Method for increasing the adhesion strength between a copper or copper alloy surface and an organic layer
The nano-roughened surface layer is formed by the acid non-etching protectant aqueous solution, which solves the problem of insufficient adhesion strength between the copper or copper alloy surface and the organic layer in the prior art, and realizes high-efficiency adhesion in thin-wire circuits and high-frequency applications Effects, reducing signal loss and metal loss.
Patent Information
- Application Number
- CN201980030663.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-08
- Filing Date
- 2019-05-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-05-06
AI Technical Summary
The prior art has shortcomings in increasing the adhesion strength between the surface of the copper or copper alloy of printed circuit board (PCB) and the organic layer, especially in thin-wire circuits and high-frequency applications, conventional methods such as high temperature and strong alkaline aqueous solutions or The etchant causes problems of surface roughening and weakening of adhesion.
Using an acidic non-etching protectant aqueous solution, including aminoazoles, organic acids or their salts, peroxides and inorganic acids, the adhesion strength is increased by forming a nano-roughened surface layer, and without etching or significant removal of copper/copper alloys In the case, keep the total surface area constant and avoid reoxidation.
It significantly improves the adhesion strength between the copper or copper alloy surface and the organic layer, is suitable for thin-wire circuits and high-frequency applications, reduces signal loss and metal copper loss, and extends the service life of the PCB.
Smart Images

Figure BDA0002764092450000161 
Figure BDA0002764092450000171 
Figure BDA0002764092450000172
Abstract
Description
Technical Field
[0001] The present invention generally relates to a method for manufacturing a printed circuit board (PCB), and in particular to a method for increasing the adhesion strength between a copper or copper alloy surface and an organic layer, such as a solder mask or a build-up layer, preferably a build-up layer, most preferably a build-up layer in a multi-layer PCB. The present invention further relates to an acidic non-etching protective agent aqueous solution. Background Art
[0002] A PCB is a thin board on which electrical parts, such as integrated circuits (ICs), resistors, switches, etc., are mounted on at least one of the surfaces to obtain a printed wiring board assembly (PCBA). During the manufacturing process of a PCB, typically, a copper circuit is formed on a non-conductive substrate / layer, which is typically made of epoxy or polyimide resin. The most common non-conductive substrate / layer is a glass-reinforced epoxy laminate, commercially known as FR-4.
[0003] To obtain a multi-layer PCB, usually, a stack of a non-conductive substrate / layer with its conductive copper circuit is formed to obtain a monolithic product.
[0004] Typically, during PCB manufacturing (specifically during multi-layer PCB manufacturing), two specific types of non-conductive substrates / layers are utilized, which are permanent: (i) the above-mentioned non-conductive substrates / layers called build-up layers (also known as prepreg, inner layers, insulating layers, etc.), which form non-conductive substrates / layers between circuits within a multi-layer PCB, and (ii) solder masks (also commonly known as solder resists, outer layers, etc.) that cover and protect the exposed outermost circuits in both multi-layer and non-multi-layer PCBs.
[0005] The solder mask, after polymerization (also called curing or hardening), is a fully polymerized, permanent layer of non-conductive material covering the surface of the outermost non-conductive substrate / layer and most of its copper circuitry. The solder mask is patterned to completely cover the circuitry except for those portions of the copper circuitry that are intended to be exposed for soldering. In such areas, the solder mask typically exhibits openings, such as pad openings.
[0006] Multilayer PCBs are formed by alternately stacking buildup layers and copper circuits. The buildup layers electrically insulate the copper circuits from each other and additionally provide stability. However, through-holes are formed at well-defined locations, electrically connecting a circuit of one layer to one or more circuits of other layers. Such through-holes are formed, for example, by using lasers, plasma, photo methods, or conventional drilling.
[0007] Typically, the buildup layer is vacuum laminated onto the corresponding non-conductive substrate / layer or core substrate and covers the copper circuitry of the substrate / layer and core substrate, respectively. The buildup layer (or multiple buildup layers) is then pressed and / or subjected to a first heat treatment step to obtain a fully pre-polymerized buildup layer. A temperature in the range of 170°C to 200°C is typically applied for approximately 30 minutes.
[0008] After the first heat treatment step, the prepolymerized buildup layer is under conditions for patterning, specifically for through-hole formation. Subsequently, the surface of the buildup layer and the through-hole surface are typically decontaminated and are substantially under conditions for forming the next copper circuit in the multilayer PCB.
[0009] The process of forming the next copper circuit is carried out, for example, by means of: (i) a subtractive process usually starting with laminating copper foil, (ii) a semi-additive process (SAP) or an advanced modified semi-additive process (AMSAP) usually starting with electroless deposition of a copper layer, or (iii) a full additive process (FAP) starting with forming a temporary structured photoresist layer for selectively depositing copper. Among these processes, SAP is usually particularly used in the manufacture of high-density PCBs.
[0010] In SAP, a copper layer is electrolessly deposited onto the buildup surface, followed by a second heat treatment step (also commonly referred to as a drying step) typically at a temperature in the range of 100° C. to 150° C. for at least 30 minutes. In this heat treatment step, heat is applied to the prepolymerized copper-plated buildup.
[0011] In the next step, a temporary photosensitive layer (photoresist layer) of non-conductive material is formed on the electroless deposited copper layer, then patterned to form openings, and cured. Subsequently, additional copper is deposited into the openings.
[0012] In the last step, the temporary photosensitive layer and the residual copper layer are removed. Thus, the copper circuit of the next layer is formed, which is then ready for lamination of the next build-up layer.
[0013] It is imperative that delamination does not occur during the life of such multilayer PCBs. Therefore, it is desirable that the adhesion between the copper circuit and the buildup layers laminated thereon is as high as possible and remains strong during the life of the corresponding PCB.
[0014] However, build-up layers sometimes suffer from the disadvantage of obtaining insufficient adhesion, which results in delamination at the interface between the copper circuit and the build-up layer.
[0015] In order to obtain strong adhesion, various preparation methods are known for copper circuit surfaces.
[0016] The conventional method is to form a layer of so-called "black oxide" on the copper surface by contacting the copper surface with a high temperature, strongly alkaline aqueous solution. Such a layer usually extends to a layer thickness of approximately 1000 nm or more. In many cases, the adhesion obtained is not sufficient so far. Moreover, in many cases, this method is not sufficient for fine-line circuits.
[0017] Another method is to apply strong etchants, which leave a strongly roughened copper surface (see, for example, JP 2740768), often referred to as a micro-roughened copper surface. Such treatments usually remove copper from the circuit surface roughly, leaving a strongly roughened copper surface, including wide and deep cavities, even in the micrometer range. Therefore, such methods are also less suitable for fine-line circuits, especially high-frequency applications, because the copper loss is too severe, the surface becomes too rough, and the obtained adhesion is usually too weak.
[0018] Other approaches utilize various chemical modifications of the copper surface to increase the adhesion.
[0019] US 2002 / 0192460 A1 discloses a coating film of an azole-copper complex compound providing a laminate having improved adhesion between a copper / copper alloy surface of a multilayer printed circuit board and a resin, and a method for producing the laminate.
[0020] WO 2009 / 109391 A1 relates to a non-etching, non-corrosive-adhesive composition for treating copper or copper alloys, and a method for preparing a workpiece having a copper or copper alloy surface using the non-etching, non-corrosive-adhesive composition for subsequent coating of the copper or copper alloy surface by polymeric deposition.
[0021] WO 2012 / 005722 A1 discloses in technical solution 1 "a method for treating a metal surface to promote adhesion between the metal surface and an organic material, characterized in that a metal oxide layer is formed on the metal surface, and the formation of the metal oxide layer is controlled by a self-limiting reaction between the metal oxide and a surface modifier compound". This reaction includes, after the formation of the metal oxide layer, the subsequent reduction of the metal oxide layer to obtain a nano-roughened surface layer exhibiting a layer thickness of generally not more than 500 nm. This is significantly smoother than, for example, a micro-roughened surface as described above. This process requires that after the reduction, the nano-roughened surface layer is protected from re-oxidation (for example by oxygen in the surrounding air).
[0022] Due to further miniaturization, there is generally a need to further improve existing methods to further increase adhesion strength. Summary of the invention
[0023] It is therefore an object of the present invention to provide an improved method for increasing the adhesion strength between a copper or copper alloy surface and an organic layer such that the adhesion strength is further increased compared to prior art methods.
[0024] The object is in particular to provide a more reliable method for further increasing the adhesion strength of copper circuits of a printed circuit board to an organic layer. DETAILED DESCRIPTION
[0025] The above mentioned object is solved by a method for increasing the adhesion strength between a copper or copper alloy surface and an organic layer, said method comprising the following steps in this order:
[0026] (i) providing a non-conductive substrate comprising, on at least one side, said surface having a total surface area of copper or a copper alloy,
[0027] (ii) contacting the substrate comprising the surface with an acidic non-etching protective agent aqueous solution comprising:
[0028] (ii-a) one or more aminoazoles,
[0029] (ii-b) one or more organic acids and / or their salts,
[0030] (ii-c) one or more peroxides in a total amount of 0.4 wt. % or less based on the total weight of the protectant solution, and
[0031] (ii-d) an inorganic acid in a total amount of 0 to 0.01 wt % based on the total weight of the protective agent solution,
[0032] wherein during step (ii), the total surface area of the surface does not increase after contact with the protectant solution.
[0033] The object is furthermore solved by means of an acidic non-etching protective agent aqueous solution comprising:
[0034] (a) one or more aminoazoles,
[0035] (b) one or more organic acids and / or their salts,
[0036] (c) one or more peroxides in a total amount of 0.4 wt. % or less based on the total weight of the protectant solution, and
[0037] (d) inorganic acid in a total amount of 0 to 0.01 wt % based on the total weight of the protective agent solution,
[0038] Wherein in the acidic non-etching protective agent aqueous solution, the molar ratio of all peroxides to all aminoazoles is 1 or less.
[0039] The inventive method and the protective agent solution of the present invention are used to increase the adhesion strength between the copper or copper alloy surface and the organic layer without etching or significantly removing the copper / copper alloy. This means that during step (ii) of the inventive method, the total surface area of the copper or copper alloy does not increase, but remains constant. In other words, after step (ii), the total surface area of the copper / copper alloy is substantially the same as when step (ii) begins. This will distinguish the inventive method from a variety of known methods, especially etching methods, the goal of which is to increase the total surface area by roughening. Therefore, the inventive method is a non-etching method.
[0040] Preferred is the process according to the invention, wherein in step (i), the copper or copper alloy surface comprises a copper or copper alloy circuit, preferably a copper or copper alloy circuit. In this case, the copper or copper alloy surface is structured. This preferably means that the non-conductive substrate exposes both non-conductive (preferably organic) areas and conductive copper / copper alloy areas on the same side. This is most preferred in the case of the process according to the invention.
[0041] Preferred is the method of the invention, wherein in step (i), the copper or copper alloy circuit comprises a line having a line width of 100 μm or less, preferably 75 μm or less, more preferably 55 μm or less. In some cases, the method of the invention is preferred, wherein in step (i), the copper or copper alloy circuit comprises a line having a line width of 30 μm or less, preferably 20 μm or less, most preferably 10 μm or less.
[0042] The non-conductive substrate comprises on at least one side said copper or copper alloy surface as defined above (preferably, as defined as preferred). Preferably, said surface is pretreated, more preferably by chemical conversion, most preferably by oxidation of copper to oxides and subsequent reduction of at least a portion of these copper oxides. Therefore, the method of the present invention is preferred, wherein in step (i), the copper or copper alloy surface comprises a nano-roughened surface layer obtained as follows:
[0043] - Oxidation of Cu-(0) to Cu-(I) and Cu-(II), respectively, and then
[0044] - at least partially reducing the Cu-(I) and Cu-(II) to Cu-(0), respectively.
[0045] Thus, a highly preferred non-conductive substrate is obtained comprising a copper or copper alloy surface on at least one side, said surface comprising a nano-roughened surface layer. Most preferably, such a copper or copper alloy surface is structured, preferably comprising an electrical circuit, most preferably an electrical circuit (for electrical circuits, see above for details).
[0046] The above-mentioned nano-roughened surface layer is a layer of predominantly copper (Cu-(0)) and residual amounts of copper oxide (including Cu-(I) and (Cu-(II)) on the surface of copper or copper alloy. This Cu-(0) and Cu-(I) need to be protected from further undesired oxidation and / or reoxidation. The nano-roughened surface layer generally has a needle-like morphology (sometimes also referred to as "hairy surface morphology"), which results in a substantial increase in the total surface area without significantly roughening the surface (hence referred to as nano-roughening). Therefore, it is preferred that the method of the present invention, wherein in step (i) or at the beginning of step (ii), the nano-roughened surface layer has a needle-like morphology. Most preferably, after step (ii), this needle-like morphology still exists. Note again that during step (ii) of the method of the present invention, this total surface area is not increased in a significant manner.
[0047] Our own experiments have shown that the method of the present invention (as defined throughout the present invention) largely prevents said undesired oxidation and / or reoxidation of the copper or copper alloy surface, most preferably of the nano-roughened surface layer, by forming a protected copper or copper alloy surface, most preferably by forming a protected nano-roughened surface layer, the formation of which results in an increased adhesion strength to the organic layer, preferably the stacking layer. This is attributed to the use of an acidic non-etching protectant aqueous solution as defined above and throughout the present invention. In particular, the acidic non-etching protectant aqueous solution does not measurably degrade the nano-roughened surface layer, because no significant etching occurs after contact in step (ii). Therefore, during step (ii), copper is not or substantially not removed from the copper or copper alloy surface; most preferably, the nano-roughened surface layer is not removed during step (ii). This includes that the total surface area is not increased in a significant manner. Therefore, the method of the present invention is highly recommended for use in the manufacture of multilayer PCBs for fine line circuits (i.e., line widths of less than 30 μm) and PCBs for high frequency applications. Such applications are generally very susceptible to intensive copper removal / etching.
[0048] Preferably, in the method of the present invention, the substrate provided in step (i) exhibits the nano-roughened surface layer described above. However, in some cases, the method of the present invention preferably comprises the following steps in this order:
[0049] (i) providing a non-conductive substrate comprising a copper or copper alloy surface on at least one side, said surface preferably comprising (most preferably being) a copper or copper alloy circuit, said surface having a total surface area of copper or copper alloy,
[0050] (ia) oxidizing Cu-(0) to Cu-(I) and Cu-(II), respectively, and then
[0051] (ib) at least partially reducing the Cu-(I) and Cu-(II) to Cu-(0), respectively,
[0052] so as to produce a copper or copper alloy surface comprising a nano-roughened surface layer, said surface preferably comprising (most preferably being) a copper or copper alloy circuit,
[0053] (ii) contacting the substrate comprising the surface with an acidic non-etching protective agent aqueous solution comprising:
[0054] (ii-a) one or more aminoazoles,
[0055] (ii-b) one or more organic acids and / or their salts,
[0056] (ii-c) one or more peroxides in a total amount of 0.4 wt. % or less based on the total weight of the protectant solution, and
[0057] (ii-d) an inorganic acid in a total amount of 0 to 0.01 wt % based on the total weight of the protective agent solution,
[0058] wherein during step (ii), the total surface area of the surface is not increased after contact with the protectant solution and the nano-roughened surface layer is not removed.
[0059] The term "subsequently" means that step (ib) substantially follows step (ia). However, in some cases it may be preferred to include a washing or conditioning step prior to step (ib).
[0060] Without wishing to be bound by theory, it is assumed that in step (ia), the copper atoms are chemically converted into oxides. Preferably, this conversion is self-limiting. After step (ia), the surface morphology is significantly changed and generally results in the needle-shaped surface morphology having an extremely low surface roughness (through nano-roughening) but a significant increase in total surface area (compared to the total surface area before step (ia)). Subsequently, these oxides are reduced by means of reduction while maintaining the needle-shaped morphology. The nano-roughened surface layer obtained (due to this conversion) produces a basic adhesion strength between the copper or copper alloy surface and the organic layer. This basic adhesion strength is preferably further increased by the method of the present invention.
[0061] In general, the nano-roughened surface layer can be studied, analyzed and measured by atomic force microscopy (AFM), Fourier transform infrared spectroscopy (FT-IR), focused ion beam high resolution scanning electron microscopy (FIB high resolution SEM), X-ray photoelectron spectroscopy (XPS) and transmission electron microscopy (TEM). Preferably, the analysis is carried out in a vertical section of the corresponding sample. More preferably, the nano-roughened surface layer thickness is observed and determined by means of FIB high resolution SEM and AFM, for example to determine the maximum layer thickness. A very preferred method is AFM.
[0062] In step (ia), the oxidation is preferably carried out by one or more than one oxidizing agent selected from the group consisting of chlorites, hypochlorites, peroxides, permanganates, perchlorates, persulfates and ozone. Preferred chlorites are chlorous acid and alkali metal chlorites, most preferably sodium chlorite. Preferred hypochlorites are hypochlorous acid and its salts. Preferred peroxides are hydrogen peroxide. Preferred perchlorates are perchloric acid and its salts. Preferred persulfates are selected from the group consisting of peroxymonosulfates, peroxydisulfates and their related acids. The oxidizing agents are present in a total concentration sufficient to achieve the desired oxidation. After step (ia), the copper is present primarily with an oxidation number of +2.
[0063] In step (ib), the reduction is preferably carried out by one or more than one reducing agent selected from the group consisting of organic reducing agents and inorganic reducing agents, preferably selected from the group consisting of aldehydes, borohydrides, boranes and substituted boranes. The preferred aldehyde is formaldehyde. After step (ib), the copper is mainly in oxidation number 0 (Cu-(0)), but a small amount of copper in oxidation number +1 is inevitable due to the immediate reoxidation of Cu-(0). However, copper in oxidation number 0 is preferred. During the reduction, the needle-shaped morphology is maintained.
[0064] In the method of the present invention, the nano-roughened surface layer is extremely smooth (in step (i) and in step (ii)) compared to conventional etching methods, which usually result in extremely significant surface roughness or even surface damage; usually including a modification of the surface morphology. This is undesirable, especially for fine-line circuits and high-frequency applications. On the contrary, the preferred nano-roughened surface layer in step (i) of the method of the present invention is very usually not more than 200 nanometers thick, is relatively smooth due to the needle-shaped morphology (i.e., nanostructured), and follows the contour of the copper or copper alloy surface without modifying its surface morphology. Such a preferred nano-roughened surface layer (in step (i) and in step (ii)) is counted as one of the so-called non-etching adhesion promoters (NEAP). The method of the present invention is preferred, wherein in step (i), the maximum layer thickness of the nano-roughened surface layer is 500nm or less, preferably 300nm or less, more preferably 180nm or less, even more preferably 150nm or less, most preferably 120nm or less.
[0065] If the maximum layer thickness exceeds 500 nm, the roughness is in some cases too high and the method is then no longer suitable for many fine-line circuit applications (eg line widths below 30 μm). If the maximum layer thickness is, for example, significantly below 30 nm, the adhesion and peel strengths are in some cases insufficient.
[0066] The preferred nano-roughened surface layer provides various advantages. PCBs used in high frequency applications benefit from a relatively smooth surface due to reduced signal losses. In addition, only an insignificant amount of metallic copper forms the surface layer, so that metallic copper losses in the circuit are reduced compared to conventional harsh etching methods. In addition, increased adhesion is obtained, which can be further increased by the method of the present invention.
[0067] In the method of the present invention, the copper or copper alloy surface is preferably a copper surface, i.e., it contains at least 99 wt% copper based on the total weight of the copper surface. In this case, the copper surface is preferably substantially free of, preferably free of, other elements than copper; more preferably substantially free of, preferably free of one, more than one or all elements selected from the group consisting of: molybdenum, cobalt, nickel, tungsten and titanium.
[0068] In the context of the present invention, the term "at least" in combination with a specific value means this value or more than this value (and is interchangeable with it). For example, "at least 99% by weight" means "99% by weight or more than 99% by weight" (and is interchangeable with it). Similarly, "at least one (kind)" means "one (kind), two (kinds), three (kinds), or more than three (kinds)" (and is interchangeable with it).
[0069] In contrast, in some cases, copper alloy surfaces are preferred. The method of the present invention is preferred, wherein in step (i), the copper alloy surface comprises at least 55 wt. %, preferably at least 75 wt. %, more preferably at least 85 wt. %, most preferably at least 90 wt. % copper based on the total weight of the copper alloy surface. Preferred alloying elements are selected from the group consisting of: molybdenum, cobalt, nickel, tungsten and titanium. In the context of the present invention, the term "copper alloy" does not include copper oxide.
[0070] In the context of the present invention, the term "substantially free" of a subject (e.g., an element, a compound, a material, etc.) means that the subject is completely absent or is present only in a very small and non-interfering amount (only to a very small and non-interfering extent) without affecting the intended purpose of the present invention. For example, such a subject may be added or utilized unintentionally, for example in the form of unavoidable impurities. "Substantially free" preferably means 0 (zero) ppm to 50 ppm, if defined for a copper or copper alloy surface as defined in the method of the present invention, then by the total weight of the surface, or if defined for a protective agent solution as defined in the method of the present invention, then by the total weight of the solution; preferably 0 ppm to 25 ppm, more preferably 0 ppm to 10 ppm, even more preferably 0 ppm to 5 ppm, most preferably 0 ppm to 1 ppm. 0 ppm means that the corresponding subject is not included. This principle also applies to nano-roughened surface layers and organic layers.
[0071] The preferred nano-roughened surface layer appropriately treated with an acidic non-etching protectant aqueous solution as defined above (preferably as defined throughout the present invention) shows an additional improved adhesion strength between the copper or copper alloy surface and the organic layer compared to the method (a) without the use of a protectant solution or (b) with the use of a protectant solution of a different composition, in particular not comprising one or more than one peroxide or comprising one or more than one peroxide in a total amount exceeding 0.4 wt. %. It is assumed that the increased adhesion strength is due to reduced copper reoxidation, in particular in subsequent processing steps involving increased temperature. This is unexpected due to the presence of trace amounts of said one or more than one peroxide and its etching potential.
[0072] Without wishing to be bound by theory, it is assumed that in step (ii), the aminoazole forms complexes with various copper species and adsorbs on the surface of the copper or copper alloy. It is further assumed that the adsorbed complexes are formed on the copper or copper alloy surface, thereby forming a thin protective film. Therefore, the process of the present invention is preferred, wherein during step (ii), one or more than one aminoazole is adsorbed on the copper or copper alloy surface, so that a protected copper or copper alloy surface is generated, preferably adsorbed on the nano-roughened surface layer, so that a protected nano-roughened surface layer is generated.
[0073] For the inventive method, it is necessary that etching does not occur after contacting with the protective agent solution. This means that the copper or copper alloy surface, preferably the nano-roughened surface layer remains intact, i.e., is not removed and its total surface area does not increase. This can be achieved mainly by avoiding too much peroxide, carefully maintaining non-etching pH and avoiding highly corrosive inorganic acids. In addition, aminoazoles are needed. Specifically, the etching potential of known peroxides in etching solutions is especially for etching copper. Therefore, surprisingly, the presence of peroxide further increases the adhesion strength between the copper or copper alloy surface and the organic layer in the non-etching method for increasing adhesion strength.
[0074] Therefore, in the context of the present invention (method and acidic non-etching protective agent aqueous solution), it is necessary that the acidic non-etching protective agent aqueous solution contains the one or more than one peroxide (preferably, as described as preferred throughout the text). The term "0.4 wt % or less total amount" (and all other preferred total amounts) in the word "less" does not mean that the peroxide can be completely absent, that is, less does not include 0 wt %. Therefore, one or more than one peroxide is present in a total amount greater than 0 wt %. Preferably, the total amount of the one or more than one peroxide is at least 0.01 wt %, more preferably at least 0.03 wt %, even more preferably at least 0.05 wt %, most preferably at least 0.07 wt % based on the total weight of the protective agent solution.
[0075] In the context of the present invention, a peroxide is a compound comprising a peroxide moiety (-OO-) wherein each oxygen atom has an oxidation number of -1 (minus one).Preferred is the process of the present invention wherein the one or more than one peroxide is selected from the group consisting of hydrogen peroxide, organic peroxides and inorganic peroxides.
[0076] The preferred organic peroxide is selected from the group consisting of organic peroxyacids and non-acidic alkyl peroxides. The preferred organic peroxyacid is peracetic acid. The preferred non-acidic alkyl peroxide is tert-butyl hydroperoxide.
[0077] Preferred inorganic peroxides are selected from the group consisting of inorganic peroxyacids and metal peroxides. Preferred inorganic peroxyacids are peroxymonosulfuric acid and peroxydisulfuric acid. Preferred metal peroxides are alkali metal peroxides, more preferably sodium peroxide and potassium peroxydisulfate.
[0078] More preferred is the method of the present invention, wherein one or more than one peroxide is selected from the group consisting of hydrogen peroxide and organic peroxides. Specifically, in some cases, the method of the present invention is preferred, wherein the acidic non-etching protective agent aqueous solution is substantially free of, preferably free of, inorganic peroxyacids; in a more preferred case, substantially free of, preferably free of, inorganic peroxyacids and metal peroxides.
[0079] Most preferably, the method of the present invention, wherein the one or more than one peroxide comprises hydrogen peroxide, preferably hydrogen peroxide. Most preferably, hydrogen peroxide is the only peroxide compound in the acidic non-etching protective agent aqueous solution. Hydrogen peroxide consists only of hydrogen and oxygen, and therefore does not pollute the working environment with other compounds or elements. In addition, hydrogen peroxide fully enhances adhesion strength by using only a very small amount in the acidic non-etching protective agent aqueous solution.
[0080] Preferred is the process of the present invention, wherein the total amount of one or more than one peroxide is 0.35 wt % or less, preferably 0.30 wt % or less, more preferably 0.25 wt % or less, even more preferably 0.20 wt % or less, most preferably 0.16 wt % or less, even most preferably 0.12 wt % or less, based on the total weight of the protective agent solution.
[0081] More preferred is the method of the present invention, wherein the one or more than one peroxide comprises hydrogen peroxide and the total amount of peroxides in the acidic non-etching protective agent aqueous solution is 0.35 wt % or less, preferably 0.30 wt % or less, more preferably 0.25 wt % or less, even more preferably 0.20 wt % or less, most preferably 0.16 wt % or less, even most preferably 0.12 wt % or less, based on the total weight of the protective agent solution. In this case, hydrogen peroxide is preferably the main peroxide in terms of weight % (> 50 wt %) based on the total weight of all peroxides in the acidic non-etching protective agent aqueous solution.
[0082] Most preferred is the method of the present invention, wherein in the acidic non-etching protective agent aqueous solution, hydrogen peroxide is the only peroxide and the total amount of peroxide in the acidic non-etching protective agent aqueous solution is 0.35 wt % or less, preferably 0.30 wt % or less, more preferably 0.25 wt % or less, even more preferably 0.20 wt % or less, most preferably 0.16 wt % or less, even most preferably 0.12 wt % or less, based on the total weight of the protective agent solution. In this case, the total amount of peroxide is equal to the total amount of hydrogen peroxide.
[0083] To avoid unwanted etching, the acidic non-etching protectant aqueous solution contains almost no mineral acid, which is well known for its etching properties, especially for etching copper. Its total amount is in the range of 0 to 0.01 wt % based on the total weight of the protectant solution.
[0084] If the acidic non-etching protective agent aqueous solution contains an inorganic acid that also contains a peroxide part (e.g., peroxymonosulfuric acid), then in the context of the present invention, such compounds are counted as one of (ii-c), i.e., are mainly regarded as peroxides. Preferably, the acidic non-etching protective agent aqueous solution is substantially free of, preferably free of, peroxymonosulfuric acid and peroxydisulfuric acid. More preferably, the acidic non-etching protective agent aqueous solution is substantially free of, preferably free of, an inorganic acid that also contains a peroxide part. This avoids undesirable etching.
[0085] Preferred is the method of the present invention, wherein the acidic non-etching protective agent aqueous solution is substantially free of, preferably free of, one, more than one or all of the following inorganic acids selected from the group consisting of: sulfuric acid, nitric acid, hydrochloric acid and phosphoric acid. In this case, the above-mentioned specific total amount (in ppm) applies individually to each of the above-mentioned inorganic acids, with the proviso that the total amount of these acids together does not exceed 0.01% by weight based on the total weight of the protective agent solution.
[0086] Very preferably, in the method of the present invention, the non-etching protectant solution contains substantially no, preferably no, sulfuric acid.
[0087] In particular, the method of the present invention is preferred, wherein the acidic non-etching protective agent aqueous solution is substantially free of, preferably free of, inorganic acids. In this case, the above-mentioned specific total amount (in ppm) applies to the sum of all inorganic acids. This applies to all inorganic acids, except for inorganic acids that additionally contain peroxide moieties.
[0088] It is also known that in etching solutions for copper, halide ions are usually present, usually to accelerate copper etching. Therefore, the method of the present invention is preferred, wherein the acidic non-etching protective agent aqueous solution is substantially free of, preferably free of chloride ions and fluoride ions, preferably substantially free of, preferably completely free of halide ions. It is also preferred that the acidic non-etching protective agent aqueous solution is substantially free of, preferably free of, compounds containing fluorine atoms. This avoids undesired etching.
[0089] The method of the present invention is preferred, wherein the acidic non-etching protectant aqueous solution is substantially free of, preferably free of, phosphate ions, preferably substantially free of, preferably free of compounds containing phosphate moieties, and more preferably substantially free of, preferably free of compounds containing phosphorus.
[0090] The method of the present invention is preferred in some cases wherein the acidic non-etching protectant aqueous solution is substantially free, preferably free of polymers.
[0091] The method of the present invention is preferred in some cases wherein the acidic non-etching protectant aqueous solution is substantially free, preferably free, of compounds comprising a quaternary nitrogen moiety.
[0092] The method of the present invention is preferred in some cases, wherein the acidic non-etching protectant aqueous solution is substantially free of, preferably free of, compounds containing one or more than one sulfhydryl group.
[0093] The acidic non-etching protective agent aqueous solution as defined in step (ii) of the method of the present invention is acidic (ie pH 6.5 or less) and aqueous, ie water is the main solvent, preferably water is the only solvent.
[0094] The method of the present invention is preferred, wherein the pH of the acidic non-etching protective agent aqueous solution is in the range of 2.5 to 6, preferably in the range of 2.7 to 5.8, more preferably in the range of 2.9 to 5.5, and most preferably in the range of 3.1 to 4.9. If the pH is significantly lower than 2.5, then undesired etching will occur, which is harmful to the copper or copper alloy surface. If the pH is significantly higher than 6, then the adsorption of aminoazoles is insufficient and the overall performance of the acidic non-etching protective agent aqueous solution is unsatisfactory. A very preferred pH range is 4.1 to 4.9. In the context of the present invention, pH refers to a temperature of 25°C.
[0095] In the process of the invention, one or more than one aminoazole is an essential compound in the acidic non-etching protective agent aqueous solution (for the reasons outlined above). Our own experiments have shown that satisfactory results are only obtained when the aminoazole is used in the acidic non-etching protective agent aqueous solution.
[0096] In the context of the present invention, aminoazole means a compound having a heterocyclic five-membered aromatic ring, the compound additionally comprising at least one (preferably one) amino moiety (-NH2), wherein the five-membered aromatic ring preferably comprises at least two nitrogen ring atoms as heteroatoms. Preferably, the nitrogen atom is the only heteroatom in the aromatic ring.
[0097] The process of the invention is preferred wherein the one or more than one aminoazole independently comprises at least three nitrogen ring atoms in the aromatic ring, more preferably independently comprises at least four nitrogen ring atoms in the aromatic ring.
[0098] Preferred are the methods of the invention, wherein at least one amino moiety, preferably one amino moiety, is directly attached to the aromatic ring, preferably to a carbon ring atom of the aromatic ring, via a covalent bond.
[0099] In some cases, the process of the invention is preferred wherein the aromatic ring is not an imidazole.
[0100] Preferred is the process of the invention wherein in each of the one or more than one aminoazoles the five-membered aromatic ring is the only ring structure.
[0101] Preferred is the process of the invention, wherein the one or more than one aminoazole is selected from the group consisting of aminotetrazole, aminotriazole, substituted aminotriazole and substituted aminotetrazole, preferably selected from the group consisting of aminotetrazole and substituted aminotetrazole, most preferably, the one or more than one aminoazole comprises 5-aminotetrazole. Preferably, the aminotetrazole also includes aminoalkyltetrazoles, such as 5-(aminomethyl)-tetrazole, but aminoalkyltetrazoles are less preferred than 5-aminotetrazole.
[0102] Preferably, the aminoazole is the only azole compound in the acidic aqueous non-etching protectant solution. Our own experiments indicate that aminoazoles provide the best increase in adhesion strength in the process of the present invention.
[0103] In substituted aminotriazoles and substituted aminotetrazoles, preferred substituents are independently alkyl. Preferred alkyl groups are methyl, ethyl and propyl. In some cases, 1-propyl-5-aminotetrazole and 1-methyl-5-aminotetrazole are preferred substituted aminotetrazoles.
[0104] Preferred is the process of the invention, wherein one or more than one aminoazole is present in a total amount of 2.0 wt % or less, preferably 1.5 wt % or less, more preferably 1.0 wt % or less, most preferably 0.8 wt % or less, based on the total weight of the protectant solution.
[0105] More preferred is the method of the present invention, wherein one or more than one aminoazole comprises 5-aminotetrazole and the total amount of aminoazoles in the acidic non-etching protective agent aqueous solution is 2.0 wt % or less, preferably 1.5 wt % or less, more preferably 1.0 wt % or less, most preferably 0.8 wt % or less, based on the total weight of the protective agent solution. In this case, 5-aminotetrazole is preferably the main aminoazole (>50 wt %) in terms of weight % based on the total weight of all aminoazoles in the acidic non-etching protective agent aqueous solution.
[0106] Most preferred is the method of the present invention, wherein in the acidic non-etching protective agent aqueous solution, 5-aminotetrazole is the only aminoazole and the total amount of aminoazoles in the acidic non-etching protective agent aqueous solution is 2.0 wt% or less, preferably 1.5 wt% or less, more preferably 1.0 wt% or less, most preferably 0.8 wt% or less, based on the total weight of the protective agent solution. Even more preferred is the method of the present invention, wherein 5-aminoazole is the only azole compound in the acidic non-etching protective agent aqueous solution and the total amount of azole compounds in the acidic non-etching protective agent aqueous solution is 2.0 wt% or less, preferably 1.5 wt% or less, more preferably 1.0 wt% or less, most preferably 0.8 wt% or less, based on the total weight of the protective agent solution.
[0107] Preferred is the method of the present invention, wherein in the acidic non-etching protective agent aqueous solution, the molar ratio of all peroxides to all aminoazoles is 1 or less, preferably 0.8 or less, more preferably 0.6 or less, even more preferably 0.5 or less, most preferably 0.4 or less. In order to avoid undesired etching, it is most desirable to have a molar ratio of no more than 1:1, more preferably, the molar concentration of all aminoazoles is higher than the molar concentration of all peroxides.
[0108] In the method of the present invention, the acidic non-etching protective agent aqueous solution comprises one or more than one organic acid and / or its salt, preferably an organic acid. The organic acid is mainly used to adjust the pH of the acidic protective agent aqueous solution. This may be required because aminoazole compounds are usually dissolved in alkaline solutions to increase solubility.
[0109] It is preferred that the acidic non-etching protectant aqueous solution is substantially free, preferably free of sulfonic acid. Typically, such acids are too strong and may cause undesirable etching.
[0110] Preferably, each of the one or more than one organic acid has a positive pKa value, preferably 3.0 or higher, preferably 3.3 or higher, more preferably a pK in the range of 3.3 to 6.5 a These pK a Values are based on a temperature of 22°C.
[0111] Preferred is the process of the present invention, wherein the one or more than one organic acid and its salts are selected from the group consisting of monocarboxylic acids, hydroxymonocarboxylic acids, dicarboxylic acids, hydroxydicarboxylic acids, tricarboxylic acids, hydroxytricarboxylic acids, aminocarboxylic acids and their salts; preferably selected from the group consisting of monocarboxylic acids, hydroxymonocarboxylic acids, dicarboxylic acids, hydroxydicarboxylic acids, tricarboxylic acids, hydroxytricarboxylic acids and their salts; most preferably selected from the group consisting of monocarboxylic acids, hydroxymonocarboxylic acids, dicarboxylic acids, hydroxydicarboxylic acids and their salts.
[0112] Particularly preferred specific organic acids and their salts are selected from the group consisting of formic acid, acetic acid, propionic acid, caprylic acid, glycolic acid, n-butyric acid, isobutyric acid, acrylic acid, crotonic acid, isomethacrylic acid, oxalic acid, malonic acid, succinic acid, adipic acid, maleic acid, acetylenedicarboxylic acid, lactic acid, glyceric acid, tartaric acid, malic acid, citric acid, threonine, tryptophan, phenylalanine and their salts.
[0113] Most preferred is the process of the present invention, wherein the one or more than one organic acid and salts thereof are selected from the group consisting of formic acid, acetic acid, lactic acid, malic acid, citric acid and salts thereof, most preferably formic acid, acetic acid and salts thereof.
[0114] One or more than one organic acid can exist in salt form. Therefore, the acidic non-etching protective agent aqueous solution preferably contains metal cations. The preferred metal cations in the acidic non-etching protective agent aqueous solution are alkali metal cations and alkaline earth metal cations, preferably alkali metal cations, more preferably sodium cations and potassium cations. Most preferably, one or more than one organic acid exists in its acidic form.
[0115] Preferred is the process of the invention, wherein the total amount of anions of organic acid residues of one or more than one organic acid and salts thereof is 4 wt% or less, preferably 3.2 wt% or less, more preferably 2.5 wt% or less, even more preferably 1.9 wt% or less, most preferably 1.5 wt% or less, based on the total weight of the protectant solution. If the total amount is too low, the desired pH cannot be properly obtained. If the total amount significantly exceeds 4 wt%, undesired etching is observed in some cases.
[0116] Preferably, the acidic non-etching protective agent aqueous solution used in the method of the present invention is substantially composed of water as a solvent, (ii-a), (ii-b), (ii-c), (ii-d) and optionally alkali metal cations and / or alkaline earth metal cations as conductive cations. In order to fully increase the adhesion strength, other compounds are not necessarily required in the acidic non-etching protective agent aqueous solution.
[0117] Based on this, it is most preferred that the acidic non-etching protective agent aqueous solution containing the solvent, (ii-a), (ii-b), (ii-c), (ii-d) and optionally alkali metal cations and / or alkaline earth metal cations as conductive cations account for at least 99 weight % of the total weight of all ingredients in the acidic non-etching protective agent aqueous solution.
[0118] In the step (ii) of the inventive method, the acidic non-etching protective agent aqueous solution contacts the substrate comprising the surface so that the adhesion strength increases.Preferably the inventive method, wherein in step (ii), the contact is carried out for 5 seconds to 600 seconds, preferably 10 seconds to 300 seconds, more preferably 15 seconds to 150 seconds, even more preferably 20 seconds to 90 seconds, most preferably 25 seconds to 45 seconds.Although etching is not observed even at 600 seconds, it is not desirable to significantly exceed 600 seconds usually without any benefit and from a commercial point of view.On the contrary, if the contact is significantly lower than 5 seconds, the increase of adhesion strength does not seem to exist in some cases.
[0119] Preferred is the process of the present invention, wherein in step (ii) the contacting is carried out at a temperature in the range of 15 to 50°C, preferably in the range of 20 to 40°C, more preferably in the range of 30 to 40°C.
[0120] The acidic non-etching protective agent aqueous solution used in the method of the present invention is preferably not used for chemical and / or mechanical polishing, such as CMP. Therefore, the method of the present invention is not a polishing method, preferably not a CMP method.
[0121] The acidic non-etching protective agent aqueous solution used in the method of the present invention does not contain abrasive particles (sometimes also referred to as grinding particles). Typical abrasive particles are silicon dioxide particles and aluminum-containing particles. Therefore, in the method of the present invention, the acidic non-etching protective agent aqueous solution is a clear solution, i.e., does not contain solid particles.
[0122] Due to the method according to the invention, the adhesion strength between the copper or copper alloy surface and the organic layer is increased. Preference is given to the method according to the invention comprising the following additional steps:
[0123] (iii) laminating an organic layer onto the substrate obtained after step (ii) so that the copper or copper alloy surface in contact with the acidic non-etching protective agent aqueous solution during step (ii) is in contact with the organic layer.
[0124] After step (iii), the organic layer is in direct contact with the copper or copper alloy surface. Since the surface is modified according to the method of the present invention, the adhesion strength between the organic layer and the surface is increased. If the copper or copper alloy surface comprises (preferably is) a copper or copper alloy circuit, the organic layer preferably covers the non-conductive areas of the non-conductive substrate and the conductive copper / copper alloy areas.
[0125] Preferably, lamination is performed under vacuum and increased temperature, preferably at a temperature in the range of 50°C to 140°C.
[0126] In a subsequent step, the laminated organic layer is preferably cured, ie subjected to a heat treatment by a higher temperature, so that the organic layer is polymerized. Therefore, preferred is a method of the present invention comprising the following additional steps after step (iii):
[0127] (iv) subjecting the substrate having the organic layer obtained after step (iii) to heat treatment at a temperature in the range of 142° C. to 220° C., preferably in the range of 145° C. to 210° C., more preferably in the range of 150° C. to 205° C., so that the organic layer is polymerized.
[0128] Preferably, the subjecting in step (iv) is carried out for 20 minutes to 180 minutes, preferably 20 minutes to 150 minutes.
[0129] The organic layer is preferably a permanent layer. The term "permanent" means that it is not intended to remove the organic layer during or after the method of the present invention. The organic layer is not a temporary layer; rather, it most preferably remains for the entire life of the non-conductive substrate, preferably the PCB. However, the term does not exclude different temporary conditions of the organic layer, such as polymerized and non-polymerized.
[0130] Preferably, the non-conductive substrate treated in the method of the present invention is a precursor of a circuit board, preferably a precursor of a multilayer printed circuit board. Such a preferred circuit board precursor is required for the final formation of a printed circuit board. In this case, preferably, in the first cycle of the method of the present invention, the organic layer laminated in step (iii) is preferably a buildup layer, which forms a non-conductive substrate in step (i) of the subsequent second cycle of the method of the present invention.
[0131] Therefore, the process of the present invention is preferred, wherein the organic layer in step (iii) is a stacked layer.
[0132] More preferably, the method of the present invention, wherein the organic layer in step (iii) is a copper layer free stacking layer, more preferably a metal layer free stacking layer. In order to form a non-conductive substrate comprising a copper or copper alloy surface (preferably a circuit, most preferably, as defined as preferred throughout the present invention) on at least one side in the subsequent second cycle step (i), the organic layer (preferably a copper layer free stacking layer, more preferably a metal layer free stacking layer) is subjected to a copper metallization process after step (iii) of the first cycle (most preferably after step (iv)) to form a corresponding copper or copper alloy surface (preferably a circuit, most preferably, as defined as preferred throughout the present invention). Subsequently, a nano-roughened surface layer is preferably formed, preferably as defined throughout the present invention. Such a cycle sequence is typical for a semi-additive process and our own experiments have shown that the method of the present invention is particularly beneficial for such a process. Therefore, the method of the present invention is preferably used in a semi-additive process for manufacturing printed circuit boards.
[0133] The non-conductive substrate provided in step (i) of the method of the present invention is preferably a core substrate or an organic layer laminated in step (iii) of a previous cycle of the method of the present invention. The core substrate is preferably the basis and starting point for accumulating a multilayer PCB. The preferred core substrate comprises a glass cloth reinforced fiber material having a copper or copper alloy surface (preferably a copper / copper alloy circuit) on at least one side. Preferably, such core substrates additionally comprise one or more than one group of filler particles selected from the group consisting of: SiO2, Al2O3, TiO2, ZrO2. Such core substrates are not build-up layers.
[0134] Preferably, in the process of the present invention, in step (iii), the organic layer is substantially free of, preferably free of, filler fibers, preferably substantially free of, preferably free of glass fibers. Alternatively, the process of the present invention is preferred, wherein in step (iii), the organic layer comprises filler particles, preferably one or more than one filler particles selected from the group consisting of SiO2, Al2O3, TiO2, ZrO2, most preferably SiO2.
[0135] The method of the invention is preferred, wherein in step (iii), the organic layer is a dry film or a liquid, preferably a dry film, most preferably a dry film stack. The skilled person knows in this context that a liquid organic layer is not completely fluid, but exhibits a certain viscosity typical of this technical field. In the same way, the skilled person knows that a dry film is not completely dry, but contains a certain amount of typical solvents.
[0136] The process according to the invention is preferred, wherein in step (iii), the layer thickness of the organic layer is 50 μm or less, preferably 33 μm or less, more preferably 21 μm or less, even more preferably 15 μm or less, most preferably 10 μm or less.
[0137] Our own experiments have shown that organic layers, preferably stacked layers, exhibiting a layer thickness of 50 μm or less, especially 21 μm or less, are highly susceptible to oxygen permeation, especially when subjected to increased temperatures. Such permeation is highly undesirable, as it leads to copper reoxidation. Therefore, the method according to the invention is particularly beneficial for very thin organic layers, especially below 21 μm, in order to prevent undesired reoxidation of copper to copper oxide.
[0138] Preferably, the organic layer comprises at least one compound selected from the group consisting of epoxy compounds, polyimides, cyanate esters, bismaleimide-triazine compounds, polypropylene ethers and polyolefins. The method of the present invention is preferred, wherein in step (iii), the organic layer comprises an epoxy compound, more preferably, the organic layer is a stacked layer comprising an epoxy compound.
[0139] The present invention also relates to an acidic non-etching protective agent aqueous solution comprising:
[0140] (a) one or more aminoazoles,
[0141] (b) one or more organic acids and / or their salts,
[0142] (c) one or more peroxides in a total amount of 0.4 wt. % or less based on the total weight of the protectant solution, and
[0143] (d) inorganic acid in a total amount of 0 to 0.01 wt % based on the total weight of the protective agent solution,
[0144] Wherein in the acidic non-etching protective agent aqueous solution, the molar ratio of all peroxides to all aminoazoles is 1 or less, preferably 0.8 or less, more preferably 0.6 or less, even more preferably 0.5 or less, most preferably 0.4 or less.
[0145] Preferred is the acidic non-etching protective agent aqueous solution of the present invention, wherein the molar concentration of all aminoazoles is higher than the molar concentration of all peroxides.
[0146] The benefits of the protectant solution have been described above in conjunction with the method of the present invention. The above discussion on the method of the present invention is also applicable to the acidic non-etching protectant aqueous solution of the present invention.
[0147] The present invention is further explained by the following non-limiting examples.
[0148] Examples
[0149] A. Sample preparation
[0150] Step (i): Providing a non-conductive substrate comprising a copper or copper alloy surface on at least one side:
[0151] Copper foil (150 mm x 75 mm x 35 μm) was used to demonstrate the method of the present invention.
[0152] In a first step, the copper surfaces of all foils were etch cleaned by using a sulfuric acid / H2O2 solution containing 180 ml / L SoftClean UC168, 200 ml / L CupraEtch Starter, 75 ml / L Hydrox (all products of Atotech) and 545 ml / L deionized water to obtain etch cleaned copper foil. Etch cleaning removes heavy oxides and other compounds such as antioxidants and / or surfactants. After etch cleaning, the etch cleaned copper foil was rinsed with cold water for approximately two minutes. Thus, etch cleaned and rinsed copper foil was obtained.
[0153] Subsequently, a nano-roughened surface layer is formed.
[0154] Subsequently, the etch-cleaned and rinsed copper foil obtained after the first step is chemically treated by oxidation and subsequent reduction reactions.
[0155] In a second step, the foil was immersed in a conditioning solution containing 15.5 ml / L NovaBond IT stabilizer (Atotech) at 50° C. for 30 seconds. The conditioning agent stabilizes the copper surface with respect to pH and electrochemical potential. Thus, a conditioned copper foil was obtained.
[0156] In the third step, the conditioned copper foil is treated in an oxidizing solution containing 100 ml / L NovaBond IT 102 (Atotech) and 15.5 ml / L NovaBond IT stabilizer (Atotech). The treatment is carried out at 70° C. for 6 minutes, resulting in a uniform and self-limiting conversion of Cu(0) to Cu(I)-oxide and Cu(II)-oxide, respectively, ultimately forming a needle-shaped layer of converted copper with a maximum layer thickness of less than 180 nm. After oxidation, the oxidized copper foil is rinsed with cold water.
[0157] In the fourth step, the oxidized and rinsed copper foil is contacted with a reducing solution comprising 20 ml / L NovaBond IT reducing agent (Amet) and 5 ml / L NovaBond IT stabilizer. The reduction is carried out at 35° C. for 5 minutes and a reduced copper foil is obtained. The reduction mainly converts copper oxide into Cu(0), thereby enhancing the stability of the needle-shaped layer of the converted copper against chemicals. During the reduction, the needle-shaped morphology is maintained. After the reduction, the copper foil is rinsed with cold water for approximately two minutes. Thus, a reduced and rinsed copper foil with a nano-roughened surface layer is obtained.
[0158] Step (ii): contacting the substrate including the surface with an acidic non-etching protective agent aqueous solution:
[0159] In the fifth step, the reduced and rinsed copper foil with nano-roughened surface layer was subjected to different acidic non-etching protectant aqueous solutions (PS) as summarized in Table 1.
[0160] Table 1. Overview of the protective agent solutions used
[0161]
[0162]
[0163] *Not according to the present invention; based on E.6 in Table 1 of US 2002 / 0192460 A1
[0164] **Not according to the invention
[0165] ***According to the present invention
[0166] In each case, the reduced and rinsed copper foil was immersed in the corresponding protectant solution (PS) for 30 seconds and the temperature of the protectant solution was approximately 35° C. After immersion, the copper foil was rinsed with cold water for approximately 30 seconds and then dried at a temperature between 60° C. and 70° C. Protected and rinsed copper foils were thus obtained. These copper foils were then subjected to lamination of organic layers and further testing.
[0167] Step (iii): Laminating an organic layer onto the substrate obtained after step (ii):
[0168] In the lamination step, each of the protected and washed copper foils obtained after the fifth step was laminated with the following commercially known buildup layers (ie, organic layers): GX-T31 and GZ-41 (both products of Ajinomoto) designed for fine-line circuit applications.
[0169] Lamination was performed in vacuum at approximately 100° C. under yellow light in a clean room with room temperature in the range of 20° C. to 25° C. and relative humidity of 50% to 60% by using a vacuum laminator (Dynachem VA 7124-HP6). The layer thickness of each build-up layer was 20 μm.
[0170] Step (iv): Subjecting the substrate having the organic layer obtained after step (iii) to heat treatment:
[0171] Each substrate obtained after step (iii) was subjected to heat treatment using a conventional hot air convection oven (Heraeus Oven UT6200) at 160° C. for 60 minutes to polymerize (ie, cure) the buildup layer.
[0172] B. Adhesion strength assessment:
[0173] For each sample, the adhesion strength (initial and HAST) was evaluated.
[0174] The adhesion strength measured "initially" after step (iv) and before any other treatment
[0175] "HAST" Adhesion strength measured after HAST test (96h, 130°C, 85% rh, HAST chamber: EHS-221M)
[0176] A summary of the results is given in Table 2.
[0177] Table 2, Summary of Adhesion Strength (GX-T31 and GZ-41)
[0178]
[0179]
[0180] The values in Table 2 show that PS3 provides significantly improved adhesion strength both "initial" and, most importantly, after "HAST".
[0181] Surprisingly, compared to known non-etching adhesion promoter processes, adding relatively small amounts of strong oxidants, such as H2O2, to the non-etching protectant solution used in the non-etching adhesion promoter process further improves the adhesion strength to the organic layer (see US 2002 / 0192460 A1). In the case of GZ-41, the adhesion strength has been doubled compared to US'460 and almost doubled compared to compositions that do not contain a small amount of strong oxidants. Although for GX-T31, the increase in adhesion strength is slight in the "initial" case, a significant increase of almost 40% compared to PS1 (which corresponds to US'460) is observed after HAST.
[0182] Increased adhesion strength was also obtained with protectant solutions similar to PS3, but with the sole exception that the concentration of acetic acid was below 1 wt % (data not shown).
[0183] In order to determine the adhesion strength of the samples, several strip-type segments have been prepared from each sample. For this, the corresponding copper foil was adhered to a rigid board (same size as the copper foil) in such a way that the rigid board and the copper foil faced the buildup layer. Thus, a copper foil with a structurally enforced buildup layer was obtained.
[0184] Subsequently, each of the mandatory copper foils was cut into strip-shaped segments (10×100 mm, Milling Cutter, Walter Lemmen CCD).
[0185] The strip segments were subjected to a peel force measurement machine (Roell Zwick Z010) to individually evaluate the adhesion strength based on the force required for forced delamination of the copper foil from its corresponding structure (angle: 90°, speed: 50 mm / min).
[0186] In another control experiment, the etching characteristics of PS3 were examined (data not shown). During immersion, no weight loss was observed, indicating that the copper and nano-roughened surface layers, respectively, were not removed but remained intact.
Claims
1. A method for increasing the adhesion strength between a copper or copper alloy surface and an organic layer, the method comprising the following steps in this order: (i) providing a non-conductive substrate comprising, on at least one side, said surface having a total surface area of copper or a copper alloy, Wherein in step (i), the copper or copper alloy surface comprises a nano-roughened surface layer obtained as follows: - Oxidation of Cu-(0) to Cu-(I) and Cu-(II), respectively, and then - reducing the Cu-(I) and Cu-(II) at least partially to Cu-(0); (ii) contacting the substrate comprising the surface with an acidic non-etching protective agent aqueous solution comprising: (ii-a) one or more aminoazoles, (ii-b) one or more organic acids and / or their salts, (ii-c) one or more peroxides in a total amount of 0.4 wt % or less based on the total weight of the acidic non-etching protectant aqueous solution, and (ii-d) an inorganic acid in a total amount of 0 to 0.01 wt % based on the total weight of the acidic non-etching protective agent aqueous solution, wherein during step (ii), the total surface area of the surface does not increase after contact with the acidic non-etching protective agent aqueous solution. 2 . The method according to claim 1 , wherein in step (i), the maximum layer thickness of the nano-roughened surface layer is 500 nm or less.
3. The method according to any one of the preceding claims, wherein during step (ii), the one or more than one aminoazole is adsorbed on the copper or copper alloy surface such that a protected copper or copper alloy surface is produced.
4. The method according to claim 1 or 2, wherein in the acidic non-etching protective agent aqueous solution, the molar ratio of all peroxides to all aminoazoles is 1 or less.
5. The method of claim 1 or 2, wherein the one or more than one peroxide comprises hydrogen peroxide.
6. The method according to claim 1 or 2, wherein the total amount of the one or more than one peroxide is 0.35 wt% or less based on the total weight of the acidic non-etching protective agent aqueous solution.
7. The method according to claim 1 or 2, wherein the pH of the acidic non-etching protective agent aqueous solution is in the range of 2.5 to 6.
8. The method of claim 1 or 2, wherein the one or more than one aminoazole is selected from the group consisting of aminotetrazole, aminotriazole, substituted aminotriazole, and substituted aminotetrazole.
9. The method according to claim 1 or 2, wherein the one or more than one aminoazole is present in a total amount of 2.0 wt% or less based on the total weight of the acidic non-etching protectant aqueous solution.
10. The method according to claim 1 or 2, wherein the total amount of organic acid residue anions of the one or more organic acids and salts thereof is 4 wt% or less based on the total weight of the acidic non-etching protective agent aqueous solution.
11. The method according to claim 1 or 2, wherein in step (ii), the contacting is performed for 5 seconds to 600 seconds.
12. The method according to claim 1 or 2, comprising the following additional steps: (iii) laminating the organic layer onto the substrate obtained after step (ii) so that the copper or copper alloy surface in contact with the acidic non-etching protective agent aqueous solution during step (ii) is in contact with the organic layer.
13. The method according to claim 12, wherein the organic layer in step (iii) is a stacked layer.
14. An acidic non-etching protective agent aqueous solution, comprising: (a) one or more aminoazoles, (b) one or more organic acids and / or their salts, (c) one or more peroxides in a total amount of 0.4 wt % or less based on the total weight of the acidic non-etching protectant aqueous solution, and (d) an inorganic acid in a total amount of 0 to 0.01 wt % based on the total weight of the acidic non-etching protective agent aqueous solution, Wherein in the acidic non-etching protective agent aqueous solution, the molar ratio of all peroxides to all aminoazoles is 1 or less.