Toner for electrostatic image development and method for producing toner for electrostatic image development
By using a combination of specific crystalline polyester resin and amorphous resin in the toner for electrostatic image development, the contradiction between low-temperature fixing performance and storage stability is solved, and excellent fixing effect and good fixing at low temperatures are achieved. Save stability and maintain productivity and cost-effectiveness.
Patent Information
- Application Number
- CN201980030990.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-11
- Filing Date
- 2019-05-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-05-10
AI Technical Summary
The existing toner for electrostatic image development is difficult to balance between low-temperature fixing performance and storage stability, and requires new equipment and high costs, affecting production efficiency and cost-effectiveness.
By using a crystalline polyester resin with a mass average molecular weight of 3000 to 5000 in the toner particles, sebacic acid is included as an acid component and 1,10-decanediol is used as an alcohol component, and amorphous resin is combined with a mold release The toner is produced by using existing equipment for kneading, cooling and curing, crushing and grading processes.
It achieves excellent fixing performance and good storage stability under low temperature conditions, while avoiding equipment upgrades and cost increases, and maintaining production efficiency and economy.
Smart Images

Figure BDA0002765425900000121
Abstract
Description
Technical Field
[0001] The present invention relates to a toner for electrostatic image development and a method for producing the toner for electrostatic image development. More specifically, the present invention relates to a toner for electrostatic image development that exhibits excellent storage stability and is capable of low-temperature fixation, and a method for producing the toner for electrostatic image development. Background Art
[0002] In the past, in printers and copiers using electronic photography, it was required to reduce the fixing temperature and shorten the standby time from the viewpoint of energy saving. Along with this, the colorant used is required to have excellent low-temperature fixing performance. If the melting point of the resin is lowered in order to improve the low-temperature fixing performance, the glass transition temperature of the colorant decreases and the storage stability deteriorates. Patent document 1 proposes a method that prevents the glass transition temperature from decreasing by performing a heat treatment when manufacturing the colorant. In addition, patent document 2 proposes a method that combines low-temperature fixing performance and storage stability by pulverizing the colorant and classifying it to form a core-shell structure.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-139752
[0006] Patent Document 2: Japanese Patent Application Publication No. 2015-157715 Summary of the invention
[0007] Here, in order to obtain low-temperature fixability, the use of crystalline resins with sharp melting properties is being studied. However, especially for toners obtained through the process of cooling and solidifying after kneading and then pulverizing and classifying, when the amorphous resin and the crystalline resin are melt-kneaded, if the amorphous resin and the crystalline resin are polyesters, etc., the glass transition temperature will drop significantly and the storage stability will easily deteriorate. If the dispersibility of the amorphous resin and the crystalline resin decreases, the charge of the toner will easily become uneven. In addition, if the glass transition temperature decreases, the toner will easily stick during storage. In addition, the methods described in Patent Documents 1 to 2 require new equipment, and the productivity is likely to decrease, and the cost will increase. Therefore, a toner that can use existing equipment and take into account both low-temperature fixability and storage stability is needed.
[0008] The present invention has been made in view of such conventional problems, and an object of the present invention is to provide a toner for electrostatic image development and a method for producing the toner for electrostatic image development which can utilize existing equipment and can achieve both low-temperature fixability and storage stability.
[0009] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that the molecular weight of the crystalline polyester resin and the carbon chains of the diol and dicarboxylic acid monomer molecules constituting the crystalline polyester resin affect the low-temperature fixability and storage stability. The present inventors have also found that the above-mentioned problems can be solved by adding a predetermined amount of a crystalline polyester resin of a predetermined molecular weight containing sebacic acid as an acid component and 1,10-decanediol as an alcohol component to toner particles, thereby completing the present invention.
[0010] A toner for electrostatic image development according to one embodiment of the present invention for solving the above-mentioned problems comprises toner particles and an external additive, wherein the toner particles comprise a binder resin containing a crystalline polyester resin, a colorant and a release agent, wherein the crystalline polyester resin comprises sebacic acid as an acid component, comprises 1,10-decanediol as an alcohol component, has a mass average molecular weight of 3000 to 5000 and is contained in the toner particles in an amount of 5 to 10% by mass.
[0011] A method for producing a toner for electrostatic image development according to one aspect of the present invention for solving the above-mentioned problems is the method for producing the above-mentioned toner for electrostatic image development, comprising the steps of cooling and solidifying after kneading, and then pulverizing and classifying for production. DETAILED DESCRIPTION
[0012] <Toner for electrostatic image development>
[0013] The electrostatic image developing toner (hereinafter also referred to as toner) of one embodiment of the present invention comprises toner particles and an external additive. The toner particles comprise a binder resin containing a crystalline polyester resin, a colorant, and a release agent. The crystalline polyester resin comprises sebacic acid as an acid component and 1,10-decanediol as an alcohol component, and has a mass average molecular weight of 3000 to 5000, and contains 5 to 10% by mass in the toner particles. In addition, the toner is used in an image forming method in an electronic photography method, and can be a two-component toner used with a carrier, or a single-component toner without a carrier. Each is described below.
[0014] (Toner particles)
[0015] The toner particles contain a binder resin including a crystalline polyester resin, a colorant, and a releasing agent.
[0016] Binder resin
[0017] The binder resin is blended for the purpose of dispersing the colorant contained in the toner and, in the fixing process during printing, being melted on the surface of the recording medium by the heat of the fixing roller and then solidified, thereby fixing the colorant on the surface of the recording medium.
[0018] As the binder resin, the crystalline polyester resin of the present embodiment and a binder resin other than the crystalline polyester resin of the present embodiment are used in combination.
[0019] The crystalline polyester resin of the present embodiment is blended to improve both low-temperature fixing property and storage stability of the toner. The crystalline polyester resin of the present embodiment contains sebacic acid as an acid component and 1,10-decanediol as an alcohol component.
[0020] By including 1,10-decanediol as the alcohol component, both the low-temperature fixing property and the storage stability of the obtained toner can be improved.
[0021] The mass average molecular weight of the crystalline polyester resin is preferably 3000 or more. In addition, the mass average molecular weight of the crystalline polyester resin is preferably 5000 or less. When the mass average molecular weight is less than 3000, the storage stability of the toner is likely to decrease. On the other hand, when the mass average molecular weight exceeds 5000, the low temperature fixing property of the toner is likely to decrease.
[0022] In the toner particles, the content of the crystalline polyester resin is preferably 5% by mass or more. In addition, in the toner particles, the content of the crystalline polyester resin is preferably 10% by mass or less. When the content is less than 5% by mass, the low-temperature fixing property of the toner is poor. On the other hand, when the content exceeds 10% by mass, the storage stability of the toner is poor.
[0023] The melting point of the crystalline polyester resin is not particularly limited. As an example, the melting point is preferably above 70°C. In addition, the melting point is preferably below 76°C. By making the melting point within the above range, the fixing property of the colorant becomes good. It should be noted that, in this embodiment, the melting point can be calculated by measuring the melting temperature in thermal analysis using a differential scanning calorimeter. The binder resin is not particularly limited.
[0024] The method for producing the crystalline polyester resin is not particularly limited, and the crystalline polyester resin can be produced by a conventional polyester polymerization method in which an acid component and an alcohol component are reacted. Examples of the method include direct polycondensation and transesterification.
[0025] The manufacture of crystalline polyester resin can be carried out within the polymerization temperature range of 180°C to 230°C. If necessary, the reaction system is set to a reduced pressure, and the reaction is carried out while removing water and alcohol produced during condensation. When the monomer is insoluble or incompatible at the reaction temperature, a high-boiling point solvent can be added as a dissolving aid to dissolve it. In the polycondensation reaction, the dissolving auxiliary solvent is distilled off while the reaction is carried out. In the copolymerization reaction, when there are monomers with poor compatibility, it is preferred to pre-condense the monomers with poor compatibility with an acid or alcohol that is intended to be polycondensed with the monomer, and then polycondense them together with the main component.
[0026] Examples of the catalyst that can be used when producing the crystalline polyester resin include alkali metal compounds such as sodium and lithium; alkaline earth metal compounds such as magnesium and calcium; metal compounds such as zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous oxide compounds, phosphorus oxide compounds, and amine compounds. Specifically, the following compounds can be mentioned.
[0027] Examples thereof include sodium acetate, sodium carbonate, lithium acetate, lithium carbonate, calcium acetate, calcium stearate, magnesium acetate, zinc acetate, zinc stearate, zinc naphthenate, zinc chloride, manganese acetate, manganese naphthenate, titanium tetraethoxide, titanium tetrapropoxide, titanium tetraisopropoxide, titanium tetrabutoxide, antimony trioxide, triphenyl antimony, tributyl antimony, tin formate, tin oxalate, tetraphenyltin, dibutyltin dichloride, dibutyltin oxide, diphenyltin oxide, zirconium tetrabutoxide, zirconium naphthenate, zirconyl carbonate, zirconyl acetate, zirconyl stearate, zirconyl octoate, germanium oxide, triphenyl phosphite, tris(2,4-tert-butylphenyl)phosphite, ethyltriphenylphosphonium bromide, triethylamine, and triphenylamine.
[0028] The binder resin that can be used in combination with the crystalline polyester resin of the present embodiment is not particularly limited. As an example, the binder resin is a styrene copolymer such as polystyrene, styrene-methyl acrylate copolymer, styrene-acrylonitrile copolymer, a polyester resin other than the crystalline polyester resin of the present embodiment, an epoxy resin, and other resin materials. These binder resins can also be used in combination. Among these, as the binder resin used in combination, polyester is preferred from the perspective of being easy to color and obtaining a toner with a bright color.
[0029] The binder resin of the present embodiment preferably contains a non-crystalline resin among the above-mentioned resin materials. In addition, the non-crystalline resin is preferably a resin having a mass average molecular weight of 4000 to 150000 and a softening point of 95 to 125°C. The mass average molecular weight is preferably above 4000, and more preferably above 5000. In addition, the mass average molecular weight is preferably below 150000, and more preferably below 12000. The softening point is preferably above 90°C, and more preferably above 95°C. In addition, the softening point is preferably below 125°C, and more preferably below 120°C. By making the mass average molecular weight and the softening point within the above range, the obtained toner shows excellent low-temperature fixing property and storage stability. It should be noted that, in the present embodiment, the mass average molecular weight can be obtained, for example, by measuring with gel permeation chromatography (GPC) and converting to polystyrene. As an apparatus for measuring the mass average molecular weight in terms of polystyrene by GPC, for example, Water 2690 (manufactured by Waters Corporation) is mentioned, and as a chromatographic column, PLgel 5 μL MIXED-D (manufactured by Polymer Laboratories Inc.) is mentioned, etc. The softening point can be measured in accordance with ASTM E28-92.
[0030] The content of the binder resin other than the crystalline polyester resin of the present embodiment is not particularly limited. As an example, the content of the binder resin is preferably 75% by mass or more in the toner. In addition, the content of the binder resin is preferably 85% by mass or less in the toner. By making the content of the binder resin within the above range, the obtained toner can easily disperse the colorant appropriately and is easy to fix on the recording medium.
[0031] Colorants
[0032] The colorant is blended to provide coloring power to the toner.
[0033] The colorant is not particularly limited. For example, the colorant is a colorant such as magnetic powder that exhibits black color, such as carbon black; a colorant that exhibits cyan color, such as copper phthalocyanine, methylene blue, Victoria blue, etc.; a colorant that exhibits magenta color, such as rhodamine dye, dimethylquinacridone, dichloroquinacridone, carmine, etc.; a colorant that exhibits yellow color, such as benzidine yellow, chrome yellow, naphthol yellow, diazo yellow, etc. The colorants may be used in combination.
[0034] The content of the colorant is not particularly limited. For example, in the toner, relative to 100 parts by mass of the binder resin, the content of the colorant is preferably used in an amount of 0.1 parts by mass or more and 30 parts by mass or less. It should be noted that a masterbatch in which a high concentration of pigment is pre-dispersed in a resin is commercially available, so the masterbatch can be purchased for use as a colorant. In this case, the concentration of the pigment contained in the masterbatch can be considered to determine its usage, so that the concentration of the pigment contained in the toner is within the above range.
[0035] Release agent
[0036] The release agent is not particularly limited, and various well-known waxes can be used. If one example is given, for example: polyolefin waxes such as polyethylene wax and polypropylene wax; branched hydrocarbon waxes such as microcrystalline wax, paraffin wax, and long-chain hydrocarbon waxes such as sasol wax; dialkyl ketone waxes such as distearyl ketone; carnauba wax, montan wax, behenyl behenate, trimethylolpropane tribehenyl ester, pentaerythritol tetrabehenyl ester, pentaerythritol diacetate dibehenyl ester, glycerol tribehenyl ester, 1,18-octadecanediol distearate, trimellitic acid tristearate, maleic acid distearate and other ester waxes; amide waxes such as ethylene bisbehenamide and trimellitic acid tristearate amide, etc. The release agent can be used in combination. Among these, the release agent is preferably an ester wax and a hydrocarbon wax.
[0037] The content of the release agent is not particularly limited. As an example, the content of the release agent can usually be set in the range of 1 to 30 parts by mass, preferably in the range of 5 to 20 parts by mass, relative to 100 parts by mass of the binder resin. The content of the release agent in the colorant particles is preferably in the range of 3 to 15% by mass. By making the content of the release agent within the above range, the obtained toner can obtain good releasability between the fixing roller and the printing surface during the fixing process during printing. In addition, the toner is not easy to ooze out the release agent, and poor charging, filming, etc. are not easy to occur.
[0038] Other ingredients
[0039] The toner particles may include, in addition to the above, a charge adjusting agent, etc. The charge adjusting agent is preferably blended in order to adjust the charge amount of the toner.
[0040] The charge adjuster is not particularly limited. For example, the charge adjuster is a metal complex such as aniline black, basic dyes, monoazo dyes; a salt or complex of a carboxylic acid such as salicylic acid and dicarboxylic acid with a metal such as chromium, zirconium, aluminum, etc.; an organic dye; a metal salt of cyclohexane acid and a higher fatty acid; a resin-type charge adjuster such as an alkoxylated amine, a quaternary ammonium salt compound, and an aromatic polycondensate. The charge adjusters can be used in combination. Among these, from the perspective of charge stability, it is preferred that the toner contains a resin-type charge adjuster.
[0041] The content of the charge adjusting agent is not particularly limited. For example, the toner particles may not contain the charge adjusting agent, and the content of the charge adjusting agent is preferably 0.5% by mass or more. In addition, the content of the charge adjusting agent is preferably 8% by mass or less in the toner particles. By making the content of the charge adjusting agent within the above range, the chargeability of the obtained toner is more excellent.
[0042] (External Additives)
[0043] The external additive is added to improve the charging characteristics of the toner particles by adhering to the surface of the toner particles, or to improve the fluidity of the toner or improve the printability by existing in a state separated from the toner particles.
[0044] There is no particular limitation on the external additive. For example, the external additive is negatively charged lubricant particles, positively charged lubricant particles, inorganic oxide particles, etc. The external additives may also be used in combination. The external additive may be appropriately selected and used according to the type of equipment and purpose.
[0045] The positively charged lubricant particles are lubricant particles that are positively charged by friction with a carrier or a charged sheet. Such lubricant particles are well known, and metal salt particles of fatty acids can be preferably exemplified. As an example of such metal salts of fatty acids, zinc stearate, aluminum stearate, calcium stearate, magnesium stearate, zinc laurate, zinc myristate, zinc palmitate, zinc oleate, etc. can be preferably cited, among which zinc stearate and magnesium stearate are more preferably cited. The positively charged lubricant particles can be a single type or a combination of two or more.
[0046] Negatively charged lubricant particles are negatively charged lubricant particles due to frictional charging with a carrier or a charged sheet. Such lubricant particles are well known, and preferably polytetrafluoroethylene (PTFE), silicone, boron nitride, polymethyl methacrylate (PMMA), polyvinylidene fluoride can be exemplified, and among them, boron nitride and polytetrafluoroethylene (PTFE) are more preferably exemplified. Negatively charged lubricant particles can be a single type or a combination of two or more.
[0047] The inorganic oxide particles are not particularly limited. For example, the inorganic oxide particles are silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, zinc oxide, chromium oxide, cerium oxide, antimony oxide, tungsten oxide, tin oxide, tellurium oxide, manganese oxide, boron oxide, etc. The inorganic oxide particles may be used in combination. Among these, silicon dioxide and titanium dioxide are preferred from the perspective of excellent fluidity and excellent charging properties of the toner.
[0048] The inorganic oxide particles are preferably surface treated with hydrophobic treatment. The method of hydrophobic treatment is not particularly limited. If an example is given, the method of hydrophobic treatment is the following method: the surface of the inorganic oxide particles before the existing known hydrophobic treatment agent is contacted with the hydrophobic treatment agent, so that the hydrophobic functional group, component chemical bonding or the method of adhering to the surface of the inorganic oxide particles. The hydrophobic treatment agent for hydrophobic treatment of inorganic oxide particles is not particularly limited. If an example is given, the hydrophobic treatment agent is octyl triethoxy silane, polydimethylsiloxane, dimethyl dichlorosilane, hexamethyldisilazane, etc. The hydrophobic treatment agent can also be used in combination.
[0049] The amount of the external additive added in this embodiment (when using multiple external additives, the total amount added) is preferably in the range of 0.05 to 5 parts by mass, and more preferably in the range of 0.1 to 3 parts by mass relative to 100 parts by mass of the toner. By making the content of the external additive within the above range, the fluidity, charging property, cleaning property, etc. of the obtained toner become good.
[0050] In summary, the toner of the present embodiment includes a crystalline polyester resin as described above, the crystalline polyester resin includes sebacic acid as an acid component, includes 1,10-decanediol as an alcohol component, has a mass average molecular weight of 3000 to 5000, and includes 5 to 10% by mass in the binder resin. This toner can achieve both excellent low-temperature fixability and storage stability.
[0051] <Method for producing toner for electrostatic image development>
[0052] The manufacturing method of the electrostatic image developing toner (hereinafter also referred to as the manufacturing method of the toner) according to one embodiment of the present invention is a manufacturing method for manufacturing the electrostatic image developing toner, which includes the steps of cooling and solidifying after kneading, and then pulverizing and classifying. It should be noted that the above steps are all steps used in the conventionally known toner manufacturing method. That is, the manufacturing method of the toner according to the present embodiment can produce the toner by the conventionally known method using the conventionally known manufacturing device.
[0053] More specifically, first, in the kneading process, each component of the toner particles is melt-kneaded to prepare a kneaded product. The mixing of each component can use various existing known mixing devices (such as double cone mixer, V-type mixer, drum mixer, super mixer, Henschel mixer, Nauta mixer, Mechano Hybrid (manufactured by COKE Industries, Ltd., Japan) etc.). In melt kneading, intermittent kneading machines such as pressure kneading machines and Banbury mixers or continuous kneading machines can be used. From the advantage of continuous production, single screw or twin screw extruders have become the mainstream. For example, KTK type twin screw extruder (manufactured by Kobe Steel Co., Ltd.), TEM type twin screw extruder (manufactured by Toshiba Machine Co., Ltd.), PCM kneader (manufactured by Ikegai Co., Ltd.), twin screw extruder (manufactured by KCK Co., Ltd.), Ko-Kneader (manufactured by BUSS Co., Ltd.), Kneadex (manufactured by COKE Industries, Ltd., Japan) etc. can be listed. It should be noted that as the toner material, a masterbatch containing the above-mentioned binder resin and a colorant can be used.
[0054] The kneaded material is then cooled and then pulverized (for example, coarsely pulverized using a crusher, hammer mill, or a pulverizer such as Feather, and then finely pulverized using, for example, a Kryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), a super rotor (manufactured by Nisshin Engineering Co., Ltd.), a turbine mixer (manufactured by Freund Turbo Co., Ltd.), or a jet-based fine pulverizer). The powder (pulverized material) obtained by the pulverization step is classified (for example, using a classifier or sifter such as Elbow Jet (manufactured by Nippon Steel Mining Co., Ltd.) of an inertial classification method, Turbo Plex (manufactured by Hosokawa Micron Co., Ltd.) of a centrifugal classification method, TSP separator (manufactured by Hosokawa Micron Co., Ltd.), or Faculty (manufactured by Hosokawa Micron Co., Ltd.)). The volume median particle size (D50) of the toner particles after pulverization and classification is preferably 4 to 10 μm. It should be noted that, in the present embodiment, the volume median particle diameter (D50) is also referred to as the median diameter of the volume basis, which is a value indicating that the volume sum of particles with a diameter less than this value and the volume sum of particles with a diameter greater than this value each account for 50% of the total volume. The volume median particle diameter (D50) can be calculated by performing a particle size distribution measurement. The particle size distribution measuring device can be listed as the "Multisizer 3" manufactured by Beckman Coulter.
[0055] As described above, the manufacturing method of the toner of the present embodiment does not require special equipment, and the toner can be manufactured using the same equipment as the existing equipment. As described above, the obtained toner can take into account both excellent low-temperature fixability and storage stability. Therefore, according to this manufacturing method, the high cost of the toner can be prevented.
[0056] One embodiment of the present invention has been described above. The present invention is not particularly limited to the above embodiment. It should be noted that the above embodiment mainly describes the invention having the following configurations.
[0057] (1) A toner for electrostatic image development, comprising toner particles and an external additive, wherein the toner particles comprise a binder resin containing a crystalline polyester resin, a colorant, and a release agent, wherein the crystalline polyester resin comprises sebacic acid as an acid component and 1,10-decanediol as an alcohol component, has a mass average molecular weight of 3000 to 5000, and is contained in the toner particles in an amount of 5 to 10% by mass.
[0058] According to such a configuration, the obtained electrostatic image developing toner can achieve both low-temperature fixability and storage stability.
[0059] (2) The electrostatic image developing toner according to (1), wherein the melting point of the crystalline polyester resin is 70 to 76°C.
[0060] According to such a configuration, the low-temperature fixing property of the electrostatic image developing toner becomes good.
[0061] (3) The electrostatic image developing toner according to (1) or (2), wherein the binder resin comprises an amorphous resin, and the amorphous resin has a mass average molecular weight of 4,000 to 150,000 and a softening point of 90 to 125°C.
[0062] According to such a configuration, the electrostatic image developing toner can achieve both excellent low-temperature fixability and storage stability.
[0063] (4) The electrostatic image developing toner according to any one of (1) to (3), further comprising a resin type charge adjusting agent.
[0064] According to such a configuration, the electrostatic image developing toner has a more excellent charging property.
[0065] (5) A method for producing a toner for electrostatic image development, which is the method for producing a toner for electrostatic image development according to any one of (1) to (4), comprising the steps of cooling and solidifying after kneading, and then pulverizing and classifying for production.
[0066] According to this structure, the obtained electrostatic image developing toner can take into account both low-temperature fixability and storage stability. In addition, the electrostatic image developing toner can be manufactured using the same equipment as the existing equipment. Therefore, according to this manufacturing method, the high cost of the toner can be prevented.
[0067] Example
[0068] The present invention is described in more detail below by way of examples. The present invention is not limited by these examples. It should be noted that, unless otherwise specified, "%" means "mass %" and "parts" means "parts by mass".
[0069] The raw materials used and the production methods are shown below.
[0070] <Binder resin>
[0071] Crystalline polyester resin
[0072] Crystalline polyester resin 1: polyester of sebacic acid and 1,10-decanediol. Mass average molecular weight 3000, melting point 74°C.
[0073] Crystalline polyester resin 2: polyester of sebacic acid and 1,10-decanediol. Mass average molecular weight 5000, melting point 74°C.
[0074] Crystalline polyester resin 3: polyester of sebacic acid and 1,10-decanediol. Mass average molecular weight 5000, melting point 75°C.
[0075] Crystalline polyester resin 4: polyester of sebacic acid and 1,6-hexanediol. Mass average molecular weight: 2600, melting point: 66°C.
[0076] Crystalline polyester resin 5: polyester of sebacic acid and 1,6-hexanediol. Mass average molecular weight 5000, melting point 67°C.
[0077] Crystalline polyester resin 6: polyester of sebacic acid and 1,6-hexanediol. Mass average molecular weight: 10,000, melting point: 69°C.
[0078] Crystalline polyester resin 7: polyester of sebacic acid and 1,10-decanediol. Mass average molecular weight: 10,000, melting point: 74°C.
[0079] Crystalline polyester resin 8: polyester of 1,12-dodecanedioic acid and 1,6-hexanediol. Mass average molecular weight 3500, melting point 71°C.
[0080] Crystalline polyester resin 9: polyester of 1,12-dodecanedioic acid and 1,10-decanediol. Mass average molecular weight 3000, melting point 78°C.
[0081] · Non-crystalline binder resin used in combination
[0082] Non-crystalline binder 1: Commercially available non-crystalline polyester resin (Tg 64°C, molecular weight 5500)
[0083] Amorphous binder 2: Commercially available amorphous polyester resin (Tg 65°C, molecular weight 110,000)
[0084] <Charge adjuster>
[0085] Trade name Copy Charge N5P-01 (manufactured by Clariant Chemicals)
[0086] <Coloring agent>
[0087] Carbon Black
[0088] <Mold release agent>
[0089] Release agent 1: fatty acid ester wax (melting point 69°C)
[0090] Release agent 2: hydrocarbon wax
[0091] <External Additives>
[0092] External additive 1: Silica particles surface treated with silicone oil (particle size: 22 nm)
[0093] External additive 2: Silica particles surface treated with dimethyldichlorosilane (particle size 12 nm)
[0094] External additive 3: Titanium oxide particles surface-treated with alkylsilane (particle size 14 nm)
[0095] <Examples 1 to 4, Comparative Examples 1 to 14>
[0096] (Preparation of Toner)
[0097] According to the mass ratio (mass %) shown in Table 1 below, crystalline polyester resin, commercial polyester resin (Tg 64°C, molecular weight 5500, amorphous), commercial polyester resin (Tg 65°C, molecular weight 110,000, amorphous), fatty acid ester wax (melting point 69°C), hydrocarbon wax, charge control agent, and carbon black were mixed with a Henschel mixer and then melt-kneaded with a twin-screw kneader. The obtained kneaded product was coarsely pulverized with a Rotoplex, finely pulverized with a jet mill, and classified with a wind classifier to obtain a toner masterbatch with a charged volume average particle size of 6.5 μm. To 100 parts by mass of the toner masterbatch, 1.0% of silica particles surface-treated with silicone oil (particle size: 22 nm), 0.5% of silica particles surface-treated with dimethyldichlorosilane (particle size: 12 nm), and 0.5% of titanium oxide particles surface-treated with alkylsilane (particle size: 14 nm) were added, and the mixture was stirred for 10 minutes using a Henschel mixer to obtain the toner of the embodiment and the comparative example.
[0098]
Table 1
[0099] Table 1
[0100]
[0101] With respect to the toners of Examples and Comparative Examples obtained above, printed materials were produced under the following conditions, and the fixing property, release property, and storage stability were evaluated.
[0102] <Evaluation of Fixing Rate>
[0103] A non-magnetic two-component negatively charged printer was used for evaluation. The printer was placed on plain paper (80 g / m 2 ) was printed on a solid image, and a friction test was performed on the solid image using a Gakushin type friction fastness tester (NR-100 manufactured by Daiei Kagaku Seiki Seisakusho Co., Ltd.) under the following conditions. The image density before and after friction was measured using a reflection densitometer (manufactured by Macbeth Co., Ltd.), and the fixing rate was calculated by the following formula.
[0104] Friction surface: Nonwoven fabric (manufactured by Honeylon Co., Ltd., trade name COTTON PADS)
[0105] Load: 500g
[0106] Reciprocating times: 5 times
[0107] Horizontal reciprocating distance: 10cm
[0108] Fixing rate (%): (image density after rubbing / image density before rubbing) × 100
[0109] ○: The fixing rate is 85% or more.
[0110] △: The fixing rate is 80% or more and less than 85%.
[0111] ×: The fixing rate is less than 80%.
[0112] <Evaluation of paper edge fixability (N / N environment)>
[0113] Using a non-magnetic two-component negatively charged printer for evaluation, 10 sheets of a solid image with 100% coverage were continuously printed in an environment of a temperature of 25° C. and a humidity of 50%.
[0114] ○: No peeling occurred due to scratching of the image in the center and all parts to the edge of the paper.
[0115] △: Only the edge of the paper peeled off due to scratching the image.
[0116] ×: The image was scratched and peeled off at both the center and the edge of the paper.
[0117] <Evaluation of paper edge fixability (L / L environment)>
[0118] Using a non-magnetic two-component negatively charged printer for evaluation, 10 sheets of a solid image with 100% coverage were continuously printed in an environment of a temperature of 10° C. and a humidity of 20%.
[0119] ○: No peeling occurred due to scratching of the image in the center and all parts to the edge of the paper.
[0120] △: Only the edge of the paper peeled off due to scratching the image.
[0121] ×: The image was scratched and peeled off at both the center and the edge of the paper.
[0122] <Evaluation of mold release properties>
[0123] A non-magnetic two-component negatively charged printer was used for evaluation to print a full-print image with 100% coverage on plain paper (64 g / m2), which was then wound onto a fixer to evaluate the peeling marks of the fixer roller and the occurrence of offset dirt.
[0124] ○: The film was wound around the fuser, and there was no peeling mark from the fuser roller or offset stain.
[0125] ×: When the film was wound around the fixing device, either peeling marks of the fixing roller or offset stains occurred.
[0126] <Storage stability 50℃ / 8 hours>
[0127] 20 g of toner was placed in a sealed plastic container and stored at 50°C for 8 hours, and then evaluated using a powder tester (manufactured by Hosokawa Micron Co., Ltd.). Sieve A (mesh size 355 μm), sieve B (mesh size 250 μm), and sieve C (mesh size 150 μm) were stacked in order from the top, 20 g of toner was placed in sieve A, and the sieve was vibrated at an amplitude of 1 mm for 30 seconds, and the weight of the remaining toner was measured.
[0128] The degree of aggregation calculated as follows was evaluated.
[0129] Aggregation degree %: (toner remaining on sieve A (g) + toner remaining on sieve B (g) × 0.6 + toner remaining on sieve A (g) × 0.2) / 20 × 100
[0130] ○: The degree of aggregation is less than 10%.
[0131] △: The degree of aggregation is 10% or more and less than 20%.
[0132] ×: The degree of aggregation is 20% or more.
[0133] <Storage stability 55℃ / 8 hours>
[0134] 20 g of toner was placed in a sealed plastic container and stored at 55°C for 8 hours, and then evaluated using a powder tester (manufactured by Hosokawa Micron Co., Ltd.). Sieve A (mesh size 355 μm), sieve B (mesh size 250 μm), and sieve C (mesh size 150 μm) were stacked in order from the top, 20 g of toner was placed in sieve A, and the sieve was vibrated at an amplitude of 1 mm for 30 seconds, and the weight of the remaining toner was measured.
[0135] The degree of aggregation calculated as follows was evaluated.
[0136] Aggregation degree %: (toner remaining on sieve A (g) + toner remaining on sieve B (g) × 0.6 + toner remaining on sieve A (g) × 0.2) / 20 × 100
[0137] ○: The degree of aggregation is less than 10%.
[0138] △: The degree of aggregation is 10% or more and less than 20%.
[0139] ×: The degree of aggregation is 20% or more.
[0140] As shown in Table 1, the toners of Examples 1 to 4 are excellent in fixability, offset printing and storage stability. On the other hand, the toners of Comparative Examples 1 to 8 using crystalline polyesters containing alcohol components with a small carbon number do not have both fixability and storage stability. The toner of Comparative Example 9 using a crystalline polyester with a large molecular weight has poor fixability at the edge of a paper in an environment of a temperature of 10°C and a humidity of 20%. The toners of Comparative Examples 10 and 11 using crystalline polyesters containing carboxylic acid components with a large carbon number and alcohol components with a small carbon number do not have both fixability and storage stability. In addition, the toner of Comparative Example 12 using a crystalline polyester containing carboxylic acid components with a large carbon number and alcohol components with a large carbon number has poor fixability at the edge of a paper in an environment of a temperature of 10°C and a humidity of 20%. In addition, the toner of Comparative Example 13 having a small content of the crystalline polyester resin of the present invention has poor fixability, and the toner of Comparative Example 14 having a large content has poor storage stability.
Claims
1. A toner for electrostatic image development, comprising toner particles and an external additive, The toner particles include a binder resin including a crystalline polyester resin, a colorant, and a release agent, The crystalline polyester resin: Contains sebacic acid as an acid component and 1,10-decanediol as an alcohol component, The mass average molecular weight is 3000-5000, The content of the toner particles is 5 to 10% by mass.
2. The electrostatic image developing toner according to claim 1, wherein The melting point of the crystalline polyester resin is 70 to 76°C.
3. The electrostatic image developing toner according to claim 1 or 2, wherein The binder resin includes a non-crystalline resin, The amorphous resin has a mass average molecular weight of 4,000 to 150,000 and a softening point of 90 to 125°C. 4 . The electrostatic image developing toner according to claim 1 , further comprising a resin type charge adjusting agent.
5. A method for producing a toner for electrostatic image development, the method for producing a toner for electrostatic image development according to any one of claims 1 to 4, The production process includes the steps of cooling and solidifying after kneading, and then pulverizing and classifying.
Citation Information
Patent Citations
Method of manufacturing toner for electrostatic image development
JP2010139752A
Dispersion solution and manufacturing method therefor, manufacturing method of coating liquid and mesoporous silica porous film
JP2015157715A
Toner for development of electrostatic image, method of producing the same, electrostatic image developer, toner cartridge, process cartridge, and image forming apparatus
CN101174112A
Electrostatic charge image developing toner, electrostatic charge image developer, toner cartridge, process cartridge, image forming device, and image forming method
JP2014063065A
Toner for electrostatic charge image development and production method of the same, and image forming method
JP2015001590A