A method for grooving the back of a strip semiconductor to eliminate stress

By fixing and mechanically cutting long strip semiconductors with negative photoresist, combined with chemical cleaning treatment, the problem of internal stress relief in semiconductor processing is solved, achieving significant stress removal effect and simple process.

CN111599671BActive Publication Date: 2024-10-18SAE TECH DELEVOPMENT DONGGUAN
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201910136434.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-02-21
Publication Date
2024-10-18
Estimated Expiration
2039-02-21

AI Technical Summary

Technical Problem

It is difficult for the existing technology to effectively eliminate internal stress during semiconductor processing, leading to deformation problems. Existing methods such as grinding and heat treatment are not satisfactory.

Method used

The long-strip semiconductor is fixed with negative photoresist for mechanical cutting, combined with the cleaning treatment of acid solution, heated alkali solution, ozone water, chlorine water, and organic solvent, and the internal stress is eliminated through specific photoresist thickness and cutting parameters.

Benefits of technology

It achieves effective elimination of the internal stress of the long strip semiconductor, has a simple process and significant effect, and eliminates the adhesion problem of the photoresist.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0001974391400000101
    Figure BDA0001974391400000101
  • Figure BDA0001974391400000111
    Figure BDA0001974391400000111
Patent Text Reader

Abstract

The present invention provides a method for grooving the back of a long strip semiconductor to eliminate stress, the method comprising the following steps: (1) coating a layer of negative photoresist on a fixture, pasting the long strip semiconductor on the surface of the photoresist, and baking until the photoresist is dry so that the long strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 50-65 μm; (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.5-0.8 mm, the cutting blade rotation speed is 4500-5500 RPM, and the cutting speed is 90-110 mm / s; (3) after the cutting is completed, washing the long strip semiconductor with an acid solution and a heated alkaline solution in turn to make it fall off the fixture, and then placing the long strip semiconductor in ozone water, chlorine water, and an organic solvent in turn for treatment. The method of the present invention has a simple preparation process and has a good effect on eliminating the internal stress of the long strip semiconductor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor device production, and in particular to a method for grooving the back side of a long strip semiconductor to eliminate stress. Background Art

[0002] With the rapid development of science and technology, the requirements for semiconductor processing capabilities are getting higher and higher. During the processing, there is deformation of the semiconductor, which is mainly caused by the stress during the processing. At present, the main methods to reduce internal stress are grinding and heat treatment. However, the effect of eliminating internal stress is not very ideal and the effect is poor. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for grooving the back side of a strip semiconductor to eliminate stress.

[0004] To achieve the above object, the technical solution adopted by the present invention is: a method for grooving the back side of a long strip semiconductor to eliminate stress, the method comprising the following steps:

[0005] (1) coating a layer of negative photoresist on a fixture, adhering a strip semiconductor to the surface of the photoresist, and baking until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 50 to 65 μm;

[0006] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.5 to 0.8 mm, the cutting blade rotation speed is 4500 to 5500 RPM, and the cutting speed is 90 to 110 mm / s;

[0007] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution and a heated alkaline solution in turn to make it fall off the fixture, and then the long strip semiconductor is placed in ozone water, chlorine water, and an organic solvent in turn for treatment.

[0008] The method of the present invention fixes a long strip semiconductor on a fixture through negative photoresist for mechanical cutting. The method of the present invention can effectively eliminate the internal stress of the prepared long strip semiconductor through specific photoresist thickness and cutting parameters; and the photoresist adhering to the semiconductor is removed through cleaning treatment with an acid solution, a heated alkaline solution, ozone water, chlorine water, and an organic solvent.

[0009] Preferably, the baking temperature in step (1) is 120-150°C.

[0010] Preferably, the baking time in step (1) is 20 minutes.

[0011] Preferably, the viscosity of the photoresist is 425-475 mPa·s at 25°C.

[0012] Preferably, the cutting blade is a diamond grinding wheel blade, the particle size of the blade is 3.0-4.5 μm, and the blade concentration is 100-110.

[0013] Preferably, the blade exposure during mechanical cutting in step (2) is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30°C.

[0014] Preferably, the thickness of the photoresist applied in step (1) is 55 to 65 μm.

[0015] Preferably, the rotation speed of the cutting blade during mechanical cutting in step (2) is 5000-5500 RPM, and the cutting speed is 100-110 mm / s.

[0016] More preferably, the cutting blade rotation speed during mechanical cutting in step (2) is 5500 RPM and the cutting speed is 110 mm / s.

[0017] Preferably, the depth of the cut groove on the semiconductor is 0.6-0.8 mm.

[0018] More preferably, the depth of the cut groove on the semiconductor is 0.7-0.8 mm.

[0019] The beneficial effects of the present invention are as follows: the present invention provides a method for grooving the back of a long strip semiconductor to eliminate stress. The method of the present invention has a simple preparation process and has a good effect on eliminating the internal stress of the long strip semiconductor. DETAILED DESCRIPTION

[0020] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0021] Example 1

[0022] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0023] (1) coating a layer of negative photoresist on a fixture, pasting a long strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the long strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 50 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0024] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0025] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0026] Example 2

[0027] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0028] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0029] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0030] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0031] Example 3

[0032] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0033] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 60 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0034] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0035] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0036] Example 4

[0037] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0038] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 65 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0039] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0040] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0041] Example 5

[0042] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0043] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0044] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.5 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0045] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0046] Example 6

[0047] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0048] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0049] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.6 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0050] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0051] Example 7

[0052] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0053] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0054] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.8 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0055] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0056] Example 8

[0057] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0058] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0059] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 4500 RPM, the cutting speed is 90 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0060] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0061] Example 9

[0062] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0063] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0064] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 4500 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0065] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0066] Example 10

[0067] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0068] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0069] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 4500 RPM, the cutting speed is 110 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0070] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0071] Embodiment 11

[0072] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0073] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0074] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 90 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0075] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0076] Example 12

[0077] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0078] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0079] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 110 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0080] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0081] Example 13

[0082] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0083] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0084] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5500 RPM, the cutting speed is 90 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0085] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0086] Embodiment 14

[0087] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0088] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0089] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5500 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0090] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0091] Embodiment 15

[0092] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0093] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0094] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5500 RPM, the cutting speed is 110 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0095] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0096] Comparative Example 1

[0097] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0098] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 70 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0099] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.7 mm, the cutting blade rotation speed is 5500 RPM, the cutting speed is 110 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0100] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0101] Comparative Example 2

[0102] A method for grooving the back side of a strip semiconductor to eliminate stress, the method comprising the following steps:

[0103] (1) coating a layer of negative photoresist on a fixture, pasting a strip semiconductor on the surface of the photoresist, and baking at 120-150° C. for 20 min until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 μm, and the viscosity of the photoresist is: 425-475 mPa·s at 25° C.;

[0104] (2) mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.4 mm, the cutting blade rotation speed is 5000 RPM, the cutting speed is 100 mm / s, the cutting blade is a diamond grinding wheel blade, the blade particle size is 3.0 to 4.5 μm, the blade concentration during mechanical cutting is 100 to 110, the blade exposure is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30° C.;

[0105] (3) After the cutting is completed, the long strip semiconductor is washed with an acid solution, and then washed with a heated alkaline solution to make it fall off the fixture, and then the long strip semiconductor is placed in water in turn and treated with ozone, and then soaked in chlorine water, and finally soaked in an organic solvent.

[0106] Experimental Example 1

[0107] The application effects of the methods of Examples 1-15 are compared.

[0108] 1. The statistical results of the shedding ratio during the cutting process and the stress magnitude of the long strip semiconductors were compared with the methods of Examples 1-4 and Comparative Example 1, as shown in Table 1.

[0109] Table 1

[0110] Photoresist thickness 50μm 55μm 60μm 65μm 70μm Shedding rate 5% 0.30% 0.25% 0.10% 0.08% Stress Effect Minimum stress Less stress Less stress High stress Too much stress

[0111] The results in Table 1 show that when the photoresist thickness exceeds 65 μm, the stress of the long strip semiconductor is too large, and the inventive method is poor in eliminating the stress of the long strip semiconductor; it shows that when the photoresist thickness is less than 50 μm, the long strip semiconductor has poor adhesion, a high detachment rate, and a large loss; therefore, the effect is better when the photoresist thickness is 55 μm-65 μm.

[0112] 2. The stress magnitudes of the long strip semiconductors obtained by applying the methods of Example 2, Examples 5-7, and Comparative Example 2 were tested, and the stress removal effects were compared as shown in Table 2.

[0113] Table 2

[0114]

[0115]

[0116] The results in Table 3 show that the effect is better when the cutting groove depth is 0.6-0.8 mm. It is also found through experiments that when the cutting groove depth exceeds 0.8 mm, it exceeds the bearing capacity of the semiconductor.

[0117] 3. The stress magnitude of the long strip semiconductor obtained by applying the methods of Examples 8-15 was tested, and the stress removal effect was compared as shown in Table 3.

[0118] Table 3

[0119] Stress relief effect 4500rpm 5000rpm 5500rpm 90mm / s Worst Poor better 100mm / s Poor generally good 110mm / s generally better most

[0120] The results in Table 3 indicate that the cutting blade rotation speed during mechanical cutting is 5000-5500 RPM, and the cutting speed is 100-110 mm / s, and the stress removal effect of the method of the present invention is better.

[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for grooving the back side of a strip semiconductor to eliminate stress, characterized in that: The method comprises the following steps: (1) coating a layer of negative photoresist on a fixture, adhering a strip semiconductor to the surface of the photoresist, and baking until the photoresist is dry so that the strip semiconductor is fixed on the fixture, wherein the thickness of the coated photoresist is 55 to 65 μm; (2) Mechanically cutting the long strip semiconductor fixed on the fixture with a cutting blade, wherein the cutting groove depth on the semiconductor is 0.6-0.8 mm, the cutting blade rotation speed is 5000-5500 RPM, and the cutting speed is 100-110 mm / s; or the cutting groove depth on the semiconductor is 0.6-0.8 mm, the cutting blade rotation speed is 4500-5000 RPM, and the cutting speed is 110 mm / s; or the cutting groove depth on the semiconductor is 0.6-0.8 mm, the cutting blade rotation speed is 5500 RPM, and the cutting speed is 90-100 mm / s; (3) After mechanical cutting is completed, the long strip semiconductor is washed with an acid solution and a heated alkaline solution in turn to make it fall off the fixture, and then the long strip semiconductor is placed in ozone water, chlorine water, and an organic solvent in turn for treatment.

2. The method according to claim 1, characterized in that The baking temperature in step (1) is 120-150°C.

3. The method according to claim 1, characterized in that The viscosity of the photoresist is 425-475 mPa·s at 25°C.

4. The method according to claim 1, characterized in that: The cutting blade is a diamond grinding wheel blade, the particle size of the blade is 3.0-4.5 μm, and the blade concentration is 100-110.

5. The method according to claim 1, characterized in that The exposed amount of the blade during mechanical cutting in step (2) is 1.0 to 1.5 mm, and the cutting water temperature is 25 to 30°C.

6. The method according to claim 1, characterized in that The baking time in step (1) is 20 minutes.

Citation Information

Patent Citations

  • Etching method and mask structure of metal layer

    CN102931075A

  • Method for improving wafer internal stress of trench gate discrete power device

    CN103854964A