wherein the polymer comprising a covalently bonded surfactant comprises one or more polymerized monomers comprising acrylic acid, methacrylic acid, an alkyl acrylate, an alkyl methacrylate, acrylonitrile, styrene, or a combination of any two or more thereof; and - a second composition comprising a coagulant present in an amount of 0.01 wt % to 20 wt % based on the total weight of the second composition, wherein the coagulant comprises aluminum sulfate; - a sound deadening agent comprising an acrylic polymer polymerization product of a molten resin mixture comprising: at least one acrylic monomer; a polymerization initiator present in a molar ratio of the polymerization initiator to the at least one acrylic monomer of 0.0005:1 to 0.06:1; and 0 wt % to 25 wt % of the reaction solvent based on the weight of the acrylic acid monomer, wherein the acrylic acid polymer polymerization product comprises unreacted acrylic acid monomer and acrylic acid polymer product, Optionally, the acrylic acid polymer polymer product is prepared via a continuous mass polymerization process comprising: charging the molten resin mixture into a continuous mixing reactor zone; maintaining a flow rate through the reaction zone; and maintaining the molten resin mixture at a high temperature of 180° C. to 270° C.; wherein the first composition and the second composition are configured to form a coating within 30 seconds of application to a substrate, and the coating is non-sag, water resistant, and dry to the touch.
2. The composition of claim 1, wherein the additive is present in the first composition, the second composition, or both the first composition and the second composition.
3. The composition of claim 2, wherein the additive comprises an expander, a dampener, an insulating agent, or a combination of two or more thereof.
4. The composition of claim 3, wherein the expansion agent comprises an acid source, a carbon source, and a gas forming agent; the vibration dampening agent comprises a first filler; and the insulating agent comprises a second filler.
5. The composition according to claim 4, wherein: The acid source comprises melamine phosphate, magnesium phosphate, boric acid and ammonium polyphosphate, polyphosphoric acid or a combination of any two or more thereof; The carbon source comprises C4-C 20 Alcohols, polyol compounds, polyhydroxylated C4-C 20 alkyl or a combination of any two or more thereof; The gas forming agent comprises melamine, melamine cyanurate, melamine borate, melamine phosphate, tris-(hydroxyethyl)isocyanurate, melamine polyphosphate, chlorinated paraffin or a combination of any two or more thereof; The first filler comprises a mineral filler, a polymeric plastic filler or a combination thereof; and The second filler comprises balsa wood, calcium silicate, cellulose, chalk, cork board, regranulated cork, cotton, raw cotton, diatomaceous earth, felt insulation, glass fiber, foam glass, glass wool, felt, kapok insulation, magnesium oxide insulation, mineral wool insulation, paper, peat, foamed plastic, polypropylene, polyethylene, polyurethane, rock wool, wool, silica aerogel, slag wool, polystyrene, vermiculite, wax, perlite, rice husk, hollow glass spheres, hollow ceramic spheres, alumina-silica fibers, alumina-silica-zirconia fibers, polycrystalline mullite fibers, calcium aluminosilicate fibers, alumina fibers, mineral fibers, or a combination of two or more thereof.
6. A method for forming a coating composition according to any one of claims 1 to 5, the method comprising: Applying the first composition to the surface of the substrate and applying the second composition to the surface of the substrate; or applying the first composition and the second composition to the surface of the substrate; as well as allowing the first composition and the second composition to crosslink within 30 seconds to form the coating; The coating is non-sag, water resistant and dry to the touch.
7. A 2-pack coating kit comprising: A first package containing a first composition according to any one of claims 1 to 5; A second package containing a second composition according to any one of claims 1 to 5; in: The first composition and the second composition are configured to form a coating within 30 seconds of application to a substrate, and the coating is non-sag, water resistant, and dry to the touch.
8. The composition of any one of claims 1-5, wherein the composition exhibits a thermal conductivity of 0.020 N / mK to 0.065 N / mK as measured according to ASTM C-518.