A device and method for testing interface strength of second-generation high-temperature superconducting tape

By using epoxy resin materials and superconducting strips to be closely adhered and combined with an electronic universal testing machine for tensile testing, the problem of poor testing results in the existing technology has been solved, and accurate measurement of the interface strength of the second-generation high-temperature superconducting strips has been achieved. Measurement and multi-angle testing improve data accuracy and consistency.

CN111879612BActive Publication Date: 2024-10-22LANZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010725444.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-24
Publication Date
2024-10-22
Estimated Expiration
2040-07-24

AI Technical Summary

Technical Problem

The existing second-generation high-temperature superconducting strip testing methods have problems such as poor interface strength testing results and low data accuracy, especially in the transverse and longitudinal tensile experiments and the lack of testing in the tilted state.

Method used

The tensile block made of epoxy resin material is closely adhered to the superconducting tape. The tensile block model is made through 3D printing and silicone mold, and the transverse tensile test is carried out with an electronic universal testing machine. The peel strength is measured through the force-displacement curve. Determine and verify the feasibility of the test plan through finite element numerical calculations.

Benefits of technology

It improves the accuracy and consistency of test data, reduces the dispersion of experimental results, and enables multi-angle strength testing of superconducting strips to study their mechanical properties under different stress conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111879612B_ABST
    Figure CN111879612B_ABST
Patent Text Reader

Abstract

The present invention discloses a device and method for testing the interface strength of a second-generation high-temperature superconducting tape, comprising a first stretching block and a second stretching block made of epoxy resin material, one end of each of the first stretching block and the second stretching block forming a clamping end, and the other end forming a fixed end, the plane where the fixed end is located forms an angle of 0 to 90 degrees with the horizontal plane, and the plane where the fixed ends of the first stretching block and the second stretching block are located is parallel; the upper and lower surfaces of the superconducting tape are respectively in close contact with the fixed ends of the first stretching block and the second stretching block, and the superconducting tape is fixed to the first stretching block and the second stretching block as a whole through epoxy resin. A method for testing the interface strength of a second-generation high-temperature superconducting tape comprises the steps of making a silicone mold, processing a superconducting tape, fixing the superconducting tape and stretching testing. The sample is integrally formed, and the experiment is simple and convenient; the epoxy resin is tightly adhered to the superconducting tape, and when stretching, the superconducting tape can be uniformly stressed, thereby improving the accuracy of the measurement data.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superconducting tape experiments, and in particular relates to a device and a method for testing the interface strength of a second-generation high-temperature superconducting tape. Background Art

[0002] The second-generation high-temperature superconducting tape is a typical multi-layer composite material. Due to the different thicknesses of each layer (0.2-50μm), large differences in material properties, and uneven interlayer bonding strength, the tape is prone to interlayer delamination during low-temperature electromagnetic field conditions, tensile fatigue testing, quenching, heat treatment and cooling, resulting in degradation of superconducting performance or even complete failure. In order to further study the interface strength performance of the tape, it is necessary to conduct a tensile delamination test on the tape.

[0003] REBCO tape has a regular geometric shape and can be easily wound into a disc or arc shape for application in engineering. However, the REBCO tape itself has a multi-layer structure, and its normal and tangential bearing capacity is limited, making it prone to damage. Studies have shown that REBCO tape only exhibits good mechanical properties in the axial direction and can withstand axial stresses of up to 700MPa; due to the layered composite structure of the tape and the brittle properties of the core functional superconducting film, the transverse tensile strength and shear strength of the tape are much smaller than the axial tensile strength; in particular, the critical delamination and dissociation stress of the REBCO tape is less than 1MPa.

[0004] At present, the anvil test method is a commonly used experimental method for testing the interfacial strength of strips. It uses anvils welded on the upper and lower surfaces of the strip to apply transverse tensile stress to cause the strip to peel off. However, this method has many factors that affect the experimental results. For example, the side wrapping state of the strip, the elastic-plastic deformation of the surface material, the welding process, the cutting edge of the strip and internal defects, etc., all of these factors will cause the results to be scattered. In addition, the existing anvils apply uneven force to the surface of the strip, the test results are poorly stable, and the data accuracy is low; at the same time, when testing with the anvil test method, only transverse and longitudinal tensile tests are performed on the strip, and the tensile test of the strip in an inclined state has not yet been conducted. Summary of the invention

[0005] The present invention provides a device and method for testing the interface strength of a second-generation high-temperature superconducting tape, aiming to solve the problems of poor testing effect and low data accuracy of existing tapes.

[0006] To this end, the present invention adopts the following technical solutions:

[0007] A second-generation high-temperature superconducting tape interface strength testing device comprises a first stretching block and a second stretching block made of epoxy resin material, one end of each of the first stretching block and the second stretching block forms a clamping end for connecting an experimental device, and the other end forms a fixed end for connecting a superconducting tape, the plane where the fixed end is located forms an angle of 0 to 90 degrees with a horizontal plane, and the plane where the fixed ends of the first stretching block and the second stretching block are located are parallel; the upper and lower surfaces of the superconducting tape are respectively tightly attached to the fixed ends of the first stretching block and the second stretching block, and the superconducting tape is fixed to the first stretching block and the second stretching block as a whole through epoxy resin.

[0008] Furthermore, the fixing end is planar or stepped.

[0009] Furthermore, the clamping ends of the first stretching block and the second stretching block are wedge-shaped, and the fixing ends are rectangular.

[0010] A method for testing the interface strength of a second-generation high-temperature superconducting tape comprises the above-mentioned device for testing the interface strength of a second-generation high-temperature superconducting tape, and comprises the following steps:

[0011] (1) Silicone mold production: first, a stretching block model is produced by 3D printing, and then the stretching block model is used to produce a corresponding silicone mold;

[0012] (2) Superconducting tape processing: Use sandpaper to grind the upper and lower surfaces of the superconducting tape, and cut off the welding areas on both sides of the superconducting tape with a cutting width of 0.5 to 2 mm, and cut the superconducting tape into rectangular blocks;

[0013] (3) Fixing the superconducting tape: Place the superconducting tape in a silicone mold and pour epoxy resin into the silicone mold so that the epoxy resin completely wraps the superconducting tape; then place the silicone mold in a vacuum chamber to exhaust the air, and then place the silicone mold in a constant temperature box to completely cure the epoxy resin. The epoxy resin on both sides of the superconducting tape forms a first stretching block and a second stretching block respectively; remove the stretching block from the silicone mold and polish the surroundings of the stretching block so that there is no adhesion between the surroundings of the superconducting tape and the stretching block;

[0014] (4) Tensile test: Finally, the tensile block is connected to the electronic universal testing machine, a tensile load is applied, and the strip is subjected to a tensile test until the strip is completely peeled off;

[0015] (5) Determine the validity of the experiment: Observe the sample morphology after the experiment and determine the validity of the experimental results.

[0016] Furthermore, when polishing the superconducting tape in step (2), sandpaper is used to polish the upper and lower surfaces of the tape at a 45° angle.

[0017] Furthermore, in the step (2), a wire cutting device is used to cut the superconducting tape.

[0018] The testing principle of the present invention is as follows:

[0019] 1. During the transverse stretching process, a load of 0.2 mm / min is applied to the strip until the strip is peeled off. On the force-displacement curve, the value at the point where the curve suddenly drops is the maximum tensile force. The interface peel strength is defined as:

[0020] (1)

[0021] Among them: F max is the maximum tensile force applied in the experiment, S del is the delamination area of ​​the strip, that is, the cross-sectional area of ​​the strip in this experiment.

[0022] 2. Numerical modeling

[0023] Numerical calculations are performed within the framework of the finite element method to verify the feasibility of the proposed test scheme in testing the interfacial peel strength of the strip.

[0024] This study is based on the existing bilinear cohesion model, which has three most important independent parameters: the critical energy release rate at fracture G ic , interfacial bonding strength , and the initial penalty stiffness K. The model uses the degradation of the interfacial stiffness K to characterize the interfacial debonding of the composite material, while the stiffness degradation is completed by the damage evolution function. The initiation displacement of stiffness degradation is defined as And define the final failure displacement as , the relationship between the two can be determined by the following relationship:

[0025] (2)

[0026] (3)

[0027] Where: n: normal (type I crack) component; s: tangential (type II, type III crack) component. Introducing variables The maximum value of the latest relative displacement of the upper and lower nodes of the tracking interface (defined in the normal and tangential directions as: , ) and The latest stiffness K after the relevant interface stiffness reduction , . And define the loading function:

[0028] The whole peeling process can be expressed as:

[0029] (4)

[0030] Where: D i is the interface damage evolution function;

[0031] (5)

[0032] in: is the maximum peeling displacement. Under the mixed loading mode, the secondary criterion is used as the criterion for judging the initiation of interface cracking:

[0033] (6)

[0034] Where: n represents the normal stress, σ s represents the tangential stress.

[0035] Once the interface cracking condition is reached, the power exponent criterion is used as the criterion for judging interface failure, which is expressed as:

[0036] (7)

[0037] Where: G n and G s They represent the energy release rates in the normal and tangential directions under the mixed loading mode. When the index α is selected as 1, the total energy release rate satisfies G = G n +G s ;

[0038] 3. Numerical calculation results:

[0039] According to the above numerical calculation method, taking type I interface cracking, i.e. transverse tensile peeling, as an example, the experiment was simulated to verify the feasibility of this scheme.

[0040] According to the experimental scheme for determining the interfacial peel strength, in the simulation, we define the equivalent tensile stress as:

[0041] (8)

[0042] in, F is the tensile force applied to the sample, S This is the strip cross section in this experiment.

[0043] Figure 7 The numerical calculation results of equivalent tensile stress and displacement are given. It can be seen that the equivalent tensile stress increases with the increase of displacement load. After reaching the maximum value, it decreases with the increase of displacement. In the experiment, the maximum value is the experimentally determined transverse tensile peel strength of the interface, and the numerical calculation shows that the result is consistent with the set transverse tensile peel strength ( ), indicating that this experimental method can accurately determine the interfacial peeling strength of the strip.

[0044] The beneficial effects of the present invention are as follows:

[0045] 1. This method uses wire cutting technology to cut off the side edge of the strip, uses 3D printing technology to prepare the sample model, and then cures the processed strip in epoxy resin to make transverse tensile peeling and longitudinal shear peeling specimens. The specimens are integrally formed, and the experiment is simple and convenient;

[0046] 2. The epoxy resin is tightly attached to the superconducting tape, which can make the superconducting tape evenly stressed during stretching, thus improving the accuracy of the measurement data;

[0047] 3. Before testing, first cut off the side edge (solder or copper) of the strip to remove the influence of the non-interface mechanical behavior (elastic-plastic deformation) of the strip; reduce the influence of measurement errors and welding process; reduce the influence of micro-cracks at the strip boundary, thereby reducing the dispersion of the experimental results;

[0048] 4. The device and method can be used to perform multi-angle strength tests on superconducting tapes, which is convenient for studying the mechanical properties of superconducting tapes under different stress conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a schematic structural diagram of the first stretching block of Example 1 of the present invention;

[0050] Figure 2 is a schematic diagram of fixing the superconducting tape in Example 1 of the present invention;

[0051] Figure 3 is a schematic structural diagram of the first stretching block of Example 2 of the present invention;

[0052] Figure 4 is a schematic diagram of fixing the superconducting tape in Example 2 of the present invention;

[0053] Figure 5 is a schematic structural diagram of the first stretching block of Example 3 of the present invention;

[0054] Figure 6 is a schematic diagram of fixing the superconducting tape in Example 3 of the present invention;

[0055] Figure 7 is a graph showing the relationship between equivalent tensile stress and displacement of the present invention;

[0056] Figure 8 is a graph showing the relationship between the transverse tensile force and the displacement of the present invention;

[0057] In the figure: 1-first stretching block, 2-second stretching block, 3-clamping end, 4-fixed end, 5-superconducting tape. DETAILED DESCRIPTION

[0058] A second-generation high-temperature superconducting tape interface strength testing device includes a first stretching block 1 and a second stretching block 2 made of epoxy resin material. The first stretching block 1 and the second stretching block 2 have the same shape and size. The first stretching block 1 and the second stretching block 2 are both Y-shaped, with a clamping end 3 formed at one end of the wedge and a fixed end 4 at one end of the rectangle. The clamping end 3 is used to connect the stretching test equipment, and the fixed end 4 is used to connect the superconducting tape 5. The fixed end 4 is planar or step-shaped, and the plane where the fixed end 4 is located forms an angle of 0 to 90 degrees with the horizontal plane, and the plane where the fixed ends 4 of the first stretching block 1 and the second stretching block 2 are located is parallel. When in use, the upper and lower surfaces of the superconducting tape 5 are respectively close to the fixed ends 4 of the first stretching block 1 and the second stretching block 2, and the superconducting tape 5 is fixed to the first stretching block 1 and the second stretching block 2 as a whole through epoxy resin.

[0059] A method for testing the interface strength of a second-generation high-temperature superconducting tape comprises the above-mentioned device for testing the interface strength of a second-generation high-temperature superconducting tape 5, and comprises the following steps:

[0060] (1) Silicone mold making: First, a stretching block model is made by 3D printing. The shape and size of the stretching block model are the size of the first stretching block 1. After printing, polishing liquid is applied to the surface of the stretching block to make the surface flat and smooth, and then the stretching block model is used to make the corresponding silicone mold.

[0061] In this experiment, Essil-296 resin produced by Axson was used to make silicone molds. First, the silicone rubber and the corresponding curing agent were mixed in a mass ratio of 10:1 and stirred for 15 minutes to ensure uniform mixing. Then the mixed silicone rubber was placed in a vacuum box and evacuated for 15 minutes to expel the bubbles mixed in during the stirring process. After taking it out, the silicone was poured into the stretching block model. Be as careful as possible during the pouring process to avoid mixing bubbles again. After the silicone fills the model and stops flowing, it can be moved to a constant temperature box with the temperature in the box set to 30°C. Keep it warm for 24 hours to allow the silicone to cure. When the silicone is completely cured, the stretching block model is removed from the cured silicone mold.

[0062] (2) Superconducting tape processing: In order to improve the bonding strength between the epoxy resin and the tape surface, the upper and lower surfaces of the superconducting tape 5 were cross-grinded at 45 degrees using sandpaper. In order to eliminate the influence of the 1 mm solder on both sides of the tape on the test results, the wire cutting method was used to cut off 1.5 mm on both sides of the tape, and finally the tape was processed into small pieces of 9 × 10 mm.

[0063] (3) Superconducting tape fixing:

[0064] First, mix the epoxy resin and curing agent in a mass ratio of 100:8, stir evenly, and put it into a vacuum box to remove the bubbles for 15 minutes; then place the treated strip in a silicone mold and pour in the epoxy resin. In order to further extract the tiny bubbles in the epoxy resin, pour a small amount of epoxy resin into the silicone mold with the strip fixed each time, put it into a vacuum box and evacuate for 5 minutes, and repeat 3 times. Since the volume of epoxy resin will shrink to a certain extent during the curing process, the epoxy resin should be slightly overflowed from the edge of the mold when the epoxy resin is added for the last time, and it is convenient to treat the surface of the epoxy resin sample. After the vacuum is completed, put the sample in a constant temperature box at 30°C for 12 hours. After the epoxy resin is completely cured, take out the sample from the silicone mold and polish the sample with a file and sandpaper to ensure that the clamping section is flat and the epoxy resin on the upper and lower sides of the strip is not adhered. The epoxy resin on both sides of the superconducting tape 5 forms the first stretching block 1 and the second stretching block 2 respectively;

[0065] (4) Tensile test: Finally, the stretching block is connected to the experimental equipment, the first stretching block 1 is connected to the upper fixture, and the second stretching block 2 is connected to the lower fixture. Then, the corresponding experimental plan is set in the stretching machine control software, and finally the sample is stretched at a loading speed of 0.2 mm / min. During the stretching process, the CCD is used to monitor the deformation of the sample, analyze whether the sample is subjected to a uniform tensile load, and determine the centering of the sample.

[0066] (5) Determine the validity of the experiment: Observe the sample morphology after the experiment and remove samples with local damage or uneven peeling to ensure the validity of the experimental results.

[0067] The specific structures of the first stretching block 1 and the second stretching block 2 refer to the following embodiments:

[0068] Embodiment 1:

[0069] like Figure 1 and 2 As shown, the fixed ends 4 of the first stretching block 1 and the second stretching block 2 are planar, and this structure can be used to perform a stretching test on the strip in the transverse direction; when this fixing scheme is selected, the stretching block model is a structure in which the first stretching block 1 and the second stretching block 2 are connected as one. In the experiment, when fixing the superconducting tape 5, the tape is vertically inserted into the middle of the silicone mold, and then epoxy resin is poured into the silicone mold. The epoxy resin on both sides of the superconducting tape 5 forms the first stretching block 1 and the second stretching block 2 respectively.

[0070] Embodiment 2:

[0071] like Figure 3 and 4As shown, when the fixed ends 4 of the first stretching block 1 and the second stretching block 2 are in the shape of horizontal steps, the structure is stretched along the longitudinal direction of the strip; when this fixing scheme is selected, two stretching block models need to be made, namely the first stretching block model and the second stretching block model, wherein the first stretching block model has the same shape as the first stretching block 1, and the second stretching block model has the same structure as the first stretching block 1 and the second stretching block 2 when connected into one; correspondingly, the first silicone mold and the second silicone mold need to be made. First, the first stretching block 1 is made using the first silicone mold, and then the first stretching block 1 is placed in the second silicone mold, and the superconducting tape 5 is placed on the horizontal step of the fixed end 4 of the first stretching block 1, and then the epoxy resin is poured, and the second stretching block 2 is formed after the epoxy resin is cured. In order to prevent the first stretching block 1 and the second stretching block 2 from being fixed into one after casting, silicone rubber can be placed at the vertical joint of the step, and the silicone rubber is taken out after the second stretching block 2 is cast, so that the first stretching block 1 and the second stretching block 2 are connected only by the strip, and there is no adhesion in the vertical direction, so as to avoid affecting the accuracy of the experiment.

[0072] Embodiment 3:

[0073] like Figure 5 and 6 As shown, when the fixed ends 4 of the first stretching block 1 and the second stretching block 2 are in the shape of inclined steps, the structure can stretch the strip along a certain inclination angle; when this structure is selected, two stretching block models need to be made, namely the first stretching block model and the second stretching block model, and the subsequent production process is the same as that of Example 2.

[0074] Experimental results:

[0075] A REBCO coated high temperature superconducting composite tape was used as the experimental tape, which was cut into small pieces of 9 mm×10 mm. Taking the transverse tensile peel strength experiment of the interface as an example, a tensile experiment was performed according to the steps described in Example 1 to obtain corresponding experimental results.

[0076] Figure 8 The effective experimental results of the relationship curve between the transverse tensile force (equivalent tensile stress) and the displacement are shown. It can be seen that the samples represented by the four solid lines show a high consistency with the test results. The effective results show that the tensile load is between 197 and 228 N. According to formula (1), the effective transverse tensile interface peel strength is 2.19 to 2.51 MPa, the average value is 2.34 MPa, the maximum relative error is 7.3%, and the discreteness of the data is greatly reduced compared with the anvil measurement method.

[0077] It should be noted that the above are only some embodiments of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A method for testing the interface strength of second-generation high-temperature superconducting tapes. It is characterized in that It comprises a second-generation high-temperature superconducting tape interface strength test device, the test device comprises a first stretching block and a second stretching block made of epoxy resin material, one end of each of the first stretching block and the second stretching block forms a clamping end for connecting the experimental equipment, and the other end forms a fixed end for connecting the superconducting tape, the plane where the fixed end is located forms an angle of 0 to 90 degrees with the horizontal plane, and the plane where the fixed ends of the first stretching block and the second stretching block are located is parallel; the upper and lower surfaces of the superconducting tape are respectively in close contact with the plane where the fixed ends of the first stretching block and the second stretching block are located, and the superconducting tape is fixed to the first stretching block and the second stretching block as a whole through epoxy resin; The testing method comprises the following steps: (1) Silicone mold production: first, a stretching block model is produced by 3D printing, and then the stretching block model is used to produce a corresponding silicone mold; (2) Superconducting tape processing: Use sandpaper to grind the upper and lower surfaces of the superconducting tape, and cut off the welding areas on both sides of the superconducting tape with a cutting width of 0.5 to 2 mm, and cut the superconducting tape into rectangular blocks; (3) Fixing the superconducting tape: Place the superconducting tape in a silicone mold and pour epoxy resin into the silicone mold so that the epoxy resin completely wraps the superconducting tape; then place the silicone mold in a vacuum chamber to exhaust the air, and then place the silicone mold in a constant temperature box to completely cure the epoxy resin. The epoxy resin on both sides of the superconducting tape forms a first stretching block and a second stretching block respectively; remove the stretching block from the silicone mold and polish the surroundings of the stretching block so that there is no adhesion between the surroundings of the superconducting tape and the stretching block; (4) Tensile test: Finally, the tensile block is connected to the electronic universal testing machine, a tensile load is applied, and the strip is subjected to a tensile test until the strip is completely peeled off; (5) Determine the validity of the experiment: Observe the sample morphology after the experiment and determine the validity of the experimental results.

2. The method for testing the interface strength of the second generation high temperature superconducting tape according to claim 1, It is characterized in that The fixing end is in a plane shape or a step shape.

3. The method for testing the interface strength of the second generation high temperature superconducting tape according to claim 1, It is characterized in that The clamping ends of the first stretching block and the second stretching block are wedge-shaped, and the fixing ends are rectangular.

4. The method for testing the interface strength of the second generation high temperature superconducting tape according to claim 1, It is characterized in that When polishing the superconducting tape in step (2), sandpaper is used to polish the upper and lower surfaces of the tape at a 45° angle.

5. The method for testing the interface strength of the second generation high temperature superconducting tape according to claim 1, It is characterized in that In the step (2), the superconducting tape is cut using a wire cutting device.

Citation Information

Patent Citations

  • Method for representing interfacial shear strength between high-performance fiber and non-transparent resin matrix

    CN108535099A

  • Second-generation high-temperature superconducting strip interface strength testing device