Copper clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and manufacturing method thereof

By coating the glass fiber mesh with high-temperature-resistant rubber and using a dry process to produce heat-resistant and temperature-resistant elastic gaskets, the problems of kraft paper failure under high temperature and pressure and the use of solvents are solved, achieving environmental protection, cost reduction and multiple effect of use.

CN111844963BActive Publication Date: 2024-10-22GUANGDONG SHUO CHENG TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202010818467.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-14
Publication Date
2024-10-22
Estimated Expiration
2040-08-14

AI Technical Summary

Technical Problem

The kraft paper material used in existing copper-clad laminate lamination loses its toughness under high temperature and pressure, and its one-time use and use of large amounts of solvents are not conducive to environmental protection, leading to environmental protection and production cost problems.

Method used

The heat-resistant and temperature-resistant elastic gasket produced by dry process is coated with a thin layer of high-temperature resistant rubber on the glass fiber mesh cloth, and the heat-resistant and temperature-resistant elastic gasket is formed by the calendering and rubbing process, replacing traditional kraft paper and reducing solvents. Use and improve productivity.

Benefits of technology

It achieves thermal resistance and micro-elasticity under high temperature and high pressure conditions, supports multiple reuse, reduces production costs and environmental pollution, meets environmental protection requirements, and replaces traditional kraft paper materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111844963B_ABST
    Figure CN111844963B_ABST
Patent Text Reader

Abstract

The present invention provides a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material, comprising at least one surface layer and at least one middle layer. Each surface layer comprises a first substrate and a protective layer, and the protective layer is located on the surface of the first substrate. Each middle layer comprises a second substrate and a rubber layer, and the rubber layer is combined with the second substrate by a calendering and rubbing process, and the surface layer and the middle layer are combined by a vulcanization process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of copper clad laminates, and in particular to a heat-resistant and temperature-resistant elastic rubber pad of a copper clad laminate composite material and a manufacturing method thereof. Background Art

[0002] With the progress of the times and the rapid development of electronic technology, the field of printed circuit board technology has been continuously improved and developed. Copper clad laminate is an extremely important basic material for printed circuit boards and an indispensable role in today's electronic industry. In other words, the processing of PCB circuit boards cannot be separated from copper clad laminate. The proportion of copper clad laminate multilayer boards is increasing year by year. An important process in the manufacture of copper clad laminate multilayer boards is lamination, among which the control of lamination quality in the manufacture of multilayer boards is becoming more and more important. In other words, the lamination quality of copper clad laminate multilayer boards further affects the quality of printed circuit boards.

[0003] When laminating copper clad laminates, kraft paper is often used as a heat transfer buffer. Kraft paper is placed between the hot plate and the steel plate of the laminating machine to ease the temperature rise curve closest to the bulk material, so that the temperature difference between the multiple substrates or multilayer boards to be pressed is as close as possible. The commonly used specifications are 90 pounds to 150 pounds. However, due to the high temperature and high pressure during lamination, the fibers in the kraft paper have been broken and it is no longer tough and difficult to function, so it must be replaced.

[0004] Furthermore, in the traditional production of copper clad laminate lamination, kraft paper is used as a gasket material, and it is used once. The large-scale use of kraft paper is not conducive to environmental protection and sustainable development. In addition, there are also products on the market that use a dip coating process, using glass fiber mesh cloth, which is coated with glue by dip coating, then cooled or dried, and pressed. In the dip coating process, a large amount of solvents are used, which increases production costs and is not conducive to environmental protection. Summary of the invention

[0005] One advantage of the present invention is that it provides a copper-clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and a manufacturing method thereof, wherein a specially formulated high-temperature resistant thin layer of rubber is used, and a calendering and rubbing rubber process is used. This method is a "dry" process. In this process, the large-scale use of solvents can be avoided in the production process, thereby reducing costs and reducing environmental pollution.

[0006] One advantage of the present invention is that it provides a copper-clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and a manufacturing method thereof, wherein a rubber is coated on a glass fiber mesh cloth by a calendering process to form a heat-resistant and temperature-resistant elastic rubber pad, which is used for PCB multi-layer board lamination production.

[0007] One advantage of the present invention is that it provides a copper-clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and a method for manufacturing the same, wherein the glass fiber mesh cloth is calendered and rubbed with a heat-resistant thin layer of rubber using a "dry process". Compared with the solvent method, this method saves solvent costs and saves electricity for rubber making. In other words, the production process of the present invention is an environmentally friendly process. Replacing traditional kraft paper in the use of finished products is also an environmentally friendly process. It is worth mentioning that the calendering rubber rubbing has the characteristics of small production space, adjustable mesh cloth rubber rubbing thickness, and flexible production conversion, which can greatly improve production efficiency.

[0008] One advantage of the present invention is that it provides a copper-clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and a manufacturing method thereof, wherein the final product is used as a substitute material for kraft paper in practical use, inherits the heat resistance of paper materials and micro-elasticity under high pressure conditions. At the same time, it has the function of multiple reuses. The formula and product size can be adjusted according to different customers to produce tailor-made products for customers.

[0009] One advantage of the present invention is that it provides a copper-clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and a manufacturing method thereof, wherein the adhesive tape used for the heat-resistant and temperature-resistant elastic rubber pad adopts an ultra-thin calendering and rubbing method, avoiding the use of a large amount of organic solvents, and is environmentally friendly and safe.

[0010] One advantage of the present invention is that it provides a copper-clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and a manufacturing method thereof, wherein the vulcanization process adopts a new process of continuous production, and the vulcanization temperature and pressure are evenly distributed, which greatly improves the uniformity of the product's pressure resistance and temperature rise, and avoids the occurrence of internal defects such as bubbles, delamination, and cracking.

[0011] One advantage of the present invention is that it provides a copper-clad laminate composite material heat-resistant and temperature-resistant elastic rubber pad and a manufacturing method thereof, wherein the heat-resistant and temperature-resistant elastic rubber pad has been tested for more than 2000 hours in a 220 degree 5MPa environment and has been used for more than 500 cycles in actual use, so as to replace traditional kraft paper and save a large amount of paper gasket material. In particular, this product complies with the EU environmental ban requirements.

[0012] One advantage of the present invention is that it provides a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material and a manufacturing method thereof, wherein the elastic rubber pad is a raw material used in manufacturing copper-clad laminates and is a pressing pad used in manufacturing copper-clad laminates.

[0013] Other advantages and features of the present invention will become more apparent from the following detailed description and may be realized by means of the instrumentalities and combinations particularly pointed out in the appended claims.

[0014] According to the present invention, the heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material of the present invention, which can achieve the above-mentioned purpose and other purposes and advantages, comprises:

[0015] At least one surface layer, wherein each surface layer comprises a first substrate and a protective layer, wherein the protective layer is located on a surface of the first substrate; and

[0016] At least one middle layer, wherein each middle layer comprises a second substrate and a rubber layer, the rubber layer is combined with the second substrate by a calendaring and rubbing process, and the surface layer and the middle layer are combined by a vulcanization process.

[0017] According to one embodiment of the present invention, the protective layer includes PTFE powder, pigment, water-based Teflon coating, thickener, and curing agent, wherein the mass fractions are as follows:

[0018] PTFE powder: 30

[0019] Pigments: 4

[0020] Water-based Teflon coating: 100

[0021] Thickener: 10

[0022] Curing agent:6.

[0023] According to one embodiment of the present invention, the protective layer includes rubber, heat-resistant material, reinforcing material, cross-linking agent, and colorant, wherein the mass fractions are as follows:

[0024] Rubber: 100

[0025] Heat-resistant material: 15-25

[0026] Reinforcement material: 15-35

[0027] Crosslinking agent: 2-6

[0028] Pigment: 1-3.

[0029] According to one embodiment of the present invention, the material of the rubber layer includes rubber, heat-resistant filler, foaming material, cross-linking agent, acid absorber, and flow agent, wherein the mass fractions are as follows:

[0030] Rubber: 100

[0031] Reinforcement material: 10-15

[0032] Heat-resistant filler: 15-30

[0033] Foam material: 5-30

[0034] Crosslinking agent: 3-6

[0035] Acid absorbent: 5-10

[0036] Flowing agent: 1-3.

[0037] According to an embodiment of the present invention, the first substrate and the second substrate are implemented as glass fiber mesh cloth.

[0038] According to one embodiment of the present invention, the cured thickness of the protective layer is 0.08-0.10 mm.

[0039] According to an embodiment of the present invention, the rubber is selected from the group consisting of fluororubber and silicone rubber.

[0040] According to an embodiment of the present invention, the heat-resistant filler is selected from the group consisting of precipitated barium sulfate, mica and vermiculite.

[0041] According to an embodiment of the present invention, the reinforcing material is precipitated silica.

[0042] According to an embodiment of the present invention, the cross-linking agent is selected from the group consisting of bisphenol AF / BPP, peroxide BIPB, bis(2,4), bis(2,5), HVA-2, and TAIC.

[0043] According to an embodiment of the present invention, the colorant is selected from the group consisting of carbon black, masterbatch and titanium dioxide.

[0044] According to an embodiment of the present invention, the foaming material is implemented as expandable microspheres.

[0045] According to an embodiment of the present invention, the acid absorber is selected from the group consisting of calcium hydroxide, magnesium oxide and zinc oxide.

[0046] According to an embodiment of the present invention, the flow agent is selected from the group consisting of fluoro wax, erucic acid, palm wax and mannitol.

[0047] According to one embodiment of the present invention, at least one middle layer is disposed between the two surface layers to perform a multi-layer vulcanization combination, wherein the protective layers of the surface layers are respectively located on the outside.

[0048] According to the present invention, a method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material of the present invention, which can achieve the above-mentioned purpose and other purposes and advantages, comprises the following steps:

[0049] (A) forming a surface layer by a coating process;

[0050] (B) forming a rubber layer through a rubber refining process;

[0051] (C) combining the rubber layer with a second substrate to form a middle layer through a calendaring and rubbing process;

[0052] (D) bonding the surface layer and the middle layer by a vulcanization process; and

[0053] (E) The heat-resistant and temperature-resistant elastic rubber pad is formed through a cutting and edge-sealing process.

[0054] According to an implementation method of the present invention, in step (A), the coating process includes forming a protective layer on a first substrate, wherein the protective layer is implemented as a water-based Teflon coating, and the curing thickness of the protective layer is 0.08-0.10 mm, the curing temperature is 250-360 degrees, and the duration is 15-30 minutes.

[0055] According to an implementation method of the present invention, in step (B), the rubber refining process includes a high temperature resistant compounding process, a high temperature resistant mixing process, a high temperature resistant open mixing process, and a high temperature resistant refining process. In the high temperature resistant compounding process, the rubber is cut according to a certain proportion, a certain proportion of heat-resistant filler, foaming material, and flow agent are weighed and put into a feeding bag, a certain proportion of acid absorber is put into the feeding bag, and a certain proportion of cross-linking agent is put into a container. In the high temperature resistant mixing process, the cut rubber is put into the mixing chamber for kneading. When the temperature rises to 50-60 degrees, the heat-resistant filler, foaming material, and flow agent in the feeding bag are put into the mixing chamber. The foaming material, the flow agent and part of the acid absorber are kneaded under pressure. When the temperature rises to 80 degrees, the hammer is lifted, and the mixing chamber is cleaned. Then the remaining acid absorber is added. When the temperature rises to 90-95 degrees, the hammer is lifted, and the mixing chamber is cleaned. Then the cross-linking agent is added. After the hammer is dropped for 30 seconds, the mixed rubber is formed. In the high temperature resistant open mixing process, the mixed rubber is put into an open mixing mill, the roller distance is adjusted to 0.5-1mm, the mixed rubber passes through the roller three times, and the triangular bag is made three times. The roller distance is adjusted to 5-10mm to form a film. In the high temperature resistant re-mixing process, the film is put into an internal mixer, and then put into the open mixing mill after the internal mixing to form the rubber layer.

[0056] According to an implementation method of the present invention, in step (C), the temperature of the upper, middle and lower rollers of a calender is set to 70-85°C, the calender roller distance is adjusted to a required rubber layer thickness, and the roller temperature of a feeding mill is set to 55-65°C to stabilize the feeding, and the second substrate is guided through the calender, and the rubber layer is evenly rubbed into the surface of the second substrate. The thickness of the calendered rubber layer can be adjusted to 0.1-0.2mm as required, wherein the rubbing width is 1420mm and the thickness range is 0.05mm.

[0057] According to an implementation method of the present invention, in step (D), at least one of the middle layers is located between the two surface layers, and the protective layer of the surface layer is an outer layer.

[0058] According to an implementation method of the present invention, in step (E), the heat-resistant and temperature-resistant elastic rubber pad is cured at 200 degrees for 6 hours in the curing box.

[0059] According to the present invention, a method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material of the present invention, which can achieve the above-mentioned purpose and other purposes and advantages, comprises the following steps:

[0060] (a) a protective layer refining process forms a protective layer on one side;

[0061] (b) a rubber refining process to form a rubber layer;

[0062] (c) combining the rubber layer with a second substrate to form a middle layer through a calendaring and rubbing process;

[0063] (d) bonding the protective layer, a first substrate and the middle layer by a vulcanization process; and

[0064] (e) The heat-resistant and temperature-resistant elastic rubber pad is formed through a cutting and edge-sealing process.

[0065] According to an implementation method of the present invention, in step (d), the protective layer, the first substrate, at least one middle layer, the first substrate and the protective layer are successively introduced into a vulcanizer in a stacked manner and combined into one through vulcanization.

[0066] Further objects and advantages of the present invention will be fully apparent from an understanding of the following description and the accompanying drawings.

[0067] These and other objects, features and advantages of the present invention will be more fully understood from the following detailed description, accompanying drawings and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1A to Figure 1B It is a schematic structural diagram of a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material according to a preferred embodiment of the present invention.

[0069] Figure 2 The present invention is a manufacturing flow chart of a heat-resistant and temperature-resistant elastic rubber pad made of a copper-clad laminate composite material according to a first preferred embodiment of the present invention.

[0070] Figure 3 It is a manufacturing flow chart of a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material according to a second preferred embodiment of the present invention. DETAILED DESCRIPTION

[0071] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0072] Those skilled in the art should understand that, in the disclosure of the present invention, the orientation or position relationship indicated by the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are based on the orientation or position relationship shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the above terms should not be understood as limiting the present invention.

[0073] It is to be understood that the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.

[0074] like Figure 1A Shown to Figure 2 As shown, a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material and a manufacturing method thereof according to the first preferred embodiment of the present invention. The heat-resistant and temperature-resistant elastic rubber pad 1 includes at least one surface layer 10 and at least one middle layer 20. The surface layer 10 and the middle layer 20 are subjected to a vulcanization process to form the heat-resistant and temperature-resistant elastic rubber pad 1. It is worth mentioning that the middle layer 20 is set according to the required number of layers. In other words, the heat-resistant and temperature-resistant elastic gasket of the copper-clad laminate composite material is formed by a multi-layer composite of the surface layer 10 and the middle layer 20. In particular, the heat-resistant and temperature-resistant elastic rubber pad 1 is composed of two surface layers 10 and at least one middle layer 20, wherein the middle layer 20 is arranged between the two surface layers 10. In addition, the surface layer 10 includes a first substrate 11 and a protective layer 12. The protective layer 12 is applied to the first substrate 11 through a coating process S1. The middle layer 20 includes a second substrate 21 and a rubber layer 22. The rubber layer 22 is combined with the second substrate 21 through a calendering and rubbing process S3. It can be understood that the structure of the heat-resistant and temperature-resistant elastic rubber pad 1 is the protective layer 12, the first substrate 11, the middle layer 20, the first substrate 11, and the protective layer 12, wherein the number of layers or the thickness of the middle layer 20 is adjusted according to actual needs. Figure 1BAs shown, the heat-resistant and temperature-resistant elastic rubber pad 1 can also be composed of a surface layer 10 and at least one middle layer 20, which is not a limitation of the present invention.

[0075] The first substrate 11 of the surface layer 10 is implemented as a glass fiber mesh cloth. The protective layer 12 includes PTFE powder, pigment, water-based Teflon coating, thickener, and curing agent. It is worth mentioning that the mass fractions of the protective layer 12 are as follows:

[0076] PTFE powder: 30

[0077] Pigments: 4

[0078] Water-based Teflon coating: 100

[0079] Thickener: 10

[0080] Curing agent: 6

[0081] Furthermore, in the coating process S1, the protective layer 12 is implemented as a water-based Teflon coating, wherein the curing thickness of the protective layer 12 is 0.08-0.10 mm, and the curing temperature of the protective layer 12 is 160 degrees for 10-15 minutes.

[0082] The second substrate 21 of the middle layer 20 is implemented as a glass fiber mesh cloth. The rubber layer 22 is formed by a rubber refining process S2. The materials for refining the rubber layer 22 include rubber, heat-resistant filler, foaming material, cross-linking agent, acid absorbent, and flow agent, wherein the mass fractions are as follows:

[0083] Rubber: 100

[0084] Heat-resistant filler: 15-30

[0085] Reinforcement material: 10-15

[0086] Foam material: 5-30

[0087] Crosslinking agent: 3-6

[0088] Acid absorbent: 5-10

[0089] Flow agent: 1-3

[0090] The rubber refining process S2 includes a high temperature resistant compounding process S201, a high temperature resistant mixing process S202, a high temperature resistant refining process S203, and a high temperature resistant refining process S204.

[0091] In the high temperature resistant compounding process S201, the rubber is cut according to a certain ratio, the heat-resistant filler, the foaming material, and the flow agent are weighed and put into a feeding bag according to a certain ratio, the acid absorber is weighed and put into the feeding bag according to the ratio, and the cross-linking agent is weighed and put into a container according to the ratio.

[0092] In the high temperature resistant mixing process S202, the cut rubber is put into a mixing chamber and hammered. When the temperature rises to a first preset temperature, a feeding bag containing heat-resistant fillers, foaming materials, flow agents and part of the acid absorber is put into the mixing chamber. When the temperature rises to a second preset temperature, the remaining acid absorber is put into the mixing chamber. When the temperature rises to a third preset temperature, a cross-linking agent is put into the mixing chamber, and then the hammer is dropped to form a mixed rubber. It is worth mentioning that the first preset temperature is implemented as 50-60 degrees; the second preset temperature is implemented as 80 degrees; and the third preset temperature is implemented as 90-95 degrees. Further, a 35-liter internal mixer is used, the air hammer pressure of the internal mixer is set to 0.6MPa, and the cooling water temperature is set to less than 30 degrees. The rubber is put into the internal mixing chamber and hammered. When the temperature rises to 50-60 degrees, a feeding bag containing heat-resistant fillers, foaming materials, flow agents and part of the acid absorber is put into the mixing chamber. When the temperature rises to 80 degrees, the hammer is lifted, the mixing chamber is cleaned, and the remaining acid absorber is added. When the temperature rises to 90-95 degrees, the hammer is lifted, the mixing chamber is cleaned, and the cross-linking agent is added. After the hammer falls for 30 seconds, the mixed rubber is formed.

[0093] In the high temperature resistant refining process S203, the mixed rubber is put into an open mill to form a film. Specifically, the mixed rubber is quickly put into an open mill, and the cooling water temperature is set to less than 30 degrees. After two thin passes, the roller distance is adjusted to 0.5-1mm to allow the mixed rubber to be quickly cooled. After three triangular packs, after three rolls, the roller distance is adjusted to 5-10mm to form the film. The film is a thick film.

[0094] In the high temperature resistant refining process S204, the rubber sheet is put into an internal mixer, and then put into the open mixer after internal mixing to form the rubber layer 22. Specifically, the rubber sheet is put into an internal mixer, and after 40-80 seconds, the hammer is lifted and cleaned once, and the material is unloaded when the temperature rises to 70-80 degrees, and then put into the open mixer after internal mixing to form the rubber layer 22.

[0095] In the calendering and rubbing process S3, the rubber layer 22 is combined with the second substrate 21, and the finished product is rolled into a roll. In other words, the rubber layer 22 is combined with the glass fiber mesh cloth to form the rolled middle layer 20. Further, the temperature of the calendering cloth drying roller is set to 95 degrees, the temperature of the upper, middle and lower rollers is 70-85 degrees Celsius, the calendering roller distance is adjusted to the required rubber layer thickness, such as 0.1-0.18mm determined according to the process requirements, and the line speed, the second substrate 21 is guided through the calender, the rubber layer 22 is evenly rubbed into the surface of the second substrate 21, and the cloth is rolled up into a roll.

[0096] In the vulcanization process, the surface layer 10 and the middle layer 20 are respectively introduced into a vulcanizing machine for vulcanization pressing, and after cooling, they are subjected to a cutting and edge sealing process S5 to form the heat-resistant and temperature-resistant elastic rubber pad 1. Further, after the surface layer 10 and the middle layer 20 are vulcanized and pressed, they are moved to a cooling rack for cooling, and then placed in a cutting table for cutting into a preset size. Then, an edge sealing glue is applied to the edge of the cut finished product and placed in a curing box for curing. Further, the pressure of the vulcanizing machine is 30-45kg / cm2, the vulcanization pressing time is 25-30Min, and the temperature is 160-180 degrees. The edge-sealed finished product is cured at 200 degrees for 6 hours in the curing box.

[0097] It is worth mentioning that in the rubber refining process s2, the rubber is selected from the group consisting of fluororubber and silicone rubber, and further, the fluororubber is implemented as a binary structure or a ternary structure fluororubber. The silicone rubber is implemented as methyl vinyl silicone rubber. The heat-resistant filler is selected from the group consisting of precipitated barium sulfate and vermiculite. The reinforcing material is implemented as precipitated white carbon black. The foaming material is implemented as expandable microspheres. The cross-linking agent is selected from the group consisting of bisphenol AF / BPP, peroxide BIPB, bis(24), bis(25) and HVA-2, TAIC. The acid absorber is selected from the group consisting of calcium hydroxide, magnesium oxide and zinc oxide. In particular, magnesium oxide is selected from highly active magnesium oxide. Calcium hydroxide is implemented as ultrafine calcium hydroxide. The flow agent is selected from the group consisting of fluoro wax, mustard amine, palm wax, and modelling.

[0098] Further, by mass proportion: fluororubber 85, silicone rubber 15, precipitated silica 10, vermiculite 10, precipitated barium sulfate 5, expandable microspheres 10, bisphenol AF 2, BPP 1, diisocyanate peroxide 1.5, HVA-2 1.5, magnesium oxide 3, calcium oxide 6, fluorowax 1, and mustard amine 1.5.

[0099] like Figure 2 As shown, this embodiment also provides a method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material, which comprises the following steps:

[0100] (A) forming a surface layer 10 by a coating process S1;

[0101] (B) forming a rubber layer 22 through a rubber refining process S2;

[0102] (C) combining the rubber layer 22 and a second substrate 21 to form a middle layer 20 through a calendering and rubbing process S3;

[0103] (D) bonding the surface layer 10 and the middle layer 20 through a vulcanization process S4; and

[0104] (E) The heat-resistant and temperature-resistant elastic rubber pad 1 is formed through a cutting and edge-sealing process S5.

[0105] In step (A), the coating process includes forming a protective layer 12 on a first substrate 11, wherein the protective layer 12 is implemented as a water-based Teflon coating. The protective layer 12 has a curing thickness of 0.08-0.10 mm, a curing temperature of 250-360 degrees, and a curing time of 15-30 minutes.

[0106] In step (A), the surface layer 10 is treated with a silane coupling agent and then coated with a fluorine coating, and then cured by baking in an oven at 250-360° C. for 15-30 minutes.

[0107] In step (A), the first substrate is implemented as a glass fiber mesh cloth.

[0108] In step (B), the rubber refining process S2 includes a high temperature resistant compounding process S201, a high temperature resistant mixing process S202, a high temperature resistant open refining process S203, and a high temperature resistant refining process S204.

[0109] In the high temperature resistant compounding process S201, the rubber is cut into pieces according to a certain proportion, a certain proportion of heat-resistant filler, foaming material and flow agent are weighed and put into a feeding bag, a certain proportion of acid absorber is put into the feeding bag, and a certain proportion of cross-linking agent is put into a container.

[0110] In the high temperature resistant mixing process S202, the cut rubber is put into the mixing chamber for kneading. When the temperature rises to a first preset temperature, the heat-resistant filler, foaming material, flow agent and part of the acid absorber in the feeding bag are put in and then pressurized and kneaded. When the temperature rises to a second preset temperature, the remaining acid absorber is put in. When it rises to a third preset temperature again, the cross-linking agent is put in, and then a hammer is dropped to form a mixed rubber. The first preset temperature is implemented as 50-60 degrees; the second preset temperature is implemented as 80 degrees; and the third preset temperature is implemented as 90-95 degrees. Further, a 35-liter internal mixer is used, the air hammer pressure of the internal mixer is set to 0.6MPa, and the cooling water temperature is set to less than 30 degrees. The rubber is put into the mixing chamber and kneaded. When the temperature rises to 50-60 degrees, the heat-resistant filler, foaming material, flow agent and part of the acid absorber in the feeding bag are put in and pressurized and kneaded. When the temperature rises to 80 degrees, the hammer is lifted, the mixing chamber is cleaned, and the remaining acid absorber is added. When the temperature rises to 90-95 degrees, the hammer is lifted, the mixing chamber is cleaned, and the cross-linking agent is added. After the hammer falls for 30 seconds, the mixed rubber is formed.

[0111] In the high temperature resistant open refining process S203, the mixed rubber is put into an open refining mill, the roller distance is adjusted to 0.5-1mm, the mixed rubber passes through the rollers three times, the triangular package is made three times, and the roller distance is adjusted to 5-10mm to form a film. The film is a thick film.

[0112] In the high temperature resistant refining process S204, the rubber sheet is put into an internal mixer, and then put into the open mixer after internal mixing to form the rubber layer 22. Specifically, the rubber sheet is put into an internal mixer, and after 40-80 seconds, the hammer is lifted and cleaned once, and the material is unloaded when the temperature rises to 70-80 degrees, and then put into the open mixer after internal mixing to form the rubber layer 22.

[0113] In step (C), in the calendering and rubbing process S3, the upper, middle and lower roller temperatures of a calender are set to 70-85°C, the calendering roller distance is adjusted to a required rubber layer thickness, and the feed mill roller temperature is set to 55-65°C to stabilize the feed. The rubber layer thickness is 0.1-0.18mm, which can be determined according to the process requirements. The second substrate 21 is guided through the calender, the rubber layer 22 is evenly rubbed into the surface of the second substrate 21, and the cloth is rolled up into a roll.

[0114] In step (D), in the vulcanization process, the two surface layers 10 and at least one middle layer 20 are introduced into a vulcanizer, the two surface layers 10 are respectively the upper layer and the lower layer, and the middle layer 20 is located between the two surface layers 10. The number of layers of the middle layer 20 is calculated according to the required material thickness. The plate is continuously vulcanized through the vulcanizer, wherein the pressure of the vulcanizer is 30-45kg / cm2, the vulcanization pressing time is 15-30Min, and the temperature is 160-180 degrees.

[0115] In step (E), the heat-resistant and temperature-resistant elastic rubber pad 1 sealed in the cutting and sealing process S5 is cured in the curing box at 200 degrees for 6 hours.

[0116] like Figure 1A , Figure 1B and Figure 3 As shown, a heat-resistant and heat-resistant elastic rubber pad of a copper-clad laminate composite material and a manufacturing method thereof according to the second preferred embodiment of the present invention. The heat-resistant and heat-resistant elastic rubber pad 1 includes at least one surface layer 10 and at least one middle layer 20. The surface layer 10 and the middle layer 20 are subjected to a vulcanization process to form the heat-resistant and heat-resistant elastic rubber pad 1. It is worth mentioning that the middle layer 20 is provided according to the required number of layers. In other words, the heat-resistant and heat-resistant elastic rubber pad of the copper-clad laminate composite material is formed by a multi-layer composite of the surface layer 10 and the middle layer 20. In particular, the heat-resistant and heat-resistant elastic rubber pad 1 is composed of two surface layers 10 and at least one middle layer 20, wherein the middle layer 20 is provided between the two surface layers 10, as shown in FIG. Figure 1AAs shown. In addition, the surface layer 10 includes a first substrate 11 and a protective layer 12. The middle layer 20 includes a second substrate 21 and a rubber layer 22. The rubber layer 22 is combined with the second substrate 21 by a calendering and rubbing process. During the vulcanization process, the first substrate 11, the protective layer 12 and the middle layer 20 are combined at the same time, wherein the protective layer 12 is located on the surface of the first substrate 11. It can be understood that the structure of the heat-resistant and temperature-resistant elastic rubber pad 1 is the protective layer 12, the first substrate 11, the middle layer 20, the first substrate 11, and the protective layer 12, wherein the number of layers or thickness of the middle layer 20 is adjusted according to actual needs. In addition, as Figure 1B As shown, the heat-resistant and temperature-resistant elastic rubber pad 1 can also be composed of a surface layer 10 and at least one middle layer 20, which is not a limitation of the present invention.

[0117] The first substrate 11 of the surface layer 10 is implemented as a glass fiber mesh cloth. The protective layer 12 includes rubber, heat-resistant material, reinforcing material, cross-linking agent, and colorant. It is worth mentioning that the mass fractions of the protective layer 12 are as follows:

[0118] Rubber: 100

[0119] Heat-resistant material: 15-25

[0120] Reinforcement material: 15-35

[0121] Crosslinking agent: 2-6

[0122] Pigment: 1-3

[0123] The second substrate 21 of the middle layer 20 is implemented as a glass fiber mesh cloth. The rubber layer 22 is formed by a rubber refining process S2. The materials for refining the rubber layer 22 include rubber, heat-resistant filler, foaming material, cross-linking agent, acid absorbent, and flow agent, wherein the mass fractions are as follows:

[0124] Rubber: 100

[0125] Reinforcement material: 10-15

[0126] Heat-resistant filler: 15-30

[0127] Foam material: 5-30

[0128] Crosslinking agent: 3-6

[0129] Acid absorbent: 5-10

[0130] Flow agent: 1-3

[0131] The rubber refining process S2 includes a high temperature resistant compounding process S201, a high temperature resistant mixing process S202, a high temperature resistant refining process S203, and a high temperature resistant refining process S204.

[0132] In the high temperature resistant compounding process S201, the rubber is cut according to a certain ratio, the heat-resistant filler, the foaming material, and the flow agent are weighed and put into a feeding bag according to a certain ratio, the acid absorber is weighed and put into the feeding bag according to the ratio, and the cross-linking agent is weighed and put into a container according to the ratio.

[0133] In the high temperature resistant mixing process S202, the cut rubber is put into a mixing chamber and hammered. When the temperature rises to a first preset temperature, a feeding bag containing heat-resistant fillers, foaming materials, flow agents and part of the acid absorber is put into the mixing chamber. When the temperature rises to a second preset temperature, the remaining acid absorber is put into the mixing chamber. When the temperature rises to a third preset temperature, a cross-linking agent is put into the mixing chamber, and then the hammer is dropped to form a mixed rubber. It is worth mentioning that the first preset temperature is implemented as 50-60 degrees; the second preset temperature is implemented as 80 degrees; and the third preset temperature is implemented as 90-95 degrees. Further, a 35-liter internal mixer is used, the air hammer pressure of the internal mixer is set to 0.6MPa, and the cooling water temperature is set to less than 30 degrees. The rubber is put into the internal mixing chamber and hammered. When the temperature rises to 50-60 degrees, a feeding bag containing heat-resistant fillers, foaming materials, flow agents and part of the acid absorber is put into the mixing chamber. When the temperature rises to 80 degrees, the hammer is lifted, the mixing chamber is cleaned, and the remaining acid absorber is added. When the temperature rises to 90-95 degrees, the hammer is lifted, the mixing chamber is cleaned, and the cross-linking agent is added. After the hammer falls for 30 seconds, the mixed rubber is formed.

[0134] In the high temperature resistant open refining process S203, the mixed rubber is put into an open mill to form a film. Specifically, the open mill adopts a 16-inch open mill, and the cooling water temperature is set to less than 30 degrees. The mixed rubber is quickly put into the open mill, and after two thin passes, the roller distance is 0.5-1mm, so that the mixed rubber is quickly cooled. Then, the triangular package is made three times, and after three rollers, the roller distance is adjusted to 5-10mm, and the film is produced.

[0135] In the high temperature resistant refining process S204, the rubber sheet is put into an internal mixer, and then put into the open mixer after internal mixing to form the rubber layer 22. Specifically, the rubber sheet is put into an internal mixer, and after 40-80 seconds, the hammer is lifted and cleaned once, and the material is unloaded when the temperature rises to 70-80 degrees, and then put into the open mixer after internal mixing to form the rubber layer 22.

[0136] In the calendering and rubbing process S3, the rubber layer 22 is combined with the second substrate 21, and the finished product is rolled into a roll. In other words, the rubber layer 22 is combined with the glass fiber mesh cloth to form the rolled middle layer 20. Further, the temperature of the calendering cloth drying roller is set to 95 degrees, the temperature of the upper, middle and lower rollers is 70-85 degrees Celsius, the calendering roller distance is adjusted to the required rubber layer thickness, such as 0.1-0.18mm determined according to the process requirements, and the line speed, the second substrate 21 is guided through the calender, the rubber layer 22 is evenly rubbed into the surface of the second substrate 21, and the cloth is rolled up into a roll.

[0137] In particular, in this embodiment, the protective layer 12 is formed into a plastic film through a protective layer refining process S1'. It is worth mentioning that the protective layer 12 formed by the protective layer refining process S1' is also stored in a roll for subsequent use. The protective layer refining process S1' is the same process as the rubber refining process S2.

[0138] In the vulcanization process S4, the surface layer 10 and the middle layer 20 are introduced into a vulcanizer respectively for vulcanization pressing, and are cut and sealed after cooling to form the heat-resistant and temperature-resistant elastic rubber pad 1. Further, after the protective layer 12 of the surface layer 10, the first substrate 11 and the middle layer 20 are vulcanized and pressed, they are moved to a cooling rack for cooling, and then placed in a cutting table for cutting into a preset size. Then, a sealing glue is applied to the edge of the cut finished product and placed in a curing box for curing. That is to say, in this embodiment, a protective layer 12, a first substrate 11, at least one middle layer 20, a first substrate 11 and a protective layer 12 are introduced into the vulcanizer respectively. In particular, the pressure of the vulcanizer is 35kg / cm2, the vulcanization pressing time is 30Min, and the temperature is 160 degrees. The heat-resistant and temperature-resistant elastic rubber pad 1 is sealed and cured at 200 degrees for 6 hours in the curing box.

[0139] It is worth mentioning that in the rubber refining process of the middle layer 20, the rubber is selected from the group consisting of fluororubber and silicone rubber, and further, the fluororubber is implemented as a binary structure or a ternary structure fluororubber. The silicone rubber is implemented as methyl vinyl silicone rubber. The heat-resistant filler is selected from the group consisting of precipitated barium sulfate and vermiculite. The reinforcing material is implemented as precipitated white carbon black. The foaming material is implemented as expandable microspheres. The cross-linking agent is selected from the group consisting of bisphenol AF / BPP, peroxide bis(2,4-dione) and TAIC. The acid absorber is selected from the group consisting of calcium hydroxide, magnesium oxide and zinc oxide. In particular, magnesium oxide is selected from highly active magnesium oxide. Calcium hydroxide is implemented as ultrafine calcium hydroxide. The flow agent is selected from the group consisting of fluoro wax, mustard amine, palm wax and modelling. Further, by mass proportion: fluororubber 90, silicone rubber 10, precipitated silica 15, vermiculite 10, precipitated barium sulfate 5, expandable microspheres 10, bisphenol AF 1.5, BPP 0.8, diquaternary peroxide 1, TAIC 1.5, magnesium oxide 3, calcium hydroxide 6, fluorowax 1, and erucic acid 1.5.

[0140] It is worth mentioning that in the rubber refining process of the protective layer 12, the rubber is selected from the group consisting of fluororubber and silicone rubber, and further, the fluororubber is implemented as a binary structure or a ternary structure fluororubber. The silicone rubber is implemented as methyl vinyl silicone rubber. The heat-resistant filler is selected from the group consisting of precipitated barium sulfate and vermiculite. The reinforcing material is implemented as precipitated white carbon black. The cross-linking agent is selected from the group consisting of bisphenol AF / BPP, peroxide bis(24) and TAIC. The colorant is selected from the group consisting of carbon black and titanium dioxide. Further, by mass fraction: fluororubber 90, silicone rubber 10, precipitated white carbon black 15, vermiculite 10, precipitated barium sulfate 5, bisphenol AF 1.5, BPP 0.8, peroxide bis(24) 1, TAIC 1.5, carbon black 0.5, titanium dioxide 1.

[0141] like Figure 3 As shown, this embodiment also provides a method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material, which comprises the following steps:

[0142] (a) a protective layer refining process S1' forms a protective layer 12 of a surface layer 10;

[0143] (b) a rubber refining process S2 to form a rubber layer 22;

[0144] (c) combining the rubber layer 22 and a second substrate 21 to form a middle layer 20 through a calendering and rubbing process S3;

[0145] (d) bonding the protective layer 12, a first substrate 11 and the middle layer 20 through a vulcanization process S4; and

[0146] (e) The heat-resistant and temperature-resistant elastic rubber pad 1 is formed through a cutting and edge-sealing process S5.

[0147] In step (d), the protective layer 12, the first substrate 11 of the surface layer 10, at least one middle layer 20, the first substrate 11 and the protective layer 12 are sequentially stacked, introduced into a vulcanizer and vulcanized into one.

[0148] Those skilled in the art should understand that the embodiments of the present invention described above and shown in the accompanying drawings are only for illustrative purposes and are not intended to limit the present invention.

[0149] The purpose of the present invention has been completely and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments, and the embodiments of the present invention may be deformed or modified in any way without departing from the principles.

Claims

1. A heat-resistant and temperature-resistant elastic rubber pad of a copper-clad laminate composite material, characterized in that: include: At least one surface layer, wherein each surface layer comprises a first substrate and a protective layer, wherein the protective layer is located on a surface of the first substrate; and At least one middle layer, wherein each middle layer comprises a second substrate and a rubber layer, the rubber layer is bonded to the second substrate by a calendering and rubbing process, and the surface layer and the middle layer are bonded by a vulcanization process; wherein the first substrate and the second substrate are implemented as glass fiber mesh cloth; At least one of the middle layers is disposed between the two surface layers to perform a multi-layer vulcanization combination, wherein the protective layers of the surface layers are respectively located on the outside; In the calendering and rubbing process, the upper, middle and lower roller temperatures of a calender are set to 70-85°C, the calendering roller distance is adjusted to a required rubber layer thickness, and the roller temperature of a feeding mill is set to 55-65°C to stabilize the feeding; the thickness of the rubber layer is 0.1-0.18mm, which can be determined according to the process requirements; the second substrate is guided through the calender, the rubber layer is evenly rubbed into the surface of the second substrate, and the cloth is rolled up; In the vulcanization process, the two surface layers and at least one middle layer are introduced into a vulcanizer, the two surface layers are respectively an upper layer and a lower layer, and the middle layer is located between the two surface layers; the number of layers of the middle layer is calculated according to the required material thickness; the plate is continuously vulcanized through the vulcanizer, wherein the pressure of the vulcanizer is 30-45kg / cm 2 The vulcanization pressing time is 15-30 minutes and the temperature is 160-180 degrees.

2. The heat-resistant and temperature-resistant elastic rubber pad according to claim 1, wherein the protective layer comprises PTFE powder, pigment, water-based Teflon coating, thickener, and curing agent, wherein the mass fractions are as follows: PTFE powder: 30 Pigments: 4 Water-based Teflon coating: 100 Thickener: 10 Curing agent:

6.

3. The heat-resistant and temperature-resistant elastic rubber pad according to claim 1, wherein the protective layer comprises rubber, heat-resistant material, reinforcing material, cross-linking agent, and colorant, wherein the mass fractions are as follows: Rubber: 100 Heat-resistant material: 15-25 Reinforcement material: 15-35 Crosslinking agent: 2-6 Pigment: 1-3.

4. The heat-resistant and temperature-resistant elastic rubber pad according to claim 1, wherein the material of the rubber layer includes rubber, heat-resistant filler, foaming material, cross-linking agent, acid absorber, and flow agent, wherein the mass fractions are as follows: Rubber: 100 Reinforcement material: 10-15 Heat-resistant filler: 15-30 Foam material: 5-30 Crosslinking agent: 3-6 Acid absorbent: 5-10 Flowing agent: 1-3.

5. The heat-resistant and temperature-resistant elastic rubber pad according to claim 2, wherein the cured thickness of the protective layer is 0.08-0.10 mm.

6. The heat-resistant and temperature-resistant elastic rubber pad according to claim 3 or 4, wherein the rubber is selected from the group consisting of fluororubber and silicone rubber.

7. The heat-resistant and temperature-resistant elastic rubber pad according to claim 4, wherein the heat-resistant filler is selected from the group consisting of precipitated barium sulfate, mica and vermiculite.

8. The heat-resistant and temperature-resistant elastic rubber pad according to claim 3 or 4, wherein the reinforcing material is precipitated silica.

9. The heat-resistant elastic rubber pad according to claim 3 or 4, wherein the cross-linking agent is selected from the group consisting of bisphenol AF / BPP, peroxide BIPB, bis(2,4), bis(2,5), HVA-2, and TAIC.

10. The heat-resistant and temperature-resistant elastic rubber pad according to claim 3, wherein the colorant is selected from the group consisting of carbon black, masterbatch and titanium dioxide.

11. The heat-resistant and temperature-resistant elastic rubber pad according to claim 4, wherein the foaming material is implemented as expandable microspheres.

12. The heat-resistant and temperature-resistant elastic rubber pad according to claim 4, wherein the acid absorber is selected from the group consisting of calcium hydroxide, magnesium oxide and zinc oxide.

13. The heat-resistant and temperature-resistant elastic rubber pad according to claim 4, wherein the flow agent is selected from the group consisting of fluoro wax, mustard amine, palm wax and modelling agent.

14. A method for manufacturing the heat-resistant and temperature-resistant elastic rubber pad of the copper-clad laminate composite material according to claim 1, characterized in that: The steps include: (A) forming a surface layer by a coating process; (B) forming a rubber layer through a rubber refining process; (C) combining the rubber layer with a second substrate to form a middle layer through a calendaring and rubbing process; (D) bonding the surface layer and the middle layer by a vulcanization process; and (E) The heat-resistant and temperature-resistant elastic rubber pad is formed through a cutting and edge-sealing process.

15. The method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad according to claim 14, wherein in step (A), the coating process includes forming a protective layer on a first substrate, wherein the protective layer is implemented as a water-based Teflon coating, and the curing thickness of the protective layer is 0.08-0.10 mm, the curing temperature is 250-360 degrees, and the curing time is 15-30 minutes.

16. The method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad according to claim 14, wherein in step (B), the rubber refining process includes a high-temperature resistant compounding process, a high-temperature resistant mixing process, a high-temperature resistant open refining process, and a high-temperature resistant refining process, wherein in the high-temperature resistant compounding process, the rubber is cut according to a certain ratio, a certain ratio of heat-resistant filler, foaming material, and flow agent are weighed and put into a feeding bag, a certain ratio of acid absorber is put into the feeding bag, and a certain ratio of cross-linking agent is put into a container, wherein in the high-temperature resistant mixing process, the cut rubber is put into a mixing chamber for kneading, and when the temperature rises to 50-60 degrees, it is put into the The heat-resistant filler, foaming material, flow agent and part of the acid absorber in the feeding bag are pressed and kneaded. When the temperature rises to 80 degrees, the hammer is lifted, the mixing chamber is cleaned, and the remaining acid absorber is added. When the temperature rises to 90-95 degrees, the hammer is lifted, the mixing chamber is cleaned, and the cross-linking agent is added. After the hammer is dropped for 30 seconds, a mixed rubber is formed. In the high-temperature resistant open mixing process, the mixed rubber is put into an open mixing mill, the roller distance is adjusted to 0.5-1mm, the rubber passes through three rollers, and the triangular bag is made three times. The roller distance is adjusted to 5-10mm to form a film. In the high-temperature resistant re-mixing process, the film is put into an internal mixer, and then put into the open mixing mill after internal mixing to form the rubber layer.

17. The method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad according to claim 14, wherein in step (C), the temperature of the upper, middle and lower rollers of a calender is set to 70-85°C, the calender roller spacing is adjusted to the required rubber layer thickness, the roller temperature of a feeding mill is set to 55-65°C to stabilize the feeding, the second substrate is guided through the calender, and the rubber layer is evenly rubbed into the surface of the second substrate, the thickness of the rubber layer can be adjusted between 0.1-0.2mm, the rubbing width is 1420mm, and the thickness range is 0.05mm.

18. The method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad according to claim 15, wherein in step (D), at least one of the middle layers is located between the two surface layers, and the protective layer of the surface layer is an outer layer.

19. The method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad according to claim 14, wherein in step (E), the heat-resistant and temperature-resistant elastic rubber pad is cured at 200 degrees for 6 hours in a curing box.

20. A method for manufacturing the heat-resistant and temperature-resistant elastic rubber pad of the copper-clad laminate composite material according to claim 1, characterized in that: The steps include: (a) a protective layer refining process forms a protective layer on one side; (b) a rubber refining process to form a rubber layer; (c) combining the rubber layer with a second substrate to form a middle layer through a calendering and rubbing process; (d) bonding the protective layer, a first substrate and the middle layer by a vulcanization process; and (e) The heat-resistant and temperature-resistant elastic rubber pad is formed through a cutting and edge-sealing process.

21. The method for manufacturing a heat-resistant and temperature-resistant elastic rubber pad according to claim 20, wherein in step (d), the protective layer, the first substrate, at least one middle layer, the first substrate and the protective layer are sequentially introduced into a vulcanizer in a stacked manner and combined into one through vulcanization.

Citation Information

Patent Citations

  • Additive material formula of halogen-free CEM-1 composite substrate copper-clad plate

    CN106675480A

  • Packing contained composite material, sheet and circuit board containing same

    CN106928660A

  • Thermosetting resin composition and application thereof

    CN110835451A

  • Dielectric material based on ethylene propylene diene monomer, prepreg and laminated plate

    CN111333965A

  • Chushioning material for forming press

    CN1129171A