A continuous uniform coating hot wire chemical vapor deposition device and method
By independently controlling the current and water flow of the hot wire heating and water cooling system in the hot wire chemical vapor deposition equipment, combined with automatic sample delivery and insulation and cooling processes, the problem of temperature control is solved, and the preparation efficiency and quality of diamond films are improved. , reducing costs and stress.
Patent Information
- Application Number
- CN202010655206.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-07-09
AI Technical Summary
The existing hot wire chemical vapor deposition equipment has defects in temperature control, resulting in low film preparation efficiency, high cost, uneven quality and excessive stress, hindering the widespread application of diamond films in the industrial and aviation fields.
A continuous and uniform coating hot wire chemical vapor deposition device is designed to ensure heat by realizing independent current and water flow control on multiple units of the hot wire heating system and the water cooling system, combining the automatic transmission and insulation and cooling process of the sample delivery device. Wire temperature field uniformization and film quality improvement.
It realizes efficient and uniform film preparation, reduces cost and manual consumption, improves the uniformity and service life of the film, and ensures automated control of the equipment and energy savings.
Smart Images

Figure CN111705304B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical vapor deposition, and relates to a hot wire chemical vapor deposition device and method. Background Art
[0002] At present, boron-doped diamond film wastewater treatment electrodes and diamond-coated tools have become new products in the field of industrial applications. Diamond film wastewater treatment electrodes can degrade industrial wastewater, difficult-to-treat organic wastewater, etc., and have great application prospects in the field of environmental protection. Diamond-coated tools are also widely used in material processing in the aviation field and microelectronic device processing. The hot wire chemical vapor deposition method can prepare diamond films on a large area. However, the hot wire needs to be replaced each time the preparation is carried out, the preparation efficiency is low, and the material and time costs are high. In addition, the uneven temperature field of the hot wire leads to poor uniformity of the film quality. The lack of a corresponding cooling process leads to excessive stress and poor stability of the film, which seriously hinders its application. In order to improve the preparation efficiency of the film and improve the quality of the film, new vacuum equipment and processes need to be developed. Summary of the invention
[0003] The purpose of the present invention is to solve the defects of existing deposition equipment in temperature control, and to provide a continuous and uniform coating hot wire chemical vapor deposition equipment and method, which can achieve uniformity of the hot wire temperature field and improve the quality of the film by adjusting and controlling the temperature of the hot wire in two-dimensional directions.
[0004] The first technical solution adopted by the present invention to solve its technical problems is: a continuous and uniformly coated hot wire chemical vapor deposition equipment, including: a coating chamber, a sample feeding and insulation chamber, and a sample feeding device. The coating chamber and the sample feeding and insulation chamber are connected by a plug valve, and a hot wire heating system is provided in the coating chamber; a water cooling system is provided under the hot wire heating system; the sample feeding and insulation chambers are symmetrically arranged on both sides of the coating chamber; the sample feeding device feeds the sample into the coating chamber through the sample feeding and insulation chamber, and the two sides are alternately performed for continuous coating.
[0005] As a preferred embodiment of the present invention, the hot wire heating system is composed of a plurality of hot wire units, each hot wire unit includes a hot wire, and the hot wire is connected to an independent power supply.
[0006] Further preferably, the hot wire units are evenly arranged on a hot wire rack, and a plurality of conductive rings are provided on the hot wire rack, and each group of conductive rings is respectively connected to the positive and negative poles of an independent power supply; both ends of the hot wire pass around the conductive rings of the positive and negative poles and are tightened by springs.
[0007] As a preferred embodiment of the present invention, the water cooling system comprises a water cooling plate, and the water cooling plate is composed of a plurality of water cooling units arranged in parallel; the water flow direction of the water cooling unit is perpendicular to the current direction of the hot wire.
[0008] Further preferably, a flow cut-off valve is provided on the water cooling unit, and the water flow in the water cooling unit is controlled by the flow cut-off valve.
[0009] Further preferably, a lifting mechanism is provided below the water cooling plate, and the lifting mechanism drives the water cooling plate to move up and down.
[0010] As a preferred embodiment of the present invention, the sample delivery device includes a sample tray, which is composed of a tray body and a resistance wire, and the resistance wire is arranged in a circuitous manner in the tray body; the two ends of the resistance wire are respectively connected to the positive and negative electrode wires; the arrangement spacing of the resistance wire is gradually dense from the middle to both sides.
[0011] Further preferably, the sample delivery device further comprises a sample delivery rod, one end of which is plug-connected to the sample tray; a joint end of the sample delivery rod and the sample tray is provided with positive and negative connection electrodes.
[0012] Further preferably, the sample delivery device also includes a conveying rack arranged in the sample delivery insulation chamber and the coating chamber, and the conveying rack is provided with a sliding device. The sample tray enters and exits the coating chamber with the help of the sliding device under the push and pull of the sample delivery rod.
[0013] The present invention further provides a method for continuous uniform coating hot wire chemical vapor deposition, comprising:
[0014] (1) Close the gate valves on both sides of the coating chamber, turn on the power, and wait for the hot wire to carbonize;
[0015] (2) Adjust the current of each hot wire heating unit so that the current increases evenly from the middle unit to the units on both sides;
[0016] (3) Open the valve on one side and place the sample to be coated on the sample tray;
[0017] (4) Use the sample delivery rod to push the sample tray to the middle of the water cooling tray, pull out the sample delivery rod, and close the gate valve;
[0018] (5) The water cooling plate is raised to 10 mm below the hot wire, and the stop valve of each water cooling unit is adjusted so that the water flow rate in the middle of the water cooling plate decreases toward both sides. The process parameters are adjusted and the deposition of the coating begins.
[0019] (6) At the end of the coating process, the water cooling plate descends, the plug valve on this side is opened, the sample delivery rod is connected to the sample delivery plate, and the sample plate is powered on for heating. The sample plate is then pulled out to the sample delivery insulation chamber and left to cool down.
[0020] (7) Open the gate valve on the other side, send the sample to be coated into the coating chamber through the sample delivery and insulation chamber on the other side, and repeat steps (4) to (6) to coat another sample;
[0021] (8) Take out the coated samples after cooling down and place new samples to be coated. The cycle is repeated in turn, with the sample delivery and insulation chambers on both sides alternately performed for continuous coating.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] Realize one-time wire drawing, multiple, large-area, continuous coating, and reduce coating costs;
[0024] Precisely control the hot wire heating unit and water cooling unit to achieve uniform temperature field, thereby achieving uniform film preparation, optimizing current and water flow, and saving energy;
[0025] Add a temperature-controllable sample tray to achieve automatic heat preservation and cooling, reduce film stress, and improve product quality and service life;
[0026] High automation control enables one person to control multiple devices, reducing labor costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the overall structure of a continuous uniform film coating hot wire chemical vapor deposition device provided by an embodiment of the present invention;
[0028] Figure 2 is a schematic diagram of the external chamber;
[0029] Figure 3 It is a schematic diagram of the structure and spatial position relationship of the internal hot wire heating system and water cooling system;
[0030] Figure 4 It is the hot wire unit structure intention;
[0031] Figure 5 It is a schematic diagram of a hot wire heating system composed of a number of hot wire units;
[0032] Figure 6 It is a schematic diagram of the structure of the water cooling plate;
[0033] Figure 7 is a schematic diagram of the internal structure of the circulation chamber;
[0034] Figure 8 It is a schematic diagram of the water cooling plate lifting mechanism;
[0035] Fig. 9 It is a perspective view of the sample delivery tray structure;
[0036] Fig.10 This is a schematic diagram of the arrangement of the resistance wires inside the sample delivery tray;
[0037] Fig.11 It is a schematic diagram of the connection between the sample delivery rod and the sample delivery plate;
[0038] Fig.12 It is a schematic diagram of the process flow of a hot wire chemical vapor deposition method for continuous uniform film coating provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0039] In order to facilitate the understanding of the present invention, the present invention is described in more detail below in conjunction with the accompanying drawings and specific embodiments. Preferred embodiments of the present invention are provided in the accompanying drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described in this specification. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0040] One of the embodiments provided by the present invention is: a continuous uniform coating hot wire chemical vapor deposition device, the overall structure of the device is as follows Figure 1 and 2 As shown, the double-layer water-cooled outer shell made of 304 stainless steel as the main material constitutes the chambers of the entire device, namely the left sample delivery insulation chamber 2, the middle coating chamber 4, and the right sample delivery insulation chamber 5. The left sample delivery insulation chamber 2 and the right sample delivery insulation chamber 5 are separated from the middle coating chamber 4 by a gate valve 3 respectively.
[0041] like Figure 1 and 3 As shown, in the coating chamber 4, there are provided a hot wire heating system running forward and backward and a water cooling system running left and right, wherein the water cooling system is placed below the hot wire heating system, and the two are spaced apart by a distance and in a vertical relationship.
[0042] like Figure 3 and 4 As shown, the hot wire heating system is composed of a plurality of hot wire units 6 arranged in parallel on a hot wire rack 11. The hot wire rack 11 is supported by four vertical copper rods 17, and a ceramic cross beam 14 is installed between two copper rods. The copper rod 17 is a hollow rod body, and water flows inside to cool the high-temperature ceramic cross beam 14 during the coating process.
[0043] like Figure 4 As shown, each hot wire unit includes a hot wire 8 and two high temperature resistant conductive molybdenum rings: a negative molybdenum ring 12 and a positive molybdenum ring 13. Multiple molybdenum rings are connected in series on a ceramic cross beam 14, and adjacent molybdenum rings are spaced a certain distance apart. The hot wire 8 uses a tantalum wire with a diameter of 0.5 to 0.8 mm. The two ends of the hot wire 8 are respectively passed around the positive molybdenum ring 13 and the negative molybdenum ring 12, and are tightened by a high temperature resistant spring 16 fixed on an insulating ceramic 18. The negative molybdenum ring 12 and the positive molybdenum ring 13 are respectively connected to the positive and negative poles of an independent power source through a high temperature resistant wire 15.
[0044] like Figure 4 and 5As shown, unlike the traditional hot wires connected in parallel and powered by the same power supply, in the entire hot wire heating system of this embodiment, each hot wire unit is connected to an independent power supply, and the independent power supply supplies power to a single hot wire separately, thereby achieving precise control of the current of the single hot wire, and further achieving precise control of the temperature.
[0045] When the traditional hot wire is powered on, the current of each hot wire is the same, and the heat generated is the same, resulting in the phenomenon that the temperature field of the entire hot wire is high in the middle and low on both sides, resulting in uneven thickness and quality of film growth. In this embodiment, the hot wire unit structure realizes the current control of a single hot wire, and the current from both sides to the middle hot wire decreases gradually, so that the heat generated by the hot wires on both sides is higher than that of the middle hot wire, and the temperature field difference in the horizontal direction of the hot wire is alleviated.
[0046] like Figure 6 As shown, the water cooling system consists of a water cooling plate 9, a circulation chamber 20 and an inlet and outlet water pipe 21. The water cooling plate 9 is composed of a plurality of water cooling units 19 arranged side by side, and the water cooling units 19 use non-standard pipe fittings processed from red copper. The two ends of the water cooling unit 19 are connected to the two ends of the circulation chamber 20, and a flow cut-off valve 22 is installed at the inlet end of each water cooling unit, and the water flow in each pipe can be controlled by the flow cut-off valve 22.
[0047] The internal structure of the circulation chamber 20 is as follows: Figure 7 As shown, a partition 23 is provided inside, and the partition divides the circulation chamber 20 into a water inlet chamber on the left and a water outlet chamber on the right, wherein the water inlet chamber is connected to the inlet end of the water cooling unit 19, and the water outlet chamber is connected to the outlet end of the water cooling unit. The bottom of the circulation chamber 20 is connected to the inlet and outlet pipes 21, and the inlet and outlet pipes 21 are of a sleeve structure, wherein the inner pipe is the outlet pipe, and the outer pipe is the inlet pipe. The inlet pipe is connected to the water inlet chamber. The partition 23 is connected to the outlet pipe, and the outlet chamber is connected to the outlet pipe through the reflux hole 24 opened on the partition. The inlet pipe outside the inlet and outlet pipes 21 carries cold water, and the inner outlet pipe carries refluxed hot water. The lower end of the inlet and outlet pipes 21 is provided with water inlets and outlets.
[0048] like Figure 8 As shown, a vacuum plate 25 is installed on the water inlet and outlet pipes 21. The function of the vacuum plate 25 is to seal the bottom of the coating chamber 4 during the coating process, so that the coating chamber forms a closed space.
[0049] A hydraulic push rod 26 is provided at the bottom of the water inlet and outlet pipes 21 , and under the action of the hydraulic push rod 26 , the entire water cooling plate 9 can achieve lifting movement.
[0050] During the lifting and lowering of the water-cooling plate 9, in order to maintain the sealing state between the vacuum plate 25 and the bottom of the coating chamber 4, the vacuum plate 25 is connected to the bottom of the circulation chamber 20 through a bellows expansion tube 27, so that during the lifting and lowering of the water-cooling plate 9, the position of the vacuum plate 25 always remains stationary, thereby sealing the bottom of the coating chamber 4.
[0051] In this embodiment, the water-cooling unit in the water-cooling plate 9 is placed vertically in space with the hot wire unit 6 in the hot wire heating system, that is, the current direction in the hot wire unit and the water flow direction of the water-cooling unit are vertical in space. The non-uniformity of the hot wire temperature field is divided into two directions: perpendicular to the hot wire and parallel to the hot wire. The vertical direction of the hot wire can be controlled by adjusting the current difference of the hot wire unit, while the temperature difference in the direction parallel to the hot wire still exists. The reason is that the heat generated at each site of the same hot wire is basically the same, but the heat radiation received in the middle of the sample stage is more than that at both ends. The water-cooling unit of the water-cooling plate can control the water flow rate passing through each tube, so that the water flow rate of the units at both ends shows an increasing trend to the middle, so the heat taken away by the middle water-cooling unit is higher than that on both sides, so as to alleviate the temperature field difference in the parallel direction of the hot wire.
[0052] In this embodiment, the separate control of the current of the hot wire unit and the separate control of the water flow of the water cooling unit, as well as the spatial vertical layout of the two play a decisive role in solving the technical problem of uneven distribution of the hot wire temperature field.
[0053] The water cooling plate 9 in the coating chamber 4 can be lifted and lowered under the action of the hydraulic push rod 26. During general coating, the distance between the hot wire and the sample plate is about 8mm to 10mm, the hot wire temperature is 2400 to 2600°C, and the radiation temperature of the sample plate is as high as 800 to 1000°C. If the sample is transported under such conditions, it is difficult to achieve due to the high temperature deformation of the transport components. In addition, the hot wire at high temperature requires a very stable surrounding environment, and the disturbance caused by the transport may cause the hot wire to break. Therefore, after the sample is coated, the hydraulic push rod 26 slowly descends to a reasonable position to achieve the appropriate temperature for sample transport, and at the same time there is no disturbance to the hot wire.
[0054] like Figure 1 and 2 As shown, in this embodiment, the left sample delivery and heat preservation chamber 2 and the right sample delivery and heat preservation chamber 5 are respectively provided with a sample tray 1 and a sample delivery rod 7, and a conveying rack 10 is provided in the sample delivery and heat preservation chamber and the coating chamber. Figure 3 As shown. The conveyor rack 10 is made of high temperature resistant ceramics and does not deform under high temperature conditions. A pulley is installed on the conveyor rack 10. The sample tray 1 is placed on the conveyor rack 10, and under the push and pull action of the sample delivery rod 7, the sample is delivered between the coating chamber 4 and the sample delivery and insulation chambers on both sides by rolling the pulley.
[0055] like Fig. 9 As shown, the sample tray 1 is composed of a ceramic tray body 33 and a heating wire 28 inside the ceramic tray body 33. The heating wire 28 is a heatable resistance wire, which is arranged in a circuitous manner inside the ceramic tray body 33, and the spacing between the heating wires gradually decreases from the middle to the sides, and the arrangement gradually becomes denser, such as Fig.10 The purpose of adopting this arrangement is to ensure that a large area of the sample can be cooled evenly during the cooling process.
[0056] like Fig. 9 and Fig.11 As shown, the two ends of the heating wire 28 are respectively connected to the positive wire 29 and the negative wire 30. The sample delivery rod 7 is connected to the sample delivery tray 1 by plugging, and a positive electrode 31 and a negative electrode 32 are provided at the joint of the sample delivery rod 7. When the sample delivery rod 7 is plugged together with the sample delivery tray 1, the positive electrode 31 and the negative electrode 32 are respectively connected to the negative wire 30 and the positive wire 29. When the power is turned on by the positive electrode 31 and the negative electrode 32, the heating wire 28 can be powered on and heated, and the coated sample placed on the ceramic tray body 33 is heated and kept warm.
[0057] Based on the equipment provided in the above embodiment, the present invention also provides another embodiment: a method for continuous uniform coating hot wire chemical vapor deposition, the process flow of the method is as follows: Fig.12 As shown, the specific steps are:
[0058] 1. The coating chamber in the middle is separated from the sample delivery and insulation chambers on both sides by a plug valve. Turn on the power of the hot wire heating system. Fig.12 As shown in (1);
[0059] 2. After the hot wire is carbonized, adjust the current of each hot wire unit, increasing from the middle to both sides;
[0060] 3. Open the right-side plug valve, place the sample to be coated on the sample tray, push the right-side sample tray to the middle position of the water cooling plate using the sample delivery rod, pull out the sample delivery rod, and close the right-side plug valve;
[0061] 4. Start the night-pressing ejector rod to raise the water cooling plate to 10mm away from the hot wire, adjust the flow cut-off valve of each water cooling unit so that the flow rate of the middle water flow is greater than that of the two sides, adjust the process parameters, and start depositing the coating, such as Fig.12 As shown in (2);
[0062] 5. At the end of the coating process, start the night push rod to lower the water cooling plate to a certain position, open the right plug valve, connect the sample delivery rod to the sample delivery plate, and connect the sample plate to the power supply for heating. That is, during the sample transfer process, the sample plate is used to heat and keep the coated sample warm to keep it at a constant temperature or a stable state with little fluctuation. Fig.12 Middle (3);
[0063] 6. Close the plug valve on the right and gradually reduce the current of the sample tray. As the temperature of the sample tray gradually decreases, the sample is cooled evenly at a certain gradient to reduce the stress state of the film, such as Fig.12 Medium (4);
[0064] 7. Push the samples in the left sample delivery and insulation chamber to the cooling plate. Fig.12As shown in (5), at the same time, the sample that has completed cooling in the right sample delivery and insulation chamber is taken out and a new non-coated sample is placed;
[0065] 8. Repeat steps 3-6 to complete the coating and uniform cooling of the samples in the left sample delivery and insulation chamber. Fig.12 As shown in (6);
[0066] 9. Reopen the right gate valve and repeat steps 3-6, cycling in sequence, alternating between left and right.
[0067] In the above method, the hot wire of the coating chamber is always in a heated state and is not connected to the atmosphere. The left and right sample feeding and heat preservation chambers play the role of cyclic sample feeding and heat preservation to achieve continuous coating.
[0068] The present invention is combined with process experience and finds that in addition to slow cooling, a lower constant temperature stage is also required to release stress when cooling down in the later stage of film preparation. Therefore, the device and method of the present invention are proposed, which can realize automatic heat preservation and gentle and uniform cooling of samples after coating, reduce film stress, and improve product quality and service life.
Claims
1. A continuous uniform coating hot wire chemical vapor deposition device, comprising: The coating chamber, the sample delivery and heat preservation chamber, and the sample delivery device are connected between the coating chamber and the sample delivery and heat preservation chamber via a plug valve; a hot wire heating system is provided in the coating chamber; a water cooling system is provided below the hot wire heating system; the hot wire heating system is composed of a plurality of hot wire units, each of which includes a hot wire, and the hot wire is connected to an independent power supply; the characteristics are as follows: the hot wire units are evenly arranged on the hot wire rack, and a plurality of conductive rings are provided on the hot wire rack, and each group of conductive rings is respectively connected to the positive and negative poles of the independent power supply; the two ends of the hot wire bypass the conductive rings of the positive and negative poles, and pass through The spring is tightened; the water cooling system includes a water cooling plate, which is composed of a number of water cooling units arranged in parallel; the water flow direction of the water cooling unit is perpendicular to the current direction of the hot wire; a flow cut-off valve is provided on the water cooling unit, and the water flow in the water cooling unit is controlled by the flow cut-off valve; a lifting mechanism is provided under the water cooling plate, and the lifting mechanism drives the water cooling plate to move up and down; the sample feeding and heat preservation chamber is arranged on both sides of the coating chamber; the sample feeding device feeds the sample into the coating chamber through the sample feeding and heat preservation chamber, and the two sides are alternately carried out for continuous coating.
2. The continuous uniform coating hot wire chemical vapor deposition equipment according to claim 1, characterized in that: The sample delivery device comprises a sample tray, which consists of a tray body and a heating wire. The heating wire is arranged in a circuitous manner in the tray body, and its two ends are respectively connected to positive and negative electrode wires; the arrangement spacing of the heating wire is gradually denser from the middle to both sides.
3. The continuous uniform coating hot wire chemical vapor deposition equipment according to claim 2, characterized in that: The sample delivery device further comprises a sample delivery rod, one end of which is plug-connected with the sample tray; positive and negative connection electrodes are arranged at the joint ends of the sample delivery rod and the sample tray.
4. The continuous uniform coating hot wire chemical vapor deposition equipment according to claim 3, characterized in that: The sample delivery device also includes a conveying rack arranged in the sample delivery insulation chamber and the coating chamber, and a sliding device is provided on the conveying rack. The sample tray enters and exits the coating chamber with the help of the sliding device under the push and pull of the sample delivery rod.
5. A method for continuous uniform coating hot wire chemical vapor deposition, using the device of claim 1, characterized in that: include: (1) Close the gate valves on both sides of the coating chamber, turn on the power, and wait for the hot wire to carbonize; (2) Adjust the current of each hot wire heating unit so that the current increases evenly from the middle unit to the units on both sides; (3) Open the valve on one side and place the sample to be coated on the sample tray; (4) Use the sample delivery rod to push the sample tray to the middle of the water cooling tray, pull out the sample delivery rod, and close the gate valve; (5) The water cooling plate is raised to 10 mm below the hot wire, and the stop valve of each water cooling unit is adjusted so that the flow rate of cold water in the middle of the water cooling plate decreases toward both sides. The process parameters are adjusted and the deposition of the coating begins. (6) At the end of the coating process, the water cooling plate is lowered, the gate valve is opened, the sample delivery rod is connected to the sample delivery plate, and the sample plate is powered on for heating. The sample plate is then pulled out to the sample delivery insulation chamber and left to cool down. (7) Open the gate valve on the other side, send the sample to be coated into the coating chamber through the sample delivery and insulation chamber on the other side, and repeat steps (4) to (6) to coat another sample; (8) Take out the coated samples after cooling down and place new samples to be coated. The cycle is repeated in turn, with the sample delivery and insulation chambers on both sides alternately performed for continuous coating.