Dicing tape and dicing die-bonding film
By optimizing the dynamic viscoelastic performance and layer structure of the cutting tape, the problem of cutting tape rupture at low temperature is solved, stable cutout in semiconductor integrated circuit manufacturing is achieved, and the reliability of the process is improved.
Patent Information
- Application Number
- CN202010563428.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-26
- Filing Date
- 2020-06-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-06-19
AI Technical Summary
The existing cutting tape is prone to rupture under low temperature conditions, resulting in poor cutting during semiconductor integrated circuit manufacturing, affecting the normal progress of subsequent processes.
By adjusting the dynamic viscoelastic measurement results of the cutting tape, the ratio of Tanδ value at -15°C to Tanδ value at -5°C is above 0.75, and the optimization design is carried out on the substrate layer and the adhesive layer to ensure that The 25% tensile strength at -15°C reaches 15 [N/20mm] or above, and the thickness of the substrate layer and the adhesive layer is controlled to suppress rupture.
It effectively suppresses the rupture of the cutting belt in the expansion process at low temperature, improves the wafer cutting ability, and ensures the stability and efficiency of the semiconductor integrated circuit manufacturing process.
Smart Images

Figure BDA0002546874250000271 
Figure HDA0002546874260000011 
Figure HDA0002546874260000021
Abstract
Description
Technical Field
[0001] The present invention relates to a dicing tape used, for example, when manufacturing a semiconductor integrated circuit, and a dicing die-bonding film including the dicing tape. Background Art
[0002] In the past, there is a known dicing die bonding film used in the manufacture of semiconductor integrated circuits. Such a dicing die bonding film, for example, comprises a dicing tape and a die bonding layer laminated on the dicing tape and bonded to a wafer. The dicing tape comprises a base material layer and an adhesive layer in contact with the die bonding layer. Such a dicing die bonding film is used in the manufacture of semiconductor integrated circuits, for example, as described below.
[0003] The method of manufacturing a semiconductor integrated circuit generally includes a front process of forming a circuit surface on one side of a wafer using a highly integrated electronic circuit, and a back process of cutting out chips from the wafer with the circuit surface formed thereon and assembling them.
[0004] The post-process includes, for example, the following processes: a mounting process, attaching the surface of the wafer on the opposite side to the circuit surface to the chip bonding layer, and fixing the wafer to the dicing tape; a dicing process, cutting the wafer attached to the dicing tape by the chip bonding layer into small chips (die) and dicing; an expansion process, expanding the interval between the diced chips; a pick-up process, peeling between the chip bonding layer and the adhesive layer, and taking out the chip (die) attached to the chip bonding layer; and a chip bonding process, bonding the chip (die) attached to the chip bonding layer to the adherend. Semiconductor integrated circuits are manufactured through these processes.
[0005] In the above manufacturing method, the expansion process is to cut the wafer and the chip bonding layer together and into small pieces by stretching the dicing tape in a radial direction under low temperature conditions, such as below 0°C, while the wafer is arranged on the chip bonding layer overlapping the dicing tape. However, there are cases where the dicing tape breaks as it is stretched. Once the dicing tape breaks, the cutting will become poor, and obstacles will occur in the subsequent picking process. In order to prevent such problems, it is urgently desired that the dicing tape has the ability to suppress the breakage in the expansion process at low temperatures.
[0006] As a conventional dicing tape that copes with the problem in the expansion process, for example, a dicing tape having a storage elastic modulus E' at 25° C. measured at a frequency of 10 Hz of 3 to 5 GPa is known (Patent Document 1).
[0007] The dicing tape described in Patent Document 1 can suppress the lifting that occurs between the die-bonding layer and the adhesive layer in the expansion step at room temperature and the subsequent steps.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-195746 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] However, it cannot be said that sufficient research has been conducted on dicing die-bonding films and dicing tapes that suppress cracking in an expansion process at a low temperature.
[0013] Therefore, an object of the present invention is to provide a dicing tape and a dicing die-bonding film in which cracks are suppressed in an expansion process at a low temperature.
[0014] Solutions for solving problems
[0015] In order to solve the above-mentioned problems, the cutting tape of the present invention is characterized in that, with respect to the ratio (E" / E') of the storage modulus E' and the loss modulus E" measured by dynamic viscoelasticity measurement, i.e., Tanδ, the ratio (A / B) of the Tanδ value (A) at -15°C to the Tanδ value (B) at -5°C is greater than 0.75.
[0016] According to the dicing tape having the above-described structure, cracking in the expansion step at a low temperature is suppressed.
[0017] The dicing tape preferably has a strength of 15 [N / 20 mm] or more at 25% tension at -15° C. This can improve the wafer dividing property in the expansion step at a low temperature.
[0018] The dicing tape preferably includes a base layer and an adhesive layer having higher adhesiveness than the base layer, and the base layer preferably has a thickness of 80 μm to 150 μm. This can further suppress cracking in the expansion step at low temperature.
[0019] In the dicing tape, it is preferable that the thickness of the adhesive layer is 5 μm or more and 40 μm or less. This can further suppress cracking in the expansion step at a low temperature.
[0020] The dicing die-bonding film of the present invention includes the dicing tape described above and a die-bonding layer bonded to the dicing tape.
[0021] In the dicing die-bonding film, the die-bonding layer may have a thickness of 50 μm to 135 μm. Even in a dicing die-bonding film having such a thick die-bonding layer, cracking of the dicing tape in an expansion step at a low temperature can be suppressed.
[0022] The dicing die-bonding film is preferably used in a cold stretching step of stretching at 0° C. or lower with a wafer bonded to the die-bonding layer, and in the cold stretching step, the wafer is cut together with the die-bonding layer.
[0023] Effects of the Invention
[0024] The dicing tape and dicing die-bonding film of the present invention exhibit an effect of further suppressing cracking in the expansion process at a low temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 : A cross-sectional view of the dicing die-bonding film of the present embodiment cut along the thickness direction.
[0026] Figure 2A : A cross-sectional view schematically showing a half-cutting process in a method for manufacturing a semiconductor integrated circuit.
[0027] Figure 2B : A cross-sectional view schematically showing a half-cutting process in a method for manufacturing a semiconductor integrated circuit.
[0028] Figure 2C : A cross-sectional view schematically showing a half-cutting process in a method for manufacturing a semiconductor integrated circuit.
[0029] Figure 2D : A cross-sectional view schematically showing a half-cutting process in a method for manufacturing a semiconductor integrated circuit.
[0030] Figure 3A : A cross-sectional view schematically showing a mounting step in a method for manufacturing a semiconductor integrated circuit.
[0031] Figure 3B : A cross-sectional view schematically showing a mounting step in a method for manufacturing a semiconductor integrated circuit.
[0032] Figure 4A : A cross-sectional view schematically showing a low-temperature expansion process in a method for manufacturing a semiconductor integrated circuit.
[0033] Figure 4B : A cross-sectional view schematically showing a low-temperature expansion process in a method for manufacturing a semiconductor integrated circuit.
[0034] Figure 4C : A cross-sectional view schematically showing a low-temperature expansion process in a method for manufacturing a semiconductor integrated circuit.
[0035] Figure 5A: A cross-sectional view schematically showing an expansion process at room temperature in a method for manufacturing a semiconductor integrated circuit.
[0036] Figure 5B : A cross-sectional view schematically showing an expansion process at room temperature in a method for manufacturing a semiconductor integrated circuit.
[0037] Figure 6 : A cross-sectional view schematically showing a pickup step in a method for manufacturing a semiconductor integrated circuit.
[0038] Description of Reference Numerals
[0039] 1: Cutting die bonding film,
[0040] 10: Chip bonding layer,
[0041] 20: cutting belt,
[0042] 21: base material layer,
[0043] 22: Adhesive layer. DETAILED DESCRIPTION
[0044] Hereinafter, one embodiment of a dicing die-bonding film and a dicing tape of the present invention will be described with reference to the drawings.
[0045] The dicing die-bonding film 1 of the present embodiment includes a dicing tape 20 and a die-bonding layer 10 which is laminated on the adhesive layer 22 of the dicing tape 20 and adhered to the semiconductor wafer.
[0046] The dicing tape 20 of this embodiment is usually a long sheet and is stored in a rolled state until use. The dicing die-bonding film 1 of this embodiment is used by being attached to an annular frame having an inner diameter slightly larger than a silicon wafer to be cut.
[0047] The dicing tape 20 of the present embodiment includes a base layer 21 and a pressure-sensitive adhesive layer 22 superposed on the base layer 21 .
[0048] In the cutting tape 20 of this embodiment, regarding the ratio (E" / E') of the storage modulus E' and the loss modulus E" measured by dynamic viscoelasticity measurement, i.e., Tanδ, the ratio (A / B) of the Tanδ value (A) at -15°C to the Tanδ value (B) at -5°C is greater than 0.75.
[0049] Since the dicing tape 20 of the present embodiment has the above-mentioned structure, cracking in a low-temperature expansion process (described in detail later) is suppressed. Low temperature generally refers to a temperature of 0°C or less.
[0050] The dynamic viscoelasticity measurement of the dicing tape 20 can be carried out according to the method described in the examples. The above-mentioned Tan δ is calculated from the average value of the measurement results obtained by performing the measurement three times.
[0051] It should be noted that the above ratio (A / B) may be 2.00 or less.
[0052] The above ratio (A / B) can be increased by, for example, increasing the value (A) of Tan δ at -15°C.
[0053] For example, the value (A) of Tan δ at -15°C can be increased by blending a material having a glass transition temperature (Tg) closer to -15°C into the dicing tape 20 or increasing the blending amount of the material.
[0054] On the other hand, the above ratio (E" / E') can be reduced by, for example, increasing the value (B) of Tan δ at -5°C.
[0055] For example, the value (B) of Tan δ at -5°C can be increased by blending a material whose glass transition temperature (Tg) is further away from -5°C into the dicing tape 20 or increasing the blending amount of the material.
[0056] The Tan δ value (A) at -15°C is preferably 0.05 or more, more preferably 0.07 or more, and further preferably 0.10 or more. When the Tan δ value (A) is 0.05 or more, there is an advantage that the relaxation property of the dicing tape 20 during stretching at -15°C is further increased.
[0057] The Tan δ value (A) at -15°C is preferably 0.50 or less, more preferably 0.40 or less, and further preferably 0.30 or less. When the Tan δ value (A) is 0.50 or less, there is an advantage that stress during stretching at -15°C can be more efficiently transmitted to the die bond layer 10 .
[0058] The Tan δ value (B) at -5°C is preferably 0.05 or more, more preferably 0.09 or more, and further preferably 0.11 or more. When the Tan δ value (B) is 0.05 or more, there is an advantage that the relaxation property of the dicing tape 20 during stretching at -5°C is further increased.
[0059] The Tan δ value (B) at -5°C is preferably 0.50 or less, more preferably 0.40 or less, and further preferably 0.27 or less. When the Tan δ value (B) is 0.50 or less, there is an advantage that stress during stretching at -5°C can be more efficiently transmitted to the die bond layer 10 .
[0060] The dicing tape 20 preferably has a strength of 15 [N / 20 mm] or more at 25% tension at -15°C. This can improve the wafer dividing property in the expansion step at a low temperature.
[0061] The strength at 25% elongation at -15°C may be 30 [N / 20 mm] or less.
[0062] The above-mentioned strength at 25% elongation is a value measured by the method described in Examples. The above-mentioned strength value is calculated from the average value of the measurement results obtained by performing the measurement three times.
[0063] For example, the strength at 25% tension can be increased by selecting a harder resin as the resin constituting the dicing tape 20 or by further increasing the thickness of the base layer 21. On the other hand, the strength at 25% tension can be reduced by selecting a softer resin as the resin constituting the dicing tape 20 or by further decreasing the thickness of the base layer 21.
[0064] The base material layer 21 may have a single-layer structure or a laminated structure.
[0065] Each layer of the base material layer 21 is, for example, a metal foil, a fiber sheet such as paper or cloth, a rubber sheet, a resin film, or the like.
[0066] Examples of the fiber sheet constituting the base material layer 21 include paper, woven fabric, and nonwoven fabric.
[0067] As the material of the resin film, for example, polyolefins such as polyethylene (PE), polypropylene (PP), and ethylene-propylene copolymers; copolymers of ethylene such as ethylene-vinyl acetate copolymers (EVA), ionomer resins, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylate (random, alternating) copolymers; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyacrylates; polyvinyl chloride (PVC); polyurethane; polycarbonate; polyphenylene sulfide (PPS); polyamides such as aliphatic polyamides and wholly aromatic polyamides (aramid); polyetheretherketone (PEEK); polyimide; polyetherimide; polyvinylidene chloride; ABS (acrylonitrile-butadiene-styrene copolymer); cellulose or cellulose derivatives; silicone-containing polymers; fluorine-containing polymers, etc. These can be used alone or in combination of two or more.
[0068] When the base material layer 21 includes a resin film, the resin film may be subjected to a stretching treatment or the like to control deformability such as elongation.
[0069] The surface of the base material layer 21 may be subjected to a surface treatment to improve adhesion with the adhesive layer 22. As the surface treatment, for example, an oxidation treatment based on a chemical method or a physical method such as chromic acid treatment, ozone exposure, flame exposure, high voltage electric shock exposure, ionizing radiation treatment, etc. may be adopted. In addition, a coating treatment using a coating agent such as an anchor coating agent, a primer, or an adhesive may also be performed.
[0070] The substrate layer 21 preferably comprises at least one selected from ethylene-vinyl acetate copolymer (EVA) resin, α-olefin-based thermoplastic elastomer resin, ethylene-methyl acrylate copolymer (EMA) resin and ionomer resin (IO). Examples of the α-olefin-based thermoplastic elastomer include homopolymers of α-olefins, copolymers of two or more α-olefins, and the like.
[0071] The substrate layer 21 may include a mixture (blend) of a plurality of the above-mentioned resins. For example, the substrate layer 21 may include a mixture of ethylene-vinyl acetate copolymer resin (EVA) and ionomer resin (IO), or may include a mixture of ethylene-vinyl acetate copolymer resin (EVA) and polypropylene-based elastomer resin. In this mixture, the proportion of ethylene-vinyl acetate copolymer resin (EVA) may be more than 60% by mass and less than 80% by mass.
[0072] The ethylene-vinyl acetate copolymer resin (EVA) may contain 10% by mass or more and 30% by mass or less of a vinyl acetate constituent unit.
[0073] The thickness of the base material layer 21 is preferably 80 μm or more and 150 μm or less. The above value is an average value of the measured values at at least three randomly selected positions. The same applies to the thickness of the adhesive layer 22 described below.
[0074] The back side of the base material layer 21 (the side not overlapped with the adhesive layer 22) may be subjected to a release treatment using a release agent (release agent) such as a silicone resin or a fluorine resin to impart releasability.
[0075] From the viewpoint of being able to supply active energy rays such as ultraviolet rays to the pressure-sensitive adhesive layer 22 from the back side, the base material layer 21 is preferably a light-transmitting (ultraviolet-transmitting) resin film or the like.
[0076] The dicing tape 20 of this embodiment may also have a release sheet covering one surface of the adhesive layer 22 (the surface of the adhesive layer 22 that does not overlap the base material layer 21) before use. When the die bonding layer 10 having an area smaller than the adhesive layer 22 is arranged so as to be contained in the adhesive layer 22, the release sheet is arranged so as to cover both the adhesive layer 22 and the die bonding layer 10. The release sheet is used to protect the adhesive layer 22 and is peeled off before the die bonding layer 10 is attached to the adhesive layer 22.
[0077] As the release sheet, for example, a plastic film or paper that has been surface-treated with a release agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide release agent can be used.
[0078] In addition, as the release sheet, films made of fluorine-based polymers such as polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, and chlorofluoroethylene-vinylidene fluoride copolymer; films made of polyolefins such as polyethylene and polypropylene; and films made of polyesters such as polyethylene terephthalate (PET).
[0079] As the release sheet, for example, a plastic film or paper whose surface is coated with a release agent such as a fluorine-based release agent or a long-chain alkyl acrylate-based release agent can be used.
[0080] It should be noted that the release sheet can be used as a supporting material for supporting the adhesive layer 22. The release sheet is particularly suitable for use when the adhesive layer 22 is overlapped on the base layer 21. Specifically, the adhesive layer 22 can be overlapped on the base layer 21 in a state where the release sheet and the adhesive layer 22 are stacked, and the release sheet can be peeled off (transferred) after the overlap, thereby overlapping the adhesive layer 22 on the base layer 21.
[0081] In the present embodiment, the adhesive layer 22 contains, for example, an acrylic polymer, an isocyanate compound, and a polymerization initiator.
[0082] The adhesive layer 22 preferably has a thickness of 5 μm or more and 40 μm or less. The shape and size of the adhesive layer 22 are usually the same as those of the base material layer 21 .
[0083] In the dicing tape 20 of the present embodiment, the ratio of the thickness of the adhesive layer 22 to the total thickness of the dicing tape 20 may be 5% or more and 30% or less.
[0084] The acrylic polymer has at least a constituent unit of an alkyl (meth)acrylate, a constituent unit of a hydroxyl group-containing (meth)acrylate, and a constituent unit of a (meth)acrylate containing a polymerizable group in the molecule. The constituent unit is a unit constituting the main chain of the acrylic polymer. Each side chain in the acrylic polymer is included in each constituent unit constituting the main chain.
[0085] In addition, in this specification, the expression "(meth)acrylate" means at least one of methacrylate and acrylate. Similarly, the expression "(meth)acrylic acid" means at least one of methacrylic acid and acrylic acid.
[0086] In the acrylic polymer contained in the adhesive layer 22, the above-mentioned constituent units can be 1 H-NMR, 13 The molar ratio of the above-mentioned structural units in the acrylic polymer can be generally calculated from the blending amount (charging amount) when the acrylic polymer is polymerized.
[0087] The constituent units of the alkyl (meth)acrylate are derived from the alkyl (meth)acrylate monomer. In other words, the molecular structure after the alkyl (meth)acrylate monomer is polymerized is the constituent unit of the alkyl (meth)acrylate. The term "alkyl" refers to a hydrocarbon portion that forms an ester bond with (meth)acrylic acid.
[0088] The hydrocarbon of the alkyl portion in the structural unit of the alkyl (meth)acrylate may be a saturated hydrocarbon or an unsaturated hydrocarbon.
[0089] It should be noted that the alkyl portion preferably does not contain polar groups containing oxygen (O), nitrogen (N), etc. This can suppress the extreme increase in polarity of the alkyl polymer. Therefore, it can suppress the adhesive layer 22 from having excessive affinity for the chip bonding layer 10. This can better peel the dicing tape 20 from the chip bonding layer 10. The number of carbon atoms in the alkyl portion can be greater than 6 and less than 10.
[0090] As a structural unit of an alkyl (meth)acrylate, each structural unit, such as hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and decyl (meth)acrylate, is mentioned, for example.
[0091] The acrylic polymer has a structural unit containing a hydroxyl group (meth)acrylate, and the hydroxyl group of the structural unit easily reacts with an isocyanate group.
[0092] By allowing the acrylic polymer having a structural unit containing a hydroxyl (meth)acrylate and the isocyanate compound to coexist in the adhesive layer 22 in advance, the adhesive layer 22 can be appropriately cured. Therefore, the acrylic polymer can be fully gelled. As a result, the adhesive layer 22 can maintain its shape and exhibit adhesive properties.
[0093] The constituent unit of the hydroxyl-containing (meth)acrylate is preferably a constituent unit of a hydroxyl-containing C2-C4 alkyl (meth)acrylate. The expression "C2-C4 alkyl" indicates the number of carbon atoms in the hydrocarbon portion that forms an ester bond with (meth)acrylic acid. In other words, the hydroxyl-containing C2-C4 alkyl (meth)acrylate monomer indicates a monomer obtained by forming an ester bond between (meth)acrylic acid and an alcohol (usually a dihydric alcohol) having 2 to 4 carbon atoms.
[0094] The hydrocarbon portion of the C2-C4 alkyl group is usually a saturated hydrocarbon. For example, the hydrocarbon portion of the C2-C4 alkyl group is a straight-chain saturated hydrocarbon or a branched saturated hydrocarbon. The hydrocarbon portion of the C2-C4 alkyl group preferably does not contain a polar group containing oxygen (O), nitrogen (N), etc.
[0095] As the constituent unit of the hydroxyl-containing C2-C4 alkyl (meth)acrylate, for example, constituent units of hydroxybutyl (meth)acrylate such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxyn-butyl (meth)acrylate, or hydroxyisobutyl (meth)acrylate can be cited. It should be noted that in the constituent unit of hydroxybutyl (meth)acrylate, the hydroxyl group (-OH group) may be bonded to the carbon (C) at the terminal of the hydrocarbon part, or may be bonded to a carbon (C) other than the terminal of the hydrocarbon part.
[0096] The acrylic polymer described above includes a structural unit of a polymerizable group-containing (meth)acrylate having a polymerizable unsaturated double bond in a side chain.
[0097] By making the acrylic polymer contain a constituent unit of a (meth)acrylate containing a polymerizable group, the adhesive layer 22 can be cured by irradiating active energy rays (ultraviolet rays, etc.) before the pickup process. In detail, by irradiating active energy rays such as ultraviolet rays, free radicals are generated by a photopolymerization initiator, and through the action of the free radicals, the acrylic polymers can be cross-linked with each other. Thus, the adhesive force of the adhesive layer 22 before irradiation can be reduced by irradiation. Moreover, the chip bonding layer 10 can be well peeled off from the adhesive layer 22.
[0098] In addition, as active energy rays, ultraviolet rays, radiation rays, and electron beams can be used.
[0099] Specifically, the constituent unit of the polymerizable group-containing (meth)acrylate may have a molecular structure in which an isocyanate group of an isocyanate group-containing (meth)acrylate monomer and a hydroxyl group in the constituent unit of the hydroxyl group-containing (meth)acrylate form a urethane bond.
[0100] The constituent unit of the polymerizable group-containing (meth)acrylate having a polymerizable group can be prepared after polymerization of an acrylic polymer. For example, after copolymerization of an alkyl (meth)acrylate monomer and a hydroxyl group-containing (meth)acrylate monomer, a part of the hydroxyl groups of the constituent unit of the hydroxyl group-containing (meth)acrylate can be subjected to a urethanization reaction with the isocyanate groups of the polymerizable monomer containing an isocyanate group, thereby obtaining the constituent unit of the polymerizable group-containing (meth)acrylate.
[0101] The isocyanate group-containing (meth)acrylate monomer preferably has one isocyanate group and one (meth)acryloyl group in the molecule. Examples of the monomer include 2-isocyanatoethyl (meth)acrylate.
[0102] The adhesive layer 22 of the dicing tape 20 in the present embodiment further contains an isocyanate compound. A part of the isocyanate compound may be in a state after reacting by a urethanization reaction or the like.
[0103] The isocyanate compound has a plurality of isocyanate groups in the molecule. By making the isocyanate compound have a plurality of isocyanate groups in the molecule, a cross-linking reaction can be performed between the acrylic polymers in the adhesive layer 22. Specifically, by making one isocyanate group of the isocyanate compound react with a hydroxyl group of the acrylic polymer and making the other isocyanate groups react with hydroxyl groups of other acrylic polymers, a cross-linking reaction with the isocyanate compound can be performed.
[0104] Examples of the isocyanate compound include diisocyanates such as aliphatic diisocyanates, alicyclic diisocyanates, and aromatic aliphatic diisocyanates.
[0105] Furthermore, as an isocyanate compound, polymeric polyisocyanates, such as dimer and trimer of diisocyanate, and polymethylene polyphenylene polyisocyanate are mentioned, for example.
[0106] Examples of the isocyanate compound include polyisocyanates obtained by reacting an excess of the above isocyanate compound with an active hydrogen-containing compound. Examples of the active hydrogen-containing compound include active hydrogen-containing low molecular weight compounds and active hydrogen-containing high molecular weight compounds.
[0107] In addition, as an isocyanate compound, allophanate polyisocyanate, biuret polyisocyanate, etc. can also be used.
[0108] The above-mentioned isocyanate compounds can be used alone or in combination of two or more.
[0109] As the above-mentioned isocyanate compound, the reaction product of an aromatic diisocyanate and an active hydrogen-containing low molecular weight compound is preferred. The reaction rate of the isocyanate group of the reaction product of the aromatic diisocyanate is relatively slow, so the adhesive layer 22 containing the reaction product can suppress over-curing. As the above-mentioned isocyanate compound, an isocyanate compound having three or more isocyanate groups in the molecule is preferred.
[0110] The polymerization initiator contained in the adhesive layer 22 is a compound that can initiate a polymerization reaction by applying heat energy or light energy. By making the adhesive layer 22 contain a polymerization initiator, a cross-linking reaction can be carried out between acrylic polymers when heat energy or light energy is applied to the adhesive layer 22. In detail, a polymerization reaction between polymerizable groups can be initiated between acrylic polymers having constituent units of (meth)acrylate containing polymerizable groups, thereby curing the adhesive layer 22. As a result, the adhesive force of the adhesive layer 22 can be reduced, and the chip bonding layer 10 can be easily peeled off from the cured adhesive layer 22 in the pickup process.
[0111] As the polymerization initiator, for example, a photopolymerization initiator or a thermal polymerization initiator can be used. As the polymerization initiator, a general commercially available product can be used.
[0112] The adhesive layer 22 may also contain other components in addition to the above components. Examples of other components include tackifiers, plasticizers, fillers, antioxidants, antioxidants, ultraviolet absorbers, light stabilizers, heat stabilizers, antistatic agents, surfactants, light peeling agents, etc. The types and amounts of other components may be appropriately selected according to the purpose.
[0113] Next, the dicing die-bonding film 1 according to the present embodiment will be described in detail.
[0114] The dicing die-bonding film 1 of the present embodiment includes the above-mentioned dicing tape 20 and a die-bonding layer 10 laminated on the adhesive layer 22 of the dicing tape 20. The die-bonding layer 10 is bonded to a semiconductor wafer in the manufacture of a semiconductor integrated circuit.
[0115] The die bonding layer 10 may include at least one of a thermosetting resin and a thermoplastic resin. The die bonding layer 10 preferably includes a thermosetting resin and a thermoplastic resin.
[0116] Examples of the thermosetting resin include epoxy resin, phenolic resin, amino resin, unsaturated polyester resin, polyurethane resin, silicone resin, and thermosetting polyimide resin. As the thermosetting resin, only one type or two or more types may be used. As the thermosetting resin, epoxy resin is preferred because it contains less ionic impurities that may cause corrosion of the semiconductor chip to be bonded to the chip. As a curing agent for the epoxy resin, phenolic resin is preferred.
[0117] Examples of the epoxy resin include bisphenol A type, bisphenol F type, bisphenol S type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol AF type, biphenyl type, naphthalene type, fluorene type, phenol novolac type, o-cresol novolac type, trihydroxyphenylmethane type, tetrahydroxyphenylethane type, hydantoin type, triglycidyl isocyanurate type, and glycidylamine type epoxy resins.
[0118] The phenolic resin can function as a curing agent for the epoxy resin. Examples of the phenolic resin include novolac-type phenolic resins, resol-type phenolic resins, and polyoxystyrene such as polyoxystyrene.
[0119] Examples of the novolac-type phenolic resin include phenol novolac resins, phenol aralkyl resins, cresol novolac resins, tert-butylphenol novolac resins, and nonylphenol novolac resins.
[0120] As the above-mentioned phenolic resin, only one kind may be used or two or more kinds may be used.
[0121] In the die bonding layer 10 , the hydroxyl group of the phenol resin is preferably 0.5 to 2.0 equivalents, more preferably 0.7 to 1.5 equivalents per 1 equivalent of the epoxy group of the epoxy resin. This allows sufficient curing reaction between the epoxy resin and the phenol resin.
[0122] When the die bonding layer 10 includes a thermosetting resin, the content ratio of the thermosetting resin in the die bonding layer 10 is preferably 5% by mass or more and 60% by mass or less, and more preferably 10% by mass or more and 50% by mass or less relative to the total mass of the die bonding layer 10. Thus, the die bonding layer 10 can appropriately function as a thermosetting adhesive.
[0123] As thermoplastic resins that can be included in the chip bonding layer 10, for example, natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylate copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resins such as 6-nylon and 6,6-nylon (trade name), phenoxy resin, acrylic resin, saturated polyester resins such as PET and PBT, polyamide-imide resin, fluororesin, etc.
[0124] As the thermoplastic resin, an acrylic resin is preferred because it contains less ionic impurities and has high heat resistance, thereby further ensuring the adhesiveness of the die-bonding layer 10 .
[0125] As the above-mentioned thermoplastic resin, only one kind may be used or two or more kinds may be used.
[0126] The acrylic resin is preferably a polymer in which the constituent unit of the (meth)acrylic acid alkyl ester is the largest in terms of mass ratio among the constituent units in the molecule. Examples of the (meth)acrylic acid alkyl ester include C2 to C4 alkyl (meth)acrylates.
[0127] The acrylic resin may further include a structural unit derived from other monomer components copolymerizable with the (meth)acrylic acid alkyl ester monomer.
[0128] Examples of the other monomer components include carboxyl group-containing monomers, acid anhydride monomers, hydroxyl group-containing monomers, glycidyl group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, functional group-containing monomers such as acrylamide and acrylonitrile, and other various polyfunctional monomers.
[0129] From the perspective of being able to exert a higher cohesive force in the chip bonding layer 10, the above-mentioned acrylic resin is preferably a copolymer of an alkyl (meth)acrylate (especially an alkyl (meth)acrylate having an alkyl part with a carbon number of 4 or less) and a carboxyl group-containing monomer and a nitrogen atom-containing monomer and a polyfunctional monomer (especially a polyglycidyl-based polyfunctional monomer), and more preferably a copolymer of ethyl acrylate, butyl acrylate, acrylic acid, acrylonitrile and polyglycidyl (meth)acrylate.
[0130] The glass transition temperature (Tg) of the acrylic resin is preferably -50°C to 50°C, more preferably 10°C to 30°C, in order to easily set the elasticity and viscosity of the die-bonding layer 10 within a desired range.
[0131] When the chip bonding layer 10 includes a thermosetting resin and a thermoplastic resin, the content ratio of the above-mentioned thermoplastic resin in the chip bonding layer 10 is preferably 30 mass % or more and 70 mass % or less, more preferably 40 mass % or more and 60 mass % or less, and further preferably 45 mass % or more and 55 mass % or less relative to the total mass of the organic components other than the filler (for example, thermosetting resin, thermoplastic resin, curing catalyst, silane coupling agent, dye). It should be noted that the elasticity and viscosity of the chip bonding layer 10 can be adjusted by changing the content ratio of the thermosetting resin.
[0132] When the thermoplastic resin of the chip bonding layer 10 has a thermosetting functional group, as the thermoplastic resin, for example, an acrylic resin containing a thermosetting functional group can be used. The acrylic resin containing a thermosetting functional group preferably contains a constituent unit derived from an alkyl (meth)acrylate in the molecule at the largest mass ratio. As the alkyl (meth)acrylate, for example: the (meth)alkyl (meth)acrylate esters exemplified above.
[0133] On the other hand, examples of the thermosetting functional group in the thermosetting functional group-containing acrylic resin include a glycidyl group, a carboxyl group, a hydroxyl group, and an isocyanate group.
[0134] The chip bonding layer 10 preferably contains a thermosetting functional group-containing acrylic resin and a curing agent. As the curing agent, the substances exemplified as curing agents that can be contained in the adhesive layer 22 can be cited. When the thermosetting functional group in the thermosetting functional group-containing acrylic resin is a glycidyl group, it is preferred to use a compound having a plurality of phenol structures as the curing agent. For example, the various phenolic resins described above can be used as the curing agent.
[0135] The die bond layer 10 preferably contains a filler. By changing the amount of the filler in the die bond layer 10, the elasticity and viscosity of the die bond layer 10 can be more easily adjusted. Furthermore, the physical properties of the die bond layer 10, such as electrical conductivity, thermal conductivity, and elastic modulus, can be adjusted.
[0136] Examples of the filler include inorganic fillers and organic fillers. As the filler, inorganic fillers are preferred.
[0137] As inorganic fillers, for example, fillers containing silicon dioxide such as aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, boron nitride, crystalline silicon dioxide, amorphous silicon dioxide, etc. can be cited. In addition, as the material of the inorganic filler, metal single substances and alloys such as aluminum, gold, silver, copper, and nickel can be cited. Fillers such as aluminum borate whiskers, amorphous carbon black, and graphite can be used. The shape of the filler can be various shapes such as spherical, needle-shaped, and flaky. As the filler, only one of the above or two or more can be used.
[0138] The average particle size of the filler is preferably 0.005 μm or more and 10 μm or less, more preferably 0.005 μm or more and 1 μm or less. By making the average particle size 0.005 μm or more, the wettability and adhesion to adherends such as semiconductor wafers are further improved. By making the average particle size 10 μm or less, the characteristics brought by the added filler can be more fully utilized, and the heat resistance of the chip bonding layer 10 can be further utilized. The average particle size of the filler can be obtained, for example, using a photometric particle size distribution meter (for example, product name "LA-910", manufactured by HORIBA, Ltd.).
[0139] When the die bonding layer 10 contains a filler, the content ratio of the filler is preferably 30 mass % to 70 mass % with respect to the total mass of the die bonding layer 10 , more preferably 40 mass % to 60 mass %, and further preferably 42 mass % to 55 mass %.
[0140] The die-bonding layer 10 may contain other components as necessary. Examples of the other components include a curing catalyst, a flame retardant, a silane coupling agent, an ion scavenger, and a dye.
[0141] Examples of the flame retardant include antimony trioxide, antimony pentoxide, and brominated epoxy resins.
[0142] Examples of the silane coupling agent include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropylmethyldiethoxysilane.
[0143] Examples of the ion scavenger include hydrotalcites, bismuth hydroxide, and benzotriazole.
[0144] As the above other additives, only one kind may be used or two or more kinds may be used.
[0145] From the viewpoint of easy adjustment of elasticity and viscosity, the die-bonding layer 10 preferably contains a thermoplastic resin (particularly an acrylic resin), a thermosetting resin, and a filler.
[0146] In the die bonding layer 10 , the content ratio of the thermoplastic resin such as acrylic resin to the total mass of organic components excluding fillers is preferably 30 mass % to 70 mass %, more preferably 40 mass % to 60 mass %, and further preferably 45 mass % to 55 mass %.
[0147] The content of the filler relative to the total mass of the die bond layer 10 is preferably 30 mass % to 70 mass %, more preferably 40 mass % to 60 mass %, and further preferably 42 mass % to 55 mass %.
[0148] The thickness of the chip bonding layer 10 is not particularly limited, for example, it is greater than 1 μm and less than 200 μm. The thickness can be greater than 50 μm and less than 135 μm. Even for a dicing chip bonding film having such a thicker chip bonding layer, the dicing tape can be prevented from breaking during the expansion process at low temperatures. It should be noted that when the chip bonding layer 10 is a laminate, the above thickness is the total thickness of the laminate.
[0149] The glass transition temperature (Tg) of the die bond layer 10 is preferably 0° C. or higher, more preferably 10° C. or higher. By setting the glass transition temperature to 0° C. or higher, the die bond layer 10 can be easily cut by cold expansion. The upper limit of the glass transition temperature of the die bond layer 10 is, for example, 100° C.
[0150] like Figure 1As shown, the die bonding layer 10 may have a single-layer structure, for example. In this specification, a single layer means a layer having only one layer formed of the same composition. A structure in which a plurality of layers formed of the same composition are stacked is also a single layer.
[0151] On the other hand, the die-bonding layer 10 may have a multilayer structure in which layers formed of two or more different compositions are stacked, for example.
[0152] For the dicing die bonding film 1 of the present embodiment, when used, the adhesive layer 22 is cured by, for example, irradiating active energy rays (e.g., ultraviolet rays). Specifically, in a state where the die bonding layer 10 having a semiconductor wafer bonded to one surface and the adhesive layer 22 bonded to the other surface of the die bonding layer 10 are stacked, at least the adhesive layer 22 is irradiated with ultraviolet rays or the like. For example, ultraviolet rays or the like are irradiated from the side where the base material layer 21 is arranged, and the ultraviolet rays or the like that pass through the base material layer 21 reach the adhesive layer 22. The adhesive layer 22 is cured by irradiating with ultraviolet rays or the like.
[0153] Since the adhesive layer 22 is cured after irradiation, the adhesive force of the adhesive layer 22 can be reduced, and thus the die bonding layer 10 (the state where the semiconductor wafer is bonded) can be relatively easily peeled from the adhesive layer 22 after irradiation.
[0154] The dicing die bonding film 1 of the present embodiment may have a release sheet covering one surface of the die bonding layer 10 (the surface of the die bonding layer 10 not overlapping the adhesive layer 22) before use. The release sheet is used to protect the die bonding layer 10 and is peeled off before attaching an adherend (e.g., a semiconductor wafer) to the die bonding layer 10.
[0155] As the release sheet, the same release sheet as the above-mentioned release sheet can be used. The release sheet can be used as a supporting material for supporting the chip bonding layer 10. The release sheet is suitable for use when the chip bonding layer 10 is overlapped on the adhesive layer 22. In detail, the chip bonding layer 10 and the adhesive layer 22 can be overlapped in a state where the release sheet and the chip bonding layer 10 are stacked, and the release sheet is peeled off (transferred) after overlapping, thereby overlapping the chip bonding layer 10 on the adhesive layer 22.
[0156] Since the dicing die-bonding film 1 of the present embodiment is configured as described above, cracking in an expansion step (described in detail later) at a low temperature can be suppressed.
[0157] Next, a method for manufacturing the dicing tape 20 and the dicing die-bonding film 1 according to the present embodiment will be described.
[0158] The method for manufacturing the dicing die-bonding film 1 according to the present embodiment includes:
[0159] A step of manufacturing the dicing tape 20 (a method of manufacturing the dicing tape), and a step of stacking the die bond layer 10 on the manufactured dicing tape 20 to manufacture the dicing die bond film 1 .
[0160] A method for manufacturing a cutting tape (a process for manufacturing a cutting tape) comprises:
[0161] A synthesis process for synthesizing acrylic polymers;
[0162] an adhesive layer forming step of volatilizing a solvent from an adhesive composition comprising the acrylic polymer, an isocyanate compound, a polymerization initiator, a solvent, and other components appropriately added according to the purpose to form an adhesive layer 22; and
[0163] In the lamination step, the adhesive layer 22 and the base layer 21 are bonded together to laminate the base layer 21 and the adhesive layer 22 .
[0164] In the synthesis step, for example, a C9-C11 alkyl (meth)acrylate monomer and a hydroxyl group-containing (meth)acrylate monomer are radically polymerized to synthesize an acrylic polymer intermediate.
[0165] Free radical polymerization can be carried out by a common method. For example, each of the above monomers can be dissolved in a solvent and stirred while heating, and a polymerization initiator can be added to synthesize an acrylic polymer intermediate. In order to adjust the molecular weight of the acrylic polymer, polymerization can also be carried out in the presence of a chain transfer agent.
[0166] Next, a part of the hydroxyl groups of the constituent units of the hydroxyl group-containing (meth)acrylate contained in the acrylic polymer intermediate is bonded to the isocyanate groups of the isocyanate group-containing polymerizable monomer by urethanization reaction. Thus, a part of the constituent units of the hydroxyl group-containing (meth)acrylate is converted into constituent units of the polymerizable group-containing (meth)acrylate.
[0167] The urethanization reaction can be carried out by a common method. For example, the acrylic polymer intermediate and the isocyanate group-containing polymerizable monomer are stirred while heating in the presence of a solvent and a urethanization catalyst. In this way, a part of the hydroxyl group of the acrylic polymer intermediate and the isocyanate group of the isocyanate group-containing polymerizable monomer can form a urethanate bond.
[0168] In the adhesive layer preparation process, for example, an acrylic polymer, an isocyanate compound, and a polymerization initiator are dissolved in a solvent to prepare an adhesive composition. The viscosity of the composition can be adjusted by changing the amount of solvent. Then, the adhesive composition is applied to a release sheet. As a coating method, for example, common coating methods such as roller coating, screen coating, and gravure coating are used. The applied composition is subjected to desolventizing treatment, curing treatment, etc., so that the applied adhesive composition is cured, thereby making an adhesive layer 22.
[0169] In the lamination step, the adhesive layer 22 in a state of being overlapped with the release sheet is overlapped with the base layer 21. In addition, the release sheet may be in a state of being overlapped with the adhesive layer 22 until use.
[0170] In order to promote the reaction between the crosslinking agent and the acrylic polymer and also to promote the reaction between the crosslinking agent and the surface of the base layer 21 , an aging treatment step may be performed at 50° C. for 48 hours after the lamination step.
[0171] It should be noted that the substrate layer 21 can use commercially available films, etc., or can be made by film-forming by a common method. As the film-forming method, for example, a calendering film-forming method, a casting method in an organic solvent, an inflation extrusion method in a closed system, a T-die extrusion method, a dry lamination method, etc. can be cited. A coextrusion molding method can also be used.
[0172] Through these steps, the dicing tape 20 can be manufactured.
[0173] The method for manufacturing a dicing die-bonding film (a process for manufacturing a dicing die-bonding film) includes the following steps:
[0174] A resin composition preparation step of preparing a resin composition for forming the die bonding layer 10;
[0175] a die bonding layer manufacturing step of manufacturing a die bonding layer 10 from a resin composition; and
[0176] In the attaching step, the die bonding layer 10 is attached to the adhesive layer 22 of the dicing tape 20 obtained as described above.
[0177] In the resin composition preparation process, for example, epoxy resin, epoxy resin curing catalyst, acrylic resin, phenolic resin, solvent, etc. are mixed and each resin is dissolved in the solvent to prepare the resin composition. The viscosity of the composition can be adjusted by changing the amount of solvent. It should be noted that commercially available products can be used as these resins.
[0178] In the chip bonding layer preparation process, for example, the resin composition prepared by the above operation is applied to the release sheet. As the coating method, there is no particular limitation, for example, a common coating method such as roller coating, screen coating, gravure coating, etc. can be adopted. Then, as needed, the applied composition is cured by desolventizing treatment, curing treatment, etc. to prepare the chip bonding layer 10.
[0179] In the pasting process, the peeling sheet is peeled off from the adhesive layer 22 of the dicing tape 20 and the chip bonding layer 10, respectively, and the chip bonding layer 10 is directly contacted with the adhesive layer 22. For example, the pasting can be performed by crimping. The temperature during pasting is not particularly limited, for example, it is 30°C or more and 50°C or less, preferably 35°C or more and 45°C or less. The linear pressure during pasting is not particularly limited, preferably 0.1kgf / cm or more and 20kgf / cm or less, more preferably 1kgf / cm or more and 10kgf / cm or less.
[0180] The dicing die-bonding film 1 manufactured as described above is used as an auxiliary tool for manufacturing a semiconductor integrated circuit, for example. A specific example of its use will be described below.
[0181] The method of manufacturing a semiconductor integrated circuit generally includes a step of cutting chips from a semiconductor wafer having a circuit surface formed thereon and assembling the chips.
[0182] This process includes, for example, the following processes: a half-cutting process, in which a groove is formed on the semiconductor wafer in order to process the semiconductor wafer into a die by cutting, and then the semiconductor wafer is ground to reduce the thickness; a mounting process, in which one side (for example, the side opposite to the circuit surface) of the semiconductor wafer processed by half-cutting is attached to the die bonding layer 10, and the semiconductor wafer is fixed to the dicing tape 20; an expansion process, in which the interval between the semiconductor chips processed by half-cutting is expanded; a pickup process, in which the die bonding layer 10 and the adhesive layer 22 are peeled off and the semiconductor die is taken out in a state where the die bonding layer 10 is attached; and a die bonding process, in which the semiconductor die in a state where the die bonding layer 10 is attached is bonded to the adherend. When performing these processes, the dicing tape (dicing die bonding film) of this embodiment is used as a manufacturing auxiliary tool.
[0183] In the half-cutting process, Figure 2A to Figure 2DAs shown, a half-cutting process for cutting a semiconductor integrated circuit into small pieces (dies) is performed. Specifically, a wafer processing tape T is attached to the surface of the semiconductor wafer on the opposite side to the circuit surface. In addition, a cutting ring R is mounted on the wafer processing tape T. A groove for dividing is formed with the wafer processing tape T attached. A back grinding tape G is attached to the surface with the groove formed, and the wafer processing tape T attached initially is peeled off. A grinding process is performed with the back grinding tape G attached until the semiconductor wafer reaches a predetermined thickness.
[0184] During the installation process, Figure 3A to Figure 3B As shown, after the dicing ring R is attached to the adhesive layer 22 of the dicing tape 20, the semiconductor wafer that has been half-cut is attached (bonded) to the exposed surface of the die bonding layer 10. Thereafter, the back grinding tape G is peeled off from the semiconductor wafer.
[0185] In the expansion process, Figure 4A to Figure 4C As shown, after the cutting ring R is installed on the adhesive layer 22 of the cutting tape 20, it is fixed to the holding tool H of the expansion device. The lifting member U possessed by the expansion device is lifted from the lower side of the cutting chip bonding film 1, thereby stretching the cutting chip bonding film 1 and expanding it in the surface direction. Thus, the semiconductor wafer that has been half-cut is cut together with the chip bonding layer 10 under specific temperature conditions. The above-mentioned temperature condition is below 0°C, for example, -20 to 0°C, preferably -15 to 0°C, and more preferably -10 to -5°C. The lifting member U is lowered to release the expansion state (so far it is a cold expansion process). Furthermore, in the expansion process, as Figure 5A to Figure 5B As shown, the dicing tape 20 is stretched under a higher temperature condition to expand the area. Thus, the adjacent semiconductor chips that have been cut are separated in the surface direction of the film surface, and the interval is further increased (room temperature expansion process).
[0186] During the picking process, Figure 6 As shown, the semiconductor chip with the die bonding layer 10 attached thereto is peeled off from the adhesive layer 22 of the dicing tape 20. Specifically, the pin member P is raised to lift up the semiconductor chip to be picked up through the dicing tape 20. The lifted semiconductor chip is held by the suction jig J.
[0187] In the die bonding step, the semiconductor chip with the die bonding layer 10 attached thereto is bonded to an adherend.
[0188] As described above, the dicing die bonding film 1 (dicing tape 20) of the present embodiment can be used in the above-mentioned process, and in the cold expansion process, the dicing tape 20 is stretched at 0°C or below with the wafer bonded to the die bonding layer 10, and the wafer is cut together with the die bonding layer 10. Furthermore, the dicing tape 20 is stretched in the expansion process at room temperature.
[0189] The temperature in the cold extension step is usually 0° C. or lower, for example, -15° C. to 0° C. The temperature in the extension step at room temperature is, for example, 10° C. to 25° C.
[0190] The matters disclosed in this specification include the following matters. (1)
[0192] A dicing tape, wherein, with respect to the ratio of storage modulus E' to loss modulus E" (E" / E') measured by dynamic viscoelasticity measurement, namely Tan δ,
[0193] The ratio (A / B) of the Tan δ value (A) at -15°C to the Tan δ value (B) at -5°C is 0.75 or more and 2.00 or less. (2)
[0195] The dicing tape according to (1) above, wherein the strength at 25% elongation at -15°C is 15 [N / 20 mm] or more and 30 [N / 20 mm] or less. (3)
[0197] The dicing tape according to (1) or (2) above, comprising a base layer and an adhesive layer having higher adhesiveness than the base layer,
[0198] The thickness of the base material layer is 80 μm or more and 150 μm or less. (4)
[0200] The dicing tape according to the above (3), wherein the adhesive layer has a thickness of 5 μm to 40 μm. (5)
[0202] The dicing tape according to any one of (1) to (4) above, wherein the value (A) of Tan δ at -15°C is 0.05 or more and 0.50 or less.
[0203] The value (B) of Tan δ at -5°C is 0.05 or more and 0.50 or less. (6)
[0205] A cutting tape according to any one of (3) to (5) above, wherein the substrate layer comprises at least one selected from ethylene-vinyl acetate copolymer (EVA) resin, α-olefin-based thermoplastic elastomer resin, ethylene-methyl acrylate copolymer (EMA) resin, and ionomer resin (IO). (7)
[0207] The cutting tape according to (6) above, wherein the substrate layer is formed by a polypropylene-based elastomer resin, an ethylene-methyl acrylate copolymer (EMA) resin, an ethylene-vinyl acetate copolymer (EVA) resin, a mixture of an ethylene-vinyl acetate copolymer (EVA) resin and an ionomer resin (IO), or a mixture of an ethylene-vinyl acetate copolymer (EVA) resin and a polypropylene-based elastomer resin. (8)
[0209] The dicing tape according to any one of (3) to (7) above, wherein the base layer has a single-layer structure. (9)
[0211] The dicing tape according to any one of (3) to (8) above, wherein the adhesive layer comprises an acrylic polymer having at least a constituent unit of an alkyl (meth)acrylate, a constituent unit of a hydroxyl (meth)acrylate, and a constituent unit of a (meth)acrylate containing a polymerizable group in the molecule. (10)
[0213] The dicing tape according to the above (9), wherein the adhesive layer further contains an isocyanate compound and a polymerization initiator. (11)
[0215] The dicing tape according to any one of (3) to (10) above, wherein a ratio of a thickness of the adhesive layer to a total thickness of the dicing tape is 5% or more and 30% or less. (12)
[0217] A dicing die-bonding film comprising the dicing tape according to any one of (1) to (11) above, and a die-bonding layer bonded to the dicing tape. (13)
[0219] The dicing die-bonding film according to the above (12), wherein the die-bonding layer has a thickness of 50 μm to 135 μm. (14)
[0221] The dicing die-bonding film according to (12) or (13) above, which is used in a cold stretching process in which the film is stretched at 0°C or lower with a wafer bonded to the die-bonding layer.
[0222] In the cold expansion step, the wafer is cut together with the die bond layer. (15)
[0224] The dicing tape according to any one of (12) to (14) above, wherein the die bond layer contains at least one of a thermosetting resin and a thermoplastic resin. (16)
[0226] The dicing tape according to the above (15), wherein the die bond layer contains epoxy resin and phenol resin as the thermosetting resin, and contains acrylic resin as the thermoplastic resin. (17)
[0228] The dicing tape according to (15) or (16), wherein the die bond layer further contains a filler.
[0229] The dicing tape and the dicing die-bonding film of the present embodiment are as exemplified above, but the present invention is not limited to the dicing tape and the dicing die-bonding film exemplified above.
[0230] That is, various methods generally used for dicing tapes and dicing die-bonding films can be adopted within a range not impairing the effects of the present invention.
[0231] Example
[0232] Next, the present invention will be described in more detail using experimental examples, but the present invention is not limited to these examples.
[0233] The dicing tape was manufactured as follows. In addition, a dicing die-bonding film was manufactured using the dicing tape.
[0234] <Base material layer>
[0235] A single-layer substrate layer was produced using the following products. Specifically, in each of the Examples and Comparative Examples, the substrate layer was formed into a film using an extrusion T-die molding machine. The extrusion temperature conditions were in the range of 180 to 230°C.
[0236] (Example 1)
[0237] ·Raw material: Vistamaxx 3980FL (thickness 125μm)
[0238] Polypropylene elastomer resin
[0239] Vistamaxx series manufactured by ExxonMobil Japan
[0240] (Example 2)
[0241] ·Raw material name: REXPEARL EMA EB330H
[0242] Ethylene-methyl acrylate copolymer resin (EMA)
[0243] REXPEARL (REXPEARL EMA) series manufactured by Japan Polyethylene Co., Ltd.
[0244] (Example 3)
[0245] Blend of ethylene-vinyl acetate copolymer resin (EVA) and ionomer resin (IO) (7:3 mass ratio)
[0246] Raw material name: EV550
[0247] Ethylene-vinyl acetate copolymer resin (EVA contains 14% by mass of vinyl acetate)
[0248] EVAFLEX series manufactured by DOW-MITSUI POLYCHEMICALS
[0249] ·Raw material name: HIMILAN1706
[0250] Ionomer resin (IO)
[0251] DOW-MITSUI POLYCHEMICALS HIMILAN (series)
[0252] (Example 4)
[0253] Blend of ethylene-vinyl acetate copolymer resin (EVA) and polypropylene elastomer resin (7:3 mass ratio)
[0254] Raw material name: EV550
[0255] Ethylene-vinyl acetate copolymer resin (EVA contains 14% by mass of vinyl acetate)
[0256] EVAFLEX series manufactured by DOW-MITSUI POLYCHEMICALS
[0257] Raw material name: Vistamaxx 3980FL
[0258] Polypropylene elastomer resin
[0259] Vistamaxx series manufactured by ExxonMobil Japan
[0260] (Comparative Example 1)
[0261] Raw material name: Novatec LC720
[0262] Low density polyethylene resin (LDPE)
[0263] Novatec LD series manufactured by Japan Polyethylene Co., Ltd.
[0264] (Comparative Example 2)
[0265] ·Raw material: WXK1233 (thickness 100μm)
[0266] Metallocene polypropylene random copolymer
[0267] WINTEC series manufactured by Japan Polypropylene Corp.
[0268] (Example 5)
[0269] ·Raw material: EV250 (thickness 125μm)
[0270] Ethylene-vinyl acetate copolymer resin (EVA contains 28% by mass of vinyl acetate)
[0271] EVAFLEX series manufactured by DOW-MITSUI POLYCHEMICALS
[0272] (Example 6)
[0273] ·Raw material: EV550 (thickness 125μm)
[0274] Ethylene-vinyl acetate copolymer resin (EVA contains 14% by mass of vinyl acetate)
[0275] EVAFLEX series manufactured by DOW-MITSUI POLYCHEMICALS
[0276] <Adhesive layer>
[0277] (Synthesis of Acrylic Polymer)
[0278] The following raw materials were added to a reaction vessel equipped with a condenser, a nitrogen inlet pipe, a thermometer and a stirrer so that the monomer concentration was about 55% by mass, and a polymerization reaction was carried out at 60° C. for 10 hours in a nitrogen stream to synthesize an acrylic polymer intermediate.
[0279] 2-Ethylhexyl acrylate (hereinafter also referred to as "2EHA"): 100 parts by mass,
[0280] 2-Hydroxyethyl acrylate (hereinafter also referred to as "HEA"): 20 parts by mass,
[0281] Polymerization initiator: appropriate amount,
[0282] Polymerization solvent: toluene
[0283] 100 parts by mass of the synthesized acrylic polymer intermediate and 1.4 parts by mass of 2-methacryloyloxyethyl isocyanate (hereinafter also referred to as "MOI") were subjected to addition reaction in the presence of dibutyltin dilaurate (0.1 parts by mass) at 50° C. for 60 hours in an air stream to synthesize an acrylic polymer.
[0284] (Preparation of Adhesive Layer)
[0285] Thereafter, a binder solution was prepared according to the following composition, and toluene was appropriately added to adjust the viscosity to 500 mPa·s.
[0286] Synthetic acrylic polymer: 100 parts by mass,
[0287] Polyisocyanate compounds
[0288] (Product name: "Coronate L", manufactured by Nippon Polyurethane Co., Ltd.)
[0289] : 1.1 parts by mass,
[0290] Photopolymerization initiator
[0291] (Product name: "Irgacure 184", manufactured by Ciba Specialty Chemicals Co., Ltd.):
[0292] : 3 parts by mass
[0293] A PET film was prepared as a release sheet. The adhesive solution prepared as above was applied to the surface of the release sheet using an applicator. It should be noted that a silicone treatment was applied to one side of the release sheet (PET film) as a release treatment, and the adhesive solution was applied to the surface subjected to the release treatment. After application, the film was heated at 120°C for 2 minutes to perform a drying treatment, thereby producing an adhesive layer with a thickness of 10 μm on the release sheet.
[0294] <Production of cutting tape>
[0295] The exposed surface of the pressure-sensitive adhesive layer formed on the release sheet was bonded to each base layer (thickness 125 μm) at room temperature using a laminator to produce a dicing tape.
[0296] <Production of chip bonding layer>
[0297] The following (a) to (d) were dissolved in methyl ethyl ketone to prepare a resin composition having a solid content concentration of 40 to 50% by mass.
[0298] (a) Acrylic resin (product name: "Teisan Resin SG-280EK23", manufactured by Nagase Chemical Co., Ltd.): 15% by mass
[0299] (b) Epoxy resin (product name: "EPPN 501H", manufactured by Nippon Kayaku Co., Ltd.): 29% by mass
[0300] (c) Novolac type phenolic resin (product name: "HF-1M", manufactured by Meiwa Chemicals Co., Ltd.) 16 mass%
[0301] (d) Inorganic filler (silicon dioxide) (product name: "SE-2050MCV", manufactured by Admatechs): 40% by mass
[0302] The resin composition is coated on a release film (peel sheet) made of polyethylene terephthalate film with a thickness of 50 μm and subjected to silicone release treatment. Thereafter, a drying process is performed at 130°C for 2 minutes. Thus, a chip bonding layer with a thickness (average thickness) of 60 μm is prepared. The prepared chip bonding layers with a thickness of 60 μm are bonded to each other to prepare a chip bonding layer with a thickness of 120 μm. It should be noted that the lamination conditions during bonding are 80°C, 0.15 MPa, and 10 mm / s (seconds).
[0303] <Manufacturing of dicing die-bonding film>
[0304] The produced die-bonding layer was cut into a circle with a diameter of 330 mm and attached to each dicing tape (temperature: 25° C., speed 10 mm / sec, pressure 0.15 MPa).
[0305] Then, only the part where the chip bonding layer was attached was irradiated with ultraviolet light (300 mJ / cm 2 ), manufacturing a dicing die bonding film.
[0306] As described above, using the base material layers having the configurations shown in Table 1, the dicing tapes and dicing die-bonding films of Examples and Comparative Examples were respectively manufactured according to the above-mentioned methods.
[0307] Table 1 shows the physical properties (Tanδ obtained by dynamic viscoelasticity measurement, etc.) of each dicing tape.
[0308] [Table 1]
[0309]
[0310] <Tanδ at each temperature (-15°C, -5°C) obtained by dynamic viscoelasticity measurement>
[0311] Tan δ at each temperature was calculated for each cut ribbon as described below.
[0312] The test sample having the following size (width) was cut out from the die-bonding film to prepare the test sample. The dynamic storage modulus was measured in a tensile mode under the following test conditions using a solid viscoelasticity measuring device (measuring device: RSA-G2, manufactured by TA Corporation).
[0313] Width of test sample: 10mm,
[0314] Distance between chucks: 20mm,
[0315] Heating rate: 10℃ / min.
[0316] Test temperature: -30~100℃
[0317] Frequency: 1Hz
[0318] The storage modulus E' and loss modulus E", at -15°C and -5°C, were measured respectively, and Tanδ was calculated by the formula Tanδ=E", / E'. The average value of each measured value of 3 measurements was used. The higher the Tanδ, the higher the viscosity. It should be noted that the measurements were carried out in both the MD direction and the TD direction, and the higher measured value was used as the result.
[0319] <Strength measurement using a tensile testing machine (at 25% stretch)>
[0320] The strength of the dicing tape having a substrate layer and an adhesive layer at 25% tension was measured under the following test conditions using a tensile testing machine. The average value of each measured value was used for 3 measurements. It should be noted that the measurement was performed in both the MD direction and the TD direction, and the higher measured value was used as the final value.
[0321] Measuring temperature: -15℃,
[0322] Width of test sample: 10mm,
[0323] Distance between chucks: 50mm,
[0324] Stretching speed: 300mm / min
[0325] <Evaluation of crack suppression performance and cutting properties during expansion>
[0326] The 12-inch wafer was half-cut by a blade in a manner of cutting with a chip size of 10 mm × 10 mm. The 12-inch wafer was back-ground (grinded) until the thickness reached 40 μm. It was then bonded to the diced chip bonding film. It should be noted that the wafer bonding temperature was 70°C and the bonding speed was 10 mm / sec.
[0327] Thereafter, the semiconductor wafer and the die bonding layer were cut using a die separation device DDS2300 manufactured by DISCO Corporation, and the dicing tape was further heat-shrunk.
[0328] Specifically, the semiconductor wafer and the chip bonding layer were severed by a cold expansion unit at an expansion temperature of -15°C, an expansion speed of 300 mm / sec, and an expansion distance of 16 mm.
[0329] Next, the dicing tape was thermally shrunk by a thermal expansion unit under the conditions of expansion amount 7 mm, heating temperature 220°C, air volume 40 L / min, heating distance 20 mm, and rotation speed 5° / sec, thereby evaluating the crack suppression performance of the dicing sheet. The case where no tape cracking occurred was evaluated as 0, and the case where tape cracking occurred was evaluated as ×.
[0330] Regarding the splitting property, the case where the splitting rate was less than 80% was evaluated as ×, the case where it was 80% or more was evaluated as 0, and the case where it was 90% or more was evaluated as ◎.
[0331] From the above evaluation results, it is understood that the dicing die-bonding film of the example suppresses cracking in the expansion step at a low temperature as compared with the dicing die-bonding film of the comparative example.
[0332] In addition, by using a dicing tape having a strength of 15 [N / 20 mm] or more at 25% tension at -15°C, it is possible to achieve good dicing properties.
[0333] In the dicing tape of the example, the ratio (A / B) of the Tan δ value (A) at -15°C to the Tan δ value (B) at -5°C was 0.75 or more.
[0334] The value of Tanδ is an indicator of the viscosity of the dicing tape at that temperature. The above ratio (A / B) of 0.75 or more indicates that the viscosity at a lower temperature of -15°C does not decrease much compared to the viscosity at -5°C. Therefore, it is believed that even if the dicing tape is stretched at -15°C, the viscosity does not decrease much, thereby suppressing cracking.
[0335] The above-mentioned properties of the dicing tape are particularly advantageous when the thickness of the chip bonding layer is relatively thick (for example, not less than 50 μm and not more than 135 μm). In detail, in the expansion process, if the thickness of the chip bonding layer is relatively thick, a relatively large force is required until the chip bonding layer is cut together with the wafer. Therefore, until the wafer and the chip bonding layer are cut, a large force is also applied to the stretched dicing tape itself. Due to this influence, until the chip bonding layer is cut, there is a risk that the stretched dicing tape itself will be deformed, that is, cracked.
[0336] However, the dicing tape of the present embodiment has the physical properties defined by Tan δ as described above, and therefore the viscosity does not decrease much at low temperatures of 0° C. or lower. As described above, it is considered that cracking in the expansion process at low temperatures can be suppressed.
[0337] Industrial Applicability
[0338] The dicing tape and dicing die-bonding film of the present invention can be suitably used as auxiliary tools in manufacturing semiconductor integrated circuits, for example.
Claims
1. A dicing tape comprising a substrate layer and an adhesive layer having higher adhesiveness than the substrate layer, The substrate layer comprises an ionomer resin or a polypropylene-based elastomer resin and comprises an ethylene-vinyl acetate copolymer, in, Regarding the ratio E" / E' of the storage modulus E' and the loss modulus E" measured by the dynamic viscoelasticity measurement, that is, Tan δ, The ratio of the Tan δ value A at -15°C to the Tan δ value B at -5°C, i.e., A / B, is 0.75 or more and 2.00 or less, The value A of Tan δ at -15°C and the value B of Tan δ at -5°C are both 0.05 or more and 0.50 or less. 2 . The dicing tape according to claim 1 , wherein the strength at 25% elongation at -15° C. is 15 [N / 20 mm] or more. 3 . The dicing tape according to claim 1 , wherein the base material layer has a thickness of 80 μm or more and 150 μm or less.
4. The cutting tape according to claim 3, wherein: The adhesive layer has a thickness of 5 μm or more and 40 μm or less. 5 . A dicing die-bonding film comprising the dicing tape according to claim 1 , and a die-bonding layer bonded to the dicing tape. 6 . The dicing die-bonding film according to claim 5 , wherein The die bonding layer has a thickness of 50 μm or more and 135 μm or less.