Method for manufacturing substrate for power module and ceramic-copper joint body
By bonding multiple copper plates to the first and second sides of the ceramic plate to form multi-layer circuits and metal layers, the problem of warping of the ceramic plate and metal plate joint is solved, and the productivity and accuracy of power module substrates are improved. .
Patent Information
- Application Number
- CN201980007310.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-01-24
- Filing Date
- 2019-01-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-01-23
AI Technical Summary
When manufacturing substrates for power modules, the joint between the ceramic plate and the metal plate is prone to warping, resulting in reduced circuit pattern accuracy and reduced productivity, especially when using larger-area ceramic plates.
By joining a plurality of first copper plates in parallel on the first surface of the ceramic plate, a circuit layer of a plurality of first copper layers is formed, and at least two second copper plates are joined on the second surface by covering the substrate area divided by the dividing groove, forming a plurality of first copper plates. For the metal layer of the second copper layer, adjust the thickness and area ratio of the copper layer to reduce warpage.
It effectively reduces the warpage of ceramic-copper joints, improves the accuracy of circuit layers and metal layers, and improves the productivity of power module substrates.
Smart Images

Figure CN111566807B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a power module substrate used in the manufacture of a power module for controlling a large current and a high voltage, and a ceramic-copper joint body. This application claims priority based on Japanese Patent Application No. 2018-009275 filed on January 24, 2018, and the contents thereof are incorporated herein by reference. Background Art
[0002] As a method for manufacturing a power module substrate used in a power module, the following method is known: for example, as described in Patent Documents 1 and 2, a dividing groove (scribe line; cutting groove) is provided on a ceramic material having a large area that can form a plurality of power module substrates in a manner divided according to the size of each power module substrate, and the ceramic material is divided into pieces along the dividing groove, thereby manufacturing a plurality of power module substrates from a single ceramic plate.
[0003] Patent Document 1 describes that a metal plate made of aluminum or copper is brazed to a ceramic base material (ceramic plate) in which cut grooves are previously formed, and then a circuit pattern is formed by etching the metal plate.
[0004] Patent Document 2 describes that after a ceramic substrate (ceramic plate) and a metal plate made of aluminum are bonded together, the metal plate is etched to form a circuit pattern, and then grooves (dividing grooves) are formed between the circuit patterns of the ceramic substrate.
[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-185606
[0006] Patent Document 2: Japanese Patent Application Publication No. 2010-50164
[0007] In this way, by using a ceramic plate having a large area on which a plurality of power module substrates can be formed, a plurality of power module substrates can be manufactured at a time, and productivity of power module substrates can be improved.
[0008] However, in the manufacturing method of a plurality of power module substrates using a ceramic material having a large area, since a dividing groove is formed in the ceramic plate and metal plates of different thicknesses are bonded to the front and back sides of the ceramic plate, a stress difference occurs between the front and back sides of the ceramic plate, and warping easily occurs in the joint body of the ceramic plate and the metal plate during the manufacturing process. If warping occurs in the joint body, it is necessary to flatten the joint body by adsorption and fixation when forming the circuit pattern, or uneven resist film thickness and poor resist pattern shape may occur during resist printing, which may easily cause problems such as position deviation of the circuit pattern and reduced inspection accuracy in the inspection process.
[0009] For the circuit layer constituting the substrate for the power module, in order to improve the heat spreader effect, it is preferred to make the thickness relatively large (thick), but for the metal layer (heat dissipation layer) arranged on the back side, in order to seek a balance with the circuit layer formed by the pattern and reduce the overall warping, the thickness will be formed to be smaller (thinner) than the circuit layer. However, before the circuit pattern is formed, since the metal plate on the circuit layer side is thicker than the metal plate on the metal layer side, the warping will become larger and the ceramic substrate may be broken. In this regard, by using a high-strength silicon nitride plate (Si3N4) on the ceramic substrate, although it is possible to manufacture a joint body in which the metal plate constituting the circuit layer is formed into a relatively thick joint body, the warping of the joint body will become larger.
[0010] For metal plates that form circuit patterns, copper is more suitable than aluminum from the perspective of conductivity and heat dissipation. However, since copper is more rigid than aluminum, when warping occurs in a joint using copper, it is difficult to flatten it when the circuit pattern is formed, which can easily lead to a decrease in the accuracy of the circuit pattern.
[0011] In order to improve the productivity of the substrate for power modules, the size (area) of the ceramic plate needs to be further increased, but in this case, the warping of the joint of the ceramic plate and the copper plate during the manufacturing process will increase, and there is a concern that the accuracy of the circuit pattern will be more seriously reduced. Summary of the invention
[0012] The present invention has been developed in view of the above circumstances, and an object of the present invention is to provide a method for manufacturing a power module substrate with high productivity and a ceramic-copper bonded body with reduced warpage.
[0013] The method for manufacturing a substrate for a power module of the present invention comprises: a junction body forming step, forming a junction body, wherein the junction body comprises: a ceramic plate having a dividing groove for dividing the ceramic plate into two or more ceramic substrates; a copper layer for forming a circuit layer, which is bonded to a first surface of the ceramic plate; and a copper layer for forming a metal layer, which is bonded to a second surface of the ceramic plate; a pattern forming step, after the junction body forming step, applying an etching treatment to the junction body, and forming a circuit layer and a metal layer in each substrate forming area of the ceramic substrate divided by the dividing groove; and a dividing step, after the pattern forming step, dividing the ceramic plate along the dividing groove to manufacture a plurality of substrates having the ceramic substrate, The power module substrate of the circuit layer and the metal layer, in the step of forming the joint body, a plurality of first copper plates are joined in parallel on the first surface of the ceramic plate, thereby forming a copper layer for forming the circuit layer composed of a plurality of first copper layers, and a second copper plate is joined on the second surface of the ceramic plate in a manner covering at least two adjacent substrate forming areas among the substrate forming areas divided by the dividing grooves, the plane area of the second copper plate is larger than the plane area of the first copper plate and the thickness is smaller than the thickness of the first copper plate, thereby forming a copper layer for forming the metal layer composed of more than one second copper layers, and the number of second copper layers arranged is less than the number of first copper layers arranged.
[0014] In the process of forming a joint body, copper plates of different thicknesses are joined to the front and back sides of the ceramic plate, but the thick copper layer for forming the circuit layer is split into multiple first copper layers (first copper plates). Therefore, in the combination with the copper layer for forming the metal layer with a thin thickness, the stress difference between the front and back sides of the ceramic plate can be reduced, and the warping of the joint body (ceramic-copper joint body) of the ceramic plate, the copper layer for forming the circuit layer (first copper plate) and the copper layer for forming the metal layer (second copper plate) can be reduced.
[0015] This can reduce the warping of the bonded body, so that in the pattern forming process, uneven resist film thickness or poor resist pattern shape is less likely to occur, and patterned circuit layers and metal layers can be formed with high precision in each substrate forming area. Therefore, multiple power module substrates can be manufactured with high precision at one time, and the productivity of power module substrates can be improved.
[0016] As a preferred embodiment of the method for manufacturing a substrate for a power module of the present invention, in a combination of a single first copper layer and a single second copper layer that are opposite to each other with the ceramic plate sandwiched therebetween, when the thickness of the first copper layer is set to t1, the bonding area between the first copper layer and the ceramic plate is set to A1, the thickness of the second copper layer is set to t2, and the bonding area between the second copper layer and the ceramic plate is set to A2, {(A1 / A2)×(t1 / t2)} obtained by multiplying the area ratio (A1 / A2) of the bonding area A1 to the bonding area A2 by the thickness ratio (t1 / t2) of the thickness t1 to the thickness t2 is 0.080 or more and 0.600 or less.
[0017] By setting the thickness t1 and the bonding area A1 of each first copper plate, and the thickness t2 and the bonding area A2 of each second copper plate to the above relationship, it is possible to form a bonded body with a small warp in which the flatness of the copper layer for forming the metal layer is set to 0.5 mm or less. Thus, in the pattern forming step, the patterned circuit layer and the metal layer can be accurately formed in each substrate forming area of the ceramic substrate.
[0018] Furthermore, the manufacturing method of the substrate for a power module of the present invention may include a dividing groove forming step before the joint body forming step, wherein the dividing groove forming step forms the dividing groove on the surface of the ceramic plate along the outer shape of the substrate forming area on at least one of the first surface and the second surface of the ceramic plate.
[0019] The ceramic-copper joint body of the present invention comprises: a ceramic plate having a dividing groove for dividing the ceramic plate into a plurality of ceramic substrates; a copper layer for forming a circuit layer, which is composed of a plurality of first copper layers joined in parallel on the first surface of the ceramic plate; and a copper layer for forming a metal layer, which is joined to the second surface of the ceramic plate and is composed of one or more second copper layers whose number of configurations is less than the number of configurations of the first copper layers, the plane area of the second copper layer being larger than the plane area of the first copper layer and the thickness being smaller than the thickness of the first copper layer, and the second copper layer covering at least two adjacent substrate forming regions among the substrate forming regions of the ceramic substrates divided by the dividing groove.
[0020] According to the present invention, warpage occurring in a ceramic-copper bonded body can be reduced, so that a circuit layer and a metal layer can be formed with high precision in each substrate forming region of a ceramic plate, thereby improving productivity of a power module substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1A to Figure 1D It is a longitudinal cross-sectional view showing the method for manufacturing the power module substrate according to the first embodiment of the present invention in order of steps.
[0022] Figure 2This is a flowchart for explaining the method for manufacturing the power module substrate according to the first embodiment of the present invention.
[0023] Figure 3A to Figure 3C is an explanatory diagram of the structure of a power module substrate manufactured by using the method for manufacturing a power module substrate according to the first embodiment, Figure 3A For the main view, Figure 3B This is a top view from the circuit layer side. Figure 3C This is a bottom view viewed from the metal layer side.
[0024] Figure 4A to Figure 4B is a top view illustrating the dividing grooves formed in the ceramic plate. Figure 4A The figure shows a ceramic plate with the first surface facing the front side. Figure 4B The figure shows a case where the second surface of the ceramic plate faces the front side.
[0025] Figure 5A to Figure 5B is a top view illustrating a ceramic-copper joint. Figure 5A The figure shows a ceramic plate with the first surface facing the front side. Figure 5B The figure shows a case where the second surface of the ceramic plate faces the front side.
[0026] Figure 6A to Figure 6B 1 is a plan view illustrating each pattern of the circuit layer and the metal layer formed in the pattern forming step. Fig. 6A The figure shows a ceramic plate with the first surface facing the front side. Figure 6B The figure shows a case where the second surface of the ceramic plate faces the front side.
[0027] Figure 7 It is a plan view showing a ceramic-copper joint body according to a second embodiment, and is a view showing a ceramic plate with the first surface facing the front side.
[0028] Figure 8A to Figure 8B 1 is a top view showing a ceramic-copper joint body according to a third embodiment. Fig. 8A The figure shows a ceramic plate with the first surface facing the front side. Figure 8B The figure shows a case where the second surface of the ceramic plate faces the front side.
[0029] Figure 9A to Figure 9B 1 is a top view showing a ceramic-copper joint body according to a fourth embodiment. Fig.9A The figure shows a ceramic plate with the first surface facing the front side. Fig. 9B The figure shows a case where the second surface of the ceramic plate faces the front side. DETAILED DESCRIPTION
[0030] Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0031] Figures 3A to 3CFIG. 1 shows a power module substrate 10 manufactured by the method for manufacturing a power module substrate according to the first embodiment of the present invention. Figure 3A The upper surface in the figure is used to mount (assemble) a semiconductor element or other element 91, thereby Figure 3A As shown, a power module 101 is manufactured.
[0032] like Figures 3A to 3C As shown, the power module substrate 10 comprises: a ceramic substrate 11; a circuit layer 12 formed on a first surface ( Figure 3A and a metal layer 13, formed on the second surface of the ceramic substrate 11 ( Figure 3A The lower surface is in the middle).
[0033] The ceramic substrate 11 is formed of a ceramic material such as AlN (aluminum nitride), Al 2 O 3 (aluminum oxide), or Si 3 N 4 (silicon nitride).
[0034] The circuit layer 12 is formed by bonding a plurality of copper plates formed of copper (copper or copper alloy) to the first surface of the ceramic substrate 11 by brazing or the like. The metal layer 13 is formed by bonding a copper plate formed of copper (copper or copper alloy) to the second surface of the ceramic substrate 11 by brazing or the like, similarly to the circuit layer 12.
[0035] like Figure 3B As shown, the circuit layer 12 is composed of a plurality of small circuit layers 121, and forms a circuit pattern. Therefore, the bonding area between the ceramic substrate 11 and the circuit layer 12 is smaller than the bonding area between the ceramic substrate 11 and the metal layer 13. Figure 3A As shown, the thickness (plate thickness) t11 of the circuit layer 12 is set to be larger (thicker) than the thickness (plate thickness) t12 of the metal layer 13. In this way, with respect to the power module substrate 10, the shape of the metal layer 13 is adjusted relative to the circuit layer 12 in such a way that the stress difference associated with the thermal expansion difference between the circuit layer 12 and the metal layer 13 bonded to both surfaces of the ceramic substrate 11 is reduced.
[0036] As an example of various dimensions of the power module substrate 10, the thickness (plate thickness) of the ceramic substrate 11 made of Si3N4 (silicon nitride) is set to 0.1 mm to 1.5 mm, the thickness t11 of the circuit layer 12 made of OFC (pure copper) is set to 0.5 mm to 2.0 mm, and the plate thickness t12 of the metal layer 13 made of OFC is set to 0.35 mm to 1.8 mm. However, these dimensions are not limited to the above numerical ranges.
[0037] The element 91 assembled on the substrate 10 for the power module is an electronic component having a semiconductor, and various semiconductor elements such as IGBT (Insulated Gate Bipolar Transistor), MOSFET (Metal Oxide Semiconductor Field Effect Transistor) or FWD (Free Wheeling Diode) are selected according to the required functions. Although the element 91 is not shown in the figure, an upper electrode portion is provided at the upper part and a lower electrode portion is provided at the lower part. The lower electrode portion of the element 91 is joined to the upper surface of the circuit layer 12 by welding or the like, whereby the element 91 is mounted on the upper surface of the circuit layer 12. The upper electrode portion of the element 91 is connected to the circuit electrode portion of the circuit layer 12 or the like through a lead frame (not shown in the figure) or the like.
[0038] Next, a method for manufacturing the power module substrate 10 will be described. Figure 2 As shown in the flowchart of FIG. 1 , the method for manufacturing a power module substrate according to the present embodiment includes a plurality of manufacturing steps S11 to S13 . Figure 1A to Figure 1D An example of the manufacturing process of the method for manufacturing the power module substrate according to the present embodiment is shown.
[0039] [Dividing groove forming step]
[0040] On at least one of the first and second surfaces of the ceramic plate 21, the surface of the ceramic plate 21 is linearly removed to the middle of the thickness direction along the boundary line of the plurality of substrate forming regions to form dividing grooves 211v and 211h. Figure 4A and 4B As shown in FIG. 1 , a large ceramic plate 21 having dividing grooves 211 v and 211 h for dividing the ceramic plate 21 into a plurality of ceramic substrates 11 is prepared. Figure 4A 2 is a top view showing the first surface of the ceramic plate 21. Figure 4B 2 is a plan view showing the second surface of the ceramic plate 21. The dividing grooves 211v and 211h are formed on at least one surface (the first surface) of the ceramic plate 21.
[0041] In this embodiment, if Figure 4A As shown, the dividing grooves 211v and 211h are formed only on the first surface of the ceramic plate 21. Figure 4B In FIG. 1 , the dividing grooves 211v and 211h formed on the first surface of the ceramic plate 21 are indicated by dotted lines. The dividing grooves 211v and 211h may be formed only on the second surface of the ceramic plate 21 or on both the first surface and the second surface.
[0042] In this way, the ceramic plate 21 is divided into a plurality of ( Figure 4A , 4B The substrate forming region 212 of the ceramic substrate 11 is 12 in the figure. For example, the dividing grooves 211v and 211h can be formed by removing the front surface of the ceramic plate 21 in a linear shape by laser processing or cutting processing.
[0043] like Figure 4A As shown, each of the dividing grooves 211 v and 211 h is formed by a straight line connecting the opposite sides of the ceramic plate 21 to each other. Figure 4A In the embodiment, four dividing grooves 211v are formed at equal intervals along the longitudinal direction connecting the long sides, and five dividing grooves 211h are formed at equal intervals along the transverse direction connecting the short sides. The nine dividing grooves 211v and 211h form a total of 12 substrate forming areas 212 divided according to the size of the outer shape of the ceramic substrate 11, four in the longitudinal direction and three in the transverse direction.
[0044] The peripheral portion of the ceramic plate 21 is divided into small blank regions 213 so as to surround the twelve substrate forming regions 212. The blank regions 213 are not used as the ceramic substrate 11 and are removed in the subsequent dividing step S13.
[0045] [Joint body forming step S11]
[0046] In the bonding body forming step S11, on the first surface of the ceramic plate 21 thus constructed, Figure 5A As shown in FIG. 1 , a copper layer 31 for forming a circuit layer is formed on the second surface of the ceramic plate 21. Figure 5B As shown, the copper layer 32 for forming the metal layer is formed, thereby forming a ceramic-copper joint 30 (hereinafter abbreviated as the joint 30) having the ceramic plate 21, the copper layer 31 for forming the circuit layer, and the copper layer 32 for forming the metal layer.
[0047] like Figure 1A As shown, a plurality of (three in the example) first copper plates 301, 302 are evenly bonded to the first surface of the ceramic plate 21, thereby Figure 1B and Figure 5A As shown in FIG. 1 , a circuit layer forming copper layer 31 is formed by a plurality of first copper layers 311 and 312. Figure 1A As shown, the second copper plate 303 is bonded to the second surface of the ceramic plate 21, thereby Figure 1B and Figure 5B As shown, the metal layer forming copper layer 32 is formed of the second copper layer 321 , and the number of the second copper layers 321 arranged is less than the number of the first copper layers 311 and 312 arranged (one in the example shown in the figure).
[0048] The first copper plates 301, 302, the second copper plate 303 and the ceramic plate 21 are joined by, for example, a brazing material (not shown) such as Ag-Cu-Ti brazing material. The brazing material may be applied in advance to each joining surface of the first copper plates 301, 302 and the second copper plate 303, thereby making it easy to handle.
[0049] The first copper plates 301, 302 and the second copper plates 303 are formed into desired external shapes by punching out a plate made of copper or a copper alloy, for example, by a stamping process. In the present embodiment, a total of three first copper plates 301, 302 are provided, and each of the first copper plates 301, 302 has a larger plane area than the plane area of the four substrate forming areas 212 arranged side by side in the longitudinal direction of the ceramic plate 21 (the sum of the plane areas of the substrate forming areas 212 covered by the first copper plates 301, 302, respectively), and is formed in a rectangular plate shape with both ends in the longitudinal direction spanning the blank areas 213 above and below (refer to Figure 5A ). Among them, about Figure 1A The first copper plates 302 arranged on the left and right (both sides in the width direction) are larger in the left and right (lateral direction) than the first copper plate 301 arranged in the center, and are formed across the blank area 213 arranged on the peripheral portion of the ceramic plate 21.
[0050] In this embodiment, the second copper plate 303 is a single piece, and the plane area of the second copper plate 303 is larger than the plane area of the 12 substrate forming areas 212 arranged vertically and horizontally along the ceramic plate 21, and is formed across the blank area 213 surrounding these substrate forming areas 212 (refer to Figure 5B ). The plane area of the second copper plate 303 is larger than the plane areas of each of the first copper plates 301 and 302, and the thickness thereof is smaller (thinner) than the thickness of the first copper plates 301 and 302. Furthermore, the plane area of the second copper plate 303 is larger than the total area of the plane areas of the three first copper plates 301 and 302 combined.
[0051] In this case, when the thickness (plate thickness) of each of the first copper plates 301 and 302 serving as the first copper layers 311 and 312 is set to t1, the plane area (joining area) of a single joining surface of the first copper plate 301 and the first copper plate 302 is set to A1, the thickness (plate thickness) of the second copper plate 303 serving as the second copper layer 321 is set to t2, and the plane area (joining area) of the joining surface of the second copper plate 303 is set to A2, it is preferred that the thickness t1 and the joining area A1 of the first copper plate 301 and the first copper plate 302, and the thickness t2 and the joining area A2 of the second copper plate 303 are adjusted so that {(A1 / A2)×(t1 / t2)}, which is obtained by multiplying the area ratio (A1 / A2) of the joining area A1 to the joining area A2 by the thickness ratio (t1 / t2), is greater than 0.080 and less than 0.600.
[0052] By adjusting the area and thickness of each copper plate 301, 302, 303 in this way, it is possible to form a bonded body 30 with a small warp in which the flatness of the copper layer 32 for forming the metal layer is set to 0.5 mm or less. In this case, the area ratio (A1 / A2) of the bonding area A1 of each of the first copper plates 301 and 302 and the bonding area A2 of the second copper plate 303 is preferably less than 0.5. The thickness ratio (t1 / t2) of the thickness t1 of each of the first copper plates 301 and 302 and the thickness t2 of the second copper plate 303 is a value exceeding 1.0 because the thickness t2 is smaller (thinner) than the thickness t1.
[0053] Each of the first copper layers 311 and 312 constituting the circuit layer forming copper layer 31 is formed by bonding each of the first copper plates 301 and 302 to the ceramic plate 21, and therefore the thickness of the first copper layers 311 and 312 is almost the same as the thickness t1 of the first copper plates 301 and 302, and the size of the bonding area between the first copper layers 311 and 312 and the ceramic plate 21 is also the same as the plane area (bonding area) A1 of the bonding surface of each of the first copper plates 301 and 302. Similarly, the second copper layer 321 is formed by bonding the second copper plate 303 to the ceramic plate 21, and therefore the thickness of the second copper layer 321 is almost the same as the thickness t2 of the second copper plate 303, and the size of the bonding area between the second copper layer 321 and the ceramic plate 21 is also the same as the plane area (bonding area) A2 of the bonding surface of the second copper plate 303.
[0054] Therefore, in the present embodiment, the thickness of the first copper layers 311 and 312 is treated as the same thickness t1 as the thickness of the first copper plates 301 and 302, and each bonding area of the first copper layers 311 and 312 is treated as the same area A1 as the plane area (bonding area) A1 of the bonding surface of the first copper plates 301 and 302. Similarly, the thickness of the second copper layer 321 is treated as the same thickness t2 as the thickness of the second copper plate 303, and the bonding area of the second copper layer 321 is treated as the same area A2 as the plane area (bonding area) A2 of the bonding surface of the second copper plate 303.
[0055] In this embodiment, the first copper plate 301 disposed in the center of the ceramic plate 21 and the first copper plates 302 disposed on the left and right are formed by copper plates having different plane areas A1. Therefore, the relationship with the second copper plate 303 is adjusted on the first copper plate 301 disposed in the center of the ceramic plate 21 and the first copper plates 302 disposed on the left and right of the ceramic plate 21. That is, the relationship between the first copper plate 301 and the second copper plate 303 in the center and the first copper plates 302 and the second copper plates 303 on the left and right, which are in a relative positional relationship through the ceramic plate 21, is adjusted.
[0056] In this way, the relationship between the first copper plates 301, 302 and the second copper plate 303 disposed at positions opposite to each other through the ceramic plate 21 is considered, so that in each combination of the first copper layers 311, 312 and the second copper layer 321 bonded to the local part of the ceramic plate 21, a symmetrical structure with the ceramic plate 21 as the center can be smoothly formed, and the warping occurring in the bonded body 30 can be reduced. The thickness t1 and the bonding area A1 of each of the first copper plates 301, 302 (first copper layers 311, 312) may be different, as long as they are adjusted to a relationship within the range of {(A1 / A2)×(t1 / t2)} being greater than 0.080 and less than 0.600 in the relationship with the second copper plate 303 (second copper layer 321) facing each other.
[0057] For example, consider a situation in which the thickness t1 of each first copper plate 301, 302 is 0.8 mm, the plane area (joining area) A1 of the first copper plate 301 arranged in the center of the ceramic plate 21 is 84 mm × 64.5 mm, and the plane area (joining area) A1 of each first copper plate 302 arranged on the left and right of the ceramic plate 21 is a rectangular plate of 84 mm × 64.5 mm, and the thickness t2 of the second copper plate 303 is 0.7 mm and the plane area (joining area) A2 is a rectangular plate of 171 mm × 126 mm.
[0058] In this case, the relationship between the first copper plate 301 arranged in the center of the ceramic plate 21 and the second copper plate 303 arranged opposite to the first copper plate 301 through the ceramic plate 21 is as follows: thickness ratio (t1 / t2) = 1.14, area ratio (A1 / A2) = 0.24, and relationship {(A1 / A2)×(t1 / t2)} = 0.27.
[0059] The relationship between the first copper plates 302 arranged on the left and right of the ceramic plate 21 and the second copper plates 303 arranged relatively to the first copper plates 302 through the ceramic plate 21 is as follows: thickness ratio (t1 / t2) = 1.14, area ratio (A1 / A2) = 0.24, and relationship {(A1 / A2)×(t1 / t2)} = 0.27.
[0060] In order to bond the first copper plates 301, 302 to the ceramic plate 21, and the second copper plate 303 to the ceramic plate 21, as Figure 1A As shown, the first copper plates 301 and 302 are overlapped on the first surface of the ceramic plate 21 via a brazing material (not shown). Similarly, the second copper plate 303 is overlapped on the second surface of the ceramic plate 21 via a brazing material (not shown).
[0061] At this time, each of the first copper plates 301 and 302 is arranged so as to expose two central dividing grooves 211v of the four dividing grooves 211v drawn in the longitudinal direction of the ceramic plate 21, avoiding the two dividing grooves 211v. Thus, each of the first copper plates 301 and 302 can be surely joined at the position including the circuit layer 12 formed in the pattern forming step S12. Figure 1A As shown in FIG. 2 , the three first copper plates 301 and 302 are arranged bilaterally symmetrically, so that the first copper plates 301 and 302 are evenly arranged in parallel on the first surface of the ceramic plate 21 .
[0062] The second copper plate 303 is arranged to cover a total of 12 substrate forming areas 212 divided on the ceramic plate 21 in such a manner that the center position of the second surface of the ceramic plate 21 overlaps with the center position of the bonding surface of the second copper plate 303. The second copper plate 303 is arranged to evenly cover the second surface of the ceramic plate 21. The second copper plate 303 is arranged at a position overlapping with the three first copper plates 301 and 302 through the ceramic plate 21.
[0063] In this state, if Figure 1BAs shown by the hollow arrows, the stack of the first copper plates 301, 302, the ceramic plate 21, and the second copper plate 303 is heated while being kept in a state of being pressurized by applying a load in the stacking direction. Thus, each of the first copper plates 301, 302 is bonded to the first surface of the ceramic plate 21 to form a circuit layer forming copper layer 31 composed of three first copper layers 311, 312. At the same time, the second copper plate 303 is bonded to the second surface of the ceramic plate 21 to form a metal layer forming copper layer 32 composed of a second copper layer 321. Thus, as Figure 1B and Figure 5A , 5B As shown, a bonded body 30 including a ceramic plate 21, a circuit layer forming copper layer 31, and a metal layer forming copper layer 32 is formed.
[0064] In this way, in the joint body forming step S11, the first copper plates 301, 302 and the second copper plate 303 of different thicknesses are respectively joined to the front and back sides (the first side and the second side) of the ceramic plate 21, thereby forming a copper layer 31 for forming a circuit layer with a large thickness (thickness) on the first side of the ceramic plate 21, and forming a copper layer 32 for forming a metal layer with a thickness smaller (thinner) than the copper layer 31 for forming the circuit layer on the second side of the ceramic plate 21.
[0065] The joint body 30 is formed by splitting into a plurality of first copper layers 311 and 312 to form a copper layer 31 for forming a circuit layer with a large thickness, and by configuring a second copper layer 321 with a smaller number than the number of first copper layers 311 and 312 to form a copper layer 32 for forming a metal layer with a small thickness, so that in the combination of the copper layers 311, 312, and 321 bonded to the front and back sides of the ceramic plate 21, a symmetrical structure centered on the ceramic plate 21 can be formed. As a result, the stress difference generated between the front and back sides of the ceramic plate 21 can be reduced, and the warping generated in the joint body 30 can be reduced.
[0066] [Pattern Forming Step S12]
[0067] like Figure 1C , Fig. 6A , 6B As shown, after the assembly forming step S11, the assembly 30 is subjected to etching treatment, and patterned circuit layers 12 and metal layers 13 are respectively formed in each substrate forming area 212 of the ceramic plate 21. The etching treatment can be performed by a well-known method. For example, after a masking operation such as coating of a resist or attaching of a masking tape, an etching solution such as ferric chloride is brought into contact with and removed from the exposed portion of the unmasked copper layer, thereby performing patterning.
[0068] In this case, the circuit layer forming copper layer 31 composed of the first copper layers 311 and 312 disposed on the first surface of the ceramic plate 21 is patterned, as shown in FIG. Fig. 6AAs shown, a circuit layer 12 composed of a plurality of independent small circuit layers 121 is formed in each substrate forming region 212. By patterning the metal layer formed by the second copper layer 321 disposed on the second surface of the ceramic plate 21, the copper layer 32 is formed. Figure 6B As shown, an independent metal layer 13 is formed in each substrate forming region 212. In the pattern forming step S12, the portions of the copper layers 311, 312, and 321 overlapping the dividing grooves 211v and 211h are removed, thereby exposing the entire dividing grooves 211v and 211h.
[0069] As described above, the warpage of the bonded body 30 formed in the bonded body forming step S11 is reduced, so defects in resist film thickness or resist pattern shape are less likely to occur in the pattern forming step S12. Therefore, the patterned circuit layer 12 and metal layer 13 can be formed with high precision in each substrate forming region 212.
[0070] [Division Step S13]
[0071] like Figure 1D As shown, after the pattern forming step S12, the ceramic plate 21 is divided along the dividing grooves 211v and 211h, thereby individualizing the substrate forming regions 212 and cutting out the blank regions 213 from the substrate forming regions 212. Figures 3A to 3C As shown, a plurality of (twelve in this embodiment) power module substrates 10 having a ceramic substrate 11 , a circuit layer 12 , and a metal layer 13 are manufactured.
[0072] Thus, in the manufacturing method of the substrate for power module of the present embodiment, in the joint body forming step S11, the first copper plates 301, 302 and the second copper plates 303 of different thicknesses are joined to the front and back sides of the large ceramic plate 21, and the thick circuit layer forming copper layer 31 is formed by splitting into multiple first copper layers 311, 312 (first copper plates 301, 302), so that in the combination with the thin metal layer forming copper layer 32 (second copper plate 303), the stress difference occurring on the front and back sides of the ceramic plate 21 can be reduced, and the warping occurring in the joint body 30 of the ceramic plate 21 and the copper layer 31 for circuit layer formation and the copper layer 32 for metal layer formation can be reduced.
[0073] The thickness t1 and the bonding area A1 of each of the first copper layers 311 and 312, and the thickness t2 and the bonding area A2 of the second copper layer 321 are adjusted so that the area ratio (A1 / A2) multiplied by the thickness ratio (t1 / t2) {(A1 / A2)×(t1 / t2)} is greater than 0.080 and less than 0.600, thereby forming a joint body 30 with a small warp in which the flatness of the copper layer 32 for forming the metal layer is set to less than 0.5 mm.
[0074] In this way, the warping of the bonded body 30 can be reduced, so that the unevenness of the resist film thickness or the poor shape of the resist pattern is less likely to occur in the pattern forming step S12, and the patterned circuit layer 12 and the metal layer 13 can be formed with high precision in each substrate forming area 212. Therefore, a plurality of power module substrates 10 can be manufactured with high precision at one time, and the productivity of the power module substrates 10 can be improved.
[0075] In addition, the present invention is not limited to the configuration of the above-described embodiment, and various changes may be made to the details without departing from the gist of the present invention.
[0076] For example, in the first embodiment, in the joint body forming step S11, the three first copper plates 301 and 302 are formed so that the first copper plate 301 in the center and the first copper plates 302 on the left and right have different shapes. Figure 7 As shown in the joint body 41 of the second embodiment, the circuit layer forming copper layer 33 having the first copper layer 313 of the same shape is formed by forming all three first copper plates into the same shape. It is not necessary to expose the dividing groove 211v of the ceramic plate 21 between each first copper layer 313, as long as the pattern shape of the circuit layer 12 formed in the pattern forming step S12 is matched, that is, each first copper layer 313 is joined at a position that actually includes the circuit layer 12.
[0077] The number of the first copper layer constituting the circuit layer forming copper layer is not limited to three. Fig. 8A , 8B The joint body 42 of the third embodiment is shown. Fig. 8A As shown in FIG. 1 , the first copper layer 314 is split into two upper and lower structures. Figure 8B As shown, the number of second copper layers 321 is less than the number of first copper layers 314 and is composed of one. In this case, by adjusting the thickness t1 and the bonding area A1 of the first copper layer 314 and the thickness t2 and the bonding area A2 of the second copper layer 321, a symmetrical structure centered on the ceramic plate 21 can be formed, thereby reducing the warping of the bonded body 42.
[0078] like Fig.9A , 9B As in the joint body 43 according to the fourth embodiment shown in FIG. 1 , the number of first copper layers is not limited to two or three. Fig.9A As shown, the number of first copper layers 315 and 316 may be set to a total of six, and the number of circuit layer forming copper layers 35 exceeding three may be provided to form the bonded body 43. Fig. 9BAs shown, if the number of second copper layers 322 is set to two, the number of second copper layers constituting the copper layer for forming a metal layer is not limited to one, and the copper layer 36 for forming a metal layer can be constituted by configuring a plurality of second copper layers 322 whose number is less than the total number of first copper layers 315 and 316.
[0079] Example
[0080] Hereinafter, the effects of the present invention will be described in detail using examples, but the present invention is not limited to the following examples.
[0081] As components constituting the samples of Inventive Examples 1 to 7 and Comparative Examples 1 and 2, a ceramic plate made of Si 3 N 4 having a plate thickness of 0.32 mm, and a first copper plate and a second copper plate made of OFC (pure copper) were prepared.
[0082] Regarding the ceramic plates, two types of planar dimensions were prepared: 190.8 mm in length and 138 mm in width (inventive examples 1, 4, 6, and comparative example 1) and 100 mm in length and 120 mm in width (inventive examples 2, 3, 5, 7, and 8). In order to correctly evaluate the warpage that occurs in the joint body formed by the combination of the copper layer for forming the circuit layer and the copper layer for forming the metal layer, a flat plate-shaped ceramic plate was used without forming a dividing groove in each ceramic plate.
[0083] Regarding the first copper plate as the first copper layer and the second copper plate as the second copper layer, copper plates having the plane dimensions (vertical and horizontal) and thicknesses t1 and t2 shown in Table 1 were prepared according to the arrangement numbers shown in Table 1. These were joined by the manufacturing method described in the first embodiment to produce a sample of a joint body (ceramic-copper joint body) having a ceramic plate and each copper layer (copper layer for forming a circuit layer and copper layer for forming a metal layer).
[0084] The first copper plate and the second copper plate are arranged side by side and evenly arranged on the bonding surface of the ceramic plate in a manner that is symmetrical in both the vertical direction and the horizontal direction. "a×b" in Table 2 represents the value of {(A1 / A2)×(t1 / t2)} obtained by multiplying the area ratio a=(A1 / A2) by the thickness ratio b=(t1 / t2).
[0085] The flatness of each sample obtained at room temperature (25° C.) after bonding was measured. The flatness of the surface of the copper layer for forming a metal layer was measured by a moire-type three-dimensional shape measuring machine. Table 2 shows the results.
[0086] [Table 1]
[0087]
[0088] [Table 2]
[0089]
[0090] It can be seen from the results in Table 2 that even when copper plates of different thicknesses are joined to the front and back sides of a large ceramic plate, in Invention Examples 1 to 7 which are composed of a combination of splitting a thick copper layer for forming a circuit layer into multiple first copper layers and setting a thin copper layer for forming a metal layer as a second copper layer with a smaller number of configurations than the first copper layer, the warping that occurs in the joint of the ceramic plate, the copper layer for forming a circuit layer, and the copper layer for forming a metal layer can be reduced compared to Comparative Examples 1 and 2 which are composed of a single copper plate of the same planar size as a combination of a copper layer for forming a circuit layer and a copper layer for forming a metal layer.
[0091] Furthermore, in Invention Examples 1 to 7 in which the relationship between the thickness t1 of each first copper layer and the bonding area A1, and the relationship between the thickness t2 of the second copper layer and the bonding area A2 is adjusted so that {(A1 / A2)×(t1 / t2)} obtained by multiplying the area ratio (A1 / A2) by the thickness ratio (t1 / t2) is greater than 0.080 and less than 0.600, a joint body with a small warpage and a flatness of the copper layer for forming a metal layer of less than 0.5 mm can be formed.
[0092] Industrial Applicability
[0093] A method for manufacturing a power module substrate with high productivity and a ceramic-copper bonded body with reduced warpage can be provided.
[0094] Explanation of symbols
[0095] 10 Power module substrate
[0096] 11 Ceramic Substrate
[0097] 12 Circuit Layer
[0098] 13 Metal layer
[0099] 21 Ceramic Plate
[0100] 30, 41, 42, 43 Joints (ceramic-copper joints)
[0101] 31, 33, 35 Copper layer for forming circuit layer
[0102] 32, 36 Copper layer for forming metal layer
[0103] 91 Components
[0104] 101 Power Module
[0105] 121 Small Circuit Layer
[0106] 211v, 211h split slot
[0107] 212 substrate forming area
[0108] 213 blank area
[0109] 301, 302 First Copper Plate
[0110] 303 The 2nd Copper Plate
[0111] 311, 312, 313, 314, 315, 316 1st copper layer
[0112] 321, 322 The second copper layer.
Claims
1. A method for manufacturing a substrate for a power module, characterized in that: have: A step of forming a bonded body, wherein the bonded body comprises: a ceramic plate having a dividing groove for dividing the ceramic plate into two or more ceramic substrates; a copper layer for forming a circuit layer, which is bonded to a first surface of the ceramic plate; and a copper layer for forming a metal layer, which is bonded to a second surface of the ceramic plate; a pattern forming step of performing an etching process on the bonded body after the bonded body forming step, and forming a circuit layer and a metal layer in each substrate forming region of the ceramic substrate divided by the dividing grooves; and a dividing step of dividing the ceramic plate along the dividing grooves after the pattern forming step to produce a plurality of power module substrates having the ceramic substrate, the circuit layer and the metal layer, In the bonding body forming step, the circuit layer forming copper layer composed of two or more first copper layers is formed by bonding two or more first copper plates in parallel to the first surface of the ceramic plate, and A second copper plate is joined to the second surface of the ceramic plate in a manner that covers at least two adjacent substrate forming areas among the substrate forming areas divided by the dividing grooves, the second copper plate having a planar area larger than a planar area of each of the first copper plates and a thickness smaller than a thickness of the first copper plates, thereby forming a copper layer for forming the metal layer composed of more than one second copper layer, and the number of second copper layers arranged is less than the number of first copper layers arranged.
2. The method for manufacturing a power module substrate according to claim 1, wherein: In the combination of the single first copper layer and the single second copper layer facing each other with the ceramic plate sandwiched therebetween, when the thickness of the first copper layer is set to t1, the bonding area between the first copper layer and the ceramic plate is set to A1, the thickness of the second copper layer is set to t2, and the bonding area between the second copper layer and the ceramic plate is set to A2, {(A1 / A2)×(t1 / t2)} obtained by multiplying the area ratio (A1 / A2) between the bonding area A1 and the bonding area A2 by the thickness ratio (t1 / t2) between the thickness t1 and the thickness t2 is 0.080 or more and 0.600 or less.
3. The method for manufacturing a power module substrate according to claim 1 or 2, characterized in that: Prior to the bonded body forming step, there is a dividing groove forming step of forming the dividing groove on the surface of the ceramic plate along the outer shape of the substrate forming region on at least one of the first surface and the second surface of the ceramic plate.
4. A ceramic-copper joint body, characterized in that: have: A ceramic plate having a dividing groove for dividing the ceramic plate into a plurality of ceramic substrates; a copper layer for forming a circuit layer, which is composed of a plurality of first copper layers joined in parallel on the first surface of the ceramic plate; and a copper layer for forming a metal layer, which is bonded to the second surface of the ceramic plate and is composed of one or more second copper layers whose number of configurations is less than the number of configurations of the first copper layer, and the second copper layer has a larger plane area than the plane area of the first copper layer and a smaller thickness than the thickness of the first copper layer, The second copper layer covers at least two adjacent substrate forming regions among the substrate forming regions of each of the ceramic substrates divided by the dividing grooves. In the combination of the single first copper layer and the single second copper layer facing each other with the ceramic plate sandwiched therebetween, when the thickness of the first copper layer is set to t1, the bonding area between the first copper layer and the ceramic plate is set to A1, the thickness of the second copper layer is set to t2, and the bonding area between the second copper layer and the ceramic plate is set to A2, {(A1 / A2)×(t1 / t2)} obtained by multiplying the area ratio (A1 / A2) between the bonding area A1 and the bonding area A2 by the thickness ratio (t1 / t2) between the thickness t1 and the thickness t2 is 0.080 or more and 0.600 or less.