Method for preparing adhesive products by single-sided gluing
By using the single-side gluing method of polar organic solvents and polyisocyanate in the shoemaking industry, the problems of high labor costs and low production efficiency in the shoemaking industry are solved, and good bonding strength and heat resistance of the bonded products are achieved. properties and hydrolysis resistance, suitable for footwear production.
Patent Information
- Application Number
- CN201910256330.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-03-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-03-29
AI Technical Summary
The shoemaking industry faces problems such as high labor costs, complex gluing processes, and low production efficiency. The existing single-sided gluing process is difficult to achieve good bonding strength, heat resistance, and hydrolysis resistance.
Using a single-side sizing method containing polar organic solvents and polyisocyanates, the cleaning agent and adhesive are applied to the surface of the substrate and dried before contact is made, thereby forming a product with good bonding strength, heat resistance and hydrolysis resistance. adhesive products.
While improving production efficiency and reducing labor costs, it also obtains good initial bonding strength, final bonding strength, heat resistance and hydrolysis resistance, and is suitable for footwear production.
Smart Images

Figure CN111746074B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a bonded product by gluing one side of the product, the bonded product prepared by the method and the application of the bonded product in the production of shoes. Background Art
[0002] The traditional process of bonding shoe materials in the shoemaking industry is a double-sided gluing process, that is, adhesive is applied to the sole, upper, midsole, and outsole of the shoe, and the midsole, outsole, and upper of the shoe often need to be cleaned and primed before applying adhesive. For example, CN1235966C discloses a laminate comprising a foamed product layer and a polyolefin material layer, and the bonding of the laminate adopts a double-sided gluing method. However, since the shoemaking industry faces the problems of high labor costs, complicated gluing procedures, and low production efficiency, the shoemaking industry hopes to find a simplified shoemaking process.
[0003] The single-sided gluing process reduces the number of gluing steps, saves labor, improves production efficiency, and avoids adhesive contamination of the shoe surface. Therefore, it is widely welcomed in the shoemaking industry. The difficulty of the single-sided gluing process lies in finding a suitable substrate treatment agent and adhesive.
[0004] Hot melt adhesives can be used in single-sided gluing processes, but their application in the shoemaking industry is limited due to their poor initial performance and high equipment costs. The industry has also tried to use water-based polyurethane dispersion adhesives for single-sided gluing processes.
[0005] CN1098154C discloses a method for preparing a laminated product by injection molding, wherein a primer comprising an organic solvent and an ethylene or propylene polymer grafted with an unsaturated carboxylic acid or its anhydride, ester, amide, imide or metal salt is applied to a substrate, and the ethylene or propylene polymer is injection molded onto the substrate coated with the primer. This method is not suitable for coating processes.
[0006] CN107802056A discloses a method for making shoes by applying powder glue to one side. The powder glue used in the method comprises common polyurethane resin and polyamide resin, and the mechanical properties of the shoe material made by the single-side glue are far different from those of the shoe material made by the double-side glue.
[0007] Therefore, the industry hopes to develop a single-sided gluing method whose product can have good bonding strength, heat resistance and hydrolysis resistance. Summary of the invention
[0008] The purpose of the present invention is to provide a method for preparing a bonded product by applying a single-sided glue, the bonded product prepared by the method and the application of the bonded product in the production of footwear.
[0009] A method for preparing an adhesive product by single-sided gluing according to the present invention comprises the following steps:
[0010] a. applying a cleaning agent to at least one surface of a first substrate, and drying the surface of the first substrate to which the cleaning agent is applied;
[0011] b. applying an adhesive to at least one surface of a second substrate, drying the surface of the second substrate to which the adhesive is applied; and
[0012] c. contacting the surface of the first substrate treated in step a with the surface of the second substrate treated in step b to obtain the bonded product;
[0013] The cleaning agent comprises a polar organic solvent and polyisocyanate; the polar organic solvent has a boiling point not higher than 135° C. and is non-reactive with isocyanate; the polyisocyanate conforms to the general formula R(NCO): n , wherein R is one or more of the following: an aliphatic hydrocarbon group containing 2 to 18 carbon atoms, an aromatic hydrocarbon group containing 6 to 15 carbon atoms, and an aromatic aliphatic hydrocarbon group containing 8 to 15 carbon atoms, and n is not less than 2; the weight of the isocyanate group of the polyisocyanate accounts for 0.005% to 6% by weight of the detergent.
[0014] According to one aspect of the present invention, a bonding product prepared according to the method provided by the present invention is provided.
[0015] According to a further aspect of the present invention, there is provided use of the bonding article provided according to the present invention in the production of footwear.
[0016] The adhesive product obtained by the single-sided gluing method of the present invention has good initial bonding strength, final bonding strength, heat resistance and hydrolysis resistance. DETAILED DESCRIPTION
[0017] The present invention provides a method for preparing an adhesive product by applying a single-sided adhesive, comprising the following steps: a. applying a cleaning agent to at least one surface of a first substrate, and drying the first substrate surface to which the cleaning agent is applied; b. applying an adhesive to at least one surface of a second substrate, and drying the second substrate surface to which the adhesive is applied; and c. contacting the first substrate surface treated in step a with the second substrate surface treated in step b to obtain the adhesive product; wherein the polar organic solvent has a boiling point of not higher than 135° C. and is isocyanate non-reactive; the polyisocyanate conforms to the general formula R(NCO): n, wherein R is one or more of the following: an aliphatic hydrocarbon group containing 2 to 18 carbon atoms, an aromatic hydrocarbon group containing 6 to 15 carbon atoms, and an aromatic aliphatic hydrocarbon group containing 8 to 15 carbon atoms, and n is not less than 2; the weight of the isocyanate group of the polyisocyanate accounts for 0.005 wt% to 6 wt% of the weight of the detergent. The present invention also provides an adhesive product prepared by the method and the use of the adhesive product in footwear production.
[0018] The description of “first” and “second” in the first substrate and the second substrate of the present invention is only for the convenience of describing the two substrates, and is not used to distinguish the order of the substrates.
[0019] The first substrate and the second substrate of the present invention may be the same or different.
[0020] There is no particular order for step a and step b, and they can be performed simultaneously, or step a can be performed first and then step b, or step b can be performed first and then step a.
[0021] Cleaning Agents
[0022] Preferably, the weight of the isocyanate groups of the polyisocyanate is 0.007 wt %-5.6 wt %, further preferably 0.01 wt %-4.5 wt %, further preferably 0.01 wt %-0.5 wt %, further preferably 0.02 wt %-0.2 wt %, more preferably 0.02 wt %-0.085 wt %, most preferably 0.04 wt %-0.085 wt %, based on the weight of the cleaning agent.
[0023] The polar organic solvent of the present invention refers to a solvent whose solvent molecules are polar molecules.
[0024] The boiling point of the polar organic solvent is preferably 35-135°C.
[0025] The polar organic solvent is preferably one or more of acetone, methyl ethyl ketone, ethyl acetate or butyl acetate, a mixture of butyl acetate, cyclohexane and methyl ethyl ketone, a mixture of methyl ethyl ketone and propylene glycol diacetate, or a mixture of butyl acetate, methyl ethyl ketone and propylene glycol methyl ether acetate.
[0026] The polar solvent is further preferably a mixture of methyl ethyl ketone and ethyl acetate, a mixture of methyl ethyl ketone and butyl acetate, a mixture of methyl ethyl ketone and propylene glycol diacetate, a mixture of acetone and butyl acetate, a mixture of ethyl acetate and butyl acetate, a mixture of ethyl acetate, butyl acetate and methyl ethyl ketone, a mixture of butyl acetate, cyclohexane and methyl ethyl ketone, a mixture of butyl acetate, methyl ethyl ketone and propylene glycol methyl ether acetate, methyl ethyl ketone or butyl acetate.
[0027] The polar solvent is most preferably methyl ethyl ketone.
[0028] The general formula R(NCO) n , wherein n is preferably 2.5-5.5, most preferably 2.5-4.
[0029] The polyisocyanate is preferably one or more of the following: derivatives of aliphatic polyisocyanates having allophanate, biuret, uretdione, isocyanurate and / or iminooxadiazinedione groups, derivatives of aromatic polyisocyanates having allophanate, biuret, uretdione, isocyanurate and / or iminooxadiazinedione groups, and derivatives of alicyclic polyisocyanates having allophanate, biuret, uretdione, isocyanurate and / or iminooxadiazinedione groups, and one or more of the following are further preferred: derivatives of aliphatic polyisocyanates having allophanate and / or isocyanurate groups, Derivatives of alicyclic polyisocyanates having allophanate and / or isocyanurate groups, and aromatic derivatives having allophanate and / or isocyanurate groups, preferably one or more of the following: toluene diisocyanate trimer, prepolymer of toluene diisocyanate and diphenylmethane diisocyanate, hexamethylene diisocyanate trimer, isophorone diisocyanate trimer, prepolymer of diphenylmethane diisocyanate and tris(p-isocyanatephenyl)phosphorothioate, most preferably one or more of the following: prepolymer of toluene diisocyanate and diphenylmethane diisocyanate, and toluene diisocyanate trimer.
[0030] The solid content of the polyisocyanate is preferably 25% by weight to 100% by weight, based on 100% by weight of the polyisocyanate.
[0031] The viscosity of the polyisocyanate is preferably 3 mPa·s-5500 mPa·s, most preferably 3 mPa·s-2200 mPa·s, according to DIN EN ISO 3219:1994-10 at 23° C. and a shear rate of 10 s -1 Next determination.
[0032] The NCO group content of the polyisocyanate is preferably 4.5% to 24% by weight, most preferably 4.5% to 14% by weight, determined by volume in accordance with DIN-EN ISO 11909:2007-05, the determined data including the free and potentially free NCO content.
[0033] The isocyanate functionality of the polyisocyanate is preferably 2-5.
[0034] The number average molecular weight of the polyisocyanate is preferably 380 g / mol-1560 g / mol, and is measured at 23° C. using gel permeation chromatography according to DIN 55672-1:2016-03 with tetrahydrofuran as the mobile phase and against a polystyrene standard.
[0035] The cleaning agent comprises a polar organic solvent and a polyisocyanate, wherein the polar organic solvent is preferably a mixture of methyl ethyl ketone and ethyl acetate, a mixture of methyl ethyl ketone and butyl acetate, a mixture of methyl ethyl ketone and propylene glycol diacetate, a mixture of acetone and butyl acetate, a mixture of ethyl acetate and butyl acetate, a mixture of ethyl acetate, butyl acetate and methyl ethyl ketone, a mixture of butyl acetate, cyclohexane and methyl ethyl ketone, a mixture of butyl acetate, methyl ethyl ketone and propylene glycol methyl ether acetate, Methyl ethyl ketone or butyl acetate; the polyisocyanate is preferably one or more of the following: toluene diisocyanate trimer, a prepolymer of toluene diisocyanate and diphenylmethane diisocyanate, hexamethylene diisocyanate trimer, isophorone diisocyanate trimer, a prepolymer of diphenylmethane diisocyanate and tris(p-isocyanate phenyl ester) of thiophosphoric acid; the weight of the isocyanate group of the polyisocyanate accounts for 0.005% to 6% by weight of the weight of the detergent.
[0036] The cleaner most preferably comprises methyl ethyl ketone and a polyisocyanate having an isocyanate functionality of 2.5-4, the polyisocyanate being one or more of the following: a prepolymer of toluene diisocyanate and diphenylmethane diisocyanate, and a trimer of toluene diisocyanate, the isocyanate groups of the polyisocyanate accounting for 0.04 wt % to 0.085 wt % of the weight of the cleaner.
[0037] The cleaning agent does not contain a binder.
[0038] The polar solvent and polyisocyanate of the present invention may be stored separately or may be pre-mixed and exist in the form of a polyisocyanate solution.
[0039] First substrate
[0040] The first substrate is commonly used in the art, especially materials that can be used for midsoles, uppers and toes. The first substrate is preferably one or more of the following: polyurethane-based materials and polyvinyl chloride-based materials, and polyurethane-based synthetic leather is most preferred.
[0041] Adhesives
[0042] The adhesive may be a one-component adhesive, a two-component adhesive or a three-component adhesive commonly used in the art.
[0043] The adhesive is preferably one or more of the following: solvent-based polyurethane, solvent-based polychloroprene rubber, water-based polyurethane dispersion, water-based polychloroprene rubber and hot-melt adhesive polyurethane, more preferably water-based polyurethane dispersion, most preferably two-component water-based polyurethane dispersion.
[0044] The two-component aqueous polyurethane dispersion preferably comprises an aqueous polyurethane dispersion and an isocyanate curing agent.
[0045] Second substrate
[0046] The second substrate is commonly used in the art, especially materials that can be used for midsoles, uppers and toes. The second substrate is preferably one or more of the following: polyurethane-based materials and polyvinyl chloride-based materials, and polyurethane-based synthetic leather is most preferred.
[0047] Pretreatment of the second substrate
[0048] Preferably, the second substrate is pretreated before applying the adhesive, comprising the following steps:
[0049] i. polishing or cleaning the second substrate; and
[0050] ii. applying a primer to the second substrate treated in step i.
[0051] The grinding is used to improve the surface roughness of the substrate. The grinding can be mechanical grinding.
[0052] The cleaning is to remove oil or dust on the surface of the substrate using a solvent, and the solvent is well known to those skilled in the art.
[0053] The primer may be a commonly used primer in the art, including but not limited to TCI coating, UV coating, solvent-based polyurethane coating or water-based polyurethane dispersion coating.
[0054] Application
[0055] The applying may be applying the cleaning agent or adhesive to the entire surface of the substrate or only to one or more portions of the surface of the substrate.
[0056] The application may be by brushing, dipping, spraying, rolling, knife coating, flow coating, pouring, printing or transfer, preferably by brushing, dipping or spraying.
[0057] dry
[0058] Drying the first substrate surface to which the cleaning agent is applied and drying the second substrate surface to which the adhesive is applied may refer to drying only the substrate surface, or may refer to drying a portion of the substrate or the entire substrate including the substrate surface to which the cleaning agent or adhesive is applied.
[0059] The drying may remove volatile components. The volatile components may be water.
[0060] The drying is preferably one or more of the following: infrared heat radiation, near infrared heat radiation, microwaves, and using a convection oven or a spray dryer under elevated temperature conditions.
[0061] The drying temperature is as high as possible, but should not be higher than a temperature limit at which the substrate deforms in an uncontrolled manner or suffers other damage.
[0062] touch
[0063] Preferably, before step c, the surface of the second substrate on which the adhesive is applied, which has been treated in step b, is thermally activated at a temperature of 45-75°C.
[0064] The thermal activation can be oven activation or infrared activation.
[0065] The contact is preferably performed before the temperature of the surface of the second substrate drops below the bonding temperature of the adhesive, and more preferably performed before the temperature of the surface of the second substrate is not less than 60°C.
[0066] The first substrate is not treated with an adhesive before contacting the second substrate.
[0067] Adhesive products
[0068] The bonded article is preferably footwear. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] The present invention will be described and explained in more detail below in conjunction with the accompanying drawings, in which:
[0070] Figure 1 is a schematic diagram of sample bonding.
[0071] Figure 2 It is a schematic diagram of the heat resistance or hydrolysis resistance test of the sample.
[0072] Example
[0073] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention belongs. When the definition of a term in this specification conflicts with the meaning commonly understood by those skilled in the art to which the invention belongs, the definition described in this article shall prevail.
[0074] Unless otherwise indicated, all numerical values expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.
[0075] As used herein, "and / or" means one or all of the mentioned elements.
[0076] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.
[0077] All percentages in the present invention are by weight, unless otherwise specified.
[0078] The analytical measurements of the present invention were all carried out at 23±2°C unless otherwise stated.
[0079] The isocyanate group (NCO) content of the polyisocyanates is stated in % by weight, determined by volume in accordance with DIN-EN ISO 11909:2007-05, the determined data comprising the free and potentially free NCO content.
[0080] The number average molecular weight of polyisocyanate was determined by gel permeation chromatography according to DIN 55672-1: 2016-03 with tetrahydrofuran as the mobile phase and compared with a polystyrene standard at 23°C.
[0081] The non-volatile content of polyisocyanate is expressed in weight % and is tested according to DIN EN ISO 3251:2008-06 at 120° C., the test time is 2 hours, the test pan diameter is 75 mm, and the test sample weight is 2.00 g±0.02.
[0082] The isocyanate functionality of polyisocyanates is calculated as follows:
[0083] Isocyanate functionality of polyisocyanate = (number average molecular weight of polyisocyanate*isocyanate group content of polyisocyanate) / (42*non-volatile content of polyisocyanate).
[0084] Materials and reagents
[0085] Polyester I: 1,4-butanediol polyadipate diol, OH value=50.
[0086] Polyester II: polyester diol composed of 1,6-hexanediol, neopentyl glycol and adipic acid, OH value=66.
[0087] H: 1,6-hexamethylene diisocyanate, available from Bayer MaterialScience AG, Germany.
[0088] I: isophorone diisocyanate, available from Bayer MaterialScience AG, Germany.
[0089] Desmodur DN: an aliphatic trimer based on hexamethylene diisocyanate (HDI), with an isocyanate group content of 21.8 wt %, a viscosity of about 1250 mPa·s (23° C.), 100 wt % solid content, an isocyanate functionality of 3.4, and a number average molecular weight of 650 g / mol. It can be purchased from Covestro AG, Germany.
[0090] Bayhydur XP 2655: an aliphatic trimer based on HDI, with an NCO group content of 20.8% by weight, a viscosity of about 3500 mPa·s (23° C.), 100% by weight solids, an isocyanate functionality of 3.2, and a number average molecular weight of 700 g / mol. It can be purchased from Covestro AG.
[0091] Desmodur N 3300: an aliphatic trimer based on HDI, 100 wt% solid content, an NCO group content of 21.7 wt%, a viscosity of about 3000 mPa·s (23° C.), an isocyanate functionality of 3.5, and a number average molecular weight of 680 g / mol, available from Covestro AG.
[0092] Bayhydur 401-60PGDA: an aliphatic trimer based on isophorone diisocyanate (IPDI), 60 wt% solid content dissolved in propylene glycol diacetate (PGDA), NCO group content of 8.5 wt%, viscosity of about 1100 mPa·s (23°C), isocyanate functionality of 2.9, number average molecular weight of 900 g / mol, available from Covestro AG.
[0093] Desmodur E 21: reaction product of aliphatic polyether polyol and diphenylmethane diisocyanate (MDI), 100 wt% solid content, NCO group content of 16.0 wt%, isocyanate functionality of about 2.8, viscosity of about 5400 mPa·s (23° C.), number average molecular weight of 720 g / mol, available from Covestro AG.
[0094] Desmodur E 29: reaction product of aliphatic polyether polyol and MDI, 100 wt% solid content, NCO group content of 24.0 wt%, isocyanate functionality of about 2.2, viscosity of about 220 mPa·s (23° C.), number average molecular weight of 380 g / mol, available from Covestro AG.
[0095] Desmodur E XP 2605 / 1: reaction product of aliphatic polyether polyol and TDI / MDI, 50 wt% solid content dissolved in butyl acetate, NCO group content of 4.5 wt%, isocyanate functionality of about 3.3, viscosity of about 350 mPa·s (23°C), number average molecular weight of 1560 g / mol, available from Covestro AG.
[0096] Desmodur IL 1351BA: an aromatic trimer based on toluene diisocyanate (TDI), 51 wt% solids dissolved in butyl acetate, NCO group content of 8.0 wt%, isocyanate functionality of about 4.5, viscosity of about 1300 mPa·s (23°C), number average molecular weight of 1280 g / mol, available from Covestro AG.
[0097] Desmodur IL 1451BA: an aromatic trimer based on TDI, 51 wt% solid content dissolved in butyl acetate, NCO group content of 7.4 wt%, isocyanate functionality of about 4.8, viscosity of about 250 mPa·s (23°C), number average molecular weight of 1290 g / mol, available from Covestro AG.
[0098] Desmodur RC: an aromatic trimer based on TDI, 35 wt% solid content dissolved in ethyl acetate, NCO group content of 7.0 wt%, isocyanate functionality of about 2.6, viscosity of about 3 mPa·s (23°C), number average molecular weight of 540 g / mol, available from Covestro AG.
[0099] Desmodur L75: an aromatic trimer based on TDI, 75 wt% solid content dissolved in ethyl acetate, NCO group content of 13.3 wt%, isocyanate functionality of about 2.7, viscosity of about 1600 mPa·s (23°C), number average molecular weight of 830 g / mol, available from Covestro AG.
[0100] Desmodur HL BA: a mixture of an aromatic trimer based on TDI and an aliphatic trimer based on HDI, 60 wt% solid content dissolved in butyl acetate, NCO group content of 10.5 wt%, isocyanate functionality of about 4.4, viscosity of about 2200 mPa·s (23°C), number average molecular weight of 1200 g / mol, available from Covestro AG.
[0101] Desmodur VP LS 2394: a mixture of an aromatic trimer based on TDI and an aliphatic trimer based on HDI, 60 wt% solid content dissolved in butyl acetate, NCO group content of 10.0 wt%, isocyanate functionality of about 4.7, viscosity of about 170 mPa·s (23°C), number average molecular weight of 1200 g / mol, available from Covestro AG.
[0102] Desmodur RN: a mixture of an aromatic trimer based on TDI and an aliphatic trimer based on HDI, 40 wt% solid content dissolved in ethyl acetate, NCO group content of 7.2 wt%, isocyanate functionality of about 4.0, viscosity of about 11 mPa·s (23°C), number average molecular weight of 940 g / mol, available from Covestro AG.
[0103] Desmodur RFE: tris(p-isocyanatephenyl)phosphorothioate, 27 wt% solid content dissolved in ethyl acetate, NCO group content of 7.2 wt%, isocyanate functionality of about 3.0, viscosity of about 3 mPa·s (23° C.), number average molecular weight of 465 g / mol, available from Covestro AG.
[0104] Dispercoll U58 / 1: anionic waterborne polyurethane dispersion with a solid content of 50±1%, available from German Polymer (China) Co., Ltd.
[0105] Dispercoll U54: anionic waterborne polyurethane dispersion with a solid content of 50±1%, available from German Polymer (China) Co., Ltd.
[0106] Desmodur XP 2802: 40 wt% solid content, hydrophilically modified polycarbodiimide, the melting point temperature of the solid component is 23.16°C, the carbodiimide functional group content is 1 mmol / g, the number average molecular weight is 1779, the weight average molecular weight is 3258, and the carbodiimide functional group functionality is 4.5, purchased from Covestro AG.
[0107] Z 2589: 100 wt% solid content, glass transition temperature 67.75°C, melting point of solid component greater than 200°C, isocyanate functionality not less than 3, particle size d50 about 1.5 μm, isophorone diisocyanate (IPDI) trimer, reaction or viscosity increasing temperature 70°C-120°C, purchased from Covestro AG.
[0108] T403: polyetheramine, purchased from Huntsman.
[0109] Tamol NN 4501: dispersant, available from BASF.
[0110] Emulvin WA: emulsifier, concentration 15 wt%, purchased from LANXESS.
[0111] MEK: methyl ethyl ketone, purchased from Yonghua Chemical Technology (Jiangsu) Co., Ltd.
[0112] MPA: Propylene glycol methyl ether acetate, purchased from Shanghai Lingfeng Chemical Reagent Co., Ltd.
[0113] Black rubber: Sole rubber made of nitrile rubber, which can be purchased from Dongguan Wantai Rubber Co., Ltd.
[0114] PVC leather: used as shoe upper, can be purchased from Shanghai Degui Trading Co., Ltd.
[0115] Borchigel L75N: thickener, purchased from OMG.
[0116] Borchigel ALA: thickener, 50 wt% in deionized water, purchased from OMG.
[0117] Preparation of adhesive 1
[0118] 99.2 wt % of Dispercoll U58 / 1 and 0.8 wt % of 25% strength Borchigel L75N were mixed to a viscosity of about 5000 mPa·s, and after stirring for 10 minutes, 3 wt % to 5 wt % of Desmodur DN was added and stirring was continued for 10 minutes to obtain Adhesive 1.
[0119] Preparation of adhesive 2
[0120] 98.7 wt % of Dispercoll U54 and 1.3 wt % of 25% strength Borchigel L75N were mixed to a viscosity of about 5000 mPa·s, and after stirring for 10 minutes, 3 wt % to 5 wt % of Desmodur DN was added and stirring was continued for 10 minutes to obtain Adhesive 2.
[0121] Preparation of adhesive 3
[0122] 2.58g T403, 0.82g Tamol NN 4501 and 0.59g Emulvin WA were added to 110.19g deionized water and mixed at 1000rpm for 10-15 minutes; then 78.55g Z 2589 was slowly added thereto and stirred for 30 minutes to 1 hour to prepare a premix for use. Then 100 g of Dispercoll U58 / 1 and 2 g of Desmodur XP 2802 were stirred and mixed at a speed of 1000 rpm for 10-15 minutes, and then 16.25 g of the above premix was added thereto, and after stirring and mixing for another 10-15 minutes, about 1.80 g of Borchigel ALA was added to adjust the viscosity to about 5000 mPa·s to obtain adhesive 3.
[0123] Preparation of adhesive 4
[0124] 450 g of polyester I and 42.5 g of polyester II were dehydrated at 110° C., 100 mbar for 1 hour, 2.25 g of 1,4-butanediol were added and the mixture was cooled while stirring. 37.84 g of H, then add 25g I, the mixture was stirred at 80-90°C until the isocyanate content reached 1.3%. The reaction mixture was dissolved in 840g of acetone and cooled to 50°C. A solution of 5.6g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 2.4g of diethanolamine and 0.8g of hydroxyethylethylenediamine in 656g of water was added to the reaction mixture solution and stirred vigorously for 30 minutes, 510g of water was added to disperse the mixture, and the acetone was then separated by distillation to obtain an aqueous polyurethane dispersion. The aqueous polyurethane urea dispersion and 1.0% by weight of Borchigel L75N with a concentration of 25% based on the weight of the adhesive were mixed to a viscosity of about 5000mPa·s, and after stirring for 10 minutes, 3% by weight to 5% by weight of Desmodur DN were added and stirring was continued for 10 minutes to obtain adhesive 4.
[0125] PU synthetic leather (first base material)
[0126] According to the amount of each component in Table 1, the components were mixed and manually stirred for 5-10 minutes to obtain a cleaning agent. The surface of the PU synthetic leather (2 cm wide and 8 cm long) to be bonded was cleaned with the fiber containing the cleaning agent, gently patted several times, and then dried in an oven at a temperature of 60° C. for 3 minutes for standby use.
[0127] Black rubber (second base material)
[0128] The polished black rubber (2 cm wide, 8 cm long) surface to be bonded was cleaned with a fiber containing methyl ethyl ketone, and the cleaned black rubber surface was exposed in a fume hood until the cleaned surface was dry, and 2% trichloroisocyanuric acid dissolved in ethyl acetate was applied to the surface, followed by drying in an oven at a temperature of 50°C for 3 minutes, and then the adhesive shown in Table 1 was applied to the black rubber surface using a fine brush, and the coating amount was 120 g / m 2 (Wet). Finally, the black rubber surface coated with the adhesive was dried in a circulating air oven at 60°C until the moisture in the adhesive film was completely removed and then used.
[0129] Performance Testing
[0130] Bond strength test
[0131] The pretreated black rubber surface was heated to 60°C, and then the pretreated black rubber and the treated PU synthetic leather were quickly laminated using a flat press (Rongtai, China) at a pressure of 4 bar. Figure 1 As shown, and maintain for 30 seconds to obtain a sample of the bonded product. According to DIN EN 1392, the bonding strength of the sample was tested using a tensile testing machine model BZ2.5 / TN1S from ZWICK. The unbonded parts of the black rubber and PU synthetic leather were clamped in the upper and lower clamps of the tensile testing machine respectively. The bonded surfaces of the black rubber and PU synthetic leather were tested to present a 180° peeling mode at a tensile rate of 100 mm / min and a tensile length of 50 mm. The tensile force used at this time was recorded as the bonding strength, and the results are listed in Table 1. The initial bonding strength (tested 30 minutes after bonding) should not be less than 3N / mm, and the final bonding strength (tested 24 hours after bonding) should not be less than 5N / mm. The greater the bonding strength obtained by the test, the greater the bonding force between the substrates and the stronger the bonding of the substrates.
[0132] Heat resistance test
[0133] The pretreated black rubber surface was heated to 60°C, and then the pretreated black rubber and the treated PU synthetic leather were quickly laminated using a flat press (Rongtai, China) at a pressure of 4 bar. Figure 1 The sample was placed at room temperature for 24 hours, and then loaded with a 1000 g weight at 80°C and maintained for 60 minutes. Figure 2As shown, record the distance of the sample being pulled apart after being kept at 80°C for 60 minutes. If the coating cannot be maintained for 60 minutes, that is, it is completely debonded, then record the time of the coating being completely debonded. The results are shown in Table 1. The distance of pulling apart is the length of separation of the sample's bonding parts measured with a ruler. The longer the distance of pulling apart, the worse the heat resistance of the sample. Complete debonding means that the bonding parts of the sample are completely separated. If the sample is completely debonded, it is considered that the sample has failed the heat resistance test. The distance of pulling apart should be less than 12mm.
[0134] Hydrolysis resistance test
[0135] The pretreated black rubber surface was heated to 60°C, and then the pretreated black rubber and the treated PU synthetic leather were quickly laminated using a flat press (Rongtai, China) at a pressure of 4 bar. Figure 1 The sample was placed at room temperature for 72 hours, and then loaded with a 1000 g weight and kept at 70°C and 95% relative humidity for 3 days. Figure 2 As shown, the time of full degumming was recorded, and the results are shown in Table 1.
[0136] Full degumming means that the bonding parts of the sample are completely separated. The shorter the full degumming time, the worse the hydrolysis resistance of the sample. The full degumming time should not be less than 32 hours.
[0137] Examples 1-69 and Comparative Examples 1-16
[0138] Table 1 lists the components and sample test results of Examples 1-69 and Comparative Examples 1-16.
[0139]
[0140]
[0141]
[0142]
[0143]
[0144]
[0145] The initial bonding strength of the bonded products of Examples 1-69 is higher than 3N / mm, the final bonding strength is higher than 5N / mm, the pulling distance is less than 12mm, and the full debonding time is no less than 32 hours. Therefore, the bonded products obtained by the single-sided gluing method of Examples 1-69 have good bonding strength, heat resistance and hydrolysis resistance, that is, have good mechanical properties.
[0146] It can be seen from Comparative Examples 1 and 7-16 that when the proportion of the isocyanate group of the polyisocyanate in the cleaner is less than 0.005 wt % of the weight of the cleaner, the bonded product obtained by the single-sided gluing method cannot have mechanical properties such as bonding strength, heat resistance and hydrolysis resistance, and cannot meet industry requirements.
[0147] It can be seen from Comparative Examples 2-6 that when the proportion of isocyanate groups of polyisocyanate to the weight of the cleaning agent exceeds 6 weight %, the bonded product obtained by the single-sided gluing method cannot have mechanical properties such as bonding strength, heat resistance and hydrolysis resistance, and cannot meet industry requirements.
[0148] It is easy for a person skilled in the art to know that the present invention is not limited to the above-mentioned specific details, and the present invention can be implemented in other specific forms without departing from the spirit or main characteristics of the present invention. Therefore, the embodiments described should be regarded as illustrative rather than restrictive from any point of view, so that the scope of the present invention is indicated by the claims rather than the above description; and therefore any changes, as long as they fall within the meaning and scope of the equivalents of the claims, should be regarded as belonging to the present invention.
Claims
1. A method for preparing an adhesive product by gluing on one side, comprising the following steps: a. applying a cleaning agent to at least one surface of a first substrate, and drying the surface of the first substrate to which the cleaning agent is applied; b. applying an adhesive to at least one surface of a second substrate, and drying the surface of the second substrate to which the adhesive is applied; and c. contacting the surface of the first substrate treated in step a with the surface of the second substrate treated in step b to obtain the bonded product; The cleaning agent comprises a polar organic solvent and polyisocyanate; the polar organic solvent has a boiling point not higher than 135° C. and is non-reactive with isocyanate; the polyisocyanate conforms to the general formula R(NCO): n , wherein R is one or more of the following: an aliphatic hydrocarbon group containing 2 to 18 carbon atoms, an aromatic hydrocarbon group containing 6 to 15 carbon atoms, and an aromatic aliphatic hydrocarbon group containing 8 to 15 carbon atoms, and n is not less than 2; the weight of the isocyanate group of the polyisocyanate accounts for 0.005% to 6% by weight of the detergent.
2. The method according to claim 1, characterized in that The weight of the isocyanate groups of the polyisocyanate is 0.007 wt % to 5.6 wt % based on the weight of the cleaning agent.
3. The method according to claim 1, characterized in that The weight of the isocyanate groups of the polyisocyanate is 0.01 wt % to 4.5 wt % based on the weight of the cleaning agent.
4. The method according to claim 1, characterized in that The weight of the isocyanate groups of the polyisocyanate is 0.01 wt % to 0.5 wt % based on the weight of the cleaning agent.
5. The method according to claim 1, characterized in that The weight of the isocyanate groups of the polyisocyanate is 0.02 wt % to 0.2 wt % based on the weight of the cleaning agent.
6. The method according to claim 1, characterized in that The weight of the isocyanate groups of the polyisocyanate is 0.04 wt % to 0.085 wt % based on the weight of the cleaning agent.
7. The method according to claim 1 or 2, characterized in that: The polar organic solvent is one or more of acetone, methyl ethyl ketone, ethyl acetate or butyl acetate, a mixture of butyl acetate, cyclohexane and methyl ethyl ketone, a mixture of methyl ethyl ketone and propylene glycol diacetate, or a mixture of butyl acetate, methyl ethyl ketone and propylene glycol methyl ether acetate.
8. The method according to claim 1 or 2, characterized in that: The polar organic solvent is a mixture of methyl ethyl ketone and ethyl acetate, a mixture of methyl ethyl ketone and butyl acetate, a mixture of methyl ethyl ketone and propylene glycol diacetate, a mixture of acetone and butyl acetate, a mixture of ethyl acetate and butyl acetate, a mixture of ethyl acetate, butyl acetate and methyl ethyl ketone, a mixture of butyl acetate, cyclohexane and methyl ethyl ketone, a mixture of butyl acetate, methyl ethyl ketone and propylene glycol methyl ether acetate, methyl ethyl ketone or butyl acetate.
9. The method according to claim 1 or 2, characterized in that: The general formula of the polyisocyanate has n of 2.5-5.
5.
10. The method according to claim 1 or 2, characterized in that: The general formula of the polyisocyanate has n of 2.5-4.
11. The method according to claim 1 or 2, characterized in that: The polyisocyanate is one or more of the following: toluene diisocyanate trimer, a prepolymer of toluene diisocyanate and diphenylmethane diisocyanate, hexamethylene diisocyanate trimer, isophorone diisocyanate trimer, a prepolymer of diphenylmethane diisocyanate, and tris(p-isocyanatephenyl)phosphothioate.
12. The method according to claim 1 or 2, characterized in that: The first substrate is one or more of the following: a polyurethane-based material and a polyvinyl chloride-based material.
13. The method according to claim 1 or 2, characterized in that: The first substrate is polyurethane-based synthetic leather.
14. The method according to claim 1 or 2, characterized in that: The cleaning agent comprises methyl ethyl ketone and polyisocyanate with an isocyanate functionality of 2.5-4, wherein the polyisocyanate is one or more of the following: prepolymers of toluene diisocyanate and diphenylmethane diisocyanate, and toluene diisocyanate trimer, and the isocyanate groups of the polyisocyanate account for 0.04 wt %-0.085 wt % of the weight of the cleaning agent.
15. The method according to claim 1 or 2, characterized in that: The second substrate is pretreated before applying the adhesive, comprising the following steps: i. polishing or cleaning the second substrate; and ii. Applying a primer to the second substrate treated in step i.
16. The method according to claim 1 or 2, characterized in that: Before the step c, the surface of the second substrate on which the adhesive is applied and treated in the step b is thermally activated at a temperature of 45-75°C.
17. A bonded article prepared according to the method of any one of claims 1 to 16.
18. Use of a bonded article according to claim 17 in the production of footwear.