A process for preparing high-purity elemental metal

By using the centrifugal remelting in situ solidification process under vacuum, the rotating arm cylinder separates gas and heavy metals, and solidifies with liquid nitrogen, the oxidation and impurities problems in beryllium ingots are solved, the purity and material yield of elemental metals are improved, and the cost is reduced .

CN111793756BActive Publication Date: 2024-11-15KINKOU SUZHOU COPPER IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010667557.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-13
Publication Date
2024-11-15
Estimated Expiration
2040-07-13

AI Technical Summary

Technical Problem

In the prior art, beryllium ingots are prone to oxidation in liquid state, and due to the small density, it is difficult to remove pores and metal impurities, resulting in low material yield, high cost and serious waste.

Method used

The centrifugal remelting in situ solidification process is adopted, and the rotating arm cylinder is heated and cooled under a vacuum environment. The gas and heavy metal are separated by centrifugal force to prevent oxidation and solidify the metal through liquid nitrogen.

Benefits of technology

It effectively improves the purity and material yield of elemental metals, reduces costs, reduces energy consumption, and solves pores and impurities problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0002581035400000011
    Figure HDA0002581035400000011
  • Figure HDA0002581035400000021
    Figure HDA0002581035400000021
  • Figure HDA0002581035400000022
    Figure HDA0002581035400000022
Patent Text Reader

Abstract

The invention proposes a process for preparing high-purity single metal, which includes: installing a remelting device, feeding, rotating and melting, rotating and cooling, cutting and other processes. The method utilizes the principle that the density of liquid metal changes when encountering centrifugal force. When the metal is melted, the arm tube is rotated to generate centrifugal force, which can make the density of the liquid metal in the arm tube reach 10 to 20 times or more of the original density, so that the gas floats upward, and the gas in the liquid single metal is effectively separated. When the arm tube rotates, the heavy metal trapped in the liquid metal is thrown to the two ends of the arm tube, thereby improving the purity of the single metal. By placing the device in a vacuum cover, the problem of oxidation of the single metal is effectively prevented. When the melt rotates, liquid nitrogen is introduced, and the liquid nitrogen is preheated to become nitrogen. The arm tube is cooled when it rotates, so that the liquid metal in the arm tube is solidified, and the working efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal material processing, in particular to a process for preparing high-purity elemental metal. Background Art

[0002] Elemental metals are pure substances composed of the same element. Elemental metals must be pure substances composed of one metal element, so a mixture cannot be a single substance. Elemental metals are usually produced by physical separation, thermal decomposition, reduction, electrolysis, oxidation and other methods. However, in the prior art, there are still various technical difficulties in producing pure substances composed of the same element. For example, beryllium is increasingly valued as an emerging material. Beryllium is an indispensable and valuable material in atomic energy, rockets, missiles, aviation, space navigation and metallurgical industries.

[0003] Although beryllium has a wide range of applications, in the prior art, if beryllium beads are directly melted into beryllium ingots for use, even if melted in a vacuum state, due to its low density, it is very easy to cause a dense beryllium oxide film to form on the surface of the liquid beryllium. At the same time, due to its light weight, the gas and metal impurities in the liquid beryllium cannot be removed and separated. Even if it is processed by vacuum remelting, the interior of the final beryllium ingot will be spongy, with a large number of pores that cannot be removed, and high-density metal impurities will settle at the bottom.

[0004] The existing technology uses remelting to make beryllium ingots. The pore inclusions in the beryllium ingots will become crack sources, resulting in a processing yield of beryllium foil made from the beryllium ingots of 15% to 20%. A large amount of scrap leads to increased costs, a large amount of labor waste, and excessive energy consumption. Summary of the invention

[0005] Purpose of the invention: In order to address the deficiencies of the prior art, the present invention provides a process for preparing high-purity elemental metals. The process is simple, ensures the purity of the prepared elemental metals, has high efficiency in preparing the elemental metals, and effectively removes pores and impurities in metal ingots.

[0006] Technical solution: In order to achieve the above purpose, the present invention provides a process for preparing high-purity elemental metal, which process includes the following steps:

[0007] Step 1: Place the remelting device on a table or a support plate, which is provided with holes for accommodating water-cooled coaxial brushes, and the water-cooled coaxial brushes are connected to the intermediate frequency power supply cabinet;

[0008] Step 2: remove the vacuum cover of the remelting device from the bottom plate of the shell, put the single metal blank into the storage barrel, and fill the tee, arm tube and storage barrel with the single metal blank;

[0009] Step 3: After the single metal blank is placed, the vacuum cover is placed on the bottom plate of the shell, and then the connection between the vacuum cover and the bottom plate of the shell is sealed and installed by a sealing material, and then the vacuum cover 20 is evacuated, and then the vacuum motor and the medium frequency power supply cabinet are started;

[0010] Step 4: The vacuum motor drives the transmission belt to work, and the transmission belt transmits power to the gear pair, and the gear pair transmits power to the lower transmission block inserted in the gear, and the lower transmission block drives the support plate and the tee and arm sleeve bushing fixed on the support plate to rotate;

[0011] While the tee and the arm sleeve are rotating, the medium frequency power supply cabinet heats the arm sleeve set on the outside of the arm sleeve through the water-cooled coaxial brush and the water-cooled coil;

[0012] Step 5: After the temperature gun measures that the temperature in the tee and the arm tube reaches the limit value, the water cooling coil continues to heat it for 7 minutes to 15 minutes to melt the elemental metal; the support plate drives the melt in the arm tube to rotate continuously for 8 minutes to 12 minutes to separate bubbles and heavy metals;

[0013] Step 6: After the water-cooling coil is powered off, the time for inputting liquid nitrogen into the input port on the vacuum cover and the time for the support plate to drive the arm cylinder to rotate are both 6 minutes to 18 minutes. After the temperature inside the three-way and the arm cylinder reaches room temperature as measured by the temperature measuring gun, the vacuum motor stops working;

[0014] Step seven, open the vacuum cover, remove the tee from the upper support block, and vertically cut off along the outer diameter direction of the first end of the tee to obtain the separated second end, the third end and the remelting section of the first end, and the remaining second end 22 and the third end 23 are vertically cut off half of their length in the direction of the original first end 21, and the section away from the second end 22 and the third end 23 is the finished pure elemental metal ingot, and the section of the second end 22 and the third end 23 is the remelting section.

[0015] As a further preferred embodiment of the present invention, the temperature measuring gun sends a signal to the PLC circuit, which controls the medium frequency power supply cabinet and the vacuum motor to open and close.

[0016] As a further preference of the present invention, in step 2, the height h of the first end of the tee is ≤ the length L of the arm tube, and the diameter D of the first end is ≥ 1.4 times the diameter d of the arm tube. This data can enable the equipment to maintain balance under high-speed and high-temperature working conditions and ensure the stability of the equipment's operation.

[0017] As a further preferred embodiment of the present invention, in step 2, the bulk density of the elemental metal is 0.6 g / cm 3 ~0.7g / cm 3 , the formula for the volume of elemental metal in the storage barrel is: V 储 =πD 2 / 2·L, the diameter of the first end is D, the length of the arm tube is L, and the volume of the single metal that should be loaded into the tee, arm tube and storage barrel is calculated based on the loose density, and then the equipment is vacuumed and powered on.

[0018] As a further preferred embodiment of the present invention, in step 2, the rotation speed of the support plate is 300 r / min to 600 r / min, which can keep the equipment balanced under high-speed and high-temperature working conditions and ensure the working stability of the equipment;

[0019] As a further preferred embodiment of the present invention, in step 2, the limit temperature in the tee and the arm tube is 1300°C to 1400°C, and the arm tube rotates when the elemental metal is melted. When the arm tube rotates, the density of the liquid elemental metal in the arm tube can be made to reach more than 20 times the original value, effectively separating the gas in the liquid elemental metal and making the gas float upward.

[0020] As a further preferred embodiment of the present invention, the temperature measuring gun, the sensor on the support plate, the input port, the output port, the vacuum motor and the medium frequency power supply cabinet on the vacuum cover are respectively connected to the PLC circuit.

[0021] As a further preferred embodiment of the present invention, the second end and the third end of the tee are respectively threadedly connected to the ends of the two arm tubes.

[0022] As a further preferred embodiment of the present invention, the arm tube bushing is connected to the tee through an interference fit, and the fireproof buffer layer sleeved on the outside of the arm tube is against the inner surface of the arm tube bushing. The fireproof buffer layer is a high-zirconium aluminum silicate fiber cloth, a high-zirconium aluminum silicate plate or a high-zirconium aluminum silicate tube. By arranging the fireproof buffer layer on the outside of the arm tube and the inside of the arm tube bushing, the arm tube is effectively prevented from shaking in the arm tube bushing, thereby increasing the reliability and stability of the connection between the arm tube and the tee and ensuring the working efficiency of the equipment.

[0023] As a further preferred embodiment of the present invention, the water-cooling coils provided on the outside of the arm barrel bushing and the storage barrel bushing are connected through a wiring groove, and the water-cooling coils on the arm barrel bushing pass through the wiring groove and the wire transmission holes on the support plate and the lower transmission block and are connected to the water-cooled coaxial brushes.

[0024] As a further preferred embodiment of the present invention, the vacuum motor is connected to the lower transmission block through a gear pair and a belt drive, one end of the lower transmission block is fixedly connected to the support plate, and the other end is installed on the bearing seat, the bearing seat is fixed on the shell bottom plate sealed with the vacuum cover, the vacuum cover is above the shell bottom plate, and then the connection between the vacuum cover and the shell bottom plate is sealed and installed by a sealing material;

[0025] As a further preferred embodiment of the present invention, an arm tube end plate is provided at the outer end of the arm tube, and the vacuum cover is provided with an input port for inputting liquid nitrogen and an output port for exhausting nitrogen.

[0026] As a further preferred embodiment of the present invention, a hole with an internal thread is provided on the lower surface of the tee, the position of the hole is opposite to the position of the first end, an upper support block is provided at the axial position on the upper surface of the support plate, and the external thread provided on the support block and the internal thread in the hole on the tee are matched and connected together

[0027] As a further preference of the present invention, a bushing limit plate close to the outside of the arm tube end plate is fixed on the arm tube bushing and connected to the limit plate by bolts. After the two arm tubes are respectively connected to the tees, the arm tube and the tee are axially fixed together as a whole, and are connected to the limit plate by bolts, thereby ensuring the coaxiality of the connection between the tee and the arm tube, and further ensuring the stability of the equipment operation.

[0028] As a further preferred embodiment of the present invention, screws pass through the pressure strip to fix the water-cooling coil on the positioning plate. Since the positioning plate and the support plate are fixed together, when the water-cooling coil mounted on the outside of the arm tube bushing is fixed on the positioning plate, radial fixation of the arm tube bushing is achieved, that is, radial fixation of the arm tube.

[0029] As a further preferred embodiment of the present invention, the heating time of the water-cooling coil is 7 minutes to 15 minutes, so that the elemental metal billet is melted into liquid elemental metal. The support plate drives the arm barrel to rotate continuously for 8 minutes to 12 minutes, so that the air in the liquid elemental metal gradually floats to the top of the first end of the tee, and the heavy metal in the liquid elemental metal gradually accumulates at both ends of the arm barrel. After the water-cooling coil is powered off, the support plate continues to rotate, driving the arm barrel to rotate. The time for inputting liquid nitrogen through the input port on the vacuum hood and the time for the support plate to drive the arm barrel to rotate are both 6 minutes to 18 minutes. The liquid nitrogen becomes nitrogen when heated, which cools the arm barrel bushing and the arm barrel as a whole, so that the liquid elemental metal in the arm barrel solidifies into an elemental metal ingot.

[0030] As a further preferred embodiment of the present invention, the material of the storage barrel liner, tee, arm tube and arm tube liner is a high-purity graphite crucible, beryllium oxide ceramic or tungsten crucible.

[0031] As a further preferred embodiment of the present invention, the single metal blank placed in the storage barrel is a single metal with low density such as beryllium beads, aluminum blanks, silver blanks, etc.

[0032] Beneficial effects: Compared with the prior art, the process for preparing high-purity elemental metal provided by the present invention has the following advantages:

[0033] 1. This method uses the principle that the density of liquid metal changes when encountering centrifugal force. When the metal is melted, the rotating arm tube generates centrifugal force, which can make the density of the liquid metal in the arm tube reach 10 to 20 times the original density, effectively separating the gas in the liquid elemental metal and making the gas float upward;

[0034] 2. When the arm rotates, the heavy metals in the liquid metal are thrown to the two ends of the arm, effectively separating the heavy metals in the melt;

[0035] 3. By placing the device in a vacuum cover, the problem of single metal being oxidized can be effectively prevented;

[0036] 4. Liquid nitrogen is introduced into the melt while it is rotating. The liquid nitrogen is preheated to become nitrogen gas. The arm tube cools down while it is rotating, causing the liquid metal in the arm tube to solidify. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a structural schematic diagram of the present invention;

[0038] Figure 2 A top view of the present invention;

[0039] Figure 3 It is a partial view of the present invention;

[0040] Figure 4 This is a schematic diagram of the structure after cutting a single metal ingot. DETAILED DESCRIPTION

[0041] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments.

[0042] like Figure 1 , Figure 2 , Figure 3 As shown, the process for preparing high-purity elemental metal described in the present invention obtains high-purity elemental metal by using a centrifugal remelting in-situ solidification device.

[0043] The centrifugal remelting in-situ solidification device comprises: a tee 2 located in a vacuum cover 20, an "eight"-shaped material storage barrel 100 sleeved on the first end 21 of the tee 2, a material storage barrel bushing 1 sleeved on the outside of the material storage barrel 100, an arm sleeve bushing 4 sleeved on the outside of the second end 22 and the third end 23 of the tee 2, respectively, an arm sleeve 3 respectively inserted into the second end 22 and the third end 23, a support plate 10 for supporting the tee 2, a lower transmission block 11 located below the support plate 10, and a vacuum motor 12 located on one side of the transmission block 11, wherein the vacuum motor 12 is connected to the lower transmission block 11 through a gear pair 19 and a belt drive 191;

[0044] One end of the lower transmission block 11 is fixedly connected to the support plate 10, and the other end is mounted on a bearing seat 171, and the bearing seat 171 is fixed on the housing bottom plate 25;

[0045] A wiring groove 24 is provided on the tee 2, and the water-cooling coil 14 provided on the outer side of the storage barrel bushing 1 and the arm barrel bushing 4 is connected through the wiring groove 24. The water-cooling coil 14 on the arm barrel bushing 4 passes through the wiring groove 24 through the support plate 10 and the wire transmission hole 18 on the lower transmission block 11 and is connected to the water-cooled coaxial brush 17. The water-cooled coaxial brush 17 is connected to the medium frequency power supply cabinet 172. The water-cooling coil 14 is connected and fixed to the positioning plate 9, and the positioning plate 9 is fixed above the support plate 10;

[0046] The outer end of the arm tube 3 is provided with an arm tube end plate 6, and the vacuum cover 20 is provided with an input port 201 for inputting liquid nitrogen and an output port 202 for exhausting nitrogen.

[0047] Example 1

[0048] Step 1: Place the remelting device on a table or a support plate, which is provided with a hole for accommodating a water-cooled coaxial brush 17, and the water-cooled coaxial brush 17 is connected to the intermediate frequency power supply cabinet 172;

[0049] Step 2: Remove the vacuum cover 20 of the remelting device from the bottom plate 25 of the shell, put the single metal blank into the storage barrel 100, and fill the tee 2, the arm 2 and the storage barrel 100 with beryllium beads;

[0050] Step 3: After the beryllium beads are placed, the vacuum cover 20 is placed on the bottom plate 25 of the housing, and then the connection between the vacuum cover 20 and the bottom plate 25 of the housing is sealed and installed by sealing glue, and then the vacuum cover 20 is evacuated, and then the vacuum motor 12 and the intermediate frequency power supply cabinet 172 are started. The voltage of the vacuum motor 12 is 380V, the current is 10A, and the voltage of the intermediate frequency power supply cabinet 172 is 700V, and the current is 70A;

[0051] Step 4: The vacuum motor 12 drives the transmission belt 191 to work. The transmission belt 191 transmits power to the gear pair 19. The gear pair 19 transmits power to the lower transmission block 11 that penetrates the gear. The lower transmission block 11 drives the support plate 10 and the tee 2 and the arm sleeve bushing 4 fixed on the support plate 10 to rotate. The rotation speed of the support plate 10 is 300r / min to 600r / min.

[0052] While the tee 2 and the arm sleeve 4 rotate, the medium frequency power supply cabinet 172 heats the arm sleeve 4 sleeved on the outside of the arm sleeve 3 through the water-cooled coaxial brush 17 and the water-cooled coil 14;

[0053] Step 5, after the temperature measuring gun 2002 measures that the temperature in the tee 2 and the arm tube 3 reaches 1300°C to 1400°C, it sends a signal to the PLC circuit, which controls the water cooling coil 14 to heat the tee 2 and the arm tube 3 for 7min to 15min to melt the beryllium bead; the support plate 10 drives the melt in the arm tube 3 to rotate continuously for 8min to 12min to separate the bubbles and heavy metals in the liquid beryllium, and then the sensor on the support plate 10 sends a signal to the intermediate frequency power supply cabinet 172, which sends a signal to control the water cooling coil to cut off the power;

[0054] Step 6: After the water-cooling coil 14 is powered off, the PLC circuit controls the input port 201 to open, and liquid nitrogen is input into the vacuum cover 20. The liquid nitrogen is preheated to become nitrogen gas, and the arm tube bushing 4 and the arm tube 3 are cooled as a whole. The support plate 20 drives the arm tube 3 to rotate continuously, so that the liquid beryllium in the arm tube 3 solidifies into a high-purity beryllium ingot. At this time, the output port 202 discharges nitrogen gas. After 6 to 18 minutes, the input of liquid nitrogen is stopped. After the temperature in the tee 2 and the arm tube 3 reaches the room temperature, the PLC circuit sends a signal to control the vacuum motor 12 to stop working.

[0055] Step seven, open the vacuum cover, remove the tee 2 from the upper support block 15, and vertically cut off along the outer diameter direction of the first end 21 of the tee 2 to obtain the separated second end 22, the third end 23 and the remelting section B of the first end 21, and the remaining second end 22 and the third end 23 are vertically cut off half of their length in the direction of the original first end 21, and the section away from the second end 22 and the third end 23 is the finished pure beryllium ingot A, and the section of the second end 22 and the third end 23 is the remelting section B.

[0056] Example 2

[0057] Step 1: Place the remelting device on a table or a support plate, which is provided with a hole for accommodating a water-cooled coaxial brush 17, and the water-cooled coaxial brush 17 is connected to the intermediate frequency power supply cabinet 172;

[0058] Step 2: Remove the vacuum cover 20 of the remelting device from the bottom plate 25 of the shell, put the aluminum billet into the storage barrel 100, and fill the tee 2, the arm 2 and the storage barrel 100 with the aluminum billet;

[0059] Step 3: After the aluminum billet is placed, the vacuum cover 20 is placed on the bottom plate 25 of the housing, and then the connection between the vacuum cover 20 and the bottom plate 25 of the housing is sealed and installed by sealing glue, and then the vacuum cover 20 is evacuated, and then the vacuum motor 12 and the intermediate frequency power supply cabinet 172 are started. The voltage of the vacuum motor 12 is 380V, the current is 10A, and the voltage of the intermediate frequency power supply cabinet 172 is 700V, and the current is 70A;

[0060] Step 4: The vacuum motor 12 drives the transmission belt 191 to work. The transmission belt 191 transmits power to the gear pair 19. The gear pair 19 transmits power to the lower transmission block 11 that penetrates the gear. The lower transmission block 11 drives the support plate 10 and the tee 2 and the arm sleeve bushing 4 fixed on the support plate 10 to rotate. The rotation speed of the support plate 10 is 300r / min to 600r / min.

[0061] While the tee 2 and the arm sleeve 4 rotate, the medium frequency power supply cabinet 172 heats the arm sleeve 4 sleeved on the outside of the arm sleeve 3 through the water-cooled coaxial brush 17 and the water-cooled coil 14;

[0062] Step 5, after the temperature measuring gun 2002 measures that the temperature in the tee 2 and the arm tube 3 reaches 1300°C to 1400°C, it sends a signal to the PLC circuit, which controls the water cooling coil 14 to heat the tee 2 and the arm tube 3 for 7min to 15min to melt the aluminum billet; after the support plate 10 drives the melt in the arm tube 3 to rotate continuously for 8min to 12min to separate the bubbles and heavy metals in the liquid aluminum, the sensor on the support plate 10 sends a signal to the intermediate frequency power supply cabinet 172, which sends a signal to control the water cooling coil to cut off the power;

[0063] Step 6: After the water-cooling coil 14 is powered off, the PLC circuit controls the input port 201 to open, and liquid nitrogen is input into the vacuum cover 20. The liquid nitrogen is preheated to become nitrogen gas, and the arm tube bushing 4 and the arm tube 3 are cooled as a whole. The support plate 20 drives the arm tube 3 to rotate continuously, so that the liquid aluminum in the arm tube 3 solidifies into a high-purity aluminum ingot. At this time, the output port 202 discharges nitrogen gas. After 6 to 18 minutes, the input of liquid nitrogen is stopped. After the temperature in the tee 2 and the arm tube 3 reaches the room temperature, the PLC circuit sends a signal to control the vacuum motor 12 to stop working.

[0064] Step 7, open the vacuum cover, remove the tee 2 from the upper support block 15, and vertically cut along the outer diameter direction of the first end 21 of the tee 2 to obtain the separated second end 22, the third end 23 and the remelting section B of the first end 21, and vertically cut the remaining second end 22 and the third end 23 half of their length in the direction of the original first end 21, and the end away from the second end 22 and the third end 23 is the finished high-purity aluminum ingot A, and the end of the second end 22 and the third end 23 is the remelting section B. .

[0065] Example 3

[0066] Step 1: Place the remelting device on a table or a support plate, which is provided with a hole for accommodating a water-cooled coaxial brush 17, and the water-cooled coaxial brush 17 is connected to the intermediate frequency power supply cabinet 172;

[0067] Step 2: Remove the vacuum cover 20 of the remelting device from the bottom plate 25 of the shell, put the silver blank into the storage barrel 100, and fill the tee 2, the arm 2 and the storage barrel 100 with the silver ingot blank;

[0068] Step 3: After the single metal blank is placed, the vacuum cover 20 is covered on the shell bottom plate 25, and then the connection between the vacuum cover 20 and the shell bottom plate 25 is sealed and installed by sealing glue, and then the vacuum cover 20 is evacuated, and then the vacuum motor 12 and the intermediate frequency power supply cabinet 172 are started. The voltage of the vacuum motor 12 is 380V, the current is 10A, and the voltage of the intermediate frequency power supply cabinet 172 is 700V, and the current is 70A;

[0069] Step 4: The vacuum motor 12 drives the transmission belt 191 to work. The transmission belt 191 transmits power to the gear pair 19. The gear pair 19 transmits power to the lower transmission block 11 that penetrates the gear. The lower transmission block 11 drives the support plate 10 and the tee 2 and the arm sleeve bushing 4 fixed on the support plate 10 to rotate. The rotation speed of the support plate 10 is 300r / min to 600r / min.

[0070] While the tee 2 and the arm sleeve 4 rotate, the medium frequency power supply cabinet 172 heats the arm sleeve 4 sleeved on the outside of the arm sleeve 3 through the water-cooled coaxial brush 17 and the water-cooled coil 14;

[0071] Step 5: After the temperature measuring gun 2002 measures that the temperature in the tee 2 and the arm tube 3 reaches 1300°C to 1400°C, it sends a signal to the PLC circuit, which controls the water cooling coil 14 to heat the tee 2 and the arm tube 3 for 7min to 15min to melt the silver blank; after the support plate 10 drives the melt in the arm tube 3 to rotate continuously for 8min to 12min to separate the bubbles and heavy metals in the liquid silver, the sensor on the support plate 10 sends a signal to the intermediate frequency power supply cabinet 172, which sends a signal to control the water cooling coil to cut off the power;

[0072] Step 6: After the water-cooling coil 14 is powered off, the PLC circuit controls the input port 201 to open, and liquid nitrogen is input into the vacuum cover 20. The liquid nitrogen is preheated to become nitrogen gas, and the arm tube bushing 4 and the arm tube 3 are cooled as a whole. The support plate 20 drives the arm tube 3 to rotate continuously, so that the liquid silver in the arm tube 3 solidifies into a high-purity silver ingot. At this time, the output port 202 discharges nitrogen gas. After 6 minutes to 18 minutes, the input of liquid nitrogen is stopped. After the temperature in the three-way 2 and the arm tube 3 reaches the room temperature, the PLC circuit sends a signal to control the vacuum motor 12 to stop working;

[0073] Step 7, open the vacuum cover, remove the tee 2 from the upper support block 15, and vertically cut along the outer diameter direction of the first end 21 of the tee 2 to obtain the separated second end 22, the third end 23 and the remelting section B of the first end 21, and vertically cut the remaining second end 22 and the third end 23 half of their length toward the original first end 21, and the end away from the second end 22 and the third end 23 is the finished high-purity silver ingot A, and the end of the second end 22 and the third end 23 is the remelting section B. .

[0074] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable technicians familiar with the technical field to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for preparing high-purity elemental metal, characterized in that: The process obtains high-purity single-element metal by using a centrifugal remelting in-situ solidification device, wherein the centrifugal remelting in-situ solidification device comprises: a tee (2) located in a vacuum cover (20), an "eight"-shaped material storage barrel (100) sleeved on the first end (21) of the tee (2), a material storage barrel bushing (1) sleeved on the outside of the material storage barrel (100), an arm sleeve bushing (4) sleeved on the outside of the second end (22) and the third end (23) of the tee (2), an arm sleeve (3) respectively inserted into the second end (22) and the third end (23), a support plate (10) for supporting the tee (2), a lower transmission block (11) located below the support plate (10), and a vacuum motor (12) located on one side of the transmission block (11), wherein the vacuum motor (12) is connected to the lower transmission block (11) via a gear pair (19) and a belt drive (191); One end of the lower transmission block (11) is fixedly connected to the support plate (10), and the other end is mounted on a bearing seat (171), and the bearing seat (171) is fixed on the housing bottom plate (25); A wiring groove (24) is provided on the tee (2), and the water-cooling coil (14) provided on the outer sides of the storage barrel bushing (1) and the arm barrel bushing (4) is connected through the wiring groove (24). The water-cooling coil (14) on the arm barrel bushing (4) passes through the wiring groove (24) through the support plate (10) and the wire transmission hole (18) on the lower transmission block (11) and is connected to the water-cooling coaxial brush (17). The water-cooling coaxial brush (17) is connected to the medium frequency power supply cabinet (172). The water-cooling coil (14) is connected and fixed to the positioning plate (9), and the positioning plate (9) is fixedly arranged above the support plate (10); An arm tube end plate 6 is provided at the outer end of the arm tube (3); the vacuum cover 20 is provided with an input port (201) for inputting liquid nitrogen and an output port (202) for exhausting nitrogen; A process for preparing high-purity elemental metal comprises the following steps: Step 1: placing the remelting device on a table or a support plate, wherein the table or the support plate is provided with a hole for accommodating a water-cooled coaxial brush (17), and the water-cooled coaxial brush (17) is connected to the medium frequency power supply cabinet (172); Step 2: Remove the vacuum cover (20) of the remelting device from the bottom plate (25) of the shell, and put a single metal blank into the storage barrel (100). The single metal blank fills the tee (2), the arm tube (2) and the storage barrel (100). The loose density of the single metal is 0.6 g / cm 3 ~0.7g / cm 3 , the formula for the volume of elemental metal in the storage barrel (100) is: V 储 =πD 2 / 2·L, the diameter of the first end (21) is D, and the length of the arm tube (3) is L; Step 3: After the single metal blank is placed, the vacuum cover (20) is placed on the bottom plate (25) of the housing, and then the connection between the vacuum cover (20) and the bottom plate (25) of the housing is sealed and installed by a sealing material, and then the vacuum cover 20 is evacuated, and then the vacuum motor (12) and the medium frequency power supply cabinet (172) are started; Step 4: The vacuum motor (12) drives the transmission belt (191) to work, and the transmission belt (191) transmits power to the gear pair (19), and the gear pair (19) transmits power to the lower transmission block (11) inserted in the gear, and the lower transmission block (11) drives the support plate (10) and the three-way (2) and the arm sleeve (4) fixed on the support plate (10) to rotate; While the tee (2) and the arm sleeve bushing (4) rotate, the medium frequency power supply cabinet (172) heats the arm sleeve bushing (4) sleeved on the outside of the arm sleeve (3) through the water-cooled coaxial brush (17) and the water-cooled coil (14); Step 5: After the temperature gun (2002) measures that the temperature inside the tee (2) and the arm tube (3) reaches a limit value, the water cooling coil (14) continuously heats them for 7 minutes to 15 minutes to melt the elemental metal; the support plate (10) drives the melt inside the arm tube (3) to continuously rotate for 8 minutes to 12 minutes to separate bubbles and heavy metals; Step 6: After the water-cooling coil (14) is powered off, the time for inputting liquid nitrogen into the input port (201) on the vacuum cover (20) and the time for the support plate (10) to drive the arm tube (3) to rotate are both 6 minutes to 18 minutes. After the temperature inside the tee (2) and the arm tube (3) reaches room temperature as measured by the temperature measuring gun (2002), the vacuum motor (12) stops working; Step 7, open the vacuum cover, remove the tee (2) from the upper support block (15), and vertically cut along the outer diameter direction of the first end (21) of the tee (2) to obtain the separated second end (22), the third end (23) and the remelting section (B) of the first end (21), and vertically cut the remaining ends of the second end 22 and the third end 23 to half of their length in the direction of the original first end 21, and the section away from the ends of the second end 22 and the third end 23 is the finished pure elemental metal ingot (A), and the section of the ends of the second end 22 and the third end 23 is the remelting section (B).

2. A process for preparing high-purity elemental metal according to claim 1, characterized in that: In step 2, the height h of the first end (21) of the tee (2) is ≤ the length L of the arm tube (3), and the diameter D of the first end (21) is ≥ 1.4 times the diameter d of the arm tube (3).

3. The centrifugal remelting in-situ solidification device according to claim 1, characterized in that: In step 4, the rotation speed of the support plate (10) is 300 r / min to 600 r / min.

4. A process for preparing high-purity elemental metal according to claim 1, characterized in that: In step five, the limit value temperature in the tee (2) and the arm tube (3) is 1300° C. to 1400° C.

5. A process for preparing high-purity elemental metal according to claim 1, characterized in that: The temperature measuring gun (2002), vacuum motor (12), and medium frequency power supply cabinet (172) are respectively connected to the PLC circuit. The heating time of the water cooling coil (14) is 7 minutes to 15 minutes. The time for the support plate (10) to drive the melt in the arm tube (3) to continuously rotate is 8 minutes to 12 minutes. After the water cooling coil (14) is powered off, the time for the input port (201) on the vacuum cover (20) to input liquid nitrogen and the time for the support plate (10) to drive the arm tube (3) to rotate are both 6 minutes to 18 minutes.

6. A process for preparing high-purity elemental metal according to claim 1, characterized in that: The second end (22) and the third end (23) of the tee (2) are respectively threadedly connected to the ends of the two arm tubes (3).

7. A process for preparing high-purity elemental metal according to claim 1, characterized in that: The arm tube bushing (4) is connected to the tee (2) by interference fit, and the fireproof buffer layer (5) sleeved on the outside of the arm tube (3) abuts against the inner surface of the arm tube bushing (4).

8. A process for preparing high-purity elemental metal according to claim 1, characterized in that: The water-cooling coil (14) provided on the outer sides of the arm sleeve bushing (4) and the storage barrel bushing (1) is connected via a wiring slot (24); the water-cooling coil (14) on the arm sleeve bushing (4) passes through the wiring slot (24) through the support plate (10) and the wire transmission hole (18) on the lower transmission block (11) and is connected to the water-cooled coaxial brush (17).

9. A process for preparing high-purity elemental metal according to claim 1, characterized in that: The vacuum motor (12) is connected to the lower transmission block (11) via a gear pair (19) and a belt drive (191).