Semiconductor device manufacturing method and semiconductor device

By using titanium nitride and titanium contact metal films in semiconductor devices, combined with the design of high-concentration dopant regions and source regions, the problems of high contact resistance and large cell spacing in semiconductor devices are solved, achieving higher Reliability and tightness.

CN111937158BActive Publication Date: 2024-10-22SHINDENGEN ELECTRIC MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880091637.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-04-11
Publication Date
2024-10-22
Estimated Expiration
2038-04-11

AI Technical Summary

Technical Problem

In semiconductor devices, the contact resistance between the high-concentration dopant region and the contact metal film is high, which may cause parasitic bipolar transistor operation when the MOSFET is turned off, and when different contact metals are used in the n-type and p-type regions There is a problem of increased unit spacing.

Method used

Using a contact metal film containing titanium nitride and titanium, a high-concentration dopant region and a source region are formed on the silicon carbide semiconductor substrate, and a contact metal film is formed on the insulating film to reduce contact resistance and improve adhesion. , avoid using nickel to prevent the production of free carbon.

Benefits of technology

It effectively reduces the contact resistance in high-concentration areas, improves the adhesion of the contact metal layer, provides higher reliability, and reduces the unit spacing of semiconductor components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111937158B_ABST
    Figure CN111937158B_ABST
Patent Text Reader

Abstract

The semiconductor device comprises: a semiconductor substrate; a drift layer of a first conductivity type; a well region of a second conductivity type; a high concentration region of the second conductivity type; a source region of the first conductivity type; an insulating film provided on the drift layer; a first contact metal film in contact with the source region and the high concentration region via a first opening provided on the insulating film; a second contact metal film formed on a surface of the first contact metal film and in contact with the high concentration region via a second opening provided on the first contact metal film; and a source electrode film formed on a surface of a contact metal layer including the first contact metal film and the second contact metal film. The first contact metal film comprises titanium nitride, and the second contact metal film comprises titanium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a semiconductor device and a semiconductor device. Background Art

[0002] Since silicon carbide (SiC) has a dielectric breakdown electric field strength approximately 10 times that of silicon (Si), it is used as a material for high withstand voltage semiconductor devices.

[0003] In a semiconductor device (e.g., MOSFET) using a semiconductor substrate (e.g., n-type SiC), a drift layer is electrically and mechanically connected to an electrode film (e.g., an alloy containing aluminum and silicon (Al-Si) or aluminum (Al)) via a contact metal film (e.g., see Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-92038

[0007] The inventors of the present invention have found that after titanium nitride (TiN) is formed as a contact metal film on a semiconductor substrate, an ohmic contact can be formed by forming an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or an electrode film containing aluminum. However, this structure has the following problem: the high concentration region of p-type dopants (SiC (p + ))At the interface between titanium nitride and silicon, the contact resistance becomes high.

[0008] The industry generally hopes that the contact resistance between the high-concentration region of p-type dopants formed on the drift layer and the contact metal film can be reduced as much as possible. Otherwise, when the MOSFET is turned off, the potential of the high-concentration region will rise, which may cause parasitic bipolar transistor operation, etc.

[0009] For example, if the contact metal film is nickel (Ni), it is expected that the contact resistance can be reduced. Patent document 1 describes the content of bonding a region where a p-type dopant with silicon carbide is introduced at a high concentration to nickel. However, if the interface between the region where a p-type dopant with silicon carbide is introduced at a high concentration and nickel is annealed, free carbon will be generated due to the formation of nickel silicide, and the adhesion between silicon carbide and the contact metal film will be reduced. In addition, if different contact metals are to be used in the n-type region and the p-type region, the contact metal formed in the n-type region and the contact metal formed in the p-type region must be separated from each other. Therefore, since the margin is indispensable when using the known photolithography technology, there is a problem of increasing the cell spacing.

[0010] Therefore, in view of the above problems, an object of the present invention is to provide a semiconductor device with higher reliability and a method for manufacturing the same. Summary of the invention

[0011] A semiconductor device according to one embodiment of the present invention is characterized by comprising:

[0012] a semiconductor substrate composed of silicon carbide;

[0013] A drift layer of a first conductivity type, which is provided on one main surface of the semiconductor substrate;

[0014] A well region of a second conductivity type, which is disposed on the drift layer;

[0015] The second conductivity type high concentration region is disposed in the well region and has a higher dopant concentration than the well region;

[0016] The source region of the first conductivity type is disposed adjacent to the high concentration region;

[0017] an insulating film disposed on the drift layer;

[0018] a first contact metal film, which contacts the source region and the high concentration region via a first opening portion provided on the insulating film;

[0019] a second contact metal film formed on a surface of the first contact metal film and in contact with the high concentration region via a second opening provided in the first contact metal film; and

[0020] a source electrode film formed on a surface of a contact metal layer including the first contact metal film and the second contact metal film,

[0021] Wherein, the first contact metal film may include titanium nitride,

[0022] The second contact metal film may include titanium.

[0023] A method for manufacturing a semiconductor device according to one embodiment of the present invention includes:

[0024] a drift layer forming step of forming a first conductivity type drift layer on a main surface of a semiconductor substrate made of silicon carbide;

[0025] a well region forming step of forming a well region of a second conductivity type opposite to the first conductivity type on the drift layer, the well region being exposed on the surface of the drift layer;

[0026] a high-concentration region forming step of forming, on the well region of the drift layer, a high-concentration region of the second conductivity type exposed on the surface of the drift layer and having a higher dopant concentration than that of the well region;

[0027] a source region forming step of forming a source region of the first conductivity type on the well region of the drift layer, the source region being exposed on the surface of the drift layer and adjacent to the high concentration region;

[0028] an insulating film forming step of forming an insulating film having a first opening on a surface of the drift layer, wherein the first opening exposes at least a portion of the high concentration region and the source region when viewed in plan from one side of the one main surface of the semiconductor substrate;

[0029] a first contact metal film forming step of forming a first contact metal film having a second opening portion exposing a portion of the high concentration region so as to contact at least a portion of the source region in the first opening portion;

[0030] a second contact metal film forming step of forming a second contact metal film on a surface of the first contact metal film so as to be in contact with the high concentration region in the second opening; and

[0031] a source electrode film forming step of forming a source electrode film on a surface of a contact metal layer including the first contact metal film and the second contact metal film;

[0032] Wherein, the first contact metal film may include titanium nitride,

[0033] The second contact metal film may include titanium.

[0034] Effects of the Invention

[0035] According to the semiconductor device and the method for manufacturing the semiconductor device of the present invention, the adhesion of the contact metal layer in the high concentration region can be improved and the contact resistance can be reduced, thereby providing a semiconductor device with high reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a cross-sectional view showing the structure of the semiconductor device according to the first embodiment.

[0037] Figure 2 This is a flowchart showing the method for manufacturing the semiconductor device according to the first embodiment.

[0038] Figure 3A It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0039] Figure 3BIt is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0040] Figure 3C It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0041] Figure 4A It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0042] Figure 4B It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0043] Figure 4C It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0044] Figure 5A It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0045] Figure 5B It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0046] Figure 5C It is a cross-sectional view showing the method for manufacturing the semiconductor device according to the first embodiment.

[0047] Figure 6 It is a cross-sectional view showing the structure of a semiconductor device according to a second embodiment.

[0048] Figure 7 This is a flowchart showing a method for manufacturing a semiconductor device according to the second embodiment.

[0049] Fig. 8A It is a cross-sectional view showing a method for manufacturing a semiconductor device according to the second embodiment.

[0050] Figure 8B It is a cross-sectional view showing a method for manufacturing a semiconductor device according to the second embodiment.

[0051] Fig.9A It is a cross-sectional view showing a method for manufacturing a semiconductor device according to the second embodiment.

[0052] Fig. 9B It is a cross-sectional view showing a method for manufacturing a semiconductor device according to the second embodiment.

[0053] Fig.10 It is a cross-sectional view showing the structure of a semiconductor device according to a third embodiment.

[0054] Fig.11AIt is a cross-sectional view showing a method for manufacturing a semiconductor device according to a third embodiment.

[0055] Fig. 11B It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a third embodiment.

[0056] Fig. 12A It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a third embodiment.

[0057] Fig. 12B It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a third embodiment. DETAILED DESCRIPTION

[0058] [First embodiment]

[0059] The following will be Figure 1 Reference to Figure 5C A first embodiment of the present invention will be described.

[0060] (Structure of Semiconductor Device)

[0061] Below, we will refer to Figure 1 The structure of the semiconductor device according to this embodiment is described below. The semiconductor device according to this embodiment is a planar MOSFET. In addition, in the semiconductor device according to this embodiment, although a plurality of semiconductor elements are arranged adjacent to each other, Figure 1 Only one of these semiconductor elements is shown.

[0062] This embodiment is a specific description for better understanding the gist of the invention, and does not limit the present invention unless otherwise specified. In addition, in order to facilitate understanding of the features of the present invention, the drawings used in the following description sometimes enlarge the main parts, and the size ratios of the various components are not necessarily the same as in reality.

[0063] like Figure 1 As shown, the semiconductor device 1 includes: a semiconductor substrate 11; a drift layer 12; a well region 13; a high concentration region 14; a source region 15; an insulating film 16; a contact metal layer 100 and a source electrode film 19. The semiconductor device 1 further includes: a drain electrode 17 and a gate electrode 18.

[0064] The semiconductor substrate 11 is made of silicon carbide (SiC) and has n-type (first conductivity type) dopants introduced into it. + The semiconductor substrate 11 is, for example, an n-type 4H-SiC substrate on the (0001) plane.

[0065] The drift layer 102 is made of silicon carbide and is formed on one main surface F1 of the semiconductor substrate 11. An n-type dopant is introduced into the drift layer 102 at a lower concentration than that of the semiconductor substrate 11.

[0066] The drain electrode 17 is formed on the other main surface F2 of the semiconductor substrate 11. The drain electrode 17 makes ohmic contact with the semiconductor substrate 11. The drain electrode 17 can be formed of, for example, titanium nitride.

[0067] The well region 13 is formed on a part of the surface of the drift layer 12 on the opposite side to the semiconductor substrate 11. In the well region 13, a p-type (second conductivity type) dopant is introduced.

[0068] The high concentration region 14 is formed on a part of the surface of the well region 13. A p-type dopant is introduced into the high concentration region 14 at a higher concentration than that of the well region 13. This can suppress the operation of a parasitic bipolar transistor in the semiconductor device 1.

[0069] The source region 15 is formed on a portion of the surface of the well region 13. In the source region 15, n-type dopants are introduced at a higher concentration than that of the drift layer 12. When viewed in a plan view from the F1 side of one main surface of the semiconductor substrate 11 (hereinafter referred to as "plan view"), the source region 15 is surrounded by the well region 13.

[0070] In this embodiment, the source region 15 is formed in a ring shape surrounding the high concentration region 14 in a plan view. Figure 1 As shown, in the present embodiment, although the source region 15 is composed of a first source region 15a which is annular in plan view and into which a relatively high concentration of n-type dopants are introduced, and a second source region 15b which is outer side of the first source region 15a into which a relatively low concentration of n-type dopants are introduced, the structure of the source region 15 is not limited thereto.

[0071] The insulating film 16 is made of an insulator and is formed on the surface of the drift layer 12. The insulating film 16 has a first opening H1. The first opening H1 is formed so that at least a portion of the source region 15 and at least a portion of the high-concentration second conductive type region 14 are exposed when viewed from a plane. In the present embodiment, the first opening H1 is formed so that a portion of the first source region 15a is exposed.

[0072] In a plan view, the gate electrode 18 is formed to span: a region of the well region 13 where the source region 15 is not formed, a region of the drift layer 12 where the well region 13 is not formed and the source region 15 that sandwich and face the above region. Next, the gate electrode 18 may also be formed to span: another well region (not shown) that sandwiches the drift layer 12 and faces the well region 13, and a source region (not shown) that sandwiches and faces the other well region.

[0073] In a state where no voltage is applied to the gate electrode 18 (or in a state where a negative voltage is applied), even if a forward bias voltage is applied between the source region 15 and the drain electrode 17, current does not flow between the source region 15 and the drain electrode 17. When a positive voltage is applied to the gate electrode 18 in a state where a forward bias voltage is applied between the source region 15 and the drain electrode 17, an inversion channel having a conductivity type opposite to that of the well region 13 is formed on the surface of the region of the well region 13 facing the gate electrode 18. In this way, current flows between the source region 15 and the drain electrode 17. That is, the current between the source region 15 and the drain electrode 17 can be controlled by applying a voltage toward the gate electrode 18.

[0074] The contact metal layer 100 includes a first contact metal film 101 and a second contact metal film 102 .

[0075] The first contact metal film 101 is formed to contact the source region 15 and the high concentration region 14 in the first opening H1. The first contact metal film 101 has a second opening H2 formed to expose a portion of the high concentration region 14. The first contact metal film 101 is formed of titanium nitride. The contact metal film 101 is the source region 15 exposed in the first opening H1, and is formed to contact a portion of the first source region 15a. In addition, the contact metal film 101 is formed to contact a portion of the high concentration region 14 located in a portion of the source region 15 formed in a ring shape when viewed from a plane. The second opening H2 is formed to expose the central portion of the high concentration region 14.

[0076] The second contact metal film 102 is formed on the surface of the first contact metal film 101. The second contact metal film 102 is formed to contact the center of the high concentration region 14 at the second opening H2. The second contact metal film 102 is formed of titanium. In addition, titanium nitride may be further formed on the surface of the second contact metal film 102.

[0077] The source electrode film 19 is formed on the surface of the contact metal film 100. The source electrode film 19 is formed using an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or aluminum. The source regions 15 of the plurality of semiconductor elements are connected to each other through the source electrode film 19. In this embodiment, the source electrode film 19 is formed on the surface of the second contact metal film 102.

[0078] In the semiconductor device 1 according to the present embodiment, nickel is not used in the formation of the contact metal film 100 (the first contact metal film 101 and the second contact metal film 102). Therefore, since free carbon is not generated during annealing, the adhesion between the contact metal film 100 and silicon carbide (the source region 15 and the high concentration region 14) can be improved.

[0079] In the semiconductor device 1 according to the present embodiment, the second contact metal film 102 in contact with the central portion of the high concentration region 14 is formed of titanium. Therefore, compared with the case where the contact metal film 100 is formed entirely of titanium nitride, the high concentration region 14 (SiC (p + )) and the contact resistance between the contact metal film 100.

[0080] As described above, the semiconductor device 1 according to the present embodiment can improve the adhesion of the contact metal film 100 in the high concentration region 14 and reduce the contact resistance. Therefore, a semiconductor device with high reliability can be provided.

[0081] Furthermore, in the semiconductor device 1 according to the present embodiment, titanium is not used in the contact metal film 100 to form the first contact metal film 101 in contact with the source region 15. Therefore, since a Schottky junction is not formed at the interface between the contact metal film 100 and the source region 15 including an n-type dopant, an ohmic contact can be formed between the source region 15 and the source electrode film 19.

[0082] In the semiconductor device 1 according to the present embodiment, the contact metal film 101 of the source region 15 mainly including the n-type dopant and the contact metal film 102 of the high concentration region 14 including the p-type dopant are not separated from each other but are formed overlappingly on the source region 15. In this way, since the margin used for the photolithography process can be reduced, the cell pitch of the semiconductor element can be reduced.

[0083] (Method for manufacturing semiconductor device)

[0084] The following will be Figure 2 Reference to Figure 5C A method for manufacturing the semiconductor device 1 according to the present embodiment will be described.

[0085] like Figure 2 As shown, the manufacturing method of the semiconductor device 1 involved in this embodiment includes: a drift layer forming step S1; a well region forming step S2; a high concentration region forming step S3; a source region forming step S4; an insulating film forming step S5; a first contact metal film forming step S6; a second contact metal film forming step S7 and a source electrode film forming step S8.

[0086] The following will use FIG. 3A to FIG. 5C Each step in the method for manufacturing the semiconductor device 1 according to the present embodiment will be described below. In the semiconductor device 1 according to the present embodiment, a plurality of semiconductor elements are arranged adjacent to each other. FIG. 3A to FIG. 5C Only one of these semiconductor elements is shown.

[0087] (S1: Drift Layer Formation Step)

[0088] First, conduct Figure 3A In the drift layer forming step S1, n + The upper surface of the silicon carbide single crystal substrate is formed by chemical vapor deposition (CVD) - Thus, an n-type silicon carbide epitaxial layer is formed on one main surface F1 of the n-type semiconductor substrate 11 composed of silicon carbide. - The drift layer 12 is composed of a silicon carbide epitaxial layer.

[0089] (S2: Well Region Formation Step)

[0090] Then, if Figure 3B As shown, the well region forming step S2 and the high concentration region forming step S3 are performed in sequence. In the well region forming step S2, the surface of the drift layer 12 is first cleaned. Subsequently, an oxide film (not shown) composed of silicon dioxide (SiO2) is formed on the surface of the drift layer 12. Then, a resist pattern (not shown) is formed only in the portion where the p-type dopant is not introduced using a known photolithography technique. Next, the oxide film in the portion not protected by the resist pattern is etched by reactive ion etching (RIE), thereby forming a mask (not shown) having an opening in the portion corresponding to the well region 13. Thereafter, the resist pattern is removed. In this state, a p-type dopant (such as aluminum) is introduced into the drift layer 12 using ion implantation. After the p-type dopant is introduced, the mask is removed. Thus, a p-type well region 13 is formed that is exposed in a portion of the drift layer 102.

[0091] (S3: High-concentration region forming step)

[0092] In the high concentration region forming step S3, a mask (not shown) having an opening is formed at a portion of the well region 13 corresponding to the high concentration region 14, similarly to the well region forming step S2. In this state, high concentration p-type dopant ions having a higher concentration than that of the well region 13 are introduced into the well region 13 using ion implantation. After the p-type dopant is introduced, the mask is removed. Thus, a p-type high concentration region 14 is formed which is exposed on the surface of the drift layer 12 and has a higher dopant concentration than that of the well region 13. The high concentration region 14 can also be formed, for example, between the source region forming step S4 and the insulating film forming step S5.

[0093] (S4: Source Region Formation Step)

[0094] Next, proceed Figure 3CThe source region forming step S4 shown in FIG. In the source region forming step S4, first, a mask (not shown) having an opening is formed at a portion corresponding to the first source region 15a in the same manner as in the well region forming step S2. In this state, an n-type dopant (e.g., phosphorus (P) or nitrogen (N)) is introduced into a portion of the well region 13 in the drift layer 12 using ion implantation. After the n-type dopant is introduced, the mask is removed. Thus, the first source region 15a is formed in a portion of the surface of the well region 13 that is exposed. In addition, the second source region 15b is also formed in a portion of the surface of the well region 13 using the same steps.

[0095] In the well region forming step S2 , the high concentration region forming step S3 , and the source region forming step S4 , after the dopant is introduced by ion implantation, annealing is performed at, for example, 1650° C. to 1800° C. in order to activate the implanted dopant.

[0096] (S5: Insulating Film Forming Step)

[0097] Next, proceed Figure 4A In the insulating film forming step S5, first, Figure 4A As shown, an oxide film 16a is formed on the surface of the drift layer 12. Subsequently, a polysilicon film is formed on the oxide film 16a by chemical vapor deposition. After the polysilicon film is formed, an n-type dopant (e.g., phosphorus) is introduced into the polysilicon film. After the dopant is introduced, a resist pattern (not shown) is formed to protect the portion corresponding to the gate electrode 18 using a known photolithography technique. Subsequently, the portion not protected by the resist pattern is removed by dry etching. Thereafter, the resist pattern is removed. Thus, as shown in FIG. Figure 4B As shown, the gate electrode 18 is formed. Next, silicon dioxide is deposited by chemical vapor deposition so as to cover the gate electrode 18, and an oxide film 16b is formed (see Figure 4C ). Then, a resist pattern (not shown) having an opening is formed at a portion corresponding to the opening H1 using a known photolithography technique. In the oxide films 16a and 16b, portions not protected by the resist pattern are removed by dry etching. Thereafter, the resist pattern is removed. Thus, Figure 4C As shown, an insulating film 16 composed of oxide films 16a and 16b and having a first opening H1 is formed on the surface of the drift layer 12. The first opening H1 is formed so that at least a portion of the high concentration region 14 and the source region 15 are exposed when viewed from a plane.

[0098] (S6: First Contact Metal Film Forming Step)

[0099] Next, proceed Figure 5AThe first contact metal film forming step S6 shown in . In the first contact metal film forming step S6, titanium nitride is first formed on the surface of the insulating film 16 by sputtering in a mixed atmosphere of nitrogen (N2) and argon (Ar) or in a nitrogen (N2) atmosphere at a substrate temperature of, for example, 150°C to 350°C. Next, a resist pattern (not shown) having an opening corresponding to the second opening H2 and protecting a portion corresponding to the first contact metal film 101 is formed using a known photolithography technique. Subsequently, the portion not protected by the resist pattern is removed by dry etching. Thereafter, the resist pattern is removed. In the first contact metal film forming step S6, titanium nitride can also be formed, for example, on the other main surface F2 of the semiconductor substrate 11.

[0100] Subsequently, annealing is performed. The annealing temperature is preferably 800-1000°C, and a more ideal temperature is, for example, 950°C. Once the temperature is greater than or equal to 1050°C, nitrogen atoms diffuse from the titanium nitride forming the contact metal 101 to the p-type silicon carbide, which causes the contact resistance of the p-type silicon carbide portion to increase. The annealing atmosphere is preferably an inert gas such as nitrogen, argon, or a mixed gas thereof. Thus, a first contact metal film 101 having a pattern corresponding to a second opening H2 in which a portion of the high concentration region 14 is exposed is formed: in the first opening H1, it contacts the source region 15 and the high concentration region 14. At the same time, a drain electrode 17 is formed on the other main surface F2 of the semiconductor substrate 11, which is ohmically connected to the drift layer 12 via the semiconductor substrate 11.

[0101] In addition, in the present embodiment, although the drain electrode 17 is formed in the first contact metal film forming step S6 , the drain electrode 17 may be formed by providing another step.

[0102] When nickel is used as the contact metal, nickel silicide is formed at the interface during annealing to generate free carbon, which reduces the adhesion between silicon carbide and the contact metal film. In this embodiment, since free carbon is not generated during annealing, the adhesion of the first contact metal film 101 can be maintained.

[0103] (S7: Second Contact Metal Film Formation Step)

[0104] Next, proceed Figure 5BThe second contact metal film forming step S7 shown in . In the second contact metal film forming step S7, titanium is first formed on the surface of the first contact metal film 101 and the high concentration region 14 exposed in the second opening H2 by sputtering or electron beam evaporation. Thereafter, a resist pattern (not shown) is formed to protect the portion corresponding to the second contact metal 102 using a known photolithography technique. Subsequently, the portion not protected by the resist pattern is removed by dry etching. Thereafter, the resist pattern is removed. Thereafter, the mask is removed. Next, annealing is performed in the same manner as in the first contact metal film forming step S6. Thus, the second contact metal film 102 is formed on the surface of the first contact metal film 101 in such a manner as to be in contact with the high concentration region 14 in the second opening H2.

[0105] In addition, when the annealing atmosphere contains nitrogen, titanium nitride is formed on at least the surface portion of the second contact metal 102 .

[0106] (S8: Source Electrode Film Formation Step)

[0107] Finally, proceed Figure 5C The source electrode film forming step S8 shown in . In the source electrode film forming step S8, an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or aluminum is formed on the surface of the contact metal layer 100 by sputtering. Thus, a source electrode film 19 connected to the source regions 15 of a plurality of semiconductor elements is formed on the surface of the contact metal layer 100. In addition, in the source electrode film 19, portions that are not necessary for the connection to the source region 15 are removed by appropriate etching. At this time, if dry etching is used, the peripheral portion of the device and the unnecessary portions can be removed simultaneously in the contact metal film 100. The manufacturing of the semiconductor device 1 can be completed by the above method.

[0108] In the method for manufacturing the semiconductor device 1 according to the present embodiment, nickel is not used in the formation of the contact metal film 100 (the first contact metal film 101 and the second contact metal film 102). As a result, free carbon is not generated during annealing, thereby improving the adhesion between the contact metal layer 100 and silicon carbide (the source region 15 and the high-concentration region 14).

[0109] In the method for manufacturing the semiconductor device 1 according to the present embodiment, the second contact metal film 102 in contact with the central portion of the high concentration region 14 is formed of titanium. Therefore, compared with the case where the contact metal film 100 is formed entirely of titanium nitride, the high concentration region 14 (SiC (p + )) and the contact resistance between the contact metal layer 100.

[0110] As described above, the method for manufacturing the semiconductor device 1 according to the present embodiment can improve the adhesion of the contact metal layer 100 in the high concentration region 14 and reduce the contact resistance. Therefore, a semiconductor device with high reliability can be provided.

[0111] Furthermore, in the method for manufacturing the semiconductor device 1 according to the present embodiment, titanium is not used in the contact metal layer 100 to form the first contact metal film 101 in contact with the source region 15. Therefore, since a Schottky junction is not formed at the interface between the contact metal layer 100 and the source region 15 including an n-type dopant, an ohmic contact can be formed between the source region 15 and the source electrode film 19.

[0112] In the semiconductor device 1 involved in this embodiment, the contact metal film 101 of the source region 15 mainly including n-type dopants and the contact metal film 102 of the high concentration region 14 including p-type dopants are not separated from each other, but are overlapped and formed on the source region 15. This can reduce the margin used for the photolithography process. In this way, it is possible to reduce the manufacturing cost while reducing the cell pitch of the semiconductor element. In addition, the contact metal 100 can be formed as follows: the first contact metal 101 contacts only a portion of the source region 15, and the second contact metal 102 contacts both a portion of the source region 15 and the high concentration region 14.

[0113] [Second embodiment]

[0114] The following will be Figure 6 Reference to Fig. 9B A second embodiment of the present invention will be described below, and description of parts common to the first embodiment will be omitted.

[0115] (Structure of Semiconductor Device)

[0116] like Figure 6 As shown, in the semiconductor device 2 of this embodiment, the contact metal layer 100 includes granular nickel silicide 205 provided on the contact surface with the high concentration region 14. The contact metal layer 100 may include titanium carbide.

[0117] In the semiconductor device 2 involved in this embodiment, the free carbon generated after the reaction of nickel and silicon carbide during annealing will be absorbed as titanium carbide in the second contact metal film 202 through the reaction with titanium, thereby improving the adhesion between the contact metal layer 200 and silicon carbide (source region 15, high concentration region 14).

[0118] In the semiconductor device 2 according to the present embodiment, nickel silicide 205 is included in a portion of the second contact metal film 202 in contact with the central portion of the high concentration region 14. Therefore, compared with the case where the contact metal layer 200 is formed entirely of titanium nitride, the high concentration region 14 (SiC (p + )) and the contact resistance between the contact metal layer 200.

[0119] As described above, the semiconductor device 2 according to the present embodiment can improve the adhesion of the contact metal layer 200 in the high concentration region 14 and reduce the contact resistance. Therefore, a semiconductor device with high reliability can be provided.

[0120] In the semiconductor device 2 according to this embodiment, the second contact metal film 202 including nickel silicide 205 is provided on at least a portion of the contact portion with the high concentration region 14. Therefore, the resistance between the high concentration region 14 and the source electrode film 19 can be reduced compared to the first embodiment.

[0121] In the semiconductor device 2 according to the present embodiment, titanium is not used in the contact metal layer 200 to form the first contact metal film 201 in contact with the source region 15. Therefore, since a Schottky junction is not formed at the interface between the contact metal layer 200 and the source region 15 including an n-type dopant, an ohmic contact can be formed between the source region 15 and the source electrode film 19.

[0122] In the semiconductor device 2 according to the present embodiment, the contact metal film 201 of the source region 15 mainly including the n-type dopant and the contact metal film 202 of the high-concentration region 14 including the p-type dopant are not separated from each other but are formed overlappingly on the source region 15. In this way, since the margin used for the photolithography process can be reduced, the cell pitch of the semiconductor element can be reduced.

[0123] (Method for manufacturing semiconductor device)

[0124] The following will be Figure 7 Reference to Fig. 9B A method for manufacturing the semiconductor device 2 according to the present embodiment will be described.

[0125] like Figure 7As shown, the process of the method for manufacturing the semiconductor device 2 according to the present embodiment includes a second contact metal film lower layer portion forming step S7a, which replaces the second contact metal film forming step S7, and forms the lower layer portion of the second contact metal film 202. The structure is the same as that of the first embodiment except that a second contact metal film upper layer portion forming step S7b for forming the upper layer portion of the second contact metal film 202 is included between the second contact metal film lower layer portion forming step S7a and the source electrode film forming step S8.

[0126] (S6: First Contact Metal Film Forming Step)

[0127] like Fig. 8A As shown, in the first contact metal film forming step S6, the first contact metal film 201 is formed of titanium nitride as in the first embodiment.

[0128] (S7a: Second Contact Metal Film Lower Layer Forming Step)

[0129] like Figure 8B As shown, in the second contact metal film lower layer portion forming step S7, the lower layer portion of the second contact metal film 202 is formed of titanium as in the first embodiment. However, in this embodiment, annealing is not performed.

[0130] (S7b: Second Contact Metal Film Upper Layer Forming Step)

[0131] Next, the second contact metal film upper portion forming step S7b is performed. In the second contact metal film upper portion forming step S7b, first, a nickel film is formed on the titanium serving as the lower portion of the second contact metal film 202 and the surface of the high concentration region 14 exposed in the second opening H2 by sputtering or electron beam evaporation. Thereafter, a resist pattern (not shown) is formed to protect the portion corresponding to the second contact metal 202 using a known photolithography technique. Subsequently, the portion not protected by the resist pattern is removed by wet etching. Thereafter, the resist pattern is removed. Thereafter, the mask is removed. Next, annealing is performed in the same manner as the first contact metal film forming step S6. At this time, although titanium nitride does not substantially react with nickel and titanium, when nickel and titanium are mixed, nickel penetrates the titanium layer and reacts with silicon carbide constituting the high concentration region 14 to become nickel silicide 205 (see Fig.9A ), free carbon reacts with titanium to form titanium carbide. In particular, nickel silicide 205 is formed in at least a portion of the portion in contact with the high concentration region 14. In addition, silicon contained in the nickel silicide 205 also diffuses into the nickel in the portion mixed with titanium, and the nickel in this portion also becomes nickel silicide 205. Thus, the second contact metal film 202 is formed on the surface of the first contact metal film 201 in such a manner as to contact the high concentration region 14 in the second opening H2.

[0132] Furthermore, when the annealing atmosphere contains nitrogen, titanium nitride is formed on at least the surface layer portion of the second contact metal film 202 similarly to the first embodiment.

[0133] like Fig. 9B As shown, in the source electrode film forming step S8, the source electrode film 19 is formed on the surface of the contact metal layer 200 using an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or aluminum, as in the first embodiment. The semiconductor device 2 is manufactured in the above manner.

[0134] In the semiconductor device 2 involved in this embodiment, the free carbon generated after the reaction of nickel and silicon carbide during annealing will be absorbed as titanium carbide in the second contact metal film 202 through the reaction with titanium, thereby improving the adhesion between the contact metal layer 200 and silicon carbide (source region 15, high concentration region 14).

[0135] In the method for manufacturing the semiconductor device 2 according to the present embodiment, the second contact metal film 202 in contact with the central portion of the high concentration region 14 is formed to include nickel silicide 205 in at least a portion of the contact portion with the high concentration region 14. Therefore, compared with the case where the contact metal layer 200 is formed entirely of titanium nitride, the high concentration region 14 containing p-type dopants (SiC (p + )) and the contact resistance between the contact metal layer 200.

[0136] As described above, the method for manufacturing the semiconductor device 2 according to the present embodiment can improve the adhesion of the contact metal layer 200 in the high concentration region 14 and reduce the contact resistance. Therefore, a semiconductor device with high reliability can be provided.

[0137] Furthermore, in the method for manufacturing the semiconductor device 2 according to the present embodiment, the second contact metal film 202 including the nickel silicide 205 is provided in at least a portion of the contact portion with the high concentration region 14. Therefore, the resistance between the high concentration region 14 and the source electrode film 19 can be reduced compared to the first embodiment.

[0138] In the method for manufacturing the semiconductor device 2 according to the present embodiment, titanium is not used in the contact metal layer 100 to form the first contact metal film 201 in contact with the source region 15. Therefore, since a Schottky junction is not formed at the interface between the contact metal layer 200 and the source region 15 including an n-type dopant, an ohmic contact can be formed between the source region 15 and the source electrode film 19.

[0139] In the semiconductor device 2 according to the present embodiment, the contact metal film 201 of the source region 15 mainly including the n-type dopant and the contact metal film 202 of the high-concentration region 14 including the p-type dopant are not separated from each other but are formed overlappingly on the source region 15. In this way, since the margin used for the photolithography process can be reduced, the cell pitch of the semiconductor element can be reduced.

[0140] [Third embodiment]

[0141] The following will be Fig.10 Reference to Fig. 12B A third embodiment of the present invention will be described below, but descriptions of parts common to the first and second embodiments will be omitted.

[0142] (Structure of Semiconductor Device)

[0143] like Fig.10 As shown, in the semiconductor device 3 according to the present embodiment, the contact metal layer 100 includes a nickel silicide layer 305 provided on the contact surface with the high concentration region 14. The contact metal layer 100 may also contain titanium carbide.

[0144] In the semiconductor device 3 according to the present embodiment, in the region of the second opening H2 excluding the third opening H3 that is annular in plan view, the second contact metal film 302 containing nickel silicide and titanium carbide is in contact with the high concentration region 14. Next, in the region of the first opening H1 excluding the second opening H2 that is annular in plan view, the first contact metal film 301 formed of titanium nitride is in contact with the high concentration region 14 and the source region 15. In these regions, free carbon generated during annealing is absorbed in the second contact metal film 302 as titanium carbide, so that the adhesion between silicon carbide and the contact metal film 300 is not reduced.

[0145] On the other hand, the nickel silicide layer 305 is in contact with the high concentration region 14 formed of silicon carbide in the third opening H3. Therefore, free carbon is generated at the interface between the nickel silicide layer 305 and the high concentration region 14 during annealing.

[0146] However, the generated free carbon is absorbed by the second contact metal film 302 in contact with the annular region of the first opening H1 excluding the second opening H2 when viewed from a plan view, thereby preventing the adhesion between silicon carbide and the contact metal film 300 from being reduced.

[0147] Secondly, after annealing is performed on the inner side of the third opening H3 which is not in direct contact with the second contact metal film 302, even if the generated free carbon is not completely absorbed by the second contact metal film 302, the portion of the contact metal layer 300 with low adhesion will be limited to the inner side of the third opening H3. On the other hand, in the annular region surrounding the third opening H3 in the inner side of the first opening H1, the adhesion will not be reduced. In this way, the contact metal layer 300 as a whole can better maintain the adhesion with silicon carbide (high concentration region 14, source region 15). In addition, titanium nitride is further formed on at least the surface portion of the second contact metal film 302 as in the second embodiment.

[0148] In the semiconductor device 3 according to the present embodiment, a nickel silicide layer 305 is provided in contact with the central portion of the high concentration region 14. Therefore, compared with the case where the contact metal layer 300 is formed entirely of titanium nitride, the high concentration region 14 (SiC (p + )) and the contact resistance between the contact metal layer 300.

[0149] As described above, the semiconductor device 3 according to the present embodiment can maintain good adhesion of the contact metal layer 300 in the high concentration region 14 and can reduce contact resistance. Therefore, a highly reliable semiconductor device can be provided.

[0150] In the semiconductor device 3 according to the present embodiment, the nickel silicide layer 305 is in contact with the high concentration region 14 formed of silicon carbide in the third opening H3. Therefore, the resistance between the high concentration region 14 and the source electrode film 19 can be reduced compared to the second embodiment.

[0151] In the semiconductor device 3 according to the present embodiment, titanium is not used in the contact metal layer 300 to form the first contact metal film 301 in contact with the source region 15. Therefore, since a Schottky junction is not formed at the interface between the contact metal layer 300 and the source region 15 including an n-type dopant, an ohmic contact can be formed between the source region 15 and the source electrode film 19.

[0152] In the semiconductor device 3 according to the present embodiment, the contact metal film 301 of the source region 15 mainly including the n-type dopant and the contact metal film 302 of the high-concentration region 14 including the p-type dopant are not separated from each other but are formed overlappingly on the source region 15. In this way, since the margin used for the photolithography process can be reduced, the cell pitch of the semiconductor element can be reduced.

[0153] (Method for manufacturing semiconductor device)

[0154] Below, we will refer to FIG. 11A to FIG. 12BNext, a method for manufacturing the semiconductor device 3 according to the present embodiment will be described. (S6: First Contact Metal Film Formation Step)

[0155] like Fig.11A As shown, in the first contact metal film forming step S6, the first contact metal film 301 is formed of titanium nitride similarly to the second embodiment.

[0156] (S7: Second Contact Metal Film Formation Step)

[0157] like Fig. 11B As shown, in the second contact metal film forming step S7, the second contact metal film 302 is formed of titanium. The second contact metal film 302 is formed to have a third opening H3 formed to expose a part of the high concentration region 14.

[0158] like Fig. 12A As shown, nickel is formed on the surface of titanium as the second contact metal film 302 and the high concentration region 14 exposed in the third opening H3 by sputtering or electron beam evaporation. After that, annealing is performed. At this time, nickel mixes with titanium on titanium and penetrates titanium directly in the third opening H3 at the part of the second opening H2 other than the third opening H3, and reacts with silicon carbide constituting the high concentration region 14 to become nickel silicide (nickel silicide layer formation process), and free carbon reacts with titanium to form titanium carbide. In addition, silicon contained in nickel silicide also diffuses into nickel in the part mixed with titanium, and nickel in this part also becomes nickel silicide. Thus, while the second contact metal film 302 containing nickel silicide and titanium carbide is formed, the nickel silicide layer 305 is formed to contact the high concentration region 14 in the third opening H3. In addition, when the annealing atmosphere contains nitrogen, titanium nitride is formed on at least the surface of the second contact metal film 302 in the same way as in the first and second embodiments.

[0159] like Fig. 12B As shown, in the source electrode film forming step S8, the source electrode film 19 is formed on the surface of the contact metal film 300 using an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or aluminum, as in the first and second embodiments. Thus, the semiconductor device 3 is formed.

[0160] In the manufacturing method of the semiconductor device 3 according to the present embodiment, in the region of the second opening H2 that is annular in plan view except for the third opening H3, the second contact metal film 302 containing nickel silicide and titanium carbide is in contact with the high concentration region 14. Next, in the region of the first opening H1 that is annular in plan view except for the second opening H2, the first contact metal film 301 formed of titanium nitride is in contact with the high concentration region 14 and the source region 15. In these regions, since free carbon generated during annealing is absorbed in the second contact metal film 302 as titanium carbide, the adhesion between silicon carbide and the contact metal film 300 is not reduced. On the other hand, the nickel silicide layer 305 is in contact with the high concentration region 14 formed of silicon carbide in the third opening H3. Therefore, free carbon is generated at the interface between the nickel silicide layer 305 and the high concentration region 14 during annealing.

[0161] However, since the generated free carbon is absorbed by the second contact metal film 302 contacting the annular region of the first opening H1 excluding the second opening H2 when viewed from a plan view, it is possible to prevent the adhesion between silicon carbide and the contact metal film 300 from being reduced.

[0162] Secondly, after annealing is performed on the inner side of the third opening H3 which is not in direct contact with the second contact metal film 302, even if the generated free carbon is not completely absorbed by the second contact metal film 302, the portion of the contact metal layer 300 with low adhesion will be limited to the inner side of the third opening H3. On the other hand, the adhesion will not be reduced in the annular region surrounding the third opening H3 in the inner side of the first opening H1 when viewed from a plane. In this way, the contact metal layer 300 as a whole can maintain good adhesion with silicon carbide (high concentration region 14, source region 15).

[0163] In the method for manufacturing the semiconductor device 3 according to the present embodiment, the nickel silicide layer 305 is provided in contact with the central portion of the high concentration region 14. Therefore, compared with the case where the contact metal layer 300 is formed entirely of titanium nitride, the high concentration region 14 (SiC (p + )) and the contact resistance between the contact metal layer 300.

[0164] As described above, the method for manufacturing the semiconductor device 3 according to the present embodiment can maintain good adhesion of the contact metal layer 300 in the high concentration region 14 and reduce contact resistance. Therefore, a semiconductor device with high reliability can be provided.

[0165] In the method for manufacturing the semiconductor device 3 according to the present embodiment, the nickel silicide layer 305 is in contact with the high concentration region 14 formed of silicon carbide in the third opening H3. Therefore, the resistance between the high concentration region 14 and the source electrode film 19 can be reduced compared to the second embodiment.

[0166] In the method for manufacturing the semiconductor device 3 according to the present embodiment, titanium is not used in the contact metal layer 300 to form the first contact metal film 301 in contact with the source region 15. Therefore, since a Schottky junction is not formed at the interface between the contact metal layer 300 and the source region 15 including an n-type dopant, an ohmic contact can be formed between the source region 15 and the source electrode film 19.

[0167] In the semiconductor device 3 according to the present embodiment, the contact metal film 301 of the source region 15 mainly including the n-type dopant and the contact metal film 302 of the high concentration region 14 including the p-type dopant are not separated from each other, but are formed overlappingly on the source region 15. This can reduce the margin for the photolithography process. In this way, the cell pitch of the semiconductor element can be reduced while reducing the manufacturing cost.

[0168] Although the embodiments of the present invention are described above, the present invention can also be implemented in other ways. For example, although the source electrode film 19 is formed of an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or aluminum, other conductive materials such as metals can also be used. In addition, although the semiconductor devices 1, 2, and 3 are planar MOSFETs, they can also be p + The insulated gate bipolar transistor (IGBT) of the type (second conductivity type) silicon carbide single crystal substrate is used as the semiconductor substrate 11. In addition, in the above embodiment, although the first conductivity type is n-type and the second conductivity type is p-type, the first conductivity type may be p-type and the second conductivity type may be n-type.

[0169] In the above embodiment, the source region 15 is surrounded by the well region 13 in a plan view and is adjacent to the high concentration region 14 while being formed in a ring shape. The structure is a "square unit structure" surrounding the high concentration region 14 in a plan view, but it is not limited to this structure. The semiconductor device of the present invention may also be, for example, Figure 1 , 6 Or a "striped cell structure" having a cross section as shown in FIG10. In this case, the well region 13 is a region extending in a direction substantially perpendicular to the cross section of the semiconductor device when viewed from a plane. The high concentration region 14 is a region included in the well region 13 and extending in the same direction as the well region 13 when viewed from a plane. The source region 15 is a pair of regions included in the well region 13 and extending adjacent to both sides of the high concentration region 14 when viewed from a plane.

[0170] Although the structure of the first opening portion H1 is formed to expose at least a portion of the source region 15 and at least a portion of the high-concentration second conductive type region 14 when viewed from a planar perspective, its structure is not limited to this. The structure of the first opening portion H1 can also be formed to not expose the source region 15 when viewed from a planar perspective, but to expose at least a portion of the high-concentration second conductive type region 14.

[0171] In addition, various design changes can be made within the scope of the matters described in the claims.

[0172] Explanation of symbols

[0173] 1, 2, 3…Semiconductor devices

[0174] 11…Semiconductor substrate

[0175] 12…Drift layer

[0176] 13… Well region

[0177] 14…High concentration area

[0178] 15…Source region

[0179] 16…Insulation film

[0180] 19…Source electrode film

[0181] 100, 200, 300...Contact metal layer

[0182] 101, 201, 301…first contact metal film

[0183] 102, 202, 302 ... second contact metal film

[0184] 305…NiSi layer

[0185] F1…a main surface

[0186] H1…First opening

[0187] H2…Second opening

[0188] H3…The third opening

[0189] S1…Drift layer formation process

[0190] S2...well region forming step

[0191] S3: High-concentration region forming step

[0192] S4: Source region forming step

[0193] S5: Insulation film forming process

[0194] S6: First contact metal film forming step

[0195] S7...second contact metal film forming step

[0196] S7a...second contact metal film lower layer forming step

[0197] S7b...second contact metal film upper layer forming step

[0198] S8...Source electrode film forming step

Claims

1. A semiconductor device, characterized in that: include: a semiconductor substrate composed of silicon carbide; A drift layer of a first conductivity type, which is provided on one main surface of the semiconductor substrate; A well region of a second conductivity type, which is disposed on the drift layer; The second conductivity type high concentration region is disposed in the well region and has a higher dopant concentration than the well region; The source region of the first conductivity type is disposed adjacent to the high concentration region; an insulating film disposed on a surface of the drift layer; a first contact metal film, which contacts the source region and the high concentration region via a first opening portion provided on the insulating film; a second contact metal film formed on a surface of the first contact metal film and in contact with the high concentration region via a second opening provided on the first contact metal film; as well as a source electrode film formed on a surface of a contact metal layer including the first contact metal film and the second contact metal film, Wherein, the first contact metal film comprises titanium nitride, The second contact metal film is a single-layer film and includes titanium.

2. The semiconductor device according to claim 1, wherein: in, The second contact metal film includes nickel silicide provided on a contact surface with the high-concentration region.

3. The semiconductor device according to claim 2, wherein: in, The nickel silicide is in granular form.

4. The semiconductor device according to any one of claims 1 to 3, characterized in that: Further including: A nickel silicide layer is in contact with the high concentration region via a third opening provided on the second contact metal film.

5. The semiconductor device according to any one of claims 1 to 3, characterized in that: in, The source electrode film is formed of an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or aluminum.

6. A method for manufacturing a semiconductor device, characterized in that: include: a drift layer forming step of forming a first conductivity type drift layer on a main surface of a semiconductor substrate made of silicon carbide; a well region forming step of forming a well region of a second conductivity type opposite to the first conductivity type on the drift layer, the well region being exposed on the surface of the drift layer; a high-concentration region forming step of forming, on the well region of the drift layer, a high-concentration region of the second conductivity type exposed on the surface of the drift layer and having a higher dopant concentration than that of the well region; a source region forming step of forming a source region of the first conductivity type on the well region of the drift layer, the source region being exposed on the surface of the drift layer and adjacent to the high concentration region; an insulating film forming step of forming an insulating film having a first opening on a surface of the drift layer, wherein the first opening exposes at least a portion of the high concentration region and the source region when viewed in plan from one side of the one main surface of the semiconductor substrate; a first contact metal film forming step of forming a first contact metal film having a second opening portion exposing a portion of the high concentration region so as to contact at least a portion of the source region in the first opening portion; a second contact metal film forming step of forming a second contact metal film on a surface of the first contact metal film in such a manner as to be in contact with the high concentration region in the second opening; as well as a source electrode film forming step of forming a source electrode film on a surface of a contact metal layer including the first contact metal film and the second contact metal film; Wherein, the first contact metal film comprises titanium nitride, The second contact metal film is a single-layer film and includes titanium.

7. The method for manufacturing a semiconductor device according to claim 6, wherein: in,The second contact metal film includes nickel silicide provided on a contact surface with the high-concentration region.

8. The method for manufacturing a semiconductor device according to claim 7, wherein: in, The nickel silicide is in granular form.

9. The method for manufacturing a semiconductor device according to any one of claims 6 to 8, characterized in that: Further including: The nickel silicide layer forming step provides a nickel silicide layer that is in contact with the high concentration region via a third opening provided in the second contact metal film.

10. The method for manufacturing a semiconductor device according to any one of claims 6 to 8, characterized in that: in, In the source electrode film forming step, the source electrode film is formed using an alloy containing aluminum and silicon, an alloy containing aluminum and copper, or aluminum.