Double antibacterial nonwoven fabric and preparation method thereof

By forming a ZIF-8 structure on non-woven fabrics and introducing nano-silver, the deficiencies in antibacterial properties and wash resistance of existing antibacterial non-woven fabrics are solved, the dual antibacterial performance and wash resistance are improved, and the non-woven fabrics are ensured Applications in Medical and Public Health.

CN111676695BActive Publication Date: 2024-10-18DONGGUAN DONGYANG SOLAR SCI RES & DEV CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202010567112.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-19
Publication Date
2024-10-18
Estimated Expiration
2040-06-19

AI Technical Summary

Technical Problem

Existing antibacterial non-woven fabrics have deficiencies in antibacterial properties and washability, especially when reused, it is difficult to achieve lasting effects.

Method used

By soaking the non-woven arrangement in a solution containing zinc salt, silver salt and 2-methylimidazole, a ZIF-8 structure is formed, and silver ions are introduced into it and then reduced to form nano-silver, combined with a specific soaking liquid composition and sequence of steps to ensure that the nanosilver load is evenly dispersed on the ZIF-8 structure to achieve dual antibacterial properties.

Benefits of technology

A dual antibacterial non-woven fabric with excellent antibacterial durability and washability was obtained. Nano-silver loading on the ZIF-8 structure avoids agglomeration, ensures good dispersion and adhesion, maintains breathability, and is green and environmentally friendly. process preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002548240860000071
    Figure BDA0002548240860000071
Patent Text Reader

Abstract

The present invention relates to a method for preparing a double antibacterial nonwoven fabric, comprising: immersing the nonwoven fabric in a solution containing zinc salt, and drying; then immersing the nonwoven fabric in a solution containing silver salt, 2-methylimidazole and an adhesive, and drying; then immersing the nonwoven fabric in a solution containing a reducing agent, and drying. The present invention loads a ZIF-8 structure on a nonwoven fabric by an in-situ growth method, and simultaneously introduces silver ions into the ZIF-8 structure, and subsequently reduces the silver ions to nanosilver, thereby obtaining a nonwoven fabric with double antibacterial properties. The present invention adopts a method for preparing an antibacterial nonwoven fabric by in-situ growth, which can ensure the uniformity of dispersion and adhesion of the ZIF-8 structure on the nonwoven fabric, and the nanosilver loading on the ZIF-8 structure also avoids the problem of easy agglomeration of nanosilver introduced on the nonwoven fabric by the traditional method, and the antibacterial nonwoven fabric thus obtained has excellent antibacterial durability and washability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite materials, and in particular to a double antibacterial non-woven fabric and a preparation method thereof. Background Art

[0002] Non-woven fabrics, also known as non-woven fabrics, are made of directional or random fibers. They are a new generation of environmentally friendly materials with the characteristics of moisture-proof, breathable, flexible, lightweight, non-combustible, easy to decompose, non-toxic and non-irritating, rich in colors, low price, and recyclable. At present, the demand for non-woven fabrics in the medical and public health fields is gradually increasing, and there are higher requirements for antibacterial properties. However, the existing antibacterial non-woven fabrics are insufficient in terms of antibacterial properties. Especially in the case of repeated use, it is more difficult for traditional non-woven fabrics to achieve the effect of washability and long-lasting antibacterial properties. Summary of the invention

[0003] The first purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a double antibacterial non-woven fabric.

[0004] Specifically, the preparation method provided by the present invention comprises the following steps:

[0005] (1) soaking the nonwoven fabric in a solution containing zinc salt and drying;

[0006] (2) soaking the non-woven fabric treated in step (1) in a solution containing silver salt, 2-methylimidazole and an adhesive, and drying;

[0007] (3) soaking the nonwoven fabric treated in step (2) in a solution containing a reducing agent and drying it.

[0008] The invention loads a ZIF-8 (sodalite methylimidazole zinc, SOD-[Zn(mim)2], zinc 2-methylimidazolate, 2-methylimidazole zinc salt, codename MAF-4, also known as ZIF-8) structure on a non-woven fabric by an in-situ growth method, and simultaneously introduces silver ions into the ZIF-8 structure, and subsequently reduces the silver ions into nanosilver. Firstly, ZIF-8 and nanosilver with excellent photocatalytic antibacterial performance are introduced into the non-woven fabric, so as to obtain a non-woven fabric with dual antibacterial performance; secondly, the method for preparing the antibacterial non-woven fabric by in-situ growth can ensure the uniformity of dispersion and adhesion of the ZIF-8 structure on the non-woven fabric; the nanosilver loading on the ZIF-8 structure also avoids the problem of easy agglomeration of nanosilver introduced into the non-woven fabric by the traditional method; the antibacterial non-woven fabric obtained thereby has excellent antibacterial durability and washability. The present invention can ensure that nanosilver is loaded on the ZIF-8 structure in the final product by limiting the specific soaking liquid composition and soaking step sequence in each step, and the ZIF-8 structure loaded with nanosilver is evenly dispersed on the surface of the non-woven fabric.

[0009] The zinc salt of the present invention can be selected from at least one of zinc nitrate, zinc acetate or zinc sulfate.

[0010] The silver salt described in the present invention can be selected from at least one of silver nitrate or silver sulfate.

[0011] The soaking described in the present invention is carried out at room temperature.

[0012] As a preferred embodiment of the present invention, the molar ratio of the zinc salt to the silver salt is (1-3): (0.1-0.3), more preferably 1: (0.1-0.2). By limiting the main raw materials of the antibacterial agent having a bactericidal effect to a specific ratio range, it can be ensured that the two bactericidal components in the final product synergistically play a bactericidal role in their specific ratio.

[0013] As a specific embodiment of the present invention, the solution in step (1) contains a zinc salt with a concentration of 0.25 to 0.75 mmol / mL; and the solution in step (2) contains a silver salt with a concentration of 0.015 to 0.05 mmol / mL.

[0014] As a preferred embodiment of the present invention, the molar ratio of the zinc salt to 2-methylimidazole is (1-3): (6-12), more preferably 1: (6-7). Limiting the above raw materials to a specific ratio range can ensure that the ZIF-8 structure can be effectively grown in situ and evenly distributed on the surface of the non-woven fabric.

[0015] As a specific embodiment of the present invention, the solution in step (1) contains a zinc salt with a concentration of 0.25 to 0.75 mmol / mL; and the solution in step (2) contains 2-methylimidazole with a concentration of 1 to 3 mmol / mL.

[0016] As a preferred embodiment of the present invention, the soaking in step (1) and / or step (2) is 4 to 10 hours. As a specific embodiment, the soaking time in step (1) can be 4 to 8 hours, and the soaking time in step (2) can be 6 to 10 hours. Limiting the soaking time to the above range can ensure that the bactericidal component is fully deposited on the surface of the non-woven fabric and fully grows in situ.

[0017] As a preferred embodiment of the present invention, the binder is selected from at least one of PEG (polyethylene glycol), PVA (polyvinyl alcohol), and PVP (polyvinyl pyrrolidone). In the present invention, the concentration of the binder in the solution of step (2) is further preferably 0.01 to 0.1 g / mL, more preferably 0.03 to 0.07 g / mL.

[0018] The purpose of step (3) of the present invention is to reduce silver ions into silver element using a reducing agent, so as to form nanosilver uniformly loaded on the ZIF-8 structure on the surface of the non-woven fabric, thereby achieving an excellent bactericidal effect.

[0019] As a preferred embodiment of the present invention, in step (3), the non-woven fabric can be firstly cleaned with clean water to wash away the residual components, dried, and then placed in a solution containing a reducing agent for reduction.

[0020] As a preferred embodiment of the present invention, the reducing agent in step (3) is selected from a reducing agent capable of converting silver ions (Ag + ) is reduced to silver. Specifically, at least one of sodium citrate, glucose or sodium borohydride can be selected.

[0021] The soaking time of step (3) of the present invention is sufficient to allow the reaction of reducing silver ions to silver element to proceed fully. As a specific embodiment, the soaking time of step (3) can be 4 to 8 hours.

[0022] As a preferred embodiment of the present invention, the drying involved in each step of the present invention is specifically: drying at 60-120°C for 10-30 minutes. As a specific implementation, the drying temperature after step (1) can be 60-100°C, the drying temperature after step (2) can be 80-120°C, and the drying temperature after step (3) can be 60-100°C. The drying temperature after washing with clean water can be 60-100°C. By limiting the drying temperature and time within the above range, it is possible to ensure that the bactericidal components on the surface of the non-woven fabric are not affected while allowing the water to evaporate fully.

[0023] As a preferred embodiment of the present invention, the non-woven fabric raw material used in the present invention is selected from one of PP non-woven fabric, polyester non-woven fabric and nylon non-woven fabric. Before the non-woven fabric is treated, it can be treated with corona or plasma to facilitate better adhesion of the bactericidal component to its surface. The preferred non-woven fabric of the present invention has a gram weight of 20 to 50 g / m 2 The thickness is 0.04 mm to 0.1 mm, which is more convenient to use. The size of the non-woven fabric is not particularly limited, as long as it can be completely immersed in the solution.

[0024] The second object of the present invention is to provide a double antibacterial non-woven fabric prepared by the method.

[0025] The third object of the present invention is to provide application of the double antibacterial nonwoven fabric in the field of medical treatment or public health.

[0026] The dual antibacterial nonwoven fabric provided by the present invention has excellent dual antibacterial effects, including the antibacterial effect of nanosilver and the photocatalytic antibacterial performance of ZIF-8. In the present invention, the ZIF-8 structure loaded with nanosilver is introduced on the nonwoven fabric by an in-situ growth method, which not only improves the dispersion uniformity and adhesion of ZIF-8 on the nonwoven fabric, but also solves the problem that nanosilver is easily agglomerated when directly loaded on the nonwoven fabric, and the obtained antibacterial nonwoven fabric has excellent wash resistance and antibacterial durability. The ZIF-8 structure in the nonwoven fabric of the present invention has a high porosity, which can ensure the good air permeability of the nonwoven fabric. The whole process of the multi-antibacterial nonwoven fabric prepared by the present invention uses water as a solvent, and the preparation process is green and environmentally friendly. DETAILED DESCRIPTION

[0027] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0028] Example 1

[0029] This embodiment provides a double antibacterial non-woven fabric, which is prepared by the following method:

[0030] 5.95 g (0.02 mol) of zinc nitrate hexahydrate was dissolved in 40 mL of water to obtain solution A; 0.34 g (0.002 mol) of silver nitrate, 9.85 g (0.12 mol) of 2-methylimidazole and 4 g of PEG were dissolved in 60 mL of water to obtain solution B; the plasma-treated PP non-woven fabric was first immersed in solution A at room temperature for 8 hours, and then dried at 100°C for 20 minutes; then immersed in solution B at room temperature for 10 hours, and then treated at 120°C for 30 minutes, and then the non-woven fabric was washed with clean water and dried at 80°C for 20 minutes; the treated non-woven fabric was immersed in a sodium citrate aqueous solution with a concentration of 0.1 mol / L again, immersed for 8 hours, and dried at 100°C for 20 minutes; and an antibacterial non-woven fabric was obtained.

[0031] Example 2

[0032] This embodiment provides a double antibacterial non-woven fabric, which is prepared by the following method:

[0033] 5.95 g (0.02 mol) of zinc nitrate hexahydrate was dissolved in 40 mL of water to obtain solution A; 0.34 g (0.002 mol) of silver nitrate, 9.85 g (0.12 mol) of 2-methylimidazole and 4 g of PEG were dissolved in 60 mL of water to obtain solution B; the plasma-treated PP non-woven fabric was first immersed in solution A at room temperature for 4 hours, and then taken out and dried at 100°C for 20 minutes; then immersed in solution B at room temperature for 6 hours, taken out and treated at 120°C for 30 minutes, and then the non-woven fabric was washed with clean water and dried at 80°C for 20 minutes; the treated non-woven fabric was immersed in a sodium citrate aqueous solution with a concentration of 0.1 mol / L again, immersed for 6 hours, and dried at 100°C for 20 minutes; and an antibacterial non-woven fabric was obtained.

[0034] Example 3

[0035] This embodiment provides a double antibacterial non-woven fabric, which is prepared by the following method:

[0036] 8.92g (0.03mol) of zinc nitrate hexahydrate was dissolved in 40mL of water to obtain solution A; 0.51g (0.003mol) of silver nitrate, 14.78g (0.18mol) of 2-methylimidazole and 4g of PEG were dissolved in 60mL of water to obtain solution B; the plasma-treated PP non-woven fabric was first immersed in solution A at room temperature for 4h, and then taken out and dried at 100℃ for 20min; then immersed in solution B at room temperature for 6h, taken out and treated at 120℃ for 30min, and then the non-woven fabric was washed with clean water and dried at 80℃ for 20min; the treated non-woven fabric was immersed in a sodium citrate aqueous solution with a concentration of 0.1mol / L again, immersed for 6h, and dried at 100℃ for 20min; and the antibacterial non-woven fabric was obtained.

[0037] Example 4

[0038] This embodiment provides a double antibacterial non-woven fabric, which is prepared by the following method:

[0039] 2.97 g (0.01 mol) of zinc nitrate hexahydrate was dissolved in 40 mL of water to obtain solution A; 0.17 g (0.001 mol) of silver nitrate, 4.93 g (0.06 mol) of 2-methylimidazole and 2 g of PEG were dissolved in 60 mL of water to obtain solution B; the plasma-treated PP non-woven fabric was first immersed in solution A at room temperature for 6 hours, and then taken out and dried at 100°C for 20 minutes; then immersed in solution B at room temperature for 8 hours, taken out and treated at 120°C for 30 minutes, and then the non-woven fabric was washed with clean water and dried at 80°C for 20 minutes; the treated non-woven fabric was immersed in a sodium citrate aqueous solution with a concentration of 0.1 mol / L again, immersed for 6 hours, and dried at 100°C for 20 minutes; and an antibacterial non-woven fabric was obtained.

[0040] Comparative Example 1

[0041] This comparative example provides a double antibacterial non-woven fabric, which is prepared by the following method:

[0042] 5.95 g (0.02 mol) of zinc nitrate hexahydrate was dissolved in 40 mL of water to obtain solution A; 0.34 g (0.002 mol) of silver nitrate, 9.85 g (0.12 mol) of 2-methylimidazole, and 4 g of PEG were dissolved in 60 mL of water to obtain solution B; solution A and solution B were uniformly mixed to obtain solution C, and the plasma-treated PP non-woven fabric was immersed in solution C at room temperature for 10 hours, taken out and dried at 120°C for 30 minutes, then the non-woven fabric was washed with clean water and dried at 80°C for 20 minutes; the treated non-woven fabric was immersed in a sodium citrate aqueous solution with a concentration of 0.1 mol / L again for 8 hours, and dried at 100°C for 20 minutes to obtain an antibacterial non-woven fabric.

[0043] Comparative Example 2

[0044] This comparative example provides a double antibacterial non-woven fabric, which is prepared by the following method:

[0045] 0.34 g (0.002 mol) of silver nitrate was dissolved in 40 mL of water to obtain solution A; 5.95 g (0.02 mol) of zinc nitrate hexahydrate, 9.85 g (0.12 mol) of 2-methylimidazole and 4 g of PEG were dissolved in 60 mL of water to obtain solution B; the plasma-treated PP non-woven fabric was first immersed in solution B at room temperature for 10 hours, taken out and dried at 120°C for 30 minutes, and then immersed in solution A at room temperature for 8 hours, taken out and dried at 100°C for 20 minutes; the non-woven fabric was washed with clean water and dried at 80°C for 20 minutes; the treated non-woven fabric was immersed in a sodium citrate aqueous solution with a concentration of 0.1 mol / L again, immersed for 8 hours, and dried at 100°C for 20 minutes; and the antibacterial non-woven fabric was obtained.

[0046] Comparative Example 3

[0047] This comparative example provides a double antibacterial non-woven fabric, which is prepared by the following method:

[0048] 5.95 g (0.02 mol) of zinc nitrate hexahydrate and 0.34 g (0.002 mol) of silver nitrate were dissolved in 40 mL of water to obtain solution A; 9.85 g (0.12 mol) of 2-methylimidazole and 4 g of PEG were dissolved in 60 mL of water to obtain solution B; the plasma-treated PP non-woven fabric was first immersed in solution A at room temperature for 8 hours, and then taken out and dried at 100°C for 20 minutes; then immersed in solution B at room temperature for 10 hours, taken out and treated at 120°C for 30 minutes, and then the non-woven fabric was washed with clean water and dried at 80°C for 20 minutes; the treated non-woven fabric was immersed in a sodium citrate aqueous solution with a concentration of 0.1 mol / L again, immersed for 8 hours, and dried at 100°C for 20 minutes; and an antibacterial non-woven fabric was obtained.

[0049] According to GB / T20944-2007 standard, the antibacterial properties of the antibacterial nonwoven fabrics obtained in each group of examples and comparative examples were tested, and the experimental bacteria were Escherichia coli and Staphylococcus aureus. The antibacterial nonwoven fabrics were then washed 100 times and their antibacterial rates were tested again. The test results are shown in Table 1:

[0050] Table 1: Antibacterial rate results

[0051]

[0052] It can be seen from Table 1 that the antibacterial non-woven fabric prepared by the present invention not only has excellent antibacterial properties against Escherichia coli and Staphylococcus aureus, but also has good washability, and still has a good antibacterial effect after being washed 100 times.

[0053] In comparison, the methods provided in Comparative Examples 1 to 3 are different from the soaking order of the present invention (Comparative Example 1 is to soak A and B solutions at the same time after mixing, Comparative Example 2 is to soak B solution first and then A solution, and Comparative Example 3 adds silver to A solution and soaks first), and the obtained non-woven fabric products are significantly lower in terms of initial antibacterial rate and antibacterial rate after washing 100 times than the embodiments of the present invention. It can be seen that the preparation method provided by the present invention can ensure that the ZIF-8 structure loaded with nanosilver is attached to the surface of the non-woven fabric with the best dispersibility, uniformity and adhesion, ensuring that it has excellent antibacterial effect and wash-resistant antibacterial effect.

[0054] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing a double antibacterial nonwoven fabric, characterized in that: The steps include: (1) soaking the nonwoven fabric in a solution containing zinc salt and drying; (2) soaking the non-woven fabric treated in step (1) in a solution containing silver salt, 2-methylimidazole and an adhesive, and drying; (3) soaking the nonwoven fabric treated in step (2) in a solution containing a reducing agent and drying it.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the zinc salt to the silver salt is (1-3):(0.1-0.3).

3. The preparation method according to claim 1, characterized in that: The molar ratio of the zinc salt to the silver salt is 1:(0.1-0.2).

4. The preparation method according to claim 1, characterized in that: The solution in step (1) contains a zinc salt at a concentration of 0.25 to 0.75 mmol / mL; and the solution in step (2) contains a silver salt at a concentration of 0.015 to 0.05 mmol / mL.

5. The preparation method according to claim 1, characterized in that: The molar ratio of the zinc salt to 2-methylimidazole is (1-3):(6-12).

6. The preparation method according to claim 1, characterized in that: The molar ratio of the zinc salt to 2-methylimidazole is 1:(6-7).

7. The preparation method according to claim 1, characterized in that: The solution in step (2) contains 2-methylimidazole at a concentration of 1 to 3 mmol / mL.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The soaking in step (1), step (2) and / or step (3) is for 4 to 10 hours.

9. The preparation method according to any one of claims 1 to 7, characterized in that: The soaking time in step (1) is 4 to 8 hours, the soaking time in step (2) is 6 to 10 hours, and the soaking time in step (3) is 4 to 8 hours.

10. The preparation method according to any one of claims 1 to 7, characterized in that: The adhesive is selected from at least one of PEG, PVA, and PVP; And / or, the reducing agent is selected from at least one of sodium citrate, glucose or sodium borohydride.

11. The preparation method according to claim 1, characterized in that: In the step (3), the non-woven fabric is first washed with clean water, dried, and then placed in a solution containing a reducing agent.

12. The preparation method according to claim 1 or 11, characterized in that: The drying step is: drying at 60-120° C. for 10-30 minutes.

13. The preparation method according to claim 1, characterized in that: The nonwoven fabric is subjected to corona or plasma treatment before step (1).

14. The preparation method according to claim 1, characterized in that: The nonwoven fabric has a gram weight of 20-50 g / m 2 , thickness is 0.04mm~0.1mm.

15. The double antibacterial nonwoven fabric prepared by the method according to any one of claims 1 to 14.

16. Use of the double antibacterial nonwoven fabric according to claim 15 in the field of medical treatment or public health.

Citation Information

Patent Citations

  • Preparation method of nano-silver-containing hydrophilic polypropylene non-woven fabric

    CN108774874A

  • Ag / ZIF-8 anti-bacterial agent and preparation method thereof

    CN109758474A