A simulation device and method for establishing cementing quality evaluation index

By setting up a fan-shaped cylinder on the outer wall of the casing to simulate the lack of annulus, and using sound wave amplitude measurement, the problem of inaccurate evaluation of low-density cement slurry is solved and accurate evaluation of cementing quality is achieved.

CN112160742BActive Publication Date: 2024-10-18CHINA PETROCHEMICAL CORP +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202010941958.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-09
Publication Date
2024-10-18
Estimated Expiration
2040-09-09

AI Technical Summary

Technical Problem

The existing cementing quality evaluation standards fail to effectively consider the differences between low-density and ultra-low-density cement slurry systems, resulting in inaccurate evaluation, especially the problem of uneven cement sheath cementation.

Method used

A simulation device was designed, including simulated formations, casings and fan-shaped cylinders. By setting a fan-shaped cylinder on the outer wall of the casing to simulate the lack of annulus, sound wave amplitude measurement was used to obtain the relative sound amplitude value of the proportion of cement slurry. Establish cementing quality evaluation indicators.

Benefits of technology

The simulation device ensures the accuracy of annulus loss, thereby improving the accuracy of cementing quality evaluation, and is suitable for the evaluation of low-density and ultra-low-density cement slurry systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112160742B_ABST
    Figure CN112160742B_ABST
Patent Text Reader

Abstract

The present invention relates to a simulation device and method for establishing cementing quality evaluation indexes, including a simulated formation, a casing and a fan-shaped annular column; wherein the simulated formation is a hollow cylinder; the fan-shaped annular column is arranged on the casing, and its outer convex cylindrical surface is raised along the radial direction of the casing, and its inner concave cylindrical surface is tightly fitted with the outer wall of the casing or the fan-shaped annular column is connected to the casing as a whole; the casing is axially arranged in the simulated formation, and the outer convex cylindrical surface of the fan-shaped annular column is tightly fitted with the inner wall of the simulated formation; the fan-shaped annular column extends at a set angle in the circumferential direction to continuously occupy the space between the inner wall of the simulated formation and the outer wall of the casing to simulate the annular space loss, and the remaining gap between the inner wall of the simulated formation and the outer wall of the casing outside the annular space loss forms a cement injection cavity for injecting cement for cementing. That is, the simulation device of the present invention can ensure the accuracy of the simulated annular space loss, thereby improving the accuracy of the established cementing quality evaluation index.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a simulation device and method for establishing cementing quality evaluation indexes, belonging to the field of petroleum exploration and development. Background Art

[0002] With the development of cementing technology, low-density, ultra-low-density and foam cement slurry systems have been widely used. Especially for low-pressure, leaky layers with narrow density windows, low-density cement slurry systems can effectively solve problems such as insufficient cement return height, cementing leakage and unqualified cementing quality.

[0003] At present, the existing evaluation standard "SY / T 6592-2016: Cementing Quality Evaluation Method" is still used for different types of low-density cement slurry systems. However, this cementing quality evaluation standard is for cement slurries with a density of 1.30 g / cm 3 For the above cement slurry systems, for low-density and ultra-low-density cement systems, due to the differences in their internal lightening materials and cement hydration processes, their cementing quality evaluation indicators will also have certain differences. Therefore, the existing conventional evaluation standards do not take into account the nature of logging response.

[0004] Therefore, the existing standards should be used to evaluate the density less than 1.30g / cm 3 The cementing quality of ultra-low density cement slurry may get wrong results. At present, when conducting indoor simulation tests, corresponding simulation devices are set up to evaluate the cement ring bonding quality. The general method is to mix cement and impurities evenly and then cast the cement ring to establish different model well structures. However, the disadvantage is that the mixed cement system contains both cement and impurities, which makes the cement bonding inevitably uneven. Therefore, when establishing the cementing quality evaluation, there must be inaccurate measurements. Summary of the invention

[0005] The purpose of the present invention is to provide a simulation device and method for establishing cementing quality evaluation indicators; it is used to solve the problem that in the prior art, when evaluating the cement ring bonding quality, the mixed cement system contains both cement and impurities, which inevitably leads to uneven cement bonding, thereby causing inaccurate cementing quality evaluation.

[0006] To achieve the above object, a technical solution of a simulation device for establishing cementing quality evaluation indexes of the present invention comprises:

[0007] Simulate formations, casing and fan annular columns;

[0008] The simulated stratum is a hollow cylinder;

[0009] The sleeve has an inner hole, and the inner hole is used for injecting liquid;

[0010] The sector annular column is arranged on the sleeve, the outer convex cylindrical surface of the sector annular column protrudes along the radial direction of the sleeve, the inner concave cylindrical surface of the sector annular column is tightly fitted with the outer wall of the sleeve, or the sector annular column and the sleeve are connected as one body;

[0011] The casing is axially arranged in the simulated formation, the outer convex cylindrical surface of the fan-shaped cylinder is closely fitted with the inner wall of the simulated formation, and the fan-shaped cylinder is a hollow structure or made of a material with a density lower than that of cement used for cementing;

[0012] The fan-shaped annular column extends at a set angle in the circumferential direction to continuously occupy the space between the inner wall of the simulated formation and the outer wall of the casing in the circumferential direction to simulate the annulus loss, and the remaining gap between the inner wall of the simulated formation and the outer wall of the casing outside the annulus loss forms a cement injection cavity for injecting cement for cementing; the simulation device is used to obtain the relative sound amplitude value of the cement slurry proportion corresponding to the circumferential extension of the fan-shaped annular column at the set angle, and the relative sound amplitude value is used to establish a cementing quality evaluation index.

[0013] The beneficial effects of the present invention are as follows: the simulation device for establishing cementing quality evaluation indicators of the present invention can ensure the accuracy of the simulated annular space loss, and further ensure the accuracy of the cementing quality evaluation standards established subsequently, by arranging a fan-shaped annular column on the outer wall of the casing that extends at a set angle in the circumferential direction and has a hollow structure or is made of a material with a density lower than that of cementing cement, so as to continuously occupy the space between the inner wall of the simulated formation and the outer wall of the casing in the circumferential direction to simulate the annular space loss.

[0014] Furthermore, the fan-shaped cylinder is made of foam plastic.

[0015] The present invention also provides a technical solution for a method of establishing cementing quality evaluation indexes using the above-mentioned simulation device solution, comprising the following steps:

[0016] 1) injecting corresponding experimental media into the cement injection cavity and the inner hole of the casing of multiple simulation devices respectively; the fan-shaped cylinders of the multiple simulation devices are set to different angles θ;

[0017] Among them, S = 1-θ / 360°, where S is the cement slurry ratio and θ is the setting angle of the fan ring column;

[0018] 2) using an acoustic amplitude logging method to measure the logging acoustic amplitude of each simulation device in step 1), comparing the acquired logging acoustic amplitude of each simulation device with the acoustic amplitude of the free casing, and obtaining a relative acoustic amplitude of the lower limit of the cement bonding state and a relative acoustic amplitude of the upper limit of the cement bonding state;

[0019] The expressions of the relative acoustic amplitudes of the lower and upper limits of the cement bonding state are as follows:

[0020]

[0021] Among them, A is the acoustic amplitude corresponding to each simulated device measured, and A0 is the acoustic amplitude of the free casing;

[0022] The free casing acoustic amplitude is the logging acoustic amplitude of the free casing well; the free casing well is the same size as the simulation device, the annulus of the free casing well is a simulation well when air or water is used, and the annulus is the annular gap formed between the outer wall of the casing and the inner wall of the simulated formation;

[0023] 3) Establish a cementing quality evaluation index based on the relative acoustic amplitude value of the lower medium limit of the cement bonding state and the relative acoustic amplitude value of the upper medium limit of the cement bonding state.

[0024] The beneficial effect of the present invention is that the present invention can ensure the accuracy of the simulated annular space loss through the above-mentioned simulation device for establishing cementing quality evaluation indicators, thereby ensuring the accuracy of the cementing quality evaluation standards established subsequently.

[0025] Furthermore, in step 2), the medium lower limit of cement bonding state corresponds to a simulation device of a sector ring-shaped column with a set angle of 36°; the medium upper limit of cement bonding state corresponds to a simulation device of a sector ring-shaped column with a set angle of 108°. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a front view of an embodiment of a simulation device for establishing cementing quality evaluation indexes of the present invention;

[0027] Figure 2 is a top view of an embodiment of a simulation device for establishing cementing quality evaluation indicators of the present invention;

[0028] Figure 3 is a flow chart of an embodiment of a method for establishing cementing quality evaluation indexes of the present invention;

[0029] Figure numerals: 1-casing, 2-simulated formation, 3-fan ring column, 4-cement injection cavity, 5-inner hole, 6-steel pipe. DETAILED DESCRIPTION

[0030] The present invention will be described in detail below with reference to the accompanying drawings.

[0031] Example of a simulation device for establishing cementing quality evaluation indicators

[0032] like Figure 1 and Figure 2As shown, the simulation device for establishing cementing quality evaluation standards provided by the present invention includes a simulated formation 2, a casing 1 and a fan-shaped annular column 3.

[0033] The simulated formation 2 of this embodiment is a hollow cylinder, which is a fully cemented cement stone cast by high-density cement slurry prepared according to API standards (API standards refer to American Petroleum Institute petroleum standards).

[0034] The casing 1 in this embodiment has a casing inner hole 5, and the casing inner hole 5 is used to inject liquid; the injected liquid in this embodiment is water, which is used to simulate the medium in the cementing casing under actual working conditions.

[0035] The fan-shaped ring-shaped column 3 is arranged on the sleeve 1, and extends at a set angle along the circumferential direction of the outer wall of the sleeve 1; the outer convex cylindrical surface of the fan-shaped ring-shaped column 3 protrudes radially along the sleeve 1, and the inner concave cylindrical surface of the fan-shaped ring-shaped column is tightly fitted with the outer wall of the sleeve 1; as other embodiments, the fan-shaped ring-shaped column 3 and the sleeve 1 can also be connected as one piece.

[0036] The casing in this embodiment is axially arranged in the simulated formation 2, and the casing 1 is concentric with the simulated formation 2, and the outer convex cylindrical surface of the fan-shaped ring column 3 is tightly fitted with the inner wall of the simulated formation 2; at the same time, the fan-shaped ring column 3 is used to continuously occupy the space between the inner wall of the simulated formation 2 and the outer wall of the casing 1 in the circumferential direction to simulate the annulus loss.

[0037] The remaining space between the inner wall of the simulated formation 2 and the outer wall of the casing 1 outside the missing annulus forms a cement injection cavity 4 for injecting cement for cementing.

[0038] The fan-shaped column 3 in the above embodiment is a column made of foam plastic. Of course, in other embodiments, the fan-shaped column 5 can also be a foam plastic with a hollow structure or other materials with a density lower than cement for cementing.

[0039] The simulation device in this embodiment is used to simulate cementing in a target area. Figure 1 and Figure 2 , introduces the specific manufacturing process of the simulation device of the present invention:

[0040] 1) Preparation: Prepare steel pipes, PVC pipes, casings, fan-shaped annular columns with set angles and steel plates in advance; the specific parameters of the steel pipes, PVC pipes and casings are shown in Table 1; the parameters of the steel plate are 1 m in length and width and 1.5 cm in height.

[0041] Table 1

[0042] Length(m) Inner diameter(cm) Outer diameter (cm) Steel pipe 2.2 70 72 PVC pipe 2.2 22 23 Casing body 2.2 16.7 17.9 Fan ring cylinder 2.2 17.9 23

[0043] The sleeve in this embodiment is a circular cylinder with an open upper end and a sealed lower end.

[0044] The fan-shaped column in this embodiment is a foam plastic column, and of course it can also be a foam column with a hollow structure.

[0045] 2) Place the PVC pipe vertically in the center of the steel plate and seal it with the steel plate. Apply a thin layer of butter or grease on the outside of the PVC pipe. The specific sealing method can be to use special glue and sealing grease for the casing to seal the lower contact surface to ensure that there will be no leakage.

[0046] 3) Put the steel pipe on the outside of the PVC pipe and ensure that it is concentric with the PVC pipe, and weld the steel pipe and steel plate to seal them.

[0047] 4) According to API standard, the density is 2.4g / cm 3 High-density cement slurry is poured into the annulus between the steel pipe and the PVC pipe, so that the annulus is filled with high-density cement slurry and waited until the cement is completely bonded;

[0048] 5) Take out the completely cemented cement ring to obtain the simulated stratum.

[0049] Specifically, a crane is used to pull out the PVC pipe coated with lubricating oil, so that the high-density cement that has been bonded is exposed. Since the acoustic properties of high-density cement stone are similar to those of sandstone, the high-density cement obtained by bonding can be regarded as a simulated stratum.

[0050] 6) The fan-shaped annular column with a set angle is tightly fitted to the outer wall of the casing, and the bottom is sealed and sleeved inside the simulated formation. It is seated on a steel plate, placed in the center, and concentric with the simulated formation to finally obtain a simulation device.

[0051] Among them, in this embodiment, the fan annular column with a set angle is closely fitted to the outer wall of the casing by using special glue and sealing grease for the casing. Of course, as other implementation methods, the fan annular column with a set angle can also be connected integrally with the outer wall of the casing.

[0052] It should be noted that the steel pipe in the above method is to consider the safety of the overall device. Since the model is relatively high, if PVC pipes are used, there will be a risk of damage and even personal safety accidents. In addition, the model needs to be moved during testing and processing, and the overall weight of the model exceeds two tons, so steel pipes are required.

[0053] Through the above-mentioned specific production process, the simulation device of the present invention can be obtained, and the above-mentioned embodiment only provides a method for implementing the production method. The selection of specific dimensions can be selected according to actual conditions, but in principle, it is necessary to ensure that the annular space gap between the simulated formation and the casing is not less than 2 cm, and the thickness of the simulated formation is not less than 20 cm. Therefore, when selecting casings of different sizes, the size of the simulated formation also needs to be modified accordingly.

[0054] Example of method for establishing cementing quality evaluation index

[0055] This embodiment is a method for establishing a cementing quality evaluation index based on the simulation device in the simulation device embodiment for establishing a cementing quality evaluation index. The method establishes a cementing quality evaluation index by measuring the acoustic amplitude of cement under different bonding states in the simulation device and by comparing the standard acoustic amplitude.

[0056] In this embodiment, when establishing the cementing quality evaluation standard, multiple simulation devices can be set according to different working conditions, and the fan-shaped cylinder of each simulation device is set to a different angle.

[0057] Specifically, before introducing the method for establishing cementing quality evaluation index of the present invention, a plurality of simulation devices are first equipped. In this embodiment, two simulation devices are taken as an example, that is, a simulation device of a fan annular column with a setting angle of 36° is used for well No. 1; a simulation device of a fan annular column with a setting angle of 108° is used for well No. 2. Figure 3 As shown, the following steps are included:

[0058] (1) Inject cement slurry that is configured according to API standards and that needs to be evaluated into the cement injection cavity of Well No. 1 and Well No. 2, respectively, inject water into the inner holes of the casing of Well No. 1 and Well No. 2, and wait for the cement to solidify until the hardness of the cement meets the logging requirements according to the ambient temperature.

[0059] In this embodiment, Well No. 1 (the setting angle of the fan annular column is 36°) corresponds to the lower limit of the scale cementing quality evaluation index medium bonding (the dividing line between high-quality and medium), and the setting angle of the fan annular column of Well No. 2 is 108°, which corresponds to the upper limit of the scale cementing quality evaluation index bonding qualification (the dividing line between medium and poor).

[0060] It should be noted that, according to the cementing quality evaluation index, if the cement bonding state is excellent, the proportion of cement slurry is high and the proportion of annular space loss is low; if the cement bonding state is poor, the proportion of cement slurry is low and the proportion of annular space loss is high; then, when the proportion of cement slurry is 90%, the annular space loss is 10%, and the corresponding setting angle of the fan-shaped annular column is 36°; when the proportion of cement slurry is 70%, the annular space loss is 30%, and the corresponding setting angle of the fan-shaped annular column is 108°; therefore, the specific setting angle in this embodiment is determined according to the proportion of cement slurry.

[0061] Specifically, the cement slurry proportion S is: S=1-θ / 360°, wherein θ is the set angle of the fan-shaped cylinder.

[0062] (2) Use the CBL logging method (CBL is acoustic amplitude logging) to measure the logging acoustic amplitudes A1 and A2 of Well 1 and Well 2 respectively, compare the obtained logging acoustic amplitudes A1 and A2 with the free casing acoustic amplitude A0, and obtain the relative acoustic amplitude P1 of the lower limit of the cement bonding state and the relative acoustic amplitude P2 of the upper limit of the cement bonding state.

[0063] Among them, the relative sound amplitude of the medium lower limit of cement bonding state is:

[0064]

[0065] The relative sound amplitude of the medium upper limit of cement bonding state is:

[0066]

[0067] Among them, A1 is the CBL sound amplitude measured by the simulation device with a setting angle of 36°, A2 is the CBL sound amplitude measured by the simulation device with a setting angle of 108°, and A0 is the free casing sound amplitude.

[0068] The free casing acoustic amplitude in this embodiment is the logging acoustic amplitude of the free casing well; the free casing well is the same size as the simulation device, and the free casing well is a simulation well when the casing inner hole and the annulus are both air or clean water, wherein the annulus is the annular space formed between the outer wall of the casing and the inner wall of the simulated formation.

[0069] (3) Based on the relative acoustic amplitude value P1 of the lower limit of cement bonding state and the relative acoustic amplitude value P2 of the upper limit of cement bonding state, cementing quality evaluation index is established, as shown in Table 2.

[0070] Table 2

[0071]

[0072] The simulation method in this embodiment can accurately establish cementing quality evaluation indicators; and for cement slurry systems of different density series and casing sizes of different specifications, the simulation device of the present invention can also be used to complete the establishment of cementing quality evaluation indicators.

[0073] The above description is only the preferred embodiment of the present invention. The present invention has been described in detail by general description and specific implementation mode, but it is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications or improvements. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of the claims of the present invention.

Claims

1. A method for establishing cementing quality evaluation index, characterized in that: The method is used for a simulation device for establishing cementing quality evaluation index, the simulation device comprising: a simulation formation, a casing and a fan annular column; The simulated stratum is a hollow cylinder; The sleeve has an inner hole, and the inner hole is used for injecting liquid; The sector annular column is arranged on the sleeve, the outer convex cylindrical surface of the sector annular column protrudes along the radial direction of the sleeve, the inner concave cylindrical surface of the sector annular column is tightly fitted with the outer wall of the sleeve, or the sector annular column and the sleeve are connected as one body; The casing is axially arranged in the simulated formation, the outer convex cylindrical surface of the fan-shaped cylinder is closely fitted with the inner wall of the simulated formation, and the fan-shaped cylinder is a hollow structure or made of a material with a density lower than that of cement used for cementing; The fan-shaped annular column extends at a set angle in the circumferential direction to continuously occupy the space between the inner wall of the simulated formation and the outer wall of the casing in the circumferential direction to simulate the annular space loss, and the remaining space between the inner wall of the simulated formation and the outer wall of the casing outside the annular space loss forms a cement injection cavity for injecting cement for cementing; The method comprises the following steps: 1) Injecting corresponding experimental media into the cement injection cavity and the inner hole of the casing of multiple simulation devices respectively; the fan-shaped annular columns of the multiple simulation devices are set to different angles θ; Among them, S=1-θ / 360°, where S is the cement slurry ratio and θ is the setting angle of the fan ring column; 2) using the acoustic amplitude logging method to measure the logging acoustic amplitude of each simulation device in step 1), comparing the obtained logging acoustic amplitude of each simulation device with the acoustic amplitude of the free casing, and obtaining the relative acoustic amplitude of the lower limit of the cement bonding state and the relative acoustic amplitude of the upper limit of the cement bonding state; The expressions of the relative acoustic amplitudes of the lower and upper limits of the cement bonding state are as follows: Among them, A is the acoustic amplitude corresponding to each simulated device measured, and A0 is the acoustic amplitude of the free casing; The free casing acoustic amplitude is the logging acoustic amplitude of the free casing well; the free casing well is the same size as the simulation device, the annulus of the free casing well is a simulation well when air or water is used, and the annulus is the annular gap formed between the outer wall of the casing and the inner wall of the simulated formation; 3) Establish cementing quality evaluation index based on the relative acoustic amplitude value of the lower medium limit of cement bonding state and the relative acoustic amplitude value of the upper medium limit of cement bonding state.

2. The method for establishing cementing quality evaluation index according to claim 1, characterized in that: Step 2) A simulation device for a sector ring-shaped column with a set angle of 36° corresponding to the medium lower limit of cement bonding state; a simulation device for a sector ring-shaped column with a set angle of 108° corresponding to the medium upper limit of cement bonding state.

3. The method for establishing cementing quality evaluation index according to claim 1, characterized in that: The fan-shaped cylinder is made of foam plastic.

Citation Information

Patent Citations

  • Well cementation cement sheath performance simulation experiment device and experiment method

    CN102979505A

  • Device and method for evaluating influence of pressure change on completeness of cement sheath

    CN104500034A

  • Method for evaluating cement bond quality of two interfaces of cased well

    CN105134170A

  • Method for evaluating integrity of well cementing barrier

    CN106499383A

  • Device and method for evaluating completeness of casing pipe in fracturing environment