Composite plated product and method for producing the same

By adding sulfonic acid and carbon particle dispersion to the silver plating solution, a high carbon content composite coating is formed, which solves the problems of uneven appearance and insufficient wear resistance in the existing technology, and realizes efficient and economical production of composite plated products. .

CN111705340BActive Publication Date: 2024-10-29DOWA METALTECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202010187161.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-03-17
Publication Date
2024-10-29
Estimated Expiration
2040-03-17

AI Technical Summary

Technical Problem

Existing composite plated products have problems with uneven appearance and insufficient wear resistance when using cyanide silver plating solution and silver nitrate silver plating solution, and have poor long-term stability, making them unsuitable for mass production.

Method used

Use silver plating solution containing sulfonic acid and carbon particle dispersion for electroplating to form a composite coating with high carbon content and good wear resistance. Avoid using silver plating solution containing cyanide and silver nitrate, and use carbon particle dispersion to increase carbon particles. Dispersion in silver plating solutions.

Benefits of technology

Composite plated products with almost no uneven appearance and good wear resistance are realized, which reduces production costs and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002414598390000101
    Figure BDA0002414598390000101
  • Figure BDA0002414598390000111
    Figure BDA0002414598390000111
  • Figure BDA0002414598390000112
    Figure BDA0002414598390000112
Patent Text Reader

Abstract

The present invention provides a composite plated product having almost no uneven appearance and good wear resistance and a method for manufacturing the same, wherein the method does not require any silver plating solution containing cyanide and any silver plating solution containing silver nitrate as a silver salt. A substrate (preferably made of copper or a copper alloy) is electroplated using a silver plating solution containing sulfonic acid to which a carbon particle dispersion (preferably containing silicate) is added to form a composite plated film of a composite material containing carbon particles in a silver layer on the substrate, thereby manufacturing the composite plated product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a composite plated article and a method for making the same. More particularly, the present invention relates to a composite plated article used as a material for sliding contact parts such as switches and connectors. Background Art

[0002] Conventionally, as materials for sliding contact parts such as switches and connectors, silver-plated products are used, in which silver is plated on a conductive material such as copper or a copper alloy to prevent oxidation of the conductive material due to heat during sliding.

[0003] However, since the silver-plated film is soft and easy to wear, and since it generally has a high friction coefficient, the silver-plated film has the problem of being easily peeled off due to sliding. In order to solve this problem, a method for improving the wear resistance of a conductive material by forming a composite coating film on a conductive material by electroplating has been proposed, wherein the composite material comprises graphite particles selected from carbon particles such as graphite particles and carbon black particles having good heat resistance, wear resistance, lubricity, etc., which are dispersed in a silver matrix (see, for example, Japanese Patent Laid-Open No. 9-7445). A method for manufacturing a silver-plated film containing graphite particles by adding a plating bath to which a wetting agent suitable for dispersing graphite particles is added is also proposed (see, for example, Japanese Patent Laid-Open No. 5-505853 (Japanese translation of the international public text of PCT / DE91 / 00241). In addition, a method for coating carbon particles with metal oxides or the like by a sol-gel method to enhance the dispersibility of carbon particles in a composite plating solution of silver and carbon particles to increase the amount of carbon particles in the composite plating film is also proposed (see, for example, Japanese Patent Laid-Open No. 3-253598).

[0004] However, the composite plated products made by the methods described in Japanese Patent Laid-Open No. 9-7445, Japanese Patent Laid-Open No. 5-505853, and Japanese Patent Laid-Open No. 3-253598 have a high friction coefficient, so there is a problem that the composite plated products cannot be used as long-life contact and terminal materials. Therefore, it is desirable to provide a composite plated product having a higher carbon content and a higher area percentage of carbon particles on its surface than the composite plated products made by the methods described in Japanese Patent Laid-Open No. 9-7445, Japanese Patent Laid-Open No. 5-505853, and Japanese Patent Laid-Open No. 3-253598, and having higher wear resistance than the composite plated products made by the methods described in Japanese Patent Laid-Open No. 9-7445, Japanese Patent Laid-Open No. 5-505853, and Japanese Patent Laid-Open No. 3-253598.

[0005] As methods for producing such composite plated products, the following methods have been proposed, among others: a method in which a substrate is electroplated using a cyanide-containing silver plating solution containing carbon particles subjected to oxidation treatment to form a composite material coating film containing carbon particles in a silver layer on the substrate (see, for example, Japanese Patent Laid-Open No. 2006-37225); a method in which a substrate is electroplated using a cyanide-containing silver plating solution containing carbon particles subjected to electrolytic treatment to form a composite material coating film containing carbon particles in a silver layer on the substrate (see, for example, Japanese Patent Laid-Open No. 2007-16261); and a method in which a substrate is electroplated using a composite plating solution prepared by adding carbon particles subjected to oxidation treatment and then subjected to silane coupling treatment to a silver plating solution containing silver nitrate and ammonium nitrate to form a composite material coating film containing carbon particles in a silver layer on the substrate (see, for example, Japanese Patent Laid-Open No. 2007-262528).

[0006] However, the methods disclosed in Japanese Patent Laid-Open Nos. 2006-37225 and 2007-16261 use a silver plating solution containing cyanide, so it is necessary to treat the aqueous solution containing cyanide, so the cost of drainage facilities is high. In the method disclosed in Japanese Patent Laid-Open No. 2007-262528, since Ag is precipitated in a dendrite-like state by electroplating in a silver plating bath containing silver nitrate and ammonium nitrate, it is possible that the appearance of the composite plated product is seriously uneven. In addition, the long-term stability of the silver plating bath is poor, so this method is not suitable for mass production of composite plated products. Summary of the invention

[0007] Therefore, an object of the present invention is to eliminate the above-mentioned problems and provide a composite plated product having almost no uneven appearance and excellent wear resistance and a method for producing the same, which method does not require any silver plating solution containing cyanide and any silver plating solution containing silver nitrate as a silver salt.

[0008] To achieve the above and other objects, the inventors have conducted intensive research and found that if a silver plating solution containing sulfonic acid (which is a cyanide-free silver plating solution) to which a carbon particle dispersion (which is a carbon particle dispersion solution) is added is used to electroplate a substrate to form a composite plated film of a composite material containing carbon particles in a silver layer on the substrate, a composite plated product having almost no uneven appearance and good wear resistance can be produced without any silver plating solution containing cyanide and any silver plating solution containing silver nitrate as a silver salt. Thus, the inventors have completed the present invention.

[0009] According to the present invention, a method for manufacturing a composite plated product is provided, the method comprising the following steps: preparing a carbon particle dispersion in which carbon particles are dispersed; adding the carbon particle dispersion to a silver plating solution containing sulfonic acid; and electroplating a substrate using the silver plating solution containing sulfonic acid to which the carbon particle dispersion is added, thereby forming a composite plated film of a composite material containing carbon particles in a silver layer on the substrate.

[0010] In the method for manufacturing the composite plated product, the carbon particle dispersion preferably contains silicate. The carbon particles are preferably graphite particles having an average particle size of 1 to 15 μm. The amount of carbon particles added to the silver plating solution containing sulfonic acid is preferably in the range of 10 g / L to 100 g / L. The electroplating for forming the composite plated film is preferably carried out at a speed of 1 to 20 A / dm 2 The substrate is preferably made of copper or a copper alloy. Before forming the composite plating film of the composite material, a nickel plating film may also be formed on the substrate.

[0011] According to the present invention, there is also provided a composite plated product, comprising: a substrate, and a composite coating formed on the substrate and comprising a composite material containing carbon particles in a silver layer; wherein the area percentage occupied by the carbon particles on the surface of the composite coating is in the range of 30 area % to 90 area %, and the composite coating contains silicon.

[0012] In the composite plated product, the silicon content in the composite plated film is preferably in the range of 0.01 wt% to 1 wt%. The composite plated film preferably has a thickness of 0.5 to 20 μm. In addition, a nickel plated film may be formed between the composite plated film and the substrate.

[0013] According to the present invention, a composite plated product having almost no uneven appearance and good wear resistance and a method for manufacturing the same can be provided without any silver plating solution containing cyanide and any silver plating solution containing silver nitrate as a silver salt. DETAILED DESCRIPTION

[0014] In a preferred embodiment of the method for manufacturing a composite plated product of the present invention, a substrate (preferably made of copper or a copper alloy) is electroplated using a sulfonic acid-containing silver plating solution (a silver plating solution containing at least one sulfonic acid) containing a carbon particle dispersion (a dispersion of carbon particles) to form a composite plating film of a composite material containing carbon particles in a silver layer on the substrate. Simply adding and suspending carbon particles in the silver plating solution does not allow the carbon particles to be included in the plating film, but if the carbon particle dispersion is added to the sulfonic acid-containing silver plating solution as in this preferred embodiment, the dispersibility of the carbon particles in the silver plating solution can be improved.

[0015] A carbon particle dispersion is a dispersion in which carbon particles are dispersed in a dispersion medium. The dispersion medium is preferably water. The carbon particle dispersion preferably contains a silicate such as potassium silicate. The amount of silicate is preferably 5 to 20% by weight, more preferably 10 to 15% by weight. The carbon particle dispersion may contain a dispersant to improve the dispersibility of the carbon particles in the carbon particle dispersion. The dispersant may be a dispersant that can prevent the carbon particles from settling. For example, the dispersant may be any one of anionic dispersants such as methylcellulose and carboxymethylcellulose, nonionic dispersants such as polyoxyethylene alkyl ethers, and cationic dispersants such as sodium alkylbenzene sulfonate. In addition, when the carbon particle dispersion is allowed to stand for 5 minutes after the carbon particles are dispersed in the dispersion medium by stirring, preferably more than 90% of the carbon particles maintain their dispersed state. The carbon particles are preferably graphite particles. The average particle size of the graphite particles is preferably 0.5 to 15 μm, more preferably 1 to 10 μm.

[0016] The silver plating solution containing sulfonic acid may contain silver sulfonate as an Ag ion source, sulfonic acid as a complexing agent, and additives such as a brightener. The Ag concentration in the silver plating solution is preferably 5 to 150 g / L, more preferably 10 to 120 g / L, and most preferably 20 to 100 g / L. As the silver sulfonate contained in the silver plating solution containing sulfonic acid, silver methanesulfonate, silver alkanolsulfonate, silver phenolsulfonate, etc. can be used.

[0017] The amount of carbon particles added to the silver plating solution containing sulfonic acid is preferably in the range of 10 g / L to 100 g / L, more preferably in the range of 20 to 90 g / L, and most preferably in the range of 30 to 80 g / L. If the amount of carbon particles in the silver plating solution containing sulfonic acid is less than 10 g / L, the amount of carbon particles in the composite plating layer may not be sufficiently increased. Even if the amount of carbon particles in the silver plating solution exceeds 100 g / L, the amount of carbon particles in the composite plating layer cannot be further increased.

[0018] The current density during electroplating for forming the composite plating film is preferably 1 to 20 A / dm 2 , more preferably 2 to 15 A / dm 2 If the Ag concentration and current density are too low, the composite coating will be formed slowly, and the composite coating cannot be formed effectively. If the Ag concentration and current density are too high, the composite coating will easily have an uneven appearance.

[0019] If the carbon particle dispersion is added to the silver plating solution containing sulfonic acid, the dispersibility of the carbon particles in the silver plating solution can be improved. If the silver plating solution is used for electroplating, a composite plated product with high wear resistance can be produced, wherein a composite plated film of a composite material including carbon particles dispersed in a silver layer is formed on a substrate, and the carbon particles occupy a high area percentage on the surface of the composite plated film.

[0020] In a preferred embodiment of the composite plated product of the present invention, a composite plated film of a composite material containing carbon particles in a silver layer is formed on a substrate (preferably made of a copper-copper alloy), the area percentage of carbon particles on the surface of the composite plated film is in the range of 30 area % to 90 area % (preferably 40 area % to 85 area %), and the composite plated product contains (preferably 0.01 to 1 weight %, more preferably 0.05 to 0.3 weight %) Si. If the area percentage of carbon particles on the surface of the composite plated film is less than 30 area %, the wear resistance of the composite plated product is insufficient. If the area percentage of carbon particles on the surface of the composite plated film exceeds 90 area %, the contact resistance of the composite plated product will increase.

[0021] The thickness of the composite plated film is preferably in the range of 0.5 μm to 20 μm, more preferably in the range of 3 μm to 10 μm, and most preferably in the range of 3 μm to 8 μm. If the thickness of the composite plated film is less than 0.5 μm, the wear resistance of the composite plated product is insufficient. If the thickness of the composite plated film exceeds 20 μm, the amount of silver therein increases, thereby increasing the manufacturing cost of the composite plated product. In order to improve the heat resistance of the composite plated product, a nickel plated film (preferably with a thickness of 0.5 to 5 μm) may be formed between the composite plated film and the substrate.

[0022] In addition, if two test pieces are cut from a preferred embodiment of the composite plated product of the present invention, one of the test pieces is used as a plate-shaped test piece (evaluation sample), and a dent is pressed on the other test piece (hemispherical punching so that the inner R is 1.0 mm) as a dent test piece (indent head), the wear resistance of the composite plated product is evaluated by performing a wear test to confirm the wear state of the plate-shaped test piece, in which a sliding wear tester is used to press the dent test piece against the plate-shaped test piece with a constant load (2N) and continuously slide back and forth (sliding distance = 10mm, sliding speed = 3mm / s) until the substrate is exposed, and the substrate is preferably not exposed after the reciprocating sliding is repeated 10,000 times. If the force applied in the horizontal direction during the above-mentioned reciprocating sliding is measured to calculate its average value F, and the dynamic friction coefficient (μ) between the plate-shaped test piece and the dent test piece is calculated from μ = F / N, the dynamic friction coefficient is preferably 0.5 or less.

[0023] Embodiments of the composite plated product and the method for producing the same according to the present invention are described in detail below.

[0024] Example 1

[0025] As a substrate, a Cu-Ni-Sn-P alloy plate (a copper alloy plate containing 1.0 wt% nickel, 0.9 wt% tin, 0.05 wt% phosphorus and the balance copper) with a thickness of 0.2 mm (NB-109EH manufactured by DOWA METALTECH CO., Ltd.) was prepared. Then, the substrate and a platinum-titanium mesh electrode plate (a platinum-plated titanium mesh material electrode plate) were used as the cathode and anode, respectively, in a sulfonic acid-containing silver base plating solution (Dyne Silver GPE-ST manufactured by Daiwa Fine Chemicals Co., Ltd.) containing sulfonic acid as a complexing agent at a temperature of 3 A / dm 2 The substrate was electroplated (silver underplating) for 10 seconds at a current density of .

[0026] Then, a carbon particle dispersion (containing 20 wt% carbon, 11-14 wt% potassium silicate and a dispersant) (PROHITE NS5 manufactured by Nippon Graphite Industries, Co., Ltd.) in which graphite particles having an average particle diameter of 4 μm were dispersed in water as carbon particles was added to a sulfonic acid-containing silver plating solution (containing sulfonic acid as a complexing agent and having a silver concentration of 80 g / L) (DyneSilver GPE-PL (matte) manufactured by Yamato Fine Chemicals Co., Ltd.) until the concentration of the carbon particle dispersion reached 260 g / L. Thus, a sulfonic acid-containing silver plating solution containing 53 g / L of carbon particles was prepared.

[0027] Then, the silver-plated substrate and the silver electrode plate were used as the cathode and the anode, respectively, in the silver plating solution containing sulfonic acid containing the carbon particle dispersion at a temperature of 25° C. and a temperature of 3 A / dm 2 The substrate was electroplated for 250 seconds at a current density of 1.500 μm (current efficiency = 95%) while the silver plating solution was stirred at 500 rpm. A composite plated product was thus prepared, wherein a composite plated film containing carbon particles was formed on the substrate in the silver plating layer.

[0028] The thickness of the composite plated film (1.0 mm diameter region at the center of the composite plated film) of the composite plated product thus obtained was measured using an X-ray fluorescence thickness gauge (FT9450 manufactured by Hitachi High-Tech Science Corporation). As a result, the thickness was 6.5 μm.

[0029] Two test pieces were cut from the composite plated product, and the surface of the test pieces was observed to calculate the area percentage (area ratio (area %)) of carbon particles on the surface of the composite plated film. The area ratio of carbon particles on the surface of the composite plated film was calculated as follows: First, an electron probe microanalyzer (EPMA) (JXA8100 manufactured by JEOL Ltd.) was used to analyze the carbon particles at 3×10 -7 The surface of the test piece was irradiated with an electron beam at an irradiation current of 1000 A and an acceleration voltage of 15 kV to obtain a composite image (COMPO image) in BE mode by a backscattered electron detector (magnification of 1000). The tone binarization of the COMPO image thus obtained was performed by using an image analysis application (image editing / processing software GIMP 2.10.6) (the maximum brightness of all pixels was set to 255 and the minimum brightness was set to 0, so that pixels with a brightness of 127 or less were black, and pixels with a brightness of more than 127 were white). Thereby, the COMPO image was divided into a silver part (white part) and a carbon particle part (black part). The ratio Y / X of the number of pixels Y of the carbon particle part to the number of pixels X of the entire image was calculated, which was the carbon particle area ratio on the surface of the composite coating. As a result, the area percentage (area ratio) of the carbon particles on the surface of the composite coating was 58% by area. The surface of the composite coating was observed with the naked eye. As a result, its surface was gray, and no uneven appearance was observed, so the appearance of the composite coating was good.

[0030] Electron probe microanalyzer (EPMA) (JXA8100 manufactured by JEOL Ltd.) was used to analyze the samples at an accelerating voltage of 15 kV and a scanning electron microscope (SEM). -7 The surface of the composite plated product was irradiated with an electron beam in an analysis area of ​​50 μm in diameter at an irradiation current of 100 A to perform surface analysis thereof by qualitative and quantitative analysis based on the ZAF method. As a result, it was found that the composite plated film contained 0.2 wt % of Si.

[0031] Then, two test pieces were cut from the composite plated product, one of which was used as a plate-shaped test piece (evaluation sample), and the other test piece was dented (hemispherical punching to make its internal R 1.0mm) as a dented test piece (indenter). Afterwards, the wear resistance of the composite plated product was evaluated by performing a wear test to confirm the wear state of the plate-shaped test piece. In the wear test, a sliding wear tester (manufactured by Yamasaki-Seiki Co., Ltd.) was used to press the dented test piece against the plate-shaped test piece with a constant load (2N) while continuously sliding back and forth (sliding distance = 10mm, sliding speed = 3mm / s) until the substrate was exposed. After the reciprocating sliding was repeated 10,000 times, the central part of the sliding scratch of the plate-shaped test piece was observed with a microscope (VKX-1000 manufactured by Keyence Corporation) at a magnification of 200 times. As a result, it was confirmed that no (brown) substrate was exposed. The thickness of the composite coating of the plate-like test piece (the area of ​​1.0 mm in diameter of the sliding scratch center portion of the composite coating) was also measured using an X-ray fluorescence analysis thickness gauge (FT9450 manufactured by Hitachi High-Technologies Co., Ltd.). As a result, the thickness was 5.2 μm, so it can be seen that the wear resistance is good. The force applied in the horizontal direction during the above-mentioned reciprocating sliding was measured to calculate its average value F, and the dynamic friction coefficient (μ) between the plate-like test piece and the indentation test piece was calculated from μ=F / N. As a result, the dynamic friction coefficient was 0.30.

[0032] Example 2

[0033] A substrate was electroplated (silver-plated) in a sulfonic acid-containing silver plating solution containing 20 g / L of carbon particles (current efficiency = 90%), wherein the sulfonic acid-containing silver plating solution was prepared by adding the same carbon particle dispersion as in Example 1 to the same sulfonic acid-containing silver plating solution as in Example 1, the sulfonic acid-containing silver plating solution being the same as in Example 1 except that the Ag concentration in the sulfonic acid-containing silver plating solution was 30 g / L and the carbon particle dispersion was added to the sulfonic acid-containing silver plating solution until the carbon particle dispersion concentration reached 100 g / L. A composite plated product was manufactured by the same method as in Example 1 except that the above-mentioned method was the same as in Example 1.

[0034] The thickness of the composite plated film of the composite plated article thus obtained was measured by the same method as in Example 1. As a result, the thickness was 5.9 μm.

[0035] For the obtained composite plated product, the area percentage (area ratio) of carbon particles on the surface of the composite plated film was calculated by the same method as in Example 1. As a result, the percentage (area ratio) was 77 area%. The surface of the composite plated film was gray, and no uneven appearance was observed thereon, so the appearance of the composite plated film was good. The surface analysis of the composite plated film was also performed by the same method as in Example 1. As a result, it was found that 0.1% by weight of Si was contained in the composite plated film.

[0036] The wear resistance of the composite plated product was evaluated by a sliding wear test in the same manner as in Example 1. As a result, it was found that after 10,000 reciprocating slidings, the substrate was not exposed and the thickness of the composite plated film was 5.1 μm, which showed that the wear resistance was good. The dynamic friction coefficient between the plate-like test piece and the indentation test piece was also calculated in the same manner as in Example 1. As a result, the dynamic friction coefficient was 0.34.

[0037] Example 3

[0038] The substrate was electroplated (silver-plated) in a sulfonic acid-containing silver plating solution containing 64 g / L of carbon particles (current efficiency = 95%), wherein the sulfonic acid-containing silver plating solution was prepared by adding a carbon particle dispersion (containing 24 wt% carbon, a small amount of silicate, a dispersant and a thickener) (PROHITE S-2 manufactured by Nippon Graphite Industries, Ltd.) in which graphite particles with an average particle size of 2 um were dispersed in water as carbon particles, to the same sulfonic acid-containing silver plating solution as in Example 1, and a composite plated product was manufactured by the same method as in Example 1 except that the above was performed.

[0039] The thickness of the composite plated film of the composite plated article thus obtained was measured by the same method as in Example 1. As a result, the thickness was 5.8 μm.

[0040] For the obtained composite plated product, the area percentage (area ratio) of carbon particles on the surface of the composite plated film was calculated by the same method as in Example 1. As a result, the percentage (area ratio) was 79 area%. The surface of the composite plated film was gray, and no uneven appearance was observed thereon, so the appearance of the composite plated film was good. The surface analysis of the composite plated film was also performed by the same method as in Example 1. As a result, it was found that the composite plated film contained 0.2% by weight of Si.

[0041] The wear resistance of the composite plated product was evaluated by a sliding wear test in the same manner as in Example 1. As a result, it was found that after 10,000 reciprocating slidings, the substrate was not exposed and the thickness of the composite plated film was 4.6 μm, which showed that the wear resistance was good. The dynamic friction coefficient between the plate-like test piece and the indentation test piece was also calculated in the same manner as in Example 1. As a result, the dynamic friction coefficient was 0.21.

[0042] Example 4

[0043] A 0.3 mm thick tough pitch copper (C1100H) plate was prepared as a substrate, and the substrate and a nickel electrode plate were used as a cathode and an anode, respectively. The nickel plating bath contained 80 g / L nickel sulfamate and 45 g / L boric acid at a liquid temperature of 45°C and a temperature of 4 A / dm 2 The substrate was electroplated (nickel-plated) at a current density of 1.0 for 140 seconds while stirring the nickel plating bath to form a nickel plating film with a thickness of 1.0 mm on the substrate, and then silver underplating and electroplating (silver plating) were performed in the same manner as in Example 1. A composite plated product was prepared by the same method as in Example 1 except that the above method and the nickel plating bath were stirred.

[0044] The thickness of the composite plated film of the composite plated article thus obtained was measured by the same method as in Example 1. As a result, the thickness was 5.1 μm.

[0045] For the obtained composite plated product, the area percentage (area ratio) of carbon particles on the surface of the composite plated film was calculated by the same method as in Example 1. As a result, the percentage (area ratio) was 57 area%. The surface of the composite plated film was gray, and no uneven appearance was observed thereon, so the appearance of the composite plated film was good. The surface analysis of the composite plated film was also performed by the same method as in Example 1. As a result, it was found that the composite plated film contained 0.2 weight % of Si.

[0046] The wear resistance of the composite plated product was evaluated by a sliding wear test in the same manner as in Example 1. As a result, it was found that after 10,000 reciprocating slidings, the substrate was not exposed and the thickness of the composite plated film was 4.1 μm, which showed that the wear resistance was good. The dynamic friction coefficient between the plate-like test piece and the indentation test piece was also calculated in the same manner as in Example 1. As a result, the dynamic friction coefficient was 0.35.

[0047] Comparative Example 1

[0048] The substrate was electroplated (silver-plated) in a silver plating solution containing sulfonic acid containing 80 g / L of hydrophobic carbon particles (current efficiency = 95%), wherein the silver plating solution containing sulfonic acid was prepared by adding hydrophobic dry carbon particles (SN-5 manufactured by SEC Carbon Co., Ltd.) having an average particle size of 5 um instead of the carbon particle dispersion to the same silver plating solution containing sulfonic acid as in Example 1 until the concentration of the carbon particles was 80 g / L, and otherwise a composite plated product was manufactured by the same method as in Example 1.

[0049] The thickness of the composite plated film of the composite plated article thus obtained was measured by the same method as in Example 1. As a result, the thickness was 5.5 μm.

[0050] For the obtained composite plated product, the area percentage (area ratio) of carbon particles on the surface of the composite plated film was calculated by the same method as in Example 1. As a result, the percentage (area ratio) was 8 area%. The surface of the composite plated film was light white, and no uneven appearance was observed thereon. The surface analysis of the composite plated film was also performed by the same method as in Example 1. As a result, it was found that the Si content in the composite plated film was 0 weight %.

[0051] The wear resistance of the composite plated product was evaluated by a sliding wear test in the same manner as in Example 1. As a result, it was found that after 10,000 reciprocating slidings were repeated, the substrate was exposed and the thickness of the composite plated film was 0 μm, which showed that the wear resistance was poor. The dynamic friction coefficient between the plate-like test piece and the indentation test piece was also calculated in the same manner as in Example 1. As a result, the dynamic friction coefficient was 1.10.

[0052] Comparative Example 2

[0053] The substrate was electroplated (silver base plating) with a cyanide-containing silver plating solution containing 3 g / L potassium silver cyanide and 100 g / L potassium cyanide instead of the silver base plating solution containing sulfonic acid, and the substrate was electroplated (silver plating) with a cyanide-containing silver plating solution containing 100 g / L potassium silver cyanide, 120 g / L potassium cyanide and 4 mg / L potassium selenocyanate instead of the silver plating solution containing sulfonic acid (current efficiency = 95%). The composite plated product was manufactured by the same method as in Example 1, except that

[0054] The thickness of the composite plated film of the composite plated article thus obtained was measured by the same method as in Example 1. As a result, the thickness was 5.6 μm.

[0055] For the obtained composite plated product, the area percentage (area ratio) of carbon particles on the surface of the composite plated film was calculated by the same method as in Example 1. As a result, the percentage (area ratio) was 0 area%. The surface of the composite plated film was a glossy whitish silver color, and no uneven appearance was observed thereon. The surface analysis of the composite plated film was also performed by the same method as in Example 1. As a result, it was found that the Si content in the composite plated film was 0 weight %.

[0056] The wear resistance of the composite plated product was evaluated by a sliding wear test in the same manner as in Example 1. As a result, it was found that after 10,000 reciprocating slidings were repeated, the substrate was exposed and the thickness of the composite plated film was 0 μm, which showed that the wear resistance was poor. The dynamic friction coefficient between the plate-like test piece and the indentation test piece was also calculated in the same manner as in Example 1. As a result, the dynamic friction coefficient was 1.20.

[0057] The production conditions and properties of the composite plated products in these Examples and Comparative Examples are shown in Tables 1 to 3.

[0058] Table 1

[0059]

[0060] Table 2

[0061]

[0062] Table 3

[0063]

Claims

1. A method for manufacturing a composite plated product, the method comprising the following steps: preparing a carbon particle dispersion in which carbon particles are dispersed; adding a dispersion of carbon particles containing silicate to a silver plating solution containing sulfonic acid; as well as The substrate is electroplated using a silver plating solution containing sulfonic acid to which a carbon particle dispersion solution is added, thereby forming a composite plating film having a composite material containing carbon particles in a silver layer on the substrate.

2. The method for manufacturing a composite plated product according to claim 1, wherein: The carbon particles are graphite particles with an average particle size of 1 to 15 μm.

3. The method for manufacturing a composite plated product according to claim 1, wherein: The amount of the carbon particles added to the silver plating solution containing sulfonic acid is in the range of 10 g / L to 100 g / L.

4. The method for manufacturing a composite plated product according to claim 1, wherein: The electroplating is carried out at 1 to 20 A / dm 2 The current density is carried out.

5. The method for manufacturing a composite plated product according to claim 1, wherein: The substrate is made of copper or a copper alloy.

6. The method for manufacturing a composite plated product according to claim 1, wherein: Before the step of forming the composite plated film of the composite material, the method further includes the step of forming a nickel plated film on the substrate.

7. A composite plated product comprising: substrate, and A composite coating of a composite material containing carbon particles formed in a silver layer on a substrate, wherein the silicon content in the composite coating is in the range of 0.01 wt% to 1 wt%, and the average particle size of the carbon particles is 2 to 15 μm; Wherein, the area percentage of the carbon particles on the surface of the composite coating is in the range of 30 area % to 90 area %.

8. The composite plated product according to claim 7, characterized in that: The composite coating has a thickness of 0.5 to 20 μm.

9. The composite plated product according to claim 7, characterized in that: Also included is a nickel plating film formed between the composite plating film and the substrate.

Citation Information

Patent Citations

  • Dispersion plating method

    JP1991253598A

  • Method for forming silver-graphite dispersion coating

    JP1993505853A

  • Sliding contact of electric equipment

    JP1997007445A

  • Composite plated material and method for producing same

    JP2006037225A

  • Method for dry-etching substrate

    JP2007016261A