Optical laminate, method for manufacturing the same, and display device
By using an optical film with adhesive on both sides in a frameless display device and using an ultraviolet laser to form openings, the problem of optical component processing alignment and adhesive layer problems is solved, and production efficiency and finished product quality are improved.
Patent Information
- Application Number
- CN202010228422.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-03-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-03-27
AI Technical Summary
In a display device with a frameless design, it is difficult to accurately align the opening processing of optical components, and problems such as poor processing of the adhesive layer and the inclusion of air bubbles result in low productivity and yield.
Optical films with adhesives on both sides are used. By setting transparent adhesive layers on both sides of the optical film, and using ultraviolet laser to form openings, the ultraviolet absorption of the adhesive layer is ensured to improve processing accuracy and production efficiency.
It simplifies the alignment process of optical components, improves productivity and yield, and reduces poor processing and air bubble mixing in the adhesive layer.
Smart Images

Figure CN111856640B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical laminate comprising an optical film and an adhesive and a method for producing the same. In addition, the present invention relates to a display device comprising an image display element and an optical element. Background Art
[0002] Mobile phones, smart phones, car navigation devices, monitors for personal computers, televisions, etc. are display devices having image display elements, and have liquid crystal display devices and organic electroluminescent (EL) display devices as image display elements. Liquid crystal display devices are provided with polarizing plates on the visible side surface of the image display unit due to their display principles. In addition, in organic EL display devices, in order to suppress external light from being reflected by the metal electrode (cathode) and observed like a mirror surface, a circular polarizing plate (a laminate of a polarizing plate and a 1 / 4 wavelength plate) is sometimes provided on the visible side surface of the image display unit.
[0003] In order to prevent damage to the image display unit due to impact from the external surface, a transparent front plate such as a transparent resin plate or a glass plate (also called a "cover window") is sometimes provided on the visible side of the image display unit. In a display device in which a cover window is provided on the front side of the image display unit, the image display unit and the cover window are attached via an adhesive sheet.
[0004] It is proposed to use an optical film with adhesive on both sides for forming a display device having an optical film such as a polarizing plate attached to the surface of an image display unit and having a cover window on the visible side surface thereof (e.g., Patent Document 1). In the optical film with adhesive on both sides, an adhesive layer for attaching to the image display unit is provided on one side of the optical film, and an adhesive layer for attaching to the cover window, etc. is provided on the other side of the optical film.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-157077 Summary of the invention
[0008] Problems to be solved by the invention
[0009] In display devices such as smartphones, tablet terminals, and notebook computers, light receiving elements such as cameras and light sensors and light emitting elements such as LEDs are usually arranged in the frame area outside the display area. In recent years, the frameless display device (made into a full-screen display) is developing, mainly in mobile devices such as smartphones.
[0010] With the borderless design, it is necessary to change the configuration of the optical elements (light receiving elements and / or light emitting elements) arranged in the border area in the previous display device. The following method is proposed: in a display device with a borderless design, an opening is set in the display area of the display, and optical elements such as a camera are accommodated below or in the opening. Since the opening set in the display area can be observed from the outside, it is expected that the shape of the opening is uniform. Therefore, a method of forming an opening by processing using an ultraviolet laser with less thermal damage and high processing accuracy is studied.
[0011] When openings are formed on optical components such as polarizing plates and adhesive sheets by laser processing and then the components are bonded together, it is not easy to accurately align the positions of the openings between the multiple optical components. It is believed that if an adhesive layer is pre-laminated on the optical component and then an ultraviolet laser is irradiated to form the opening, alignment between the components is not necessary, thereby improving productivity and yield.
[0012] However, when an opening is formed by irradiating a laminate having an adhesive layer with an ultraviolet laser, processing failure of the adhesive layer, mixing of bubbles in the adhesive layer, peeling at the bonding interface of the adhesive layer, mixing of bubbles in the bonding interface, etc. may occur. In view of these problems, an object of the present invention is to provide an optical laminate for a display device having excellent processability using an ultraviolet laser or the like, and an optical laminate having an opening penetrating a plurality of optical components.
[0013] Means used to solve problems
[0014] The optical laminate of the present invention comprises: an optical film including a polarizer, a first adhesive layer provided on one main surface of the optical film, a first adherend bonded to the first adhesive layer, a second adhesive layer provided on the other main surface of the optical film, and a second adherend bonded to the second adhesive layer. The adherend bonded to the adhesive layer may be fixedly laminated on the adhesive layer or temporarily bonded to the adhesive layer.
[0015] The first adhesive layer and the second adhesive layer are transparent adhesive layers with a transmittance of 85% or more for light with a wavelength of 420 nm. The first adhesive layer has ultraviolet absorption and a transmittance of 80% or less for light with a wavelength of 355 nm. The transmittance of the first adhesive layer for light with a wavelength of 355 nm may be 20% or more.
[0016] The thickness of the first adhesive layer is, for example, 30 μm or more. The storage elastic modulus of the first adhesive layer at 25° C. is preferably 0.35 MPa or less. The first adhesive layer may be a photocurable adhesive containing a photocurable compound and a photopolymerization initiator.
[0017] The second adhesive layer may or may not be ultraviolet absorbing. The thickness of the second adhesive layer may be less than the thickness of the first adhesive layer. When the thickness of the second adhesive layer is greater than 30 μm, the second adhesive layer preferably has ultraviolet absorbing properties, and the transmittance of light of a wavelength of 355 nm is preferably 80% or less. The transmittance of light of a wavelength of 355 nm of the second adhesive layer may be greater than the transmittance of light of a wavelength of 355 nm of the first adhesive layer. The storage elastic modulus of the second adhesive layer at 25° C. may be greater than the storage elastic modulus of the first adhesive layer at 25° C.
[0018] The optical film may have a resin film on one side or both sides of the polarizer. The transmittance of the resin film bonded to the polarizer at a wavelength of 355 nm may be 10% or less.
[0019] As an adherend temporarily attached to the adhesive layer, a release film can be cited. The adherend fixedly laminated on the first adhesive layer is, for example, a cover window. The adherend fixedly laminated on the second adhesive layer is, for example, an image display unit. The image display unit is, for example, an organic EL unit, and the organic EL unit may include a polyimide film.
[0020] An opening (through hole) penetrating the first adherend, the first adhesive layer, the optical film, the second adhesive layer, and the second adherend is formed by irradiating the main surface of the first adherend side or the main surface of the second adherend side of the optical laminate. The adherend arranged on the irradiation surface of the ultraviolet laser preferably has ultraviolet absorption, and the transmittance of light with a wavelength of 355nm is preferably 70% or less.
[0021] For example, when forming a through hole by irradiating an optical laminate having release films temporarily attached to the first adhesive layer and the second adhesive layer with ultraviolet laser, it is preferred that the transmittance of light at a wavelength of 355 nm of the release film on either side is 70% or less. The transmittance of light at a wavelength of 355 nm of the release film on the ultraviolet irradiation side may be 15% or more.
[0022] The through hole can also be formed by irradiating an optical laminate having a release film temporarily attached to the first adhesive layer and an image display unit fixedly laminated on the second adhesive layer with an ultraviolet laser. In the case of irradiating the ultraviolet laser from the image display unit side, it is preferred that the image display unit has ultraviolet absorption. For example, in the case where the image display unit includes a polyimide film, the polyimide film has ultraviolet absorption. In the case of irradiating the ultraviolet laser from the release film side, it is preferred that the release film has ultraviolet absorption. In this case, the transmittance of light of a wavelength of 355nm of the release film is preferably 15% to 70%.
[0023] The adherend on the adhesive layer can be replaced with another adherend. For example, the release film temporarily attached to the second adhesive layer can be peeled off and the image display unit can be attached, or the release film temporarily attached to the first adhesive layer can be peeled off and the cover window can be attached. In addition, the release film temporarily attached to the adhesive layer can be replaced with another release film.
[0024] The adherend may be replaced after the through hole is formed. For example, a through hole may be formed in an optical laminate in which a release film is temporarily attached to a first adhesive layer and an image display unit is fixedly laminated on a second adhesive layer, and then the release film is peeled off from the first adhesive layer and a cover window is attached to the first adhesive layer.
[0025] By disposing an optical element in or below the through hole, a display device including an image display element and an optical element is formed. Examples of the optical element disposed in or below the through hole include light receiving elements such as cameras and optical sensors, and light emitting elements such as LEDs.
[0026] Effects of the Invention
[0027] The optical laminate of the present invention has excellent processability using ultraviolet lasers because the adherend on the laser irradiation surface and the adhesive layer also have ultraviolet absorbency, and can be used to form a display device in which optical elements such as cameras are arranged in the display area of the display. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1A This is a perspective view of an optical layered body according to one embodiment.
[0029] Figure 1B This is a cross-sectional view of an optical layered body according to one embodiment.
[0030] Figure 2 This is a cross-sectional view of an optical layered body according to one embodiment.
[0031] Figure 3 This is a cross-sectional view of an optical layered body according to one embodiment.
[0032] Figure 4 A cross-sectional view of a display device according to one embodiment.
[0033] Figure 5 This is a cross-sectional view of an optical layered body according to one embodiment.
[0034] Figure 6 This is a cross-sectional view of an optical layered body according to one embodiment.
[0035] Figure 7 It is a cross-sectional view showing a mid-stage of the process of cutting out a single optical layered body from a mother substrate.
[0036] Figure 8 It is a cross-sectional view showing a mid-stage of the process of cutting out a single optical layered body from a mother substrate.
[0037] Fig. 9 This is a cross-sectional view of an optical layered body according to one embodiment.
[0038] Fig.10 This is a cross-sectional view of an optical layered body according to one embodiment.
[0039] Fig.11 This is a cross-sectional view of an optical layered body according to one embodiment.
[0040] Fig.12 This is a cross-sectional view of an optical layered body according to one embodiment.
[0041] Fig.13 It is a cross-sectional view showing a mid-stage of the process of cutting out a single optical layered body from a mother substrate.
[0042] Fig.14 This is a microscopic photograph of a mold release film in which bubbles were generated around the through-holes.
[0043] Reference numerals
[0044] 10 Optical film
[0045] 11. Polarizer
[0046] 13, 15 Transparent film
[0047] 21, 22 Adhesive layer
[0048] 25 Optical film with adhesive on both sides
[0049] 41, 42, 43, 46, 47, 48 Release film
[0050] 49 slide(キャリアシート)
[0051] 70 Image display unit (organic EL unit)
[0052] 5, 7, 8, 9 through holes
[0053] 101, 102, 103, 105, 106, 109, 110, 111, 112 Optical laminate
[0054] 91 Optical Components
[0055] 204 Display device DETAILED DESCRIPTION
[0056] The optical laminate of the present invention comprises: an optical film including a polarizer, and adhesive layers arranged on both sides of the optical film. An adherend is attached to each adhesive layer arranged on both sides of the optical film. The adherend can be fixedly laminated on the adhesive layer, or can be releasably attached (temporarily attached) to the adhesive layer. At least one of the adhesive layers arranged on both sides of the optical film has ultraviolet absorption.
[0057] One embodiment of the optical laminate has a through hole that penetrates the optical film and the adhesive layers disposed on both sides of the optical film. The through hole may also penetrate the adherend attached to the surface of the adhesive layer. Another embodiment of the optical laminate is a laminate before the through hole is formed, and since at least one of the adhesive layers disposed on both sides of the optical film has ultraviolet absorption, it is suitable for processing using ultraviolet laser.
[0058] Figure 1A 1 is a perspective view of an optical laminate 101 having a through hole. The optical laminate 101 has a first adhesive layer 21 (visible side adhesive layer) on one surface of an optical film 10, and a second adhesive layer 22 (unit side adhesive layer) on the other surface of the optical film 10. A release film 41 as a first adherend is temporarily attached to the first adhesive layer 21, and an image display unit 70 as a second adherend is fixed to the second adhesive layer 22. The optical laminate 101 is provided with a through hole 5 that penetrates the image display unit 70, the second adhesive layer 22, the optical film 10, the first adhesive layer 21, and the first release film 41.
[0059] Figure 1B is a cross-sectional view of the optical laminate 101, corresponding to Figure 1A The cross section of the BB line. Figure 2 1 is a cross-sectional view of an optical laminate 102 in which release films 41 and 42 are temporarily attached to both main surfaces of an optical film 25 with an adhesive on both sides. The optical film 25 with an adhesive on both sides has a first adhesive layer 21 on one main surface of the optical film 10 and a second adhesive layer 22 on the other main surface of the optical film 10. Release films 41 and 42 as adherends are temporarily attached to the surfaces of the adhesive layers 21 and 22. Figure 5 As shown, the release films 41 and 42 may protrude outward from the end surfaces of the optical film 25 with an adhesive on both sides.
[0060] The release film 42 temporarily attached to the second adhesive layer 22 is peeled off, and the image display unit 70 is attached to the second adhesive layer 22, thereby obtaining Figure 3 The optical stack 103 shown. Figure 3In the figure, the end faces of the optical components constituting the optical laminate 103 are aligned, but the end faces of the optical components may not be consistent. For example, the release film 41 may extend outward compared to the end face of the first adhesive layer 21, and the image display unit 70 may extend outward compared to the end face of the second adhesive layer 22.
[0061] The optical laminate 101 is formed by providing the through hole 5 in the optical laminate 103. If the laminate including the optical film 25 with adhesive on both sides is subjected to hole-forming processing, through holes penetrating the optical film 10 and the adhesive layers 21 and 22 arranged on both sides of the optical film 10 are formed, so that the hole-forming process can be simplified and the yield can be expected to be improved.
[0062] Will temporarily paste Figure 1B The first release film 41 on the first adhesive layer 21 of the optical laminate 101 shown in the figure is peeled off, and the cover window 80 is attached to the first adhesive layer 21, thereby obtaining Figure 4 The display device 204 shown. An optical element 91 is arranged below the through hole 5. The optical element 91 is, for example, a light receiving element such as a camera or a light sensor. By providing a through hole 5 that passes through the image display unit 70 to the first adhesive layer 21, light from the outside passes through the cover window 80 and reaches the optical element 91. In the case where the optical element 91 is a light emitting element, the light from the optical element 91 passes through the through hole 5 and the cover window 80 and then is emitted to the outside. The optical element 91 can be arranged in the through hole 5.
[0063] The through hole 5 of the optical stack 101 is formed, for example, by: Figure 3 The image display unit 70 side (lower side in the figure) of the stacked body 103 shown is irradiated with ultraviolet laser to perform hole drilling. If the hole drilling is performed in a manner that penetrates the stacked body 103 in a state where the optical film 10 and the image display unit 70 are stacked in advance, it is not necessary to align the holes during stacking, so the manufacturing process of the device can be simplified and the yield rate can be expected to be improved.
[0064] When the laminate 103 is irradiated with ultraviolet laser to perform hole-forming processing on the laminate, it is preferred that the adherend on the laser irradiation surface has ultraviolet absorptivity. For example, when the ultraviolet laser is irradiated from the image display unit 70 side of the laminate 103, it is preferred that the image display unit 70 has ultraviolet absorptivity. When the ultraviolet laser is irradiated from the first release film 41 side of the laminate 103, it is preferred that the first release film 41 has ultraviolet absorptivity.
[0065] The adherend passing through the laser irradiation surface has ultraviolet absorption, and the adherend absorbs the ultraviolet laser to generate heat and vaporize, and the adhesive layer, optical film, etc. provided on the adherend are dissipated along with the vapor, thereby forming a through hole.
[0066] In order to effectively absorb the ultraviolet laser, the transmittance of the adherend at the laser irradiation surface at a wavelength of 355 nm is preferably 70% or less, more preferably 60% or less, and further preferably 50% or less. The transmittance of the adherend at the laser irradiation surface at a wavelength of 355 nm may be 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, or 1% or less.
[0067] When the image display unit 70 includes a polyimide film as the substrate 71 , since the polyimide film has high ultraviolet absorption, the hole-forming processability by ultraviolet laser irradiation from the image display unit 70 side is excellent.
[0068] The first adhesive layer 21 disposed on the visible side of the optical film 10 in the display device 204 may require high level absorption, and a thick and flexible adhesive layer is used. The first adhesive layer 21 has a thickness of, for example, 30 μm or more, and preferably has a storage elastic modulus of 0.35 MPa or less at 25° C.
[0069] As described above, if the component disposed on the laser irradiation surface has ultraviolet absorption, the component disposed thereon is also processed by laser. Therefore, if only a hole is formed, the adhesive layer and optical film disposed on the adherend do not necessarily need to have ultraviolet absorption. However, since the adhesive layer is soft and has lower processability than film materials, etc., sometimes the through hole is not formed sufficiently or bubbles are generated around the laser processed part.
[0070] In particular, the first adhesive layer 21 is sometimes required to have a high-grade absorption property, but due to its large thickness and softness, it is easy to cause processing failure during laser processing. Figure 3 In the optical laminate 103 shown, the first pressure-sensitive adhesive layer 21 and the release film 41 are temporarily attached. Since the adhesive force at the interface is weak, the release film may peel off from the pressure-sensitive adhesive layer around the laser irradiation area.
[0071] If the first adhesive layer 21 has ultraviolet absorption, the first adhesive layer 21 absorbs ultraviolet laser light, thereby improving processability and preventing processing defects, peeling of the release film, etc. The transmittance of the first adhesive layer 21 at a wavelength of 355 nm is preferably 80% or less, more preferably 75% or less.
[0072] The second adhesive layer 22 may also have ultraviolet absorption. In the case where the second adhesive layer has ultraviolet absorption, the transmittance of the second adhesive layer of light with a wavelength of 355nm is preferably 80% or less, and more preferably 75% or less. The second adhesive layer 22 used to bond the optical film 10 and the image display unit 70 generally does not require height difference absorption. Compared with the first adhesive layer 21, the second adhesive layer 22 is thinner and harder, so even if the second adhesive layer 22 does not have ultraviolet absorption, it is not easy to cause processing defects. In particular, when the thickness of the second adhesive layer 22 is 30μm or less, even if the second adhesive layer 22 does not have ultraviolet absorption, processing defects are almost not likely to occur.
[0073] [Components of the optical laminate]
[0074] Hereinafter, preferred embodiments of the respective optical elements constituting the optical layered body will be described in order.
[0075] <Image Display Unit>
[0076] exist Figure 1B , Figure 3 , Figure 4 In the optical laminate shown, the image display unit 70 is a top emission type organic EL unit, which has a metal electrode 73, an organic light emitting layer 75 and a transparent electrode 77 in sequence on a substrate 71. A sealing material 79 is stacked on the transparent electrode 77. Although not shown in the figure, the sealing material 79 is preferably provided in a manner covering the side surfaces of the electrodes 73, 77 and the organic light emitting layer 75.
[0077] As the substrate 71, a glass substrate or a plastic substrate can be used. In the top emission type organic EL unit, the substrate 71 does not need to be transparent, and a high heat-resistant film such as a polyimide film can also be used as the substrate 71. In addition to the organic layer that functions as a light-emitting layer, the organic light-emitting layer 75 can also have an electron transport layer, a hole transport layer, etc. The transparent electrode 77 is a metal oxide layer or a metal film that allows light from the organic light-emitting layer 75 to pass through. In order to protect or strengthen the substrate, a backplane (not shown) can be provided on the back side of the substrate 71.
[0078] The organic EL unit may also be a bottom emission type organic EL unit in which a transparent electrode, an organic light emitting layer, and a metal electrode are sequentially stacked on a substrate. In a bottom emission type organic EL unit, a transparent substrate is used, and the substrate is arranged on the visible side (the second adhesive layer 22 side). The image display unit is not limited to an organic EL unit, and may also be a liquid crystal unit, an electrophoretic display unit (electronic paper), etc. A touch panel sensor (not shown) may be arranged on the visible side surface of the image display unit 70.
[0079] <Optical Film>
[0080] The optical film 10 is bonded to the organic EL unit 70 via the second adhesive layer 22. The optical film 10 includes a polarizer 11. Transparent films 13 and 15 as polarizer protective films are laminated on both surfaces of the polarizer 11. The polarizer protective films on one or both surfaces of the polarizer may be omitted and an adhesive layer may be directly provided on the polarizer 11.
[0081] As the polarizer 11, for example, there can be listed: a polarizer obtained by adsorbing a dichroic substance such as iodine or a dichroic dye onto a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or a partially saponified film of ethylene-vinyl acetate copolymer and then uniaxially stretching it; a polyolefin oriented film such as a dehydrated product of polyvinyl alcohol or a dehydrochlorinated product of polyvinyl chloride, etc.
[0082] As the polarizer 11, a thin polarizer with a thickness of 10 μm or less may be used. Examples of the thin polarizer include polarizers described in Japanese Patent Application Laid-Open No. 51-069644, Japanese Patent Application Laid-Open No. 2000-338329, WO2010 / 100917, Japanese Patent No. 4691205, and Japanese Patent No. 4751481. The thin polarizer may be obtained, for example, by a manufacturing method including the steps of stretching a polyvinyl alcohol resin layer and a stretching resin substrate in a laminated state and dyeing with a dichroic material such as iodine.
[0083] As the transparent films 13 and 15, transparent resin films such as cellulose resins, cyclic polyolefin resins, acrylic resins, phenylmaleimide resins, and polycarbonate resins are preferably used. The transmittance of the transparent films 13 and 15 for light of a wavelength of 420 nm is preferably 85% or more. When the transparent films 13 and 15 are provided on both surfaces of the polarizer 11, the transparent films 13 and 15 may be films made of the same resin material or films made of different resin materials.
[0084] The transparent films 13 and 15 disposed on one or both surfaces of the polarizer 11 may have ultraviolet absorption. When the transparent films 13 and 15 have ultraviolet absorption, there is a tendency that the processability of the adhesive layers 21 and 22 disposed adjacent to the optical film 10 using ultraviolet laser is improved. The transmittance of the transparent film disposed on one or both surfaces of the polarizer 11 at a wavelength of 355 nm may be 10% or less, or 5% or less.
[0085] If the transparent film 13 disposed on the visible side of the polarizer 11 has ultraviolet absorption, ultraviolet rays contained in external light are absorbed by the transparent film 13, thereby suppressing the degradation of the polarizer 11 due to ultraviolet rays. The transmittance of the transparent film 13 for light of a wavelength of 355 nm may be 10% or less or 5% or less.
[0086] The transparent film can be given ultraviolet absorption by applying an ultraviolet absorption coating on the film surface or by including an ultraviolet absorber in the film. Examples of ultraviolet absorbers include benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, salicylate ultraviolet absorbers, triazine ultraviolet absorbers, and cyanoacrylate ultraviolet absorbers. As the transparent film, a resin material having ultraviolet absorption, such as polyethylene naphthalate (PEN), can be used.
[0087] The optical film 10 may have an optical functional film laminated on one or both surfaces of the polarizer 11 via an appropriate adhesive layer or adhesive layer as needed. As optical functional films, there can be listed: phase difference plate, viewing angle expansion film, viewing angle limiting (anti-peep) film, brightness enhancement film, etc. The optical film 10 may include a touch panel sensor as an optical functional film. The transparent films 13 and 15 in contact with the polarizer may have the functions of a polarizer protective film and an optical functional film. The transparent films 13 and 15 may also have the function of an electrode substrate film of a touch panel sensor.
[0088] The metal electrode 73 of the organic EL unit 70 is light reflective. Therefore, when external light enters the interior of the organic EL unit, the light is reflected on the metal electrode 73, and the reflected light is observed from the outside like a mirror. By configuring a circular polarizing plate as the optical film 10 on the visible side surface of the organic EL unit 70, it is possible to prevent the reflected light on the metal electrode 73 from being re-emitted to the outside, thereby improving the visibility and appearance design of the screen of the display device.
[0089] The circular polarizing plate has a phase difference film on the surface of the polarizer 11 on the side of the organic EL unit 70. The transparent film 15 arranged adjacent to the polarizer 11 can be a phase difference film. When the phase difference film has a delay of λ / 4 and the angle between the slow axis direction of the phase difference film and the absorption axis direction of the polarizer 11 is 45°, the stack of the polarizer and the phase difference film acts as a circular polarizing plate for suppressing the re-emission of reflected light on the metal electrode 73. The phase difference film constituting the circular polarizing plate can be a phase difference film obtained by stacking more than two layers of films. For example, by stacking polarizers, λ / 2 plates and λ / 4 plates in a manner such that their respective optical axes form a specified angle, a broadband circular polarizing plate that acts as a circular polarizing plate in a wide band of the entire visible light can be obtained.
[0090] <First Adhesive Layer>
[0091] The first adhesive layer 21 is disposed on the visible side of the optical film 10 in the display device 204, and is used to bond the optical film 10 to a transparent member such as a cover window 80. The first adhesive layer 21 is preferably a transparent adhesive sheet and has a high visible light transmittance. The transmittance of the first adhesive layer 21 at a wavelength of 420 nm is 85% or more, preferably 88% or more, and more preferably 90% or more. The haze of the first adhesive layer 21 is preferably 2% or less, and more preferably 1% or less.
[0092] The first adhesive layer 21 may be an adhesive layer obtained by laminating two or more adhesive sheets. The second adhesive layer 22 described later may also be an adhesive layer obtained by laminating two or more adhesive sheets. When the adhesive layer is a laminated adhesive sheet, the light transmittance and haze of the laminate are preferably within the above ranges.
[0093] As the adhesive constituting the adhesive layer 21, an adhesive having a base polymer such as acrylic polymer, polysiloxane polymer, polyester, polyurethane, polyamide, polyvinyl ether, vinyl acetate-vinyl chloride copolymer, modified polyolefin, epoxy, fluorine-containing, natural rubber, synthetic rubber, etc. can be appropriately selected and used.
[0094] As the adhesive constituting the first adhesive layer 21, an acrylic adhesive having an acrylic polymer as a base polymer is preferred, because it has excellent optical transparency, exhibits appropriate adhesive properties such as wettability, cohesiveness and tackiness, and is also excellent in weather resistance, heat resistance, etc. The adhesive constituting the second adhesive layer 22 described later is also preferably an acrylic adhesive as in the first adhesive layer 21. In the acrylic adhesive, the content of the acrylic base polymer is preferably 50% by weight or more, more preferably 70% by weight or more, and even more preferably 80% by weight or more relative to the total solid content of the adhesive composition.
[0095] As the acrylic base polymer, it is preferable to use a polymer having a monomer unit of an alkyl (meth)acrylate as a main skeleton. It should be noted that in the present specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid.
[0096] As the alkyl (meth)acrylate, it is preferred to use an alkyl (meth)acrylate in which the number of carbon atoms of the alkyl group is 1 to 20. The alkyl group in the alkyl (meth)acrylate may have a branched chain. The content of the alkyl (meth)acrylate is preferably 40% by weight or more, more preferably 50% by weight or more, and further preferably 60% by weight or more, relative to the total amount of the monomer components constituting the base polymer. The acrylic base polymer may be a copolymer of multiple alkyl (meth)acrylates. The arrangement of the constituent monomer units may be random or blocky.
[0097] The acrylic base polymer may contain an acrylic monomer unit having a crosslinkable functional group as a copolymer component. When the base polymer has a crosslinkable functional group, it is easy to increase the gel fraction of the adhesive by thermal crosslinking or photocuring of the base polymer. Examples of acrylic monomers having a crosslinkable functional group include hydroxyl-containing monomers and carboxyl-containing monomers. Among them, it is preferred to contain a hydroxyl-containing monomer as a copolymer component of the base polymer. When the base polymer has a hydroxyl-containing monomer as a monomer unit, there is a tendency to improve the crosslinking property using an isocyanate crosslinking agent and suppress the white turbidity of the adhesive in a high temperature and high humidity environment, and to obtain an adhesive with high transparency.
[0098] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and 4-hydroxymethylcyclohexylmethyl (meth)acrylate.
[0099] The content of the hydroxyl group-containing monomer is preferably 0.1 to 50% by weight, more preferably 1 to 40% by weight, and even more preferably 3 to 30% by weight, based on the total amount of monomer components constituting the base polymer.
[0100] The acrylic base polymer preferably contains a highly polar monomer unit such as a nitrogen-containing monomer in addition to a hydroxyl-containing monomer unit. By containing a highly polar monomer such as a nitrogen-containing monomer in addition to a hydroxyl-containing monomer, the adhesive has high adhesion and holding power and can suppress white turbidity in a high temperature and high humidity environment.
[0101] Examples of the nitrogen-containing monomer include N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyl Vinyl monomers such as oxazole, vinyl morpholine, (meth) acryloyl morpholine, N-vinyl carboxylic acid amide, and N-vinyl caprolactam; cyano acrylic monomers such as acrylonitrile and methacrylonitrile, etc. Among them, N-vinyl pyrrolidone and (meth) acryloyl morpholine are preferably used.
[0102] The content of the nitrogen-containing monomer is preferably 0.1 to 50% by weight, more preferably 1 to 40% by weight, and even more preferably 3 to 30% by weight, based on the total amount of monomer components constituting the base polymer.
[0103] The monomer components forming the acrylic polymer may contain a multifunctional monomer component. The multifunctional monomer is a monomer having at least two polymerizable functional groups having unsaturated double bonds, such as (meth)acryloyl groups or vinyl groups. The multifunctional monomer may have three or more polymerizable functional groups in one molecule.
[0104] The acrylic base polymer can be prepared by known polymerization methods such as solution polymerization, UV polymerization, bulk polymerization, and emulsion polymerization. From the perspectives of transparency, water resistance, and cost of the adhesive, solution polymerization or UV polymerization is preferred. As a solvent for solution polymerization, ethyl acetate, toluene, etc. are generally used.
[0105] When preparing the base polymer, a polymerization initiator such as a photopolymerization initiator or a thermal polymerization initiator can be used according to the type of polymerization reaction. As the photopolymerization initiator, a benzoin ether photopolymerization initiator, an acetophenone photopolymerization initiator, an α-ketol photopolymerization initiator, an aromatic sulfonyl chloride photopolymerization initiator, a photoactive oxime photopolymerization initiator, a benzoin photopolymerization initiator, a benzyl photopolymerization initiator, a benzophenone photopolymerization initiator, a ketal photopolymerization initiator, a thioxanthone photopolymerization initiator, an acylphosphine oxide photopolymerization initiator, etc. can be used. As the thermal polymerization initiator, an azo initiator, a peroxide initiator, a redox initiator obtained by combining a peroxide and a reducing agent (for example, a combination of a persulfate and sodium bisulfite, a combination of a peroxide and sodium ascorbate, etc.) can be used.
[0106] In order to adjust the molecular weight of the base polymer, a chain transfer agent can be used. The chain transfer agent has the function of accepting free radicals from the growing polymer chain to stop the elongation of the polymer and the chain transfer agent that accepts the free radical attacks the monomer to restart the polymerization. As the chain transfer agent, for example, thiols such as α-thioglycerol, lauryl mercaptan, glycidyl mercaptan, thioglycolic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, and 2,3-dimercapto-1-propanol can be appropriately used.
[0107] In the case of using a multifunctional monomer as a monomer component to form a base polymer in addition to a monofunctional monomer, the monofunctional monomer can be polymerized to form a prepolymer composition (prepolymerization) with a low degree of polymerization, a multifunctional monomer is added to the slurry of the prepolymer composition, and the prepolymer and the multifunctional monomer are polymerized (postpolymerization). By carrying out the prepolymer prepolymerization in this way, the branching point generated by the multifunctional monomer component can be uniformly introduced into the base polymer. In addition, the mixture (adhesive composition) of the prepolymer composition and the unpolymerized monomer component can also be coated on a substrate, and then postpolymerized on the substrate to form an adhesive layer. Since the viscosity of the prepolymer composition is low and the coating is excellent, the method of postpolymerization on the substrate after coating the adhesive composition as a mixture of the prepolymer composition and the unpolymerized monomer can improve the productivity of the adhesive layer, and the thickness of the adhesive layer can be made uniform.
[0108] The prepolymer composition can be prepared, for example, by partially polymerizing (prepolymerizing) a composition obtained by mixing monomer components constituting an acrylic base polymer and a polymerization initiator (referred to as a "prepolymer-forming composition"). It should be noted that the monomer in the prepolymer-forming composition is preferably a monofunctional monomer such as an alkyl (meth)acrylate and a monomer containing a polar group in the monomer components constituting the acrylic polymer. The prepolymer-forming composition may also contain a polyfunctional monomer. For example, a part of the polyfunctional monomer component as a raw material of the base polymer may be contained in the prepolymer-forming composition, and the remaining part of the polyfunctional monomer component may be added after polymerization into a prepolymer, and then supplied to the post-polymerization.
[0109] The prepolymer-forming composition may contain a chain transfer agent or the like as needed in addition to a monomer and a polymerization initiator. The polymerization method of the prepolymer is not particularly limited, but from the viewpoint of adjusting the reaction time so that the molecular weight (polymerization rate) of the prepolymer is within the desired range, polymerization by irradiation with active light such as UV light is preferred. The polymerization initiator and chain transfer agent used for prepolymerization are not particularly limited, and for example, the above-mentioned photopolymerization initiator and chain transfer agent can be used.
[0110] The polymerization rate of the prepolymer is not particularly limited, but is preferably 3% to 50% by weight, more preferably 5% to 40% by weight, from the viewpoint of adjusting the viscosity suitable for coating on the substrate. The polymerization rate of the prepolymer can be adjusted to a desired range by adjusting the type or amount of the photopolymerization initiator, the irradiation intensity and irradiation time of active light such as UV light, etc.
[0111] The remaining part of the monomer components constituting the acrylic base polymer (post-polymerization monomer) and, as required, a polymerization initiator, a chain transfer agent, a silane coupling agent, a cross-linking agent, etc. are mixed with the above-mentioned prepolymer composition to form an adhesive composition. The post-polymerization monomer preferably contains a multifunctional monomer. In addition to the multifunctional monomer, a monofunctional monomer may be added as a post-polymerization monomer.
[0112] The photopolymerization initiator and chain transfer agent used for post-polymerization are not particularly limited, and for example, the above-mentioned photopolymerization initiators and chain transfer agents can be used. When the polymerization initiator in the pre-polymerization remains in the prepolymer composition in an undeactivated state, the addition of the polymerization initiator for post-polymerization can be omitted.
[0113] The base polymer may have a cross-linked structure as required. The formation of the cross-linked structure is performed, for example, by adding a cross-linking agent after prepolymerization or after polymerization of the base polymer. As the cross-linking agent, an isocyanate cross-linking agent, an epoxy cross-linking agent, Commonly used crosslinking agents include oxazoline crosslinking agents, aziridine crosslinking agents, carbodiimide crosslinking agents, metal chelate crosslinking agents, etc. The content of the crosslinking agent is usually in the range of 0 to 5 parts by weight, preferably 0 to 3 parts by weight, based on 100 parts by weight of the acrylic base polymer.
[0114] When the adhesive composition contains a crosslinking agent, it is preferably subjected to a crosslinking treatment by heating before lamination to an adherend to form a crosslinked structure. The heating temperature and heating time in the crosslinking treatment are appropriately set according to the type of crosslinking agent used, and crosslinking is usually carried out by heating at a temperature within a range of 20°C to 160°C for about 1 minute to about 7 days.
[0115] The adhesive constituting the adhesive layer 21 may be a light-curing adhesive that can be cured by light irradiation after being bonded to an adherend such as the cover window 80. For example, if a light-curing adhesive is used in bonding a cover window having a raised portion such as decorative printing, the adhesive before light curing has a height difference absorption property by bonding in a soft state, thereby suppressing the mixing of bubbles near the raised portion, etc. The adhesive can be light-cured by irradiating ultraviolet rays, etc. after bonding, thereby improving the bonding reliability.
[0116] The photocurable adhesive preferably contains a photocurable compound (a monomer or oligomer having a photopolymerizable functional group) and a photopolymerization initiator in addition to a polymer. The photocurable adhesive preferably contains a polyfunctional compound having two or more polymerizable functional groups in one molecule as a photopolymerizable compound. The amount of the polyfunctional compound used varies depending on its molecular weight, the number of functional groups, etc., and is preferably 10% by weight or less, and more preferably 5% by weight or less, relative to the total amount of the monomer components constituting the base polymer.
[0117] The mixture of the above-mentioned prepolymer composition and the unpolymerized monomer component (adhesive composition) can be used as a photocurable adhesive. In addition, a part of the monomers can be left in an uncured state by applying the adhesive composition on the substrate and then adjusting the polymerization rate during post-polymerization to form a photocurable adhesive layer.
[0118] In addition to the above-exemplified components, the adhesive layer 21 may further contain additives such as a silane coupling agent, a tackifier, a plasticizer, a softener, an anti-degradation agent, a filler, a colorant, an antioxidant, a surfactant, and an antistatic agent.
[0119] In order to make the adhesive layer 21 have ultraviolet absorption, an ultraviolet absorber can be used. The content of the ultraviolet absorber in the adhesive layer 21 is about 0.05% by weight to about 10% by weight, and it can be adjusted in a way that the transmittance of light with a wavelength of 355nm of the adhesive layer 21 reaches 80% or less. As ultraviolet absorbers, benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, triazine ultraviolet absorbers, salicylate ultraviolet absorbers, and cyanoacrylate ultraviolet absorbers can be listed. From the perspective of high ultraviolet absorption, excellent compatibility with acrylic polymers, and easy to obtain highly transparent acrylic adhesive sheets, triazine ultraviolet absorbers and benzotriazole ultraviolet absorbers are preferred, among which triazine ultraviolet absorbers containing hydroxyl groups and benzotriazole ultraviolet absorbers having one benzotriazole skeleton in one molecule are preferred.
[0120] As the ultraviolet absorber, a commercial product can be used. Commercial products of the triazine ultraviolet absorber include: 2-[4-[2-hydroxy-3-(alkoxy)propoxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine ("TINUVIN 400" manufactured by BASF), a reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and glycidyl acid (2-ethylhexyl) ester ("TINUVIN 405" manufactured by BASF), 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine ("TINUVIN 405" manufactured by BASF), 460”), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-(hexyloxy)-phenol (“TINUVIN 577” manufactured by BASF), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (“TINUVIN 479” manufactured by BASF), 2,4-bis[{4-(2-ethylhexyloxy)-2-hydroxy}phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (“Tinosorb S” manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (“ADK STAB LA-46” manufactured by ADEKA), and the like.
[0121] Examples of commercially available benzotriazole ultraviolet absorbers include 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (“TINUVIN 928” manufactured by BASF), 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (“TINUVIN PS” manufactured by BASF), 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (“TINUVIN PS” manufactured by BASF), 900”), 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (“TINUVIN 928” manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (“TINUVIN 571” manufactured by BASF), 2-(2H-benzotriazol-2-yl)-p-cresol (“TINUVIN P” manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (“TINUVIN 234” manufactured by BASF), 2-[5-chloro-(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (“TINUVIN 326”), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-amylphenol (“TINUVIN 328” manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (“TINUVIN 329” manufactured by BASF), ester compound of phenylpropionic acid and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy (C7 to C9 branched and linear alkyl) (“TINUVIN 384-2” manufactured by BASF), reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol (“TINUVIN 1130”), reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol 300 (“TINUVIN 213” manufactured by BASF), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole (“Sumisorb 250” manufactured by Sumitomo Chemical), etc.
[0122] The adhesive composition is applied in a layered manner on the substrate, and the solvent is dried, the base polymer is crosslinked and cured as required to form an adhesive layer. In the case where the adhesive composition is photocurable, the adhesive composition can be applied to the supporting substrate, and then irradiated with ultraviolet rays and / or short-wavelength visible light to perform photocuring. When performing photocuring, a cover plate is preferably provided on the surface of the coating layer, and light is irradiated while the adhesive composition is sandwiched between two cover plates, thereby preventing inhibition caused by oxygen.
[0123] The thickness of the first adhesive layer 21 is not particularly limited and is generally about 5 μm to about 1000 μm. When the adherend (covering window 80, etc.) fixedly laminated on the first adhesive layer 21 has a raised portion such as a printed height difference and requires height difference absorption, the thickness of the first adhesive layer 21 is preferably 30 μm or more. The thickness of the first adhesive layer 21 may be 40 μm or more or 50 μm or more. Considering the viewpoints of lightweight and thinning of the display device, the ease of forming the adhesive layer, operability, etc., the thickness of the first adhesive layer 21 is preferably 500 μm or less, more preferably 300 μm or less, and further preferably 250 μm or less.
[0124] The transmittance of the first adhesive layer 21 to light of a wavelength of 355 nm is 80% or less. The first adhesive layer 21 has ultraviolet absorption, so that when the laminate is processed by ultraviolet laser, the processability of the first adhesive layer is improved, and peeling at the bonding interface and the mixing of bubbles in the bonding interface can be suppressed.
[0125] From the viewpoint of improving processability by ultraviolet laser, the transmittance of the first adhesive layer 21 at a wavelength of 355 nm is preferably smaller. The transmittance of the first adhesive layer 21 at a wavelength of 355 nm may be 75% or less, 70% or less, or 65% or less.
[0126] If the first adhesive layer 21 has ultraviolet absorption, ultraviolet rays contained in the external light are absorbed by the first adhesive layer 21, so that it is possible to suppress the degradation of the polarizer 11 due to ultraviolet rays. On the other hand, in the case where the transparent film 13 arranged on the visible side of the polarizer 11 has ultraviolet absorption, the first adhesive layer 21 is not required to have high ultraviolet absorption, as long as the first adhesive layer 21 has ultraviolet absorption to a degree that enables the processability using ultraviolet laser.
[0127] In the case where the first adhesive layer 21 is a photocurable adhesive, when the amount of ultraviolet light absorbed by the ultraviolet absorber or the like is large, the amount of ultraviolet light absorbed by the photopolymerization initiator is reduced, which may become a cause of hindering curing. From the viewpoint of improving the photocuring efficiency, the transmittance of the first adhesive layer 21 at a wavelength of 355 nm may be 20% or more, 25% or more, or 30% or more. Even if the ultraviolet shielding property generated by the first adhesive layer 21 is insufficient, if the transparent film 13 has ultraviolet light absorptivity, ultraviolet degradation of the polarizer 11 can be suppressed.
[0128] When the first adhesive layer 21 is required to have high differential absorption, the storage elastic modulus G' of the first adhesive layer 21 at 25°C is preferably 0.35 MPa or less, and more preferably 0.30 MPa or less. On the other hand, when the first adhesive layer 21 is too soft, it is easy for the adhesive to transfer to the cutting knife or the like when the optical film with adhesive is cut into single sheets, and the adhesive to protrude from the end surface of the single optical film with adhesive. In addition, when the first adhesive layer 21 is too soft, it may cause poor processing when processing with a laser. Therefore, the storage elastic modulus G' of the first adhesive layer 21 at 25°C is preferably 0.01 MPa or more, and more preferably 0.02 MPa or more. The storage modulus G' of the first adhesive layer 21 at 25°C may be 0.03 MPa or more, 0.05 MPa or more, or 0.1 MPa or more.
[0129] <Second Adhesive Layer>
[0130] The second adhesive layer 22 is used for bonding the optical film 10 and the image display unit 70 in the display device 204. The second adhesive layer 22 is preferably a transparent adhesive sheet and has a high visible light transmittance. The transmittance of the second adhesive layer 22 for light of a wavelength of 420 nm is 85% or more, preferably 88% or more, and more preferably 90% or more. The haze of the second adhesive layer 22 is preferably 2% or less, and more preferably 1% or less.
[0131] The adhesive constituting the second adhesive layer 22 is not particularly limited, and adhesives having various polymers as base polymers can be appropriately selected and used. As described above, the adhesive constituting the second adhesive layer 22 is preferably an acrylic adhesive having an acrylic polymer as a base polymer.
[0132] There is no particular limitation on the thickness of the second adhesive layer 22. Since the second adhesive layer 22 is not required to have height difference absorption, the thickness of the second adhesive layer 22 may be smaller than the thickness of the first adhesive layer 21. The thickness of the second adhesive layer 22 is preferably 3 μm to 30 μm, more preferably 5 μm to 27 μm, and further preferably 10 μm to 25 μm.
[0133] The storage elastic modulus G′ of the second adhesive layer 22 at 25° C. is, for example, about 0.02 MPa to 5 MPa. Since the second adhesive layer 22 is not required to have high-difference absorbency, the storage elastic modulus G′ of the second adhesive layer at 25° C. may be greater than G′ of the first adhesive layer 21 .
[0134] The second adhesive layer 22 may or may not have ultraviolet absorption. If the thickness of the second adhesive layer 22 is 30 μm or less, even if the second adhesive layer does not have ultraviolet absorption, through holes can be formed in the second adhesive layer 22 by irradiating the laminate with ultraviolet laser. Therefore, the transmittance of light of wavelength 355 nm of the second adhesive layer can be 80% or more, 83% or more, or 85% or more. In the case where the thickness of the second adhesive layer 22 is greater than 30 μm, from the viewpoint of improving the processability using ultraviolet laser, the transmittance of light of wavelength 355 nm of the second adhesive layer 22 is preferably 80% or less, more preferably 75% or less. The transmittance of light of wavelength 355 nm of the second adhesive layer 22 can be greater than the transmittance of light of wavelength 355 nm of the first adhesive layer 21.
[0135] <Optical film with adhesive on both sides>
[0136] A first adhesive layer 21 is provided on the main surface of the visible side of the optical film 10, and a second adhesive layer 22 is provided on the main surface of the second main surface side of the optical film 10, thereby forming an optical film 25 with an adhesive on both sides. As a method for forming the first adhesive layer 21 and the second adhesive layer 22 on the optical film 10, for example, the following methods can be cited: an adhesive composition is applied to a release film, and the solvent is removed by drying, and a cross-linking treatment is performed as needed to form an adhesive layer, and then the adhesive layer is transferred to the optical film 10; or an adhesive composition is applied to the optical film 10, and the solvent is removed by drying, so as to form an adhesive layer on the optical film; etc. In the method of transferring the adhesive layer to the optical film, the release film used in the formation of the adhesive layer can be used as the release film 41, 42 of the optical film with an adhesive on both sides. In the case of applying an adhesive composition to the optical film 10 to form an adhesive layer, a release film is provided on the adhesive layer after the solvent is removed by drying.
[0137] <Release film>
[0138] As the release films 41, 42 temporarily attached to the adhesive layers 21, 22, it is preferable to use a release film having a release layer on the surface of the film substrate. As the material of the release layer, polysiloxane release agents, fluorine-containing release agents, long-chain alkyl release agents, fatty acid amide release agents, etc. can be cited. From the perspective of being able to have both adhesion and releasability to acrylic adhesives, polysiloxane release agents are preferred.
[0139] As the film substrate of the release film, a transparent resin film is preferred. As the resin material, polyester resins such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth) acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, polyvinyl alcohol resins, polyarylate resins, polyphenylene sulfide resins, etc. can be cited. Among them, polyester resins such as polyethylene terephthalate (PET) are particularly preferred.
[0140] The thickness of the release films 41 and 42 is preferably 10 μm to 200 μm, and more preferably 25 μm to 150 μm. The thickness of the release film 41 and the thickness of the release film 42 may be the same or different.
[0141] When the laminate obtained by bonding the image display unit 70 to the second adhesive layer 22 is processed by irradiating an ultraviolet laser, since the release film 42 is peeled off and removed, the optical properties of the release film 42 have no particular effect on the laser processability. When irradiating the ultraviolet laser from the image display unit 70 side, the release film 41 may or may not have ultraviolet absorption. Therefore, the transmittance of light with a wavelength of 355nm of the release films 41 and 42 may be 80% or more, 85% or more, or 90% or more. As described in detail later, when irradiating the ultraviolet laser from the surface of the release film side of the laminate, it is preferred that the release film on the laser irradiation surface has ultraviolet absorption, and the transmittance of light with a wavelength of 355nm of the release film on the laser irradiation surface is preferably 15% to 70%.
[0142] [Cutting of optical films]
[0143] The laminate 102 having release films 41, 42 temporarily adhered to the surfaces of the adhesive layers 21, 22 of the optical film 25 with adhesive on both sides is cut into the desired size as needed, and then the release film temporarily adhered to the surface of the adhesive layer is peeled off and adhered to an adherend such as an image display unit 70 and a cover window 80.
[0144] A large-area sheet (mother substrate) is produced in a roll-to-roll manner, and then cut into a specified size that matches the size of the adherend, thereby obtaining a single optical film with adhesive on both sides. This method can obtain a large number of single sheets from the mother substrate, so the productivity can be improved. Usually, the mother substrate is cut into a single product size that is consistent with the size (screen size) of the image display unit 70. As cutting methods, there can be listed: a method of punching using a Thomson knife, etc.; a method using a cutter such as a circular knife and a disc knife, a laser, a water pressure, etc.
[0145] exist Figure 2 In the laminated body 102 shown, release films 41 and 42 are temporarily attached to the surfaces of the adhesive layers 21 and 22, so that the main surface of the adhesive layer is protected. On the other hand, the end surface of the adhesive layer is exposed, and since the adhesive protrudes from the end surface, sometimes adhesive loss and adhesive stains may occur. In a single optical film with adhesive, in order to prevent adhesive loss and adhesive stains, the end surface of the adhesive layer can be set at a position closer to the inside than the end surface of the optical film 10 and the end surface of the release films 41 and 42.
[0146] For example, you can Figure 5 As shown in the laminated body 105, the release films 41 and 42 are arranged to extend outward from the end faces of the optical film 10 and the adhesive layers 21 and 22, and the end faces of the adhesive layers 21 and 22 are located at a position further inward than the end faces of the release films 41 and 42. Figure 6 As shown in the laminated body 106, near the interface between the adhesive layers 21, 22 and the release films 41, 42, the end faces of the adhesive layers 21, 22 are basically consistent with the end faces of the release films 41, 42, and near the center of the thickness direction of the adhesive layers 21, 22, the end faces of the adhesive layers 21, 22 are located at a position closer to the inside than the end faces of the release films 41, 42.
[0147] The double-sided adhesive optical film 25 with release films 41 and 42 temporarily attached to both sides is pressurized from the main surface (the surface provided with the release film) so that the ends of the adhesive layers 21 and 22 protrude from the ends of the optical film 10, and then the pressure is released, so that the optical film 25 can be cut as shown in FIG. Figure 6 In the case of adopting this method, the end faces of the adhesive layers 21 and 22 are located at a position further inside than the end faces of the optical film 10 and the end faces of the release films 41 and 42, as in the laminated body 106 shown in FIG. When this method is adopted, the following method is preferred: a mother substrate produced in a roll-to-roll manner is punched out by a Thomson knife or the like, a plurality of punched-out laminated bodies are overlapped, and pressure is applied from the stacking direction, and the inner side of the cut surface produced by punching out is cut (cut) by a rotary knife or the like while the adhesive layer protrudes from the end face, thereby processing into a product size.
[0148] For example, by controlling the area of the adhesive layers 21 and 22 on the optical film 10, or removing only a portion of the adhesive layers after the adhesive layers 21 and 22 are provided, a structure such as the above can be formed. Figure 5 The release films 41 and 42 shown are a single laminate 105 that protrudes outward from the end surfaces of the adhesive layers 21 and 22 .
[0149] From the viewpoint of productivity, it is preferred to produce the mother substrate in a roll-to-roll manner and cut the optical film with adhesive and the release film. For example, the mother substrate with adhesive optical film is cut according to the following steps, thereby forming a single laminate 105 in which the release films 41 and 42 extend outward from the end faces of the adhesive layers 21 and 22.
[0150] First, the release film 42 side of the laminated body provided with release films 41 and 42 on both sides is half-cut to cut the release film 42 and the optical film 25 with adhesive on both sides. Then, the optical film with adhesive on both sides in the area surrounded by the cut line and the release film 42 on the entire surface are peeled off from the surface of the release film 41. Another release film 43 is attached to the second adhesive layer 22 of the optical film 25 with adhesive on both sides, thereby forming a laminated body as shown in FIG. Figure 7 In the figure, a stacked body 307 of a plurality of single optical films 25 with an adhesive on both sides is arranged between two release films 41 and 43 .
[0151] By cutting the laminate 307, a single laminate is obtained in which the release films 41 and 43 protrude outward from the end surface of the optical film 25 with adhesive on both sides. When the laminate is cut, if the release film 41 in the area where the optical film 25 with adhesive on both sides is not provided is cut, the laminate is obtained as shown in FIG. Figure 5 The laminated body shown has a large protrusion amount of the release film 43.
[0152] The mother substrate may also be laminated on a carrier sheet and cut into single sheets. A carrier sheet 49 is laminated on the surface of the release film 41 side of the laminate having release films 41 and 42 on both sides, and half-cutting is performed from the release film 42 side. At this time, half-cutting is performed in a manner that cuts the release film 42 and the optical film 25 with adhesive on both sides, and half-cutting is performed in a manner that cuts the release film 42, the optical film 25 with adhesive on both sides, and the release film 42 is cut at a position further to the outside than the cutting line. The release film 42 surrounded by the cutting line, the optical film 25 with adhesive on both sides surrounded by the cutting line, and the entire surface of the release film 42 are peeled off and removed from the surface of the carrier sheet 49. Another release film 43 is laminated on the second adhesive layer 22 of the optical film 25 with adhesive on both sides, thereby obtaining Figure 8 The stack 308 is shown.
[0153] The release film 43 of the laminated body 308 is cut and the laminated body of the release film 41, the optical film 25 with an adhesive on both sides and the release film 43 is peeled off from the carrier sheet 49 to obtain a laminated body as shown in FIG. Figure 5 The laminated body shown has a large protrusion amount of the release film 43.
[0154] When the release film is provided so as to protrude outward from the end surface of the adhesive layer, the protrusion amount of the release film on one surface may be the same as or different from the protrusion amount of the release film on the other surface. Figure 5 As shown, by making the extension amount of the release films on both sides different, it is easy to selectively grab the release film to be peeled. By increasing the extension amount of the release film to be peeled off first, the workability is further improved. When the second release film 42 (43) is peeled off from the second adhesive layer 22, the image display unit 70 is attached to the second adhesive layer 22, and then the first release film 41 is peeled off from the first adhesive layer 21, and the cover window 80 is attached to the first adhesive layer 21, the extension amount of the second release film 42 (43) can be increased.
[0155] [Formation of through hole]
[0156] The second release film 42 temporarily attached to the surface of the second adhesive layer 22 is peeled off, and the image display unit 70 is bonded to the second adhesive layer 22 for fixed lamination, thereby forming the optical laminate 103. The optical laminate 103 may also be formed by bonding the optical film 10 to the image display unit 70 via the second adhesive layer 22, and laminating the first adhesive layer 21 and the first release film 41 thereon.
[0157] By irradiating the image display unit 70 side of the laminate 103 with ultraviolet laser, a through hole (hole) is formed in a manner that penetrates the image display unit 70, the second adhesive layer 22, the optical film 10, the first adhesive layer 21, and the release film 41 temporarily attached to the first adhesive layer 21. As the ultraviolet laser, there is no particular limitation as long as it can irradiate a laser with a wavelength of 400nm or less. From the viewpoint of high output power and excellent processability, the third harmonic of YAG laser (wavelength 355nm) is preferred. The laser power is, for example, about 0.1W to about 50W.
[0158] The shape of the through hole 5 is not particularly limited, and can be appropriately set according to the shape of the optical element 91 disposed below the image display unit 70. The shape of the through hole 5 can be circular, elliptical, triangular, quadrilateral, polygonal, linear, etc. In the case of configuring a camera as the optical element 91, a circular through hole can be provided in the shape of a camera lens. A plurality of through holes can be formed in the optical laminate.
[0159] When the laser light source and the optical stack are fixed and laser irradiation is performed, the through hole formed by laser processing is a hole of the same degree as the laser beam diameter. When the size of the through hole 5 is larger than the laser beam diameter, by moving the laser light source relative to the optical stack, a through hole 5 having a target size and shape can be formed. The entire area where the through hole 5 is to be formed can be irradiated with laser to form an opening. In addition, the laser can be irradiated along the periphery of the shape of the through hole 5 and the inside can be dug out to form a through hole 5 having a target size and shape.
[0160] Since the image display unit 70 includes an ultraviolet absorbing member such as a polyimide film, the image display unit 70 absorbs the ultraviolet laser. By absorbing the ultraviolet laser, the image display unit 70 generates heat and vaporizes, and the second adhesive layer 22, the optical film 10, the first adhesive layer 21, and the release film 41 provided on the image display unit 70 are blown away together with the vapor, thereby forming a through hole.
[0161] If the second adhesive layer 22, the optical film 10, and the first adhesive layer 21 have ultraviolet absorption, these optical components also absorb ultraviolet laser light, so the processing accuracy is improved. As mentioned above, when the thickness of the second adhesive layer 22 is small (for example, less than 30 μm), even if the second adhesive layer 22 does not have ultraviolet absorption, sufficient processability is exhibited. The release film 41 may have ultraviolet absorption or may not have ultraviolet absorption.
[0162] Since the first adhesive layer 21 has ultraviolet absorption and absorbs ultraviolet laser light, good processability is exhibited even when the first adhesive layer 21 is thick and soft. If the first adhesive layer 21 has ultraviolet absorption, the release film 41 temporarily attached to the first adhesive layer 21 is also processed due to heating and gasification during processing, so that the release film 41 around the laser irradiation area can be prevented from peeling off and mixing of bubbles.
[0163] [Formation of Display Device]
[0164] The release film 41 temporarily attached to the first adhesive layer 21 is peeled off, and the cover window 80 is attached, thereby forming an optical laminate (image display element) in which the cover window 80 is fixedly laminated on the first adhesive layer 21 and the image display unit 70 is fixedly laminated on the second adhesive layer 22. The optical laminate has a through hole 5 that penetrates from the image display unit 70 to the first adhesive layer 21.
[0165] A display device with an optical element is obtained by disposing the optical element 91 below the through hole 5. The optical element 91 may be a light receiving element such as a camera or a photosensor, or a light emitting element such as an LED.
[0166] As the cover window 80, a transparent plate with appropriate mechanical strength and thickness can be used. As such a transparent plate, a transparent resin plate such as an acrylic resin, a polycarbonate resin, a transparent polyimide resin, or a glass plate can be used. The thickness of the cover window 80 is, for example, about 20 μm to about 2000 μm. In a flexible device, a transparent resin film is preferably used as the cover window 80, and its thickness is preferably 20 μm to 500 μm, more preferably 30 μm to 300 μm, and further preferably 50 μm to 200 μm. A thin glass substrate that can be bent can also be used as the cover window 80.
[0167] The cover window 80 may be a cover window integrated with the touch panel sensor. An anti-reflection layer, a hard coating layer, etc. may be disposed on the visible side surface of the cover window 80 .
[0168] After the cover window 80 is bonded to the first adhesive layer 21, heating, pressurization, decompression, etc. may be performed to remove bubbles at the bonding interface and near the printing height difference. Autoclave treatment may be performed to suppress delayed bubbles, etc.
[0169] When the first adhesive layer 21 is a photocurable adhesive, it is preferred to photocure the first adhesive layer 21 after attaching the cover window 80 to the first adhesive layer 21. For example, the first adhesive layer 21 is photocured by irradiating active light such as ultraviolet rays through the cover window 80. By photocuring the adhesive, the bonding reliability is improved.
[0170] [Variation of hole processing]
[0171] In the above example, the description is centered on the case where the through hole 5 is formed by irradiating the stacked body 103 having the image display unit 70 fixedly laminated as the adherend on the second adhesive layer 22 with ultraviolet laser from the image display unit 70 side, but other embodiments can also be applied to the formation of through holes using ultraviolet laser.
[0172] For example, the through hole 5 can be formed by irradiating the release film 41 temporarily attached to the first adhesive layer 21 of the optical laminate 103 with ultraviolet laser light. When irradiating the release film 41 with ultraviolet laser light, the release film 41 preferably has ultraviolet absorption, and the transmittance of the release film 41 at a wavelength of 355 nm is preferably 70% or less, more preferably 60% or less.
[0173] The higher the ultraviolet absorption of the release film 41 disposed on the laser irradiation surface (the lower the transmittance of light with a wavelength of 355 nm), the higher the processing efficiency using the ultraviolet laser tends to be. On the other hand, when the ultraviolet absorption of the release film 41 is too high, bubbles may be generated around the through hole formed in the release film 41 (around the laser irradiation area) (see Fig.14 ). The reason why bubbles are generated in the release film is not clear, but one of the reasons is believed to be that the heat resistance of the film substrate (such as PET film) of the release film is lower than that of a polyimide film, so bubbles are easily generated due to the heat generated when absorbing ultraviolet laser.
[0174] When forming a display device, the release film 41 is peeled off and the adherend such as the cover window is attached, so even if bubbles are generated around the through hole of the release film 41, no quality problems will occur. However, when bubbles are generated in the release film 41, it is difficult to distinguish them from bubbles mixed in the adhesive layer, etc., and sometimes the process inspection becomes difficult or becomes a cause of misjudgment. In addition, sometimes the deformation caused by the bubbles generated in the release film 41 will be transferred to the first adhesive layer 21 and become a cause of poor appearance. Therefore, when the opening process is performed by irradiating ultraviolet laser from the side of the release film 41, it is preferred that no bubbles are generated in the release film 41.
[0175] When the ultraviolet light absorptivity of the release film 41 is low (the ultraviolet light transmittance is high), there is a tendency to suppress the generation of bubbles. From the viewpoint of suppressing the generation of bubbles in the release film 41 due to laser processing, the transmittance of light of a wavelength of 355 nm of the release film 41 is preferably 15% or more, more preferably 20% or more, and further preferably 30% or more. The transmittance of light of a wavelength of 355 nm of the release film 41 may be 35% or more or 40% or more.
[0176] <Hole-drilling Processing Before Lamination with Image Display Unit>
[0177] The laminated body before the image display unit is attached to the second adhesive layer 22 can be irradiated with ultraviolet laser to perform the hole-opening process. For example, the laminated body 102 in which the release film 41 is temporarily attached to the first adhesive layer 21 and the release film 42 is temporarily attached to the second adhesive layer 22 can be irradiated with ultraviolet laser to form the following hole-opening process: Fig. 9 The laminated body 105 having the through hole 7 is shown. When the through hole 7 is formed, ultraviolet laser light may be irradiated from either the release film 41 side or the release film 42 side.
[0178] The release film on the laser irradiation side preferably has ultraviolet light absorptivity, and the transmittance of light of wavelength 355 nm of the release film on the laser irradiation side is preferably 70% or less, more preferably 60% or less. From the viewpoint of suppressing the generation of bubbles around the laser processing area, the transmittance of light of wavelength 355 nm of the release film on the laser irradiation side is preferably 15% or more, more preferably 20% or more, and further preferably 30% or more. The transmittance of light of wavelength 355 nm of the release film on the laser irradiation side may be 35% or more or 40% or more.
[0179] For example, when ultraviolet laser is irradiated from the release film 42 side, the transmittance of light of wavelength 355nm of the release film 42 is preferably within the above range. When ultraviolet laser is irradiated from the release film 42 side, the release film 41 may or may not have ultraviolet absorptivity.
[0180] When irradiating the release film 41 with ultraviolet laser light, the transmittance of the release film 41 at a wavelength of 355 nm is preferably within the above range. When irradiating the release film 41 with ultraviolet laser light, the release film 42 may or may not have ultraviolet absorptivity.
[0181] The laminated body in which a release film is temporarily attached to the surfaces of the adhesive layers 21 and 22 of the optical film 25 with adhesive on both sides only needs to have through holes penetrating the first adhesive layer 21, the optical film 10 and the second adhesive layer 22, and the release film on one or both sides may not have through holes.
[0182] For example, in Fig.10 In the optical laminate 110 shown, the through hole 8 provided in the optical film 25 with adhesive on both sides penetrates the release film 41 temporarily attached to the first adhesive layer 21, but no through hole is provided in the release film 47 temporarily attached to the second adhesive layer 22. Alternatively, the release film temporarily attached to the second adhesive layer 22 may be provided with a through hole, while the release film temporarily attached to the first adhesive layer 21 may not be provided with a through hole.
[0183] exist Fig.11 In the optical laminate 111 shown, through holes 9 are provided in the first adhesive layer 21, optical film 10 and second adhesive layer 22 constituting the double-sided adhesive optical film 25, but no through holes are provided in the release films 46 and 47 temporarily attached to the adhesive layers 21 and 22.
[0184] An optical laminate 102 having release films 41, 42 temporarily adhered to adhesive layers 21, 22 is irradiated with ultraviolet laser to form a through hole 7, and then one or both of the release films 41, 42 of the laminate 109 having through holes are replaced with other release films 46, 47, thereby obtaining an optical laminate without through holes formed on one or both sides of the release films.
[0185] After forming the through hole by laser processing, the release film is replaced, and the through hole of the optical film 25 with adhesive on both sides is blocked by the release film, thereby preventing foreign matter from mixing into the through hole during handling or storage of the optical laminate. When the release film temporarily attached to the adhesive layer is replaced after forming the through hole in the optical film and the adhesive layer, the replaced release film may or may not have ultraviolet absorption.
[0186] The release film temporarily attached to the adhesive layers 21 and 22 provided with through holes may extend outwards compared to the end faces of the adhesive layers 21 and 22. The release film temporarily attached to the first adhesive layer 21 may extend outwards compared to the end face of the first adhesive layer, and the release film temporarily attached to the second adhesive layer 22 may extend outwards compared to the end face of the second adhesive layer 22. Fig.12 As shown, the double-sided release films 41 and 48 may extend outwards from the end faces of the first adhesive layer 21 and the second adhesive layer 22, respectively. When the double-sided release films extend outwards from the end faces of the adhesive layers (end faces of the double-sided adhesive optical film 25), the extension amount of the release film on one side may be the same as or different from the extension amount of the release film on the other side.
[0187] When a single optical laminate is cut out from a large-area mother substrate, the formation of through holes by laser processing can be performed before or after cutting. After the through holes are formed by irradiating the mother substrate with ultraviolet laser, the release film on one or both sides can be replaced before or after cutting.
[0188] The release film may be replaced during the process of cutting into single sheets after forming a through hole by irradiating the mother substrate with a laser. In one embodiment, after forming a through hole in a laminated body having release films 41 and 42 on both sides, the release film 42 and the optical film with adhesive on both sides are cut by half cutting. The optical film with adhesive on both sides in the area surrounded by the cutting line and the release film 42 on the entire surface are peeled off from the surface of the release film 41. Another release film 48 is attached to the second adhesive layer 22 of the optical film with adhesive on both sides 25, thereby forming a laminated body as shown in FIG. Fig.13 In the figure, a laminate 313 is shown in which a plurality of single optical films 25 with an adhesive on both sides and provided with through holes 8 are arranged between two release films 41 and 48 .
[0189] In the laminate 313, the through hole 8 penetrates the release film 41 on the first adhesive layer 21, but no through hole is provided in the release film 48. Fig.12 The second adhesive layer 22, the optical film 10, the first adhesive layer 21 and the release film 41 temporarily attached to the first adhesive layer 21 are provided with through holes, and the release films 41 and 48 protrude outward from the end surfaces of the adhesive layers 21 and 22.
[0190] The release film temporarily attached to the second adhesive layer 22 is peeled off from the optical laminate after the through hole is formed, the image display unit 70 is attached to the second adhesive layer 22, the release film temporarily attached to the first adhesive layer 21 is peeled off, and the covering window is attached to the first adhesive layer 21, thereby forming an image display element.
[0191] A through hole may be previously formed in the image display unit 70. In this case, the through hole provided in the image display unit 70 and the through hole provided in the double-sided adhesive optical film 25 may be aligned so that the positions thereof coincide.
[0192] When forming a through hole in the image display unit 70 after bonding the image display unit 70 to the second adhesive layer 22, the position of the through hole provided in the optical film with adhesive on both sides can be irradiated with ultraviolet laser or the like. In this case, laser irradiation can be performed from either side.
[0193] [Example]
[0194] Hereinafter, the present invention will be described in more detail by showing test examples of laser processing of an optical layered body, but the present invention is not limited to these examples.
[0195] [Production of polarizing plate with adhesive on both sides]
[0196] <Production example 1>
[0197] As an optical film, a polarizing plate was used in which a 40 μm thick triacetyl cellulose film was bonded to both surfaces of a polarizer including a 25 μm thick stretched polyvinyl alcohol film impregnated with iodine. The triacetyl cellulose film contained an ultraviolet absorber and had a transmittance of 0% for light of a wavelength of 355 nm.
[0198] On one side of the polarizing plate, a 150 μm thick acrylic adhesive sheet (transmittance of light at a wavelength of 355 nm: 64%, transmittance of light at a wavelength of 420 nm: 92%, storage elastic modulus at 25°C: 0.1 MPa) containing a benzotriazole ultraviolet absorber and a 75 μm thick release film (a biaxially stretched PET film having a polysiloxane release layer on the surface, transmittance of light at a wavelength of 355 nm: 85%) were attached as a first adhesive layer. On the other side of the polarizing plate, a 20 μm thick acrylic adhesive sheet (transmittance of light at a wavelength of 355 nm: 85%, transmittance of light at a wavelength of 420 nm: 92%, storage elastic modulus at 25°C: 0.12 MPa) not containing an ultraviolet absorber and a 38 μm thick release film were attached as a second adhesive layer, thereby obtaining a laminate having adhesive layers on each side of the polarizing plate and release films temporarily attached to the adhesive layers.
[0199] <Production Examples 2 to 4>
[0200] A laminate was formed in the same manner as in Production Example 1 except that the amount of the ultraviolet absorber in the first adhesive layer was changed. In Production Example 4, an adhesive containing no ultraviolet absorber was used as the first adhesive layer. The transmittance of the first adhesive layer in Production Examples 2 to 4 at a wavelength of 355 nm is shown in Table 1.
[0201] <Production example 5>
[0202] A laminate was formed in the same manner as in Production Example 1 except that the thickness of the second adhesive layer was changed to 40 μm.
[0203] <Production example 6>
[0204] A biaxially stretched PET film containing no ultraviolet absorber was used as a release film on the first adhesive layer. The transmittance of the release film at a wavelength of 355 nm was 1%. A laminate was formed in the same manner as in Preparation Example 1 except that the release film on the first adhesive layer was changed.
[0205] [Preparation of Samples for Processability Evaluation]
[0206] The release film on the second adhesive layer of the laminated bodies of Production Examples 1 to 6 was peeled off, and a 25 μm-thick polyimide film ("Kapton EN100" manufactured by DuPont Toray, transmittance of 0% for light at a wavelength of 355 nm) was bonded to the second adhesive layer to prepare samples for processability evaluation.
[0207] [Processing using ultraviolet laser]
[0208] The sample for processability evaluation was irradiated with a YAG third harmonic ultraviolet laser (wavelength 355nm, frequency 40Hz, output power 0.4W) to form a through hole. The laser light source was moved along the outer periphery (circumference) of a circle with a diameter of 3mm at a speed of 10mm / second while the laser irradiation was performed, and the circumference was circled 30 times, and the inside of the circumference was dug out, thereby forming a circular through hole with a diameter of about 3mm. For the samples of Preparation Examples 1 to 5, the laser was irradiated from the polyimide film side (second adhesive layer side); for the sample of Preparation Example 6, the laser was irradiated from the PET release film side (first adhesive layer side).
[0209] [evaluate]
[0210] <Presence or Absence of Bubbles in the First Adhesive Layer>
[0211] The release film was peeled off from the sample after the through-holes were formed, and the surface of the first adhesive layer was observed by optical microscopy (direct magnification 5 times) to check for the presence of bubbles. Samples with no bubbles were evaluated as ○, and samples with bubbles were evaluated as ×.
[0212] <Cutting Processability>
[0213] The cutting processability when the laser processing was performed 30 times along the circumference was judged according to the following criteria.
[0214] ○: The inside of the circumference has fallen off after laser processing, or the inside of the circumference can be hollowed out without deformation of the outside of the circumference.
[0215] ×: The inside of the circumference did not fall off after laser processing, but the outside of the circumference was deformed when the inside of the circumference was hollowed out, or the inside of the circumference could not be hollowed out.
[0216] Table 1 shows the structure of the laminated body of each production example and the evaluation results of laser processability.
[0217] Table 1
[0218]
[0219] In the production examples 1 to 3 in which the first adhesive layer has ultraviolet absorbency, good processability was shown. In the production example 4 in which the first adhesive layer does not contain an ultraviolet absorber, bubbles were observed in the first adhesive layer, and the laser processability was poor. From these results, it can be seen that by making the first adhesive layer have ultraviolet absorbency, the processability using ultraviolet laser is improved, and high-precision cutting processing can be achieved.
[0220] In Production Example 5, in which the thickness of the second adhesive layer was large, although the generation of bubbles in the first adhesive layer was not observed, poor cutting of the second adhesive layer was confirmed. In Production Examples 1 to 4, in which the thickness of the second adhesive layer was small, poor cutting of the second adhesive layer was not observed, so it can be said that the large thickness of the second adhesive layer is the cause of the reduced processability using the laser. Therefore, it is known that the thickness of the second adhesive layer is preferably small, and when the thickness of the second adhesive layer is large, it is preferred to make it have ultraviolet absorption by adding an ultraviolet absorber or the like.
[0221] In Production Example 6, in which laser irradiation was performed from the first pressure-sensitive adhesive layer side, the pressure-sensitive adhesive layer had good processability as in Production Examples 1 to 3. These results show that as long as the adherend on the laser irradiation surface has ultraviolet absorptivity, it can be processed by ultraviolet laser.
[0222] It should be noted that in Preparation Example 6, although the processability of the adhesive layer was good, in the optical microscope observation of the release film on the laser irradiation surface, as shown in FIG. Fig.14 As shown in FIG. 1 , bubbles of about 20 μm were generated around the through-holes. In Preparation Examples 1 to 5, no bubbles were observed in the polyimide film or the release film. Fig.14 In addition, in the polyimide film of Production Example 6, no bubbles were confirmed.
[0223] Based on the above results, it can be considered that in Production Example 6, since the ultraviolet absorption of the release film on the ultraviolet laser irradiation surface is high, the heat generated during ultraviolet laser irradiation is large, so bubbles are generated in the release film. Therefore, it can be said that when the ultraviolet laser is irradiated from the surface of the release film side, it is preferable to adjust the ultraviolet absorption (ultraviolet transmittance) of the release film so that it has ultraviolet absorption to the extent that laser processing can be performed and the generation of bubbles caused by excessive ultraviolet absorption is suppressed.
Claims
1. An optical laminate comprising: Optical films including polarizers, a first adhesive layer disposed on a first main surface of the optical film, a first adherend attached to the first adhesive layer, a second adhesive layer disposed on the second main surface of the optical film, and fixing the organic electroluminescent unit stacked on the second adhesive layer; The transmittance of the first adhesive layer and the second adhesive layer for light with a wavelength of 420 nm is 85% or more. The transmittance of the first adhesive layer to light of a wavelength of 355 nm is 80% or less, The second adhesive layer satisfies at least one of a thickness of 30 μm or less and a transmittance of light of a wavelength of 355 nm of 80% or less, The transmittance of the organic electroluminescent unit for light with a wavelength of 355 nm is 70% or less, The optical laminate is provided with a through hole penetrating at least the organic electroluminescent unit, the second adhesive layer, the optical film, and the first adhesive layer.
2. The optical laminate according to claim 1, wherein: The organic electroluminescent unit includes a polyimide film.
3. The optical layered body according to claim 1 or 2, wherein: The first adherend is a first release film temporarily attached to the first adhesive layer.
4. The optical layered body according to claim 1 or 2, wherein: The first adherend is a first release film temporarily attached to the first adhesive layer, and the through hole penetrates the first adherend.
5. The optical layered body according to claim 1 or 2, wherein: The first adhesive layer has a thickness of 30 μm or more.
6. The optical layered body according to claim 1 or 2, wherein: The second adhesive layer has a thickness smaller than that of the first adhesive layer.
7. The optical layered body according to claim 1 or 2, wherein: The first adhesive layer has a transmittance of light of a wavelength of 355 nm of 20% or more.
8. The optical layered body according to claim 1 or 2, wherein: The first adhesive layer has a storage elastic modulus at 25° C. of 0.35 MPa or less.
9. The optical layered body according to claim 1 or 2, wherein: The first adhesive layer is a photocurable adhesive including a photocurable compound and a photopolymerization initiator.
10. The optical layered body according to claim 1 or 2, wherein: The storage elastic modulus of the second adhesive layer at 25° C. is greater than the storage elastic modulus of the first adhesive layer at 25° C.
11. The optical layered body according to claim 1 or 2, wherein: The transmittance of the second adhesive layer at a wavelength of 355 nm is greater than the transmittance of the first adhesive layer at a wavelength of 355 nm.
12. The optical layered body according to claim 1 or 2, wherein: The optical film includes a resin film provided in contact with at least one surface of a polarizer, and the transmittance of the resin film for light of a wavelength of 355 nm is 10% or less.
13. A method for producing an optical laminate, wherein a through hole is formed in the laminate by laser processing, wherein: The laminate comprises: Optical films including polarizers, a first adhesive layer disposed on a first main surface of the optical film, a first adherend attached to the first adhesive layer, a second adhesive layer disposed on the second main surface of the optical film, and fixing the organic electroluminescent unit stacked on the second adhesive layer; The transmittance of the first adhesive layer and the second adhesive layer for light with a wavelength of 420 nm is 85% or more. The transmittance of the first adhesive layer to light of a wavelength of 355 nm is 80% or less, The second adhesive layer satisfies at least one of a thickness of 30 μm or less and a transmittance of light of a wavelength of 355 nm of 80% or less, The transmittance of the organic electroluminescent unit for light with a wavelength of 355 nm is 70% or less, A through hole penetrating the organic electroluminescent unit, the second adhesive layer, the optical film, the first adhesive layer, and the first adherend is formed by irradiating the main surface on the organic electroluminescent unit side with ultraviolet laser light.
14. A display device comprising an image display element and an optical element, wherein: The image display element comprises: Optical films including polarizers, a first adhesive layer disposed on a first main surface of the optical film, a transparent adherend attached to the first adhesive layer, a second adhesive layer disposed on the second main surface of the optical film, and an organic electroluminescent unit attached to the second adhesive layer; The transmittance of the first adhesive layer and the second adhesive layer for light with a wavelength of 420 nm is 85% or more. The transmittance of the first adhesive layer to light of a wavelength of 355 nm is 80% or less, The second adhesive layer satisfies at least one of a thickness of 30 μm or less and a transmittance of light of a wavelength of 355 nm of 80% or less, The transmittance of the organic electroluminescent unit for light with a wavelength of 355 nm is 70% or less, The image display element is provided with a through hole penetrating the organic electroluminescent unit, the second adhesive layer, the optical film and the first adhesive layer, One or more optical elements selected from the group consisting of a light receiving element and a light emitting element are arranged in or below the through hole.
Citation Information
Patent Citations
Hakumakujinkohenkomakuno seiho
JP1976069644A
Polarizing plate and its production
JP2000338329A
Polarizing film with adhesive layer, and image display device
JP2016157077A
Highly functional thin polarizing film and process for producing same
WO2010100917A1
Polarizing plate and image display device
JP2017151162A