Indoor corrosion damage test system and test method for defective prestressed anchor structures
By designing the corrosion damage test system for prestressed anchor structures in the room, the problem of inaccurate evaluation of corrosion damage and controlling tension in the existing technology is solved, and precise control and disturbance-free disassembly of the prestressed anchor structure is achieved, and corrosion is improved. Accuracy and simulation capabilities of injury assessment.
Patent Information
- Application Number
- CN202011080225.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-10-10
AI Technical Summary
The existing prestressed anchor structure corrosion test system is difficult to accurately evaluate corrosion damage indoors, and cannot accurately control tension, and cannot reflect local corrosion conditions and anchor structure performance under different prestress levels.
A corrosion damage test system for prestressed anchoring structures with indoor defects was designed, including steel bars, grouting containers, corrosion tanks, tension pressure sensors, mortar bodies and corrosion liquids. By precisely controlling tension and simulated defects, combined with electrochemical testing, Achieve disturbance-free disassembly and corrosion damage assessment of prestressed anchor structures.
Accurate control and disturbance-free disassembly of the prestressed anchor structure are achieved, the accuracy of corrosion damage assessment is improved, the corrosion conditions in different environments can be simulated, and the mechanical properties of the anchor structure are weakened.
Smart Images

Figure CN112098313B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of prestressed anchor structure corrosion test design, in particular to an indoor defective prestressed anchor structure corrosion damage test system and test method. Background Art
[0002] Since the 1960s, anchoring structures have been widely used in various geotechnical engineering projects in my country. Among them, prestressed anchor rods play an important role in geotechnical anchoring projects due to their excellent stability maintenance ability and huge economic benefits. However, the physical and mechanical properties of prestressed anchor rods are often degraded due to corrosion in the surrounding harsh geotechnical environment. The corrosion damage of prestressed anchoring structures in high slopes is usually caused by insufficient grouting and cracking of the grouting body. As the rust products gradually accumulate on the contact surface between the steel bars and the mortar, the oxides, which consume about 2-6 times the volume of the steel bars, produce huge rust expansion forces, leading to further development of mortar defects, and the engineering performance of the anchoring structure may drop sharply.
[0003] Unlike permanent prestressed anchor structures in actual projects (such as slopes, tunnels, etc.), a series of mechanical property tests are usually required after conducting indoor durability tests of prestressed anchor structures. Therefore, how to minimize the external disturbance to the prestressed anchor structure after the corrosion test, and then more objectively and accurately evaluate the actual damage of the prestressed anchor structure under indoor set conditions, is a question worth considering. Secondly, previous test devices rarely considered the impact of defects on the corrosion damage of prestressed anchor structures, and thus could not objectively reflect local corrosion, which is a more common corrosion condition than uniform corrosion. Furthermore, since the existing prestressed anchor structure corrosion test system usually uses hydraulic jacks for tensioning, even if there is a tension display that can read the applied tension value, it is impossible to accurately control the locking tension, resulting in the inability to evaluate the corrosion of the anchor structure under different prestress levels. Summary of the invention
[0004] In view of this, the present invention provides an indoor corrosion damage test system and test method for a defective prestressed anchor structure, which can better realize the disturbance-free disassembly of the prestressed anchor structure after corrosion and the local corrosion of the prestressed anchor structure caused by grouting defects, and can accurately control the locking tension force, thereby being more suitable for practical use.
[0005] In order to achieve the first objective, the present invention provides an indoor corrosion damage test system for a prestressed anchor structure with defects, comprising a steel bar, a grouting container, a corrosion pool, a rigid groove, a tension and pressure sensor, a mortar body, and a corrosion liquid.
[0006] The corrosion pool is contained in the rigid tank;
[0007] The grouting container is placed in the corrosion pool;
[0008] The two ends of the steel bar are detachably fixed to the two side walls of the rigid groove after passing through the grouting container and the corrosion pool in sequence from the inside to the outside;
[0009] The corrosive liquid is contained in the containing space between the grouting container and the corrosion tank;
[0010] The mortar body is accommodated in the accommodation space between the steel bar and the grouting container;
[0011] The grouting container is provided with a defective through hole;
[0012] When a pulling force is applied to the steel bar, the pulling force sensor is used to obtain data of the pulling force.
[0013] Furthermore, a first seal is provided at the connection between the steel bar and the grouting container; and a second seal is provided at the connection between the steel bar and the corrosion pool.
[0014] Furthermore, it also includes a first nut and a second nut, the steel bar is a ribbed steel bar, the first nut is used to fix the ribbed steel bar and the first side wall of the rigid groove; the second nut is used to fix the ribbed steel bar and the second side wall of the rigid groove; the first side wall and the second side wall are corresponding side walls.
[0015] Further, the tension and pressure sensor is arranged between the first side wall and the first nut, or the tension and pressure sensor is arranged between the second side wall and the second nut.
[0016] Furthermore, it also includes a first gasket and a second gasket, the first gasket is arranged between the first nut and the first side wall; the second gasket is arranged between the second nut and the second side wall; the tension and pressure sensor is arranged between the first gasket and the first nut, or the tension and pressure sensor is arranged between the second gasket and the second nut.
[0017] Furthermore, the grouting container is provided with grouting holes, and the grouting holes include a first grouting hole and a second grouting hole, and the first grouting hole and the second grouting hole are symmetrically arranged at two axial ends of the grouting container.
[0018] Furthermore, the grouting container is cylindrical, and the cylinder is split into a first half mold and a second half mold along two corresponding busbars. When in use, the first half mold and the second half mold are combined into one by using the two corresponding busbars.
[0019] Further, it also includes an auxiliary electrode graphite rod, a reference electrode saturated calomel electrode, and an electrochemical workstation. Among them, the auxiliary electrode graphite rod is disposed in the corrosion solution, and the saturated calomel electrode is an external electrode, which is placed into the corrosion solution during electrochemical testing. The steel bar is used as the working electrode. The electrochemical workstation is connected to the auxiliary electrode graphite rod, the reference electrode saturated calomel electrode, and the steel bar, and is used to collect and process electrochemical data. The electrochemical data includes electrochemical polarization curves and electrochemical impedance spectra. The instantaneous corrosion rate is obtained through the electrochemical polarization curves, and an equivalent circuit is fitted based on the characteristic curves of the electrochemical impedance spectra. The time-varying corrosion damage mechanism of the defective prestressed anchorage structure is explained based on the equivalent circuit.
[0020] In order to achieve the second above-mentioned purpose, the present invention provides a test method for corrosion damage of an indoor detachable defective prestressed anchorage structure, which is carried out based on the above test system. The method includes the following steps:
[0021] Assemble the indoor test system for corrosion damage of the defective prestressed anchorage structure;
[0022] The mortar body in the test system is soaked in the corrosion solution for a set time to obtain the mortar body corroded by the corrosion solution;
[0023] Dismantle the corrosion cell and take out the mortar body;
[0024] Conduct a pull-out test on the taken-out mortar body.
[0025] Further, the method specifically includes:
[0026] Step 1: Prepare a "mesh"-shaped reinforced concrete anchorage groove as a rigid groove, and evenly arrange a number of reserved holes for steel bars to pass through in each grid according to needs;
[0027] Step 2: Prepare the anchor rod specimen. Select a ribbed steel bar, and process one end into a threaded shape. First, gradually polish the steel bar with 200-600 mesh sandpaper until it is smooth. For steel bars with obvious rust, clean them with dilute hydrochloric acid, then use acetone to remove the surface oil, wipe off the surface moisture with a dry cloth, and place it in a vacuum box for standby;
[0028] Step 3: Make the corrosion cell. Use a PMMA plate with a thickness of 3 mm to process it into an uncovered cubic hollow box with a length of 30 cm, a width of 20 cm, and a height of 20 cm. Circular holes for the anchorage structure to pass through are opened on both side walls in the width direction of the corrosion cell, and the corrosion cell is fixed to the grid wall of the anchorage groove;
[0029] Step 4: Make a mortar pouring mold as a grouting container, divide a round tube made of PMMA, 2mm thick and 20cm long into two parts, drill a round hole at each end of the upper half as a grouting hole, drill at least one round hole in the middle as a defect through hole according to the defect design type, and prepare two thin wooden boards with round holes drilled in the center for blocking the two ends of the mold;
[0030] Step 5: Make a defective prestressed anchor structure, pass the processed ribbed steel bar with thread on one end through the rigid groove, corrosion pool, and grouting container bonded with epoxy resin glue in sequence, and fix one end of the steel bar with an anchor, install a tension and pressure sensor on the threaded end and fix it with a nut;
[0031] Step 6: Pour mortar. Before pouring mortar, check the gap of the mold to ensure that the contact between the steel bar and the wooden board and the upper and lower parts of the mold are tightly bonded to prevent water loss during the grouting process. Tie the steel bar to the wire and use epoxy resin to seal the wire. Lead the wire out of the mold, prepare cement mortar, use iron rods of different diameters to seal the defective through holes, and control the depth of the iron rod inserted into the hole as different types of defects. Use a mortar syringe to slowly inject mortar into the mold from the round hole at one end of the casting mold until the round hole at the other end overflows with mortar and stop grouting.
[0032] Step 7: Remove the mold for curing. After 24 hours, remove the mortar casting mold, pull out the small iron rods at the defects, and sprinkle water on the surface of the anchor body to keep the surface of the mortar inclusion in a moist state for curing.
[0033] Step 8: Pull out the steel bars. According to the specification, apply prestress to the steel bars after 7 days. Apply the prestress required by the design to the steel bars by twisting the nuts. The readings are directly reflected by the data acquisition instrument.
[0034] Step 9: Check the tightness of the corrosion pool, especially the contact position between the two side walls and the steel bars, and use sealant to seal the water; apply waterproof glue to the exposed steel bar surface in the corrosion pool to avoid unnecessary corrosion;
[0035] Step 10: After ensuring that there is no water seepage, inject a 10% NaCl solution into the corrosion pool, and after the ions in the solution are relatively stable, test the electrochemical impedance and self-corrosion potential of the defective prestressed anchor body;
[0036] Step 11: After a period of soaking, gradually remove the corrosion pool, take out the prestressed anchor body by rotating the nut, and perform a pull-out test on it.
[0037] The indoor corrosion damage test system and test method for defective prestressed anchoring structures provided by the present invention have simple principles, low manufacturing costs, and are convenient and practical. They can realize precise control of applied prestress, and can remove the prestressed anchoring structure with almost no disturbance, thereby making the anchor body pull-out test data more accurate. In addition, various factors (pH, prestress, defect type, protective layer thickness, etc.) affecting the mechanical properties of the prestressed anchoring structure can be controlled as needed, thereby realizing corrosion simulation under different environments, which is helpful for analyzing the corrosion mechanism and evolution law of the weakening of the mechanical properties of the prestressed anchoring structure in complex rock and soil environments, and provides a reference for conducting indoor accelerated corrosion tests on prestressed anchoring structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 A schematic diagram of the overall structure of an indoor corrosion damage test system for a prestressed anchor structure with defects provided by an embodiment of the present invention;
[0039] Figure 2 A schematic diagram of the front view of the structure of a grouting container used in the indoor corrosion damage test system for a prestressed anchor structure with defects provided by an embodiment of the present invention;
[0040] Figure 3 A schematic diagram of the top view of the structure of a grouting container used in the indoor corrosion damage test system for a prestressed anchor structure with defects provided by an embodiment of the present invention;
[0041] Figure 4 A flow chart of a corrosion damage test method for an indoor detachable defective prestressed anchor structure provided by an embodiment of the present invention;
[0042] Figure 5 An example schematic diagram of an electrochemical polarization curve (E-logi) provided for an embodiment of the present invention;
[0043] Figure 6 A schematic diagram of an example of an electrochemical impedance spectroscopy characteristic curve (Nyquist diagram) provided in an embodiment of the present invention;
[0044] Figure 7 Another type of electrochemical impedance spectroscopy characteristic curve example schematic diagram (Bode diagram) provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] See attached Figure 1-3 An embodiment of the present invention provides an indoor corrosion damage test system for a defective prestressed anchor structure, including a steel bar 1, a grouting container 6, a corrosion pool 4, a rigid groove 24, a tension and pressure sensor 10, a mortar body 2, and a corrosion liquid 7.
[0047] The corrosion pool 4 is accommodated in the rigid groove 24, the grouting container 6 is accommodated in the corrosion pool 4, and the two ends of the steel bar 1 pass through the grouting container 6 and the corrosion pool 4 from the inside to the outside in turn, and are fixed on the two side walls of the rigid groove 24; the corrosive liquid 7 is accommodated in the accommodating space between the grouting container 6 and the corrosion pool 4; the mortar body 2 is accommodated in the accommodating space between the steel bar 1 and the grouting container 6; a defective through hole 8 is provided on the grouting container 6; when a pulling force is applied to the steel bar 1, the tensile pressure sensor 10 is used to obtain the pulling force data.
[0048] The indoor corrosion damage test system and test method for defective prestressed anchoring structures provided by the present invention have simple principles, low manufacturing costs, and are convenient and practical. They can realize precise control of applied prestress, and can remove the prestressed anchoring structure with almost no disturbance, thereby making the anchor body pull-out test data more accurate. In addition, various factors (pH, prestress, defect type, protective layer thickness, etc.) affecting the mechanical properties of the prestressed anchoring structure can be controlled as needed, thereby realizing corrosion simulation under different environments, which is helpful for analyzing the corrosion mechanism and evolution law of the weakening of the mechanical properties of the prestressed anchoring structure in complex rock and soil environments, and provides a reference for conducting indoor accelerated corrosion tests on prestressed anchoring structures.
[0049] Among them, a first seal is provided at the connection between the steel bar 1 and the grouting container 6; a second seal is provided at the connection between the steel bar 1 and the corrosion pool 4. In this case, the corrosive liquid 7 can be prevented from penetrating into the mortar body 2 through the connection between the steel bar 1 and the grouting container 6, and the corrosive liquid 7 can be prevented from leaking into the rigid groove 24 through the connection between the steel bar 1 and the corrosion pool 4, which may cause inaccurate experimental data.
[0050] Among them, the indoor corrosion damage test system for defective prestressed anchoring structures also includes a first nut 13 and a second nut 14. The steel bar 1 is a ribbed steel bar, and the first nut 13 is used to fix the ribbed steel bar and the first side wall of the rigid groove 24; the second nut 14 is used to fix the ribbed steel bar and the second side wall of the rigid groove 24; the first side wall and the second side wall are corresponding side walls. In this case, the steel bar 1 can be fixed not only between the two side walls of the rigid groove 24 through the first nut 13 and the second nut 14, but also the position of the steel bar 1 in the rigid groove can be fixed, making the test process more convenient.
[0051] Among them, the indoor corrosion damage test system for defective prestressed anchoring structures also includes a first gasket 11 and a second gasket 12. The first gasket 11 is arranged between the first nut 13 and the first side wall; the second gasket 12 is arranged between the second nut 14 and the second side wall. In this case, the connection between the steel bar 1 and the rigid groove 24 can be made more stable. In this embodiment, the first gasket 11 and the second gasket 12 can be made of a compressive and deformable material. On this basis, the problem of displacement of the corrosion pool 4 caused by looseness between the first nut 13, the second nut 14 and the steel bar 1 can be avoided.
[0052] The tension and pressure sensor 10 is disposed between the first gasket 11 and the first nut 13, or the tension and pressure sensor 10 is disposed between the second gasket 12 and the second nut. In this case, the process of measuring tension and pressure using the tension and pressure sensor 10 is more convenient.
[0053] The grouting container 6 is provided with grouting holes, so that mortar can be easily injected into the grouting container 6 through the grouting holes to form the mortar body 2.
[0054] The grouting holes include a first grouting hole 20 and a second grouting hole 21 (such as Figure 3 As shown). The first grouting hole 20 and the second grouting hole 21 are symmetrically arranged at the axial ends of the grouting container 6. In this case, the process of grouting into the grouting container 6 to form the mortar body 2 is more uniform, so that the density of the mortar body 2 in the axial direction is more uniform; at least one circular hole is drilled on the grouting container 6 as the defective through hole 8 according to the defect design type, and two thin wooden boards with circular holes drilled in the center are prepared for plugging the two ends of the grouting container 6. In subsequent tests, iron rods of different diameters are used to plug the defective through hole 8, and the depth of the iron rod inserted into the hole is controlled to serve as different types of defects.
[0055] The grouting container 6 is cylindrical, and the cylinder is split along two corresponding generatrixes into a first half mold 16 and a second half mold 17 (such as Figure 2 As shown in the figure, when in use, the first half mold 16 and the second half mold 17 are combined into one body by using the corresponding two busbars. In this case, the grouting container 6 is easy to manufacture, use and demold. For example, when demolding, it is only necessary to separate the first half mold 16 and the second half mold 17 from the combined position before demolding, thereby facilitating the recycling of the grouting container 6. In this embodiment, in order to facilitate demolding, lubricating oil can be applied to the inner walls of the first half mold 16 and the second half mold 17, or an isolation film can be pasted. In this case, the lubricating oil or the isolation film can be used to achieve isolation between the mortar body 2 and the inner wall of the grouting container 6, making demolding more convenient.
[0056] Wherein, the first sealing member and the second sealing member are made of epoxy resin. Epoxy resin is a general term for a class of polymers containing two or more epoxy groups in the molecule. It is a condensation product of epichlorohydrin and bisphenol A or polyol. Due to the chemical activity of the epoxy group, it can be opened with a variety of compounds containing active hydrogen, and cured and cross-linked to form a network structure, so it is a thermosetting resin. It has good bonding strength and chemical resistance, so it can ensure the sealing effect of the first sealing member and the second sealing member.
[0057] The indoor corrosion damage test system for defective prestressed anchoring structures also includes an auxiliary electrode graphite rod 25, a reference electrode saturated calomel electrode and an electrochemical workstation 5, wherein the auxiliary electrode graphite rod 25 is arranged in the corrosive solution 7, the saturated calomel electrode is an external electrode, the steel bar 1 is used as a working electrode, and the saturated calomel electrode is used as a reference electrode. When performing electrochemical testing, it is placed in the corrosive solution 7, and its wire is connected to the electrochemical workstation to form a voltage loop with the working electrode for measuring the self-corrosion potential of the working electrode. The electrochemical workstation 5 is connected to the auxiliary electrode graphite rod 25, the reference electrode saturated calomel electrode and the steel bar 1, and is used to collect and process electrochemical data. The electrochemical workstation used in this embodiment is a CS350 electrochemical workstation produced by Wuhan Cost Instrument Co., Ltd., wherein the electrochemical data includes electrochemical polarization curves, electrochemical impedance spectrum characteristic curves (such as Figure 6 and Figure 7 The electrochemical workstation 5 plots an electrochemical polarization curve by monitoring the self-corrosion potential and corrosion current density of the working electrode, and plots an electrochemical impedance spectrum curve by monitoring the impedance and frequency of the working electrode.
[0058] The corrosion current density is obtained by the electrochemical polarization curve, and then the corrosion rate is obtained by formula (1):
[0059]
[0060] Where CR is the corrosion rate, μm / a; K is the corrosion current density coefficient, 3.27×10 -3 mm·g / μA·cm·year;i corr is the corrosion current density, μA / cm 2 , obtained from the polarization curve (such as Figure 5 As shown, the anode is the working electrode, in this embodiment, it is the anchor to be corroded; the cathode is oxygen); ρ is the steel density, g / cm 3 ; EW is steel bar molar equivalent (loss of two electrons), 28.
[0061] The electrochemical workstation can be used to obtain the characteristic curve of electrochemical impedance spectroscopy. The obtained characteristic curve of electrochemical impedance spectroscopy is obtained by the electrochemical workstation based on the acquired frequency data f and real part data Z real and imaginary data Z imag The curve directly outputted, on this basis, the corrosion solution resistance, mortar body resistance, and steel bar surface charge transfer resistance are set as R s , R c , R ct , the double-layer capacitances of the corrosion solution-mortar protective layer interface and the protective layer-steel interface are set as C dl , Q dl , where R ct Reflects the impedance of the passive film on the steel bar surface, Q dl Characterize the roughness of the steel bar surface. According to the characteristic curve of the electrochemical impedance spectroscopy and the above R s , R c , R ct , C dl , Q dl , a person skilled in the art can fit an equivalent circuit based on the existing knowledge, and according to the equivalent circuit, a person skilled in the art can analyze the corrosion mechanism of the working electrode, i.e., the anchor used in the test process, based on the existing knowledge.
[0062] In this embodiment, the etching liquid 7 is a NaCl solution, the raw material of which is cheap and easy to use.
[0063] See also Figure 4 The embodiment of the present invention also provides a method for testing corrosion damage of an indoor detachable prestressed anchor structure containing defects, comprising the following steps:
[0064] Step S1: assembling the indoor defective prestressed anchor structure corrosion damage test system provided by the present invention;
[0065] Step S2: the mortar body 2 in the test system is immersed in the corrosive liquid 7 for a set time to obtain the mortar body 2 corroded by the corrosive liquid 7;
[0066] Step S3: dismantling the corrosion pool 4 and taking out the mortar body 2;
[0067] Step S4: performing a pull-out test on the taken-out mortar body 2 .
[0068] Example
[0069] like Figure 1 As shown, the indoor corrosion damage test system for defective prestressed anchor structure includes an anchor system, an electrochemical test system and a data acquisition system.
[0070] Among them, the anchoring system is a "mesh"-shaped three-grid reinforced concrete anchoring groove, and each grid is equipped with two sets of detachable defective mortar anchoring structures, upper and lower. On both side walls of each grid, there are two circular holes, upper and lower, respectively, for the prestressed anchor body to penetrate into.
[0071] The detachable defective mortar anchoring structure is a ribbed steel bar with a thread at one end wrapped by a mortar body 2. One end of the ribbed steel bar is fixed to the left side wall through an anchor and a thick gasket in sequence, and the other end passes through the reinforced concrete anchoring groove (rigid groove 24), corrosion pool 4, thick gasket (11 or 12), and tensile-compressive force sensor 10, and is fixed to the right side wall of the reinforced concrete anchoring groove through a nut; there is a cylindrical defect on the mortar body 2.
[0072] The corrosion pool 4 is an uncovered cubic groove made of PMMA. There are circular holes with the same diameter as the ribbed steel bar at the centers of the left and right side walls of the corrosion pool 4. After locking the prestress of the anchoring structure, the contact part between the circular hole and the ribbed steel bar is sealed with epoxy resin glue; the corrosion pool 4 is fixed to the partition wall of the grid of the reinforced concrete anchoring groove through iron wires.
[0073] The electrochemical test system includes a working electrode ribbed steel bar, an auxiliary electrode graphite rod, and a reference electrode saturated calomel electrode. The working electrode and the auxiliary electrode are respectively connected to the electrochemical workstation through wires.
[0074] The data acquisition system is the tensile-compressive force sensor 10, which is used for the acquisition of prestress application.
[0075] As Figure 2 shown, the mortar anchor body is formed by injecting mortar into a pouring mold (grouting container 6). The pouring mold is evenly divided into an upper half mold and a lower half mold, and both ends are blocked by wooden boards; there is a circular hole in the center of the wooden board. As Figure 3 shown, there are grouting holes at both ends of the upper half mold, and a defect arrangement hole is provided at the center position.
[0076] In the past, after the prestressed anchor body corrosion test, it was necessary to cut the steel bar with a steel bar shear to take out the anchor body. This operation caused severe disturbance to the anchor body, seriously affected the integrity of the inclusion, and further affected the accuracy of the subsequent pull-out test results. At the same time, in the past, the prestress was applied through a hydraulic jack, and this method had the defect that it could not accurately apply the predetermined tensile force. In view of this problem, the present invention is designed such that there are holes for the anchor body to pass through at both ends of the anchoring groove, and the two ends of the steel bar are processed with threads, and the prestress can be accurately applied effectively by screwing the nut. The magnitude of the applied prestress is sensed by the tensile-compressive force sensor, which is convenient for studying other corrosion influencing factors under the condition of the same prestress magnitude. After the corrosion test is completed, the prestressed anchor body can be taken out, which is convenient and efficient.
[0077] A test method for corrosion damage of an indoor detachable prestressed anchorage structure with defects provided by the present invention has the following test operation process:
[0078] Step 1: Prepare a "mesh"-shaped reinforced concrete anchorage groove, and evenly arrange several (usually less than 3) reserved holes with a diameter of 10 cm for steel bars to pass through in each grid according to requirements.
[0079] Step 2: Prepare the anchor rod specimens. Select Q235 ribbed steel bars with a diameter of Φ6, process one end into a threaded shape. According to the American Society for Testing and Materials (ASTM) standard, first grind the steel bars layer by layer with 200-600 mesh sandpaper until smooth. For steel bars with obvious rust, clean them with dilute hydrochloric acid, then use acetone to remove the surface oil, wipe off the surface moisture with a dry cloth, and place them in a vacuum box for standby.
[0080] Step 3: Make the corrosion cell. Use a 3-mm-thick PMMA plate to process into an uncovered cube-shaped hollow box with a length of 30 cm, a width of 20 cm, and a height of 20 cm. Open circular holes with a diameter of 5 cm for the anchorage structure to pass through on both side walls in the width direction of the corrosion cell, and fix the corrosion cell to the grid wall of the anchorage groove with iron wire.
[0081] Step 4: Make the mortar pouring mold. Divide a 2-mm-thick, 20-cm-long round tube made of PMMA into two equal parts. Drill a circular hole with a diameter of 9 mm at each end of the upper half part, and drill a circular hole in the middle according to the defect design type (the circular hole diameter in this test is 4 mm, 7 mm, 9 mm). Prepare two thin wooden boards with circular holes drilled in the center for sealing the two ends of the mold.
[0082] Step 5: Make the prestressed anchorage structure with defects. Pass the processed ribbed steel bar with a threaded end through the reinforced concrete anchorage groove, the corrosion cell, and the mortar pouring mold bonded with epoxy resin in sequence, fix one end of the steel bar with an anchor, install a tension-compression sensor at the threaded end and fix it with a nut.
[0083] Step 6: Pour the mortar. Before pouring the mortar, check the gaps of the mold to ensure that the contact between the steel bar and the wooden board and the bonding of the upper and lower parts of the mold are tight to prevent water loss during the grouting process; bind the wire to the steel bar and seal the binding place with epoxy resin, and lead the wire out of the mold. Prepare cement mortar with a water-cement-sand ratio of 0.55:1:1, block the defect openings with iron rods of different diameters, and at the same time control the depth of the iron rods inserted into the holes to represent different types of defects. Slowly inject the mortar into the mold from one circular hole at one end of the pouring mold with a mortar syringe until the mortar overflows from the circular hole at the other end and stop grouting.
[0084] Step 7: Remove the mold and maintain the body. After 24 hours, remove the mold, pull out the small iron rods at the defects, and sprinkle water on the surface of the anchor body to keep the surface of the mortar inclusion moist for maintenance.
[0085] Step 8: Pull out the steel bar and apply prestress to the steel bar after 7 days according to the specification. Apply the prestress required by the design to the steel bar by twisting the nut, and the reading is directly reflected by the data acquisition instrument.
[0086] Step 9: Check the tightness of the corrosion pool, especially the contact position between the two side walls and the steel bars, and use sealant to seal the water; apply waterproof glue to the exposed steel bar surface in the corrosion pool to avoid unnecessary corrosion.
[0087] Step 10: After ensuring that there is no water seepage, inject a 10% NaCl solution into the corrosion pool, and after the ions in the solution are relatively stable, test the electrochemical parameters such as the electrochemical impedance and self-corrosion potential of the defective prestressed anchor body.
[0088] Step 11: After a period of soaking, gradually remove the corrosion pool, take out the prestressed anchor body by rotating the nut, and perform a pull-out test on it.
[0089] The invention has a simple principle, low production cost, convenience and practicality, can realize precise control of applied prestress, can dismantle the prestressed anchor structure almost without disturbance, thereby making the anchor body pull-out test data more accurate, and can control various factors affecting the mechanical properties of the prestressed anchor structure (pH, prestress, defect type, protective layer thickness, etc.) as needed, thereby realizing corrosion simulation under different environments (pH can be achieved by adjusting different acidity and alkalinity; prestress is achieved by knob nut; defect types are mainly diameter, depth, distribution, and protective layer thickness can be achieved by designing different casting molds), which is helpful to analyze the corrosion mechanism and evolution law of the weakening of the mechanical properties of the prestressed anchor structure in complex geotechnical environment, and provides a reference for conducting indoor accelerated corrosion tests of prestressed anchor structures.
[0090] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. An indoor corrosion damage test system for defective prestressed anchoring structures, characterized in that: It comprises a steel bar (1), a grouting container (6), a corrosion pool (4), a rigid groove (24), a tension and pressure sensor (10), a mortar body (2), and a corrosion liquid (7). The corrosion pool (4) is accommodated in the rigid groove (24); The grouting container (6) is accommodated in the corrosion pool (4); The two ends of the steel bar (1) are detachably fixed to the two side walls of the rigid groove (24) after passing through the grouting container (6) and the corrosion pool (4) in sequence from the inside to the outside; The corrosive liquid is contained in the containing space between the grouting container (6) and the corrosion pool (4); The mortar body (2) is accommodated in the accommodation space between the steel bar (1) and the grouting container (6); The grouting container (6) is provided with a defective through hole (8); When a pulling force is applied to the steel bar (1), the pulling force sensor (10) is used to obtain data of the pulling force; The system further comprises a first nut (13) and a second nut (14), The steel bar (1) is a ribbed steel bar. The first nut (13) is used to fix the ribbed steel bar and the first side wall of the rigid groove (24); The second nut (14) is used to fix the ribbed steel bar and the second side wall of the rigid groove (24); The first side wall and the second side wall are corresponding side walls; The system also includes an auxiliary electrode graphite rod (25), a reference electrode saturated calomel electrode and an electrochemical workstation (5), wherein the auxiliary electrode graphite rod (25) is arranged in the corrosion liquid (7), the saturated calomel electrode is an external electrode, which is placed in the corrosion liquid (7) when performing electrochemical testing, and the steel bar (1) is used as a working electrode. The electrochemical workstation (5) is connected to an auxiliary electrode graphite rod (25), a reference electrode saturated calomel electrode and a steel bar (1) to collect and process electrochemical data, wherein the electrochemical data includes an electrochemical polarization curve and an electrochemical impedance spectrum, and an instantaneous corrosion rate is obtained through the electrochemical polarization curve, and an equivalent circuit is fitted based on the characteristic curve of the electrochemical impedance spectrum, and a time-varying corrosion damage mechanism of a prestressed anchor structure containing defects is explained based on the equivalent circuit; The corrosion current density is obtained through the electrochemical polarization curve, and then the corrosion rate is obtained: ; Where CR is the corrosion rate, μm / a; K is the corrosion current density coefficient, 3.27×10 -3 mm·g / μA·cm·year;i corr is the corrosion current density, μA / cm 2 ; ρ is the steel density, g / cm 3 ; EW is steel bar molar equivalent; A first sealing member is provided at the connection between the steel bar (1) and the grouting container (6); A second sealing member is provided at the connection between the steel bar (1) and the corrosion pool (4); The tension and pressure sensor (10) is arranged between the first side wall and the first nut (13), or the tension and pressure sensor (10) is arranged between the second side wall and the second nut; The system further comprises a first gasket (11) and a second gasket (12), The first gasket (11) is arranged between the first nut (13) and the first side wall; The second gasket (12) is arranged between the second nut (14) and the second side wall; The tensile and compressive force sensor (10) is arranged between the first gasket (11) and the first nut (13), or the tensile and compressive force sensor (10) is arranged between the second gasket (12) and the second nut; The grouting container (6) is provided with grouting holes, the grouting holes include a first grouting hole (20) and a second grouting hole (21), and the first grouting hole (20) and the second grouting hole (21) are symmetrically arranged at two axial ends of the grouting container (6); The grouting container (6) is in the shape of a cylinder, and the cylinder is split into a first half mold (16) and a second half mold (17) along two corresponding generatrices. When in use, the first half mold (16) and the second half mold (17) are combined into one body by the two corresponding generatrices; An indoor detachable corrosion damage test method for a prestressed anchorage structure with defects by a system, the method comprising the following steps: Specifically including: Step 1: Prepare a "mesh"-shaped reinforced concrete anchorage groove as a rigid groove (24), and evenly arrange a number of reserved holes in each grid for the reinforcement to pass through as required; Step 2: Prepare an anchor rod specimen, select a ribbed steel bar, process one end into a threaded shape. First, gradually polish the steel bar with 200-600 mesh sandpaper until it is smooth. For steel bars with obvious rust, clean them with dilute hydrochloric acid, then use acetone to remove the surface oil, wipe off the surface moisture with a dry cloth, and place it in a vacuum box for standby; Step 3: Make a corrosion cell (4), use a plate made of PMMA with a thickness of 3 mm to process into an uncovered cubic hollow box with a length of 30 cm, a width of 20 cm, and a height of 20 cm. Circular holes for the anchorage structure to pass through are opened on both side walls in the width direction of the corrosion cell, and the corrosion cell is fixed to the grid wall of the anchorage groove; Step 4: Make a mortar casting mold as the grouting container (6), divide a round pipe made of PMMA with a thickness of 2 mm and a length of 20 cm into two equal parts, drill a round hole at each end of the upper half as a grouting hole, and drill at least one round hole as a defect through hole (8) in the middle according to the defect design type. Prepare two thin wooden boards with round holes drilled in the center for blocking the two ends of the mold; Step 5: Make a prestressed anchorage structure with defects, sequentially pass the processed ribbed steel bar with a threaded end through the rigid groove (24), the corrosion cell (4), and the grouting container (6) bonded with epoxy resin glue, and fix one end of the steel bar with an anchor, install a tensile and compressive force sensor at the threaded end and fix it with a nut; Step 6: Pour mortar. Before pouring mortar, check the gaps of the mold to ensure that the contact between the steel bar and the wooden board and the bonding of the upper and lower parts of the mold are tight to prevent water loss during the grouting process; Bind wires to the steel bars and seal the binding places with epoxy resin. Lead the wires out of the mold, prepare cement mortar, block the defect through holes (8) with iron rods of different diameters, and at the same time control the depth of the iron rods inserted into the holes to represent different types of defects. Use a mortar syringe to slowly inject mortar into the mold from a round hole at one end of the casting mold until mortar overflows from the round hole at the other end and stop grouting; Step 7: Remove the mold for curing. After 24 hours, remove the mortar casting mold, pull out the small iron rods at the defects, and sprinkle water on the surface of the anchor body to keep the surface of the mortar inclusion in a moist state for curing. Step 8: Pull out the steel bars. According to the specification, apply prestress to the steel bars after 7 days. Apply the prestress required by the design to the steel bars by twisting the nuts, and the readings are directly reflected by the data acquisition instrument. Step 9: Check the tightness of the corrosion pool, and seal the contact points between the two side walls and the steel bars with sealant; apply waterproof glue to the exposed steel bars in the corrosion pool to avoid unnecessary corrosion; Step 10: After ensuring that there is no water seepage, inject a 10% NaCl solution into the corrosion pool, and after the ions in the solution are relatively stable, test the electrochemical impedance and self-corrosion potential of the defective prestressed anchor body; Step 11: After a period of soaking, gradually remove the corrosion pool, take out the prestressed anchor body by rotating the nut, and perform a pull-out test on it.