Positive photosensitive resin composition, cured film and pattern processing method thereof

By using the substance of structural formula (a3) ​​in the positive photosensitive resin composition to generate a polyimide structure, the problems of low alkali solubility and difficulty in controlling the imidization rate of alkali-soluble resins before exposure are solved, and the exposure sensitivity is improved. and developing resolution, suitable for insulation layer applications in a variety of electronic components.

CN112180684BActive Publication Date: 2024-10-11WUHAN ROUXIAN SCIENCE & TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011171907.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-28
Publication Date
2024-10-11
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

The existing positive-type photosensitive resin composition has low alkali solubility before exposure to the alkali-soluble resin and the imidization rate is difficult to accurately control, resulting in low exposure sensitivity and low image resolution.

Method used

A substance containing structural formula (a3) ​​is used to participate in the reaction to generate a polyimide structure. By regulating the proportion of the substance, the imidization rate in the alkali-soluble resin is precisely controlled to improve exposure sensitivity and development resolution.

Benefits of technology

It achieves precise control of the imidization rate of alkali-soluble resins at lower temperatures, improves exposure sensitivity and development resolution, and is suitable for applications such as semiconductor components, EL components, and the insulating layer of TFTs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The present invention provides a positive photosensitive resin composition that can be developed by alkali after exposure and has good exposure sensitivity and high pattern resolution, a cured film obtained by curing the positive photosensitive resin composition, and a pattern processing method of the cured film. The positive photosensitive resin composition of the present invention contains (a) 100 parts by weight of an alkali-soluble resin, (b) 10-30 parts by weight of a photoacid generator, (c) 20-60 parts by weight of a thermal crosslinking agent, and (d) an organic solvent, wherein the main chain structure of the alkali-soluble resin (a) contains a structural unit having a structural formula (a1) and a structural unit having a structural formula (a2), and a part of the structural unit of the structural formula (a2) is a product of a reaction between a structural unit of the structural formula (a3) ​​and a diamine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive photosensitive resin composition and a cured film. More specifically, the present invention relates to a positive photosensitive resin composition suitable for use as a surface protective film of a semiconductor element, an interlayer insulating film, an insulating layer of an organic electroluminescent (EL) element, an insulating layer of a thin film transistor (TFT), etc., and a cured film using the same. Background Art

[0002] Polyimide (PI) is an ideal polymer material with excellent heat resistance, mechanical properties, electrical insulation and chemical stability, and is often used in aerospace, semiconductor, optoelectronics and microelectronics. Compared with ordinary polyimide, photosensitive polyimide (PSPI) does not require other photoresists to achieve graphic processing, shortening the process route, and is an ideal insulating material in the electronics and microelectronics fields.

[0003] In recent years, with the miniaturization of semiconductor components, the intermediate insulating film, passivation layer, etc. of the semiconductor components also require finer exposure and development sensitivity and image resolution; based on this, in the prior art, a photosensitive polyimide resin composition varnish is often used on the surface of the semiconductor component, and developed under alkaline conditions after exposure, so as to obtain an ideal pattern; but this often places high requirements on the exposure sensitivity and development resolution of the photosensitive polyimide resin composition.

[0004] At present, known positive photosensitive resin compositions include: soluble resins such as polyamic acid, polyamic acid / polyimide, polyamic acid ester / polyamic acid, and photoacid generators (such as naphthoquinone diazide), thermal crosslinking agents, and solvent compositions. Known, polyamic acid has a large solubility in alkaline solutions, and adding a photoacid generator naphthoquinone diazide can make the photosensitive resin composition resistant to alkali to a certain extent, but after exposure, it is almost impossible to obtain a desired pattern (CN1246389C) (low image resolution). Therefore, in order to regulate the alkali solubility of polyamic acid, polyamic acid / polyimide resin compositions (CN1154708C, CN104854508A, CN102985877A, CN1457454A) have been developed. However, due to the close relationship between the ratio of polyimide in the polyamic acid / polyimide resin composition to solubility and the transmittance of ultraviolet light, exposure sensitivity and image resolution have a greater impact. Therefore, the polyamic acid / polyimide resin composition can have higher exposure sensitivity and development resolution by controlling the ratio of polyimide in the composition.

[0005] At present, the publicly reported methods for synthesizing polyamic acid / polyimide include chemical imide method, thermal imide method and imide monomer polymerization method. Among them, chemical imide and thermal imide can easily obtain polymers with an imide rate of more than 80%. It is still difficult to accurately control the imidization rate in the resin composition within a specific range, especially in actual production and process. Summary of the invention

[0006] The object of the present invention is to provide a positive photosensitive resin composition, a cured film and a pattern processing method thereof, wherein the positive photosensitive resin composition can solve the problems of low alkali solubility of alkali-soluble resin before exposure (unexposed) and difficulty in controlling the imidization rate. The alkali-soluble resin in the positive photosensitive resin composition provided by the present invention uses a substance containing structural formula (a3) ​​to participate in the reaction, directly generating a polyimide structure, and can accurately control the imidization rate in the alkali-soluble resin, thereby obtaining higher exposure sensitivity and development resolution.

[0007] The first aspect of the present invention adopts the following technical solution:

[0008] A positive photosensitive resin composition, characterized in that it contains the following components:

[0009] (a) 100 parts by weight of an alkali-soluble resin, wherein the main chain structure of the alkali-soluble resin comprises a structural unit having a structural formula (a1) and a structural unit having a structural formula (a2);

[0010] (b) a photoacid generator, 10-30 parts by weight;

[0011] (c) thermal crosslinking agent, 20-60 parts by weight;

[0012] (d) organic solvents;

[0013]

[0014] In the above structural formula (a1) and structural formula (a2), X represents a reaction residue of a tetraacid or a dianhydride, and P and Q represent reaction residues of a diamine; at least one of the groups X, Y, P, and Q contains a fluorine atom, and the mass ratio of the fluorine atom to the alkali-soluble resin (a) is 5-25%, and at least one of the groups X, Y, P, and Q also contains one or more of a hydroxyl group, a carboxyl group, and a sulfonic acid group;

[0015] The structural formula (a2) is prepared from a methylene derivative of a dianhydride having a structural formula (a3);

[0016]

[0017] The methylene derivative of the dianhydride R 1It represents the reaction residues of dianhydrides including the following structures: 2,2-bis(3,4-dicarboxylic acid phenyl)hexafluoropropane dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, fluoropyromellitic dianhydride, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, cyclobutanetetracarboxylic dianhydride.

[0018] As a further embodiment, the tetraacid comprises one or more combinations of tetraacids prepared from the following structural dianhydrides: 2,2-bis(3,4-dicarboxylic acid phenyl)hexafluoropropane dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, cyclobutane tetracarboxylic dianhydride, 3,3',4, 4'-biphenyltetracarboxylic dianhydride and dianhydrides of the following structures;

[0019]

[0020] As a further embodiment, the diamine comprises one or more combinations of the following diamine compounds: 4,4'-diaminodiphenyl ether, bis(4-aminophenyl)hexafluoropropane, 3,5-diaminobenzoic acid, bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 4,4'-diaminotetrafluorodiphenyl ether, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 1,1,3,3-tetramethyl-1,3-bis(3-aminopropyl)disiloxane, and diamines of the following structures.

[0021]

[0022] Furthermore, in the methylene derivative of the dianhydride, R 1 represents the reaction residue of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride;

[0023] Furthermore, the structural unit of the structural formula (a3) ​​reacts with the diamine at low temperature, and the reaction temperature is 20-120°C.

[0024] Furthermore, the ratio of the structural unit of the structural formula (a1) to the alkali-soluble resin (a) is 20-80 mol%, the ratio of the structural unit of the structural formula (a2) to the alkali-soluble resin (a) is 10-80 mol%, 10 mol%-25 mol% of the alkali-soluble resin (a) is derived from the structural formula (a3), and the imidization rate of the alkali-soluble resin (a) is 20-50%.

[0025] Furthermore, the end-capping groups of the main chain structure of the (a) alkali-soluble resin have structures represented by general formula (1) and / or (2), A is derived from a primary monoamine, and B is derived from a dianhydride.

[0026]

[0027] Furthermore, X and Y are one or more of an aromatic structure or an aliphatic structure, and P and Q are one or more of an aromatic structure, an aliphatic structure, and a silicon-containing structure.

[0028] A second aspect of the present invention provides a cured film obtained by curing the positive photosensitive resin composition.

[0029] The third aspect of the present invention provides a method for pattern processing of a cured film, which comprises the following steps: coating the positive photosensitive resin composition on a substrate, drying at 40-120°C for 1-10 minutes to form a photosensitive resin composition film; exposing the film under a mask; removing the exposed portion of the film using an alkaline developer, developing and cleaning; curing and drying the developed film at 100-400°C to obtain a cured film containing a desired pattern.

[0030] The beneficial effects of the present invention are to provide a positive photosensitive resin composition, a cured film and a pattern processing method thereof. The alkali-soluble resin in the positive photosensitive resin composition uses a substance containing structural formula (a3) ​​to participate in the reaction at a relatively low temperature to directly generate a polyimide structure. Therefore, by controlling the proportion of the substance containing structural formula (a3) ​​during feeding, the imidization rate in the alkali-soluble resin can be accurately controlled, and the solubility of the alkali-soluble resin can be regulated, thereby obtaining higher exposure sensitivity and development resolution. DETAILED DESCRIPTION

[0031] Hereinafter, specific embodiments of the positive photosensitive resin composition, cured film and pattern processing method thereof according to the present invention are described in detail, but the present invention is not limited to the embodiments including the following examples and can be modified in various ways within the scope of the gist of the invention so as to achieve the purpose of the invention.

[0032] <Positive photosensitive resin composition>

[0033] The positive photosensitive resin composition of the present invention is composed of (a) an alkali-soluble resin, (b) a photoacid generator, (c) a thermal crosslinking agent and (d) an organic solvent.

[0034] (a) Alkali soluble resin

[0035] The above-mentioned (a) alkali-soluble resin contains a structural unit having a structural formula (a1) and a structural unit having a structural formula (a2), that is, the (a) alkali-soluble resin has a main chain structure represented by the general formula (1).

[0036]

[0037] Wherein m is an integer from 10 to 50,000, and n is an integer from 10 to 50,000.

[0038] In the general formula (1), X and Y represent the reaction residues of tetravalent dianhydrides or dicyanomethylene derivatives of dianhydrides, P and Q represent the reaction residues of divalent diamines, the structural unit of the structural formula (a1) represents a polyimide precursor, and the structural unit of the structural formula (a2) represents a polyimide; the structural unit of the structural formula (a2) can be obtained by the imidization reaction of dianhydrides and diamines, and can also be obtained by the reaction of a substance containing the structural formula (a3) ​​and diamines.

[0039] Structural unit of formula (a1)

[0040] As the dianhydride required for synthesizing the structural unit of the structural formula (a1), X represents a reaction residue of the dianhydride, and the dianhydride containing X can be specifically selected from pyromellitic dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 2,3,5,6-pyridinetetracarboxylic dianhydride, bicyclo[3.1.1]hept-2-enetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, bicyclo[2.2.2]octanetetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, adamantanetetracarboxylic dianhydride, 2,2',3,3'- Biphenyltetracarboxylic dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, cyclobutanetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, cyclohexanetetracarboxylic dianhydride, 2,2-bis(3,4- Other aromatic dianhydrides or aliphatic dianhydrides such as 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride and bicyclo[3.3.1]tetracarboxylic dianhydride, and dianhydrides of the following structures can be used alone or in combination of two or more.

[0041]

[0042] Here, R 2 Indicates the selection of oxygen atoms, -C(CF 3 ) 2 -、-C(CH 3 ) 2 -, -CO-, -COO- or -SO 2- The group in R3 and R 4 Respectively indicate the selection of -H and -CF 3 , -OH and -SH groups.

[0043] The appropriate introduction of F atoms can inhibit the penetration to the interface during development in alkaline aqueous solution, have appropriate hydrophobicity at the membrane interface, and improve the solubility of the polymer in organic solvents. Some X structures containing F dianhydride can also be listed as follows:

[0044]

[0045] Among the above dianhydrides, 2,2-bis(3,4-dicarboxylic acid phenyl)hexafluoropropane dianhydride 6FDA, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride ODPA, cyclobutane tetracarboxylic dianhydride CBDA, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dianhydrides of the following structures;

[0046]

[0047] As the diamine required for synthesizing the structural unit of the structural formula (a1), P represents a diamine residue, and the diamine containing P can be selected specifically from m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methane, bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxy)biphenyl, bis(3-amino-4-hydroxyphenyl)fluorene, 1,4-bis(4-aminophenoxy)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3, 3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-5,5'-dihydroxybenzidine, 3,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, 4, 4'-diaminodiphenyl ether, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 3,5-diaminobenzoic acid, 3-carboxy-4,4'-diaminodiphenyl ether, and diamines of the following structures. These diamines may be used alone or in combination of two or more.

[0048]

[0049]

[0050] Here, R 5 Indicates selection -O-, -C(CF 3 ) 2 -、-C(CH 3 ) 2 -, -CO-, -COO- or -SO 2 -The group in R 3 ~R 11 Respectively indicate the selection of -H and -CF 3 , -OH and -SH groups.

[0051] Among the above diamines, 4,4'-diaminodiphenyl ether, bis(4-aminophenyl)hexafluoropropane, 3,5-diaminobenzoic acid, bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 4,4'-diaminotetrafluorodiphenyl ether, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, and diamines of the following structures are preferred.

[0052]

[0053] Structural unit of formula (a2)

[0054] The structural unit of the structural formula (a2) can be obtained by the imidization reaction of a methylene derivative of a dianhydride as shown in the structural formula (a3) ​​and a diamine.

[0055] Y represents the residue of the reaction product of a dianhydride derivative and a diamine, wherein the dianhydride derivative is as shown in the structural formula (a3), and R 1 The reaction residue of a dicyanomethylene derivative of a dianhydride. In particular, the dianhydride derivative can directly react with a diamine to form a polyimide structure at a relatively low temperature. The dianhydride derivative can be derived from the dianhydride required for the structural unit of the synthetic structural formula (a2) listed above. The dianhydride derivative can also be used alone or in combination of two or more.

[0056] Among the above-mentioned dianhydride derivatives, dianhydride derivatives formed from 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, cyclobutanetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylethertetracarboxylic dianhydride, fluoropyromellitic dianhydride and dianhydrides of the following structures are preferred:

[0057]

[0058] Here, R 2 Indicates selection -O-, -C(CF 3 ) 2- 、-C(CH 3 ) 2 -, -CO-, -COO- or -SO 2 -The group in R 3 and R 4 Respectively indicate the selection of -H and -CF 3 , -OH and -SH groups.

[0059] Among the above-mentioned dianhydride derivatives, the structure shown below is more preferred:

[0060]

[0061]

[0062] R 12 Indicates the selection of -O- or -C(CF 3 ) 2- ; R 3 and R 4 Represent -OH respectively.

[0063] As the diamine required for synthesizing the structural unit of the structural formula (a2), Q represents the reaction residue of the diamine, and the selection range of the diamine containing Q is the same as the selection range of the diamine containing P, and the preferred range is also the same. These diamines can be used alone or in combination of two or more. However, P and Q in the general formula (1) may be the same or different.

[0064] When synthesizing the (a) alkali-soluble resin, according to the reaction rules of different monomers, a suitable dicyanomethylene derivative of dianhydride / dianhydride is selected to react with a diamine. By adjusting the ratio of the dianhydride derivative Y represented by the structural formula (a3) ​​and the tetravalent dianhydride X of the structural formula (a1), the ratio of the structural units of the structural formula (a2) to the structural units of the structural formula (a1) in the (a) alkali-soluble resin, i.e., n / m, can be adjusted, thereby adjusting the imidization rate of the (a) alkali-soluble resin, and finally achieving the goal of adjusting the alkali solubility of the positive photosensitive resin composition and improving the development resolution.

[0065] Furthermore, in order to improve adhesion to the substrate, etc., 0-10 mol% of the total diamine may be an aliphatic group having a siloxane structure within a range that does not reduce heat resistance. Specifically, diamines such as 1,1,3,3-tetramethyl-1,3-bis(3-aminopropyl)disiloxane and bis(p-aminophenyl)octamethylpentasiloxane are listed, and 1,1,3,3-tetramethyl-1,3-bis(3-aminopropyl)disiloxane is preferred.

[0066] End-capping group

[0067] At the end of the main chain structure of the (a) alkali-soluble resin represented by the general formula (1), there is an end-capping group represented by the general formula (2) and / or the general formula (3).

[0068] In the general formula (2), A is derived from a primary monoamine of an end-capping group. Examples of the primary monoamine of an end-capping group include 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 2-aminophenol, 3-aminophenol, 4-aminophenol, 3-amino-4,6-dihydroxypyrimidine, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, etc., which can be used alone or in combination of two or more. The primary monoamine of the end-capping group accounts for 0-50 mol %, and particularly preferably 5-30 mol %, of the total amine components.

[0069] In the general formula (3), B is derived from the dianhydride of the end-capping group. Examples of the dianhydride of the end-capping group include phthalic anhydride, maleic anhydride, nadic anhydride, cyclohexanedicarboxylic anhydride, etc., which can be used alone or in combination of two or more. The dianhydride of the end-capping group accounts for 0-50 mol %, and particularly preferably 5-30 mol % of the total anhydride components.

[0070] (b) Photoacid generator

[0071] The positive photosensitive resin composition of the present invention also uses (b) a photoacid generator, which can include quinonediazide compounds (naphthoquinonediazidesulfonate compounds), sulfonium salts, phosphonium salts, diazonium salts, iodonium salts, etc., which can be used alone or in combination of two or more. These quinonediazide compounds can be synthesized by esterification reaction of phenolic hydroxyl compounds with quinonediazidesulfonyl chloride. In the present invention, the quinonediazide compound preferably uses a compound in which 5-naphthoquinonediazidesulfonyl or 4-naphthoquinonediazidesulfonyl is bonded to a compound having a phenolic hydroxyl group.

[0072] Specific examples of phenolic hydroxy compounds include the following structures:

[0073]

[0074]

[0075] As the quinonediazide compound, the molecular structure preferably has any one or more of the naphthoquinonediazidesulfonate structures. Specifically, the following commercial photoacid generators PAC-1 to PAC-20 can be used, and any one or more of the following substances can be used in combination.

[0076]

[0077]

[0078] The amount of the photoacid generator (b) added is 5 to 40 parts by weight, preferably 10 to 30 parts by weight, based on 100 parts by weight of the alkali-soluble resin (a).

[0079] (c) Thermal crosslinking agent

[0080] The positive photosensitive resin composition of the present invention contains (c) a thermal crosslinking agent. The thermal crosslinking agent can react with the alkali-soluble resin (a) by heating to crosslink, thereby improving the chemical resistance of the cured film. Examples of the thermal crosslinking agent (c) include (c1) epoxy compounds and (c2) alkoxy / hydroxymethyl compounds. The (c1) epoxy compound is preferably a compound containing two or more epoxy groups in one molecule, and examples thereof include bisphenol A type epoxy resin, bisphenol A type oxetane resin, bisphenol F type epoxy resin, bisphenol F type oxetane resin, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, polymethyl (glycidyloxypropyl) siloxane and other epoxy-containing silicones, but are not limited to these. Specifically, there are Dainippon Ink and Chemical Industry EPICLON, EXA and other series products, Yuka Shell Epoxy Co. Ltd.'s Epikote series of bisphenol A type epoxy compounds and ADEKA's EP series. (c2) Alkoxy / hydroxymethyl compounds preferably have two or more functional groups of 2 to 8 in one molecule, and examples thereof include Honshu Chemical's trade names DML, TriML, DMOM, HMOM, TMOM and the like series, and Sanwa Chemical's MX and MW series. The positive photosensitive resin composition of the present invention may contain one or more of the above-mentioned thermal crosslinking agents.

[0081] The amount of the thermal crosslinking agent (c) added is 15 to 100 parts by weight, preferably 20 to 60 parts by weight, based on 100 parts by weight of the alkali-soluble resin (a).

[0082] (d) Organic solvents

[0083] The positive photosensitive resin composition of the present invention contains (d) an organic solvent. Specific examples of usable organic solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, propyl acetate, butyl acetate, methyl lactate, ethyl lactate, butyl lactate, bis(2-methoxyethyl) ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, methyl ethyl ketone, cyclohexanone, cyclopentanone, butanol, isobutanol, amyl alcohol, γ-butyrolactone, N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, etc., but are not limited to these.

[0084] <Cured film>

[0085] The cured film involved in the present invention is a film obtained by curing the positive photosensitive resin composition of the present invention.

[0086] <Pattern processing method>

[0087] The following is a detailed description of a pattern processing method for forming a resin pattern using the positive photosensitive resin composition of the present invention.

[0088] The coating method of the positive photosensitive resin composition may include spin coating, spray coating, blade coating, screen coating, slit coating and the like. It is usually preferred to coat the composition in such a manner that the film thickness after drying becomes 0.5 to 50 μm. Drying may be performed using an oven, a hot plate, an infrared oven, etc., at 40°C to 120°C for 1 min to 10 min, or by step-programmed temperature drying to volatilize the organic solvent. The substrate may be a silicon wafer, a ceramic, a gallium arsenic, an organic circuit board, an inorganic circuit board, and a substrate having a circuit component material arranged thereon, but is not limited thereto.

[0089] After the coating and drying process, a positive photosensitive resin composition film is formed on the substrate. The film is exposed by irradiating exposure light through a mask having a desired pattern. The exposure light source is preferably the i (365nm), h (405nm), and g (436nm) rays of a mercury lamp. The exposure device can use a reduced projection type exposure device, a mask aligner, a mirror projection type exposure device, etc.

[0090] After exposure, the exposed part of the film is removed using a developer. As the developer, aqueous solutions of alkaline compounds such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, dimethylamine, dimethylaminoethanol, cyclohexylamine, and ethylenediamine are preferred. In addition, one or a combination of organic solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, methanol, ethanol, isopropanol, ethyl lactate, cyclopentanone, cyclohexanone, and acetone can be added to these alkaline aqueous solutions.

[0091] The developing method can be spray developing, immersion developing, ultrasonic immersion developing and other methods. The developing time, developing temperature, developing steps and other conditions are the conditions for removing the exposed part. After development, the film is preferably rinsed with water, or it can be rinsed with an aqueous solution of alcohols and esters such as ethanol, isopropanol, ethyl lactate, etc. If necessary, the film can be baked before development, the baking temperature is 60-150°C, preferably 60-120°C, and the baking time is 5s-60min. After rinsing, the film is heated and dried in the range of 60-200°C, and the drying time is controlled in 1min-60min.

[0092] After exposure, development and rinsing, the positive photosensitive resin composition of the present invention is subjected to a staged program temperature rise / constant temperature heat treatment in the range of 100 to 400°C to cure and form a cured film. The temperature rise / constant temperature heat treatment method can be listed as, for example, starting from room temperature at a heating rate of 5°C / min, and then performing constant temperature heat treatment at 120°C and 180°C for 30 minutes, respectively, and then heating to 250°C for constant temperature heat treatment for 2 hours. Alternatively, the temperature is raised from room temperature to 250°C within 2 hours, and then the temperature is kept constant for 2 hours at 250°C. The temperature rise / constant temperature heat treatment can be carried out under normal pressure, nitrogen or vacuum. Curing obtains a cured film containing an ideal pattern with heat resistance.

[0093] The cured film having a desired pattern formed by the positive photosensitive resin composition of the present invention can be used as a surface protection film of a semiconductor element, an interlayer insulating film, an insulating layer of an organic electroluminescent (EL) element, an insulating layer of a thin film transistor (TFT), etc., but is not limited to these.

[0094] Example

[0095] The present invention is described below with reference to examples, but the present invention is not limited to these examples. First, the evaluation method in each example and comparative example is described. The evaluation used a resin composition (hereinafter referred to as varnish) that was previously filtered using a 1 μm polytetrafluoroethylene filter.

[0096] < Imidization rate of alkali-soluble resin >

[0097] (a) The imidization rate of the alkali-soluble resin was obtained by applying a 50% by mass N-methylpyrrolidone (hereinafter referred to as NMP) solution of the alkali-soluble resin on a 6-inch silicon wafer by spin coating, followed by baking for 3 minutes using a 120°C hot plate (SKW-636 manufactured by Dainippon Screen Manufacturing Co., Ltd.) to prepare a pre-baked film having a thickness of 10 μm ± 1 μm. The film was divided into two halves, one half of which was placed in an inert gas oven (INH-21CD manufactured by Koyo ThermoSystems), raised to a curing temperature of 350°C over 30 minutes, and heated at 350°C for 60 minutes. Then, the film was slowly cooled to a temperature of 50°C or less in the oven to obtain a cured film. The infrared absorption spectrum of the obtained cured film (A) and the film before curing (B) was measured using a Fourier transform infrared spectrophotometer FT-720 (manufactured by Horiba, Ltd.). Calculate the 1377cm wavelength derived from the CN stretching vibration of the imide ring -1 The peak intensity near the imidization ratio was determined as "peak intensity of the film before curing (B) / peak intensity of the cured film (A)".

[0098] <Production of Developed Film>

[0099] The positive photosensitive resin composition of the present invention (hereinafter referred to as varnish) was coated on a 6-inch silicon wafer to a film thickness of 10 μm after prebaking, and then prebaked at 120°C for 4 minutes using a hot plate (SCW-636; Dainippon Screen Manufacturing Co., Ltd.) to obtain a prebaked film. A small photolithography developer (AC3000) was used at the i, g, and h lines with an exposure of 0 to 1000 mJ / cm 2 In the case of 10mJ / cm 2 After exposure, the film was developed in a 2.38 mass % TMAH aqueous solution for 90 seconds and then rinsed with water to obtain a developed film having an isolated pattern.

[0100] <Calculation of residual film rate>

[0101] Residual film rate (%) = film thickness after development ÷ film thickness after pre-baking × 100%

[0102] <Sensitivity>

[0103] Using a coating and developing device ACT-8 (manufactured by Tokyo Electron Limited), the varnish was applied to a 6-inch silicon wafer by spin coating and pre-baked at 120°C for 3 minutes. Exposure was performed using an i-line stepper exposure machine NSR-2005i9C (manufactured by Nikon). After exposure, the ACT-8 developing device was used to repeatedly develop twice using a 2.38 wt % tetramethylammonium aqueous solution (hereinafter referred to as TMAH, manufactured by Tama Chemical Industry) using a puddle method (the developer discharge time was 10 seconds and the puddle time was 40 seconds). After washing with pure water, the film was spun dry, and the minimum exposure when the exposed part was completely dissolved was used as the sensitivity. If the minimum exposure is 400mJ / cm 2 Below 300 mJ / cm2, it can be judged as high sensitivity. More preferably, it is 300 mJ / cm2. 2 the following.

[0104] <Resolution>

[0105] The film obtained by coating the varnish was patterned exposed using the i-line (wavelength 365nm), h-line (wavelength 405nm) and g-line (wavelength 436nm) of an ultra-high pressure mercury lamp using a double-sided alignment single-sided exposure device (mask aligner PEM-6M; manufactured by Union Optical Co., Ltd.) through a grayscale mask for sensitivity measurement (MDRM MODEL 4000-5-FS; manufactured by OptoLine International), and then developed using a small developer for photolithography (AD-2000; manufactured by Takizawa Sangyo Co., Ltd.), and then cured using a high-temperature inert oven (INH-9CD-S; manufactured by Koyo Thermo Systems Co., Ltd.) to obtain a cured film. The resolution pattern of the cured film was observed using an FPD / LSI inspection microscope (OPTIPHOT-330; manufactured by Union Co., Ltd.). The minimum pattern size of the line and space pattern obtained without residue was taken as the resolution.

[0106] <Pattern Evaluation of Developed Film>

[0107] The photosensitive resin composition film formed by development was visually observed for tackiness in the unexposed portion and residue in the exposed portion. The developed film was judged as good if there was no problem with the pattern, and judged as poor if tackiness occurred in the unexposed portion or residue occurred in the exposed portion.

[0108] The following is a detailed description of the embodiments of the present invention. First, the abbreviations corresponding to some monomers involved in the embodiments are described.

[0109] 6FDA: 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride

[0110] ODPA: 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride

[0111] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0112] TFMB: 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl

[0113] CBDA: Cyclobutanetetracarboxylic dianhydride

[0114] ODA: 4,4'-diaminodiphenyl ether

[0115] SiDA: 1,1,3,3-Tetramethyl-1,3-bis(3-aminopropyl)disiloxane

[0116] 6FAP: Bis(3-amino-4-hydroxyphenyl)hexafluoropropane

[0117] 6FODA: 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether

[0118] THF: Tetrahydrofuran

[0119] DIPA: Diisopropylamine

[0120] NMP: N-methylpyrrolidone

[0121] Synthesis example 1

[0122] Synthesis of 6FDA Dianhydride Derivative Y1

[0123] Add 6FDA (0.0245 mol) and dicyanomethane (0.049 mol) to a three-necked flask, dissolve them in 300 ml of tetrahydrofuran (THF), and add DIPA (0.099 mol, about 14 ml) dropwise within 1 hour. After the addition is complete, continue stirring at room temperature for 20 hours to obtain a yellow precipitate, which is filtered. The filter cake is washed with dry THF and vacuum dried at 100°C for 2 days.

[0124] Take the dried filter cake (3.36 mol) and dissolve it in 50 ml of dichloromethane. Then, add nitrogen and 1.2 ml of phosphorus oxychloride (POCl 3 ), under nitrogen, stirred at room temperature for 20 hours, filtered. The filter cake was washed with dry dichloromethane to obtain a crude product. The crude product was recrystallized in acetic anhydride and then dried to obtain the dianhydride derivative Y1 of 6FDA.

[0125] Synthesis example 2

[0126] Synthesis of ODPA Dianhydride Derivative Y2

[0127] The 6FDA in Synthesis Example 1 was replaced by ODPA, while other conditions remained unchanged, to obtain the dianhydride derivative Y2 of ODPA.

[0128] Synthesis example 3

[0129] Synthesis of BPDA Dianhydride Derivative Y3

[0130] The dianhydride derivative Y3 of BPDA was obtained by replacing 6FDA in Synthesis Example 1 with BPDA while keeping other conditions unchanged.

[0131] Synthesis example 4

[0132] Synthesis of Dianhydride Derivative Y4 of F-Generated Pyromellitic Dianhydride

[0133] The 6FDA in Synthesis Example 1 is replaced by F-generation pyromellitic dianhydride (structural formula is as follows), and other conditions remain unchanged to obtain the dianhydride derivative Y4 of F-generation pyromellitic dianhydride.

[0134]

[0135] Synthesis example 5

[0136] Synthesis of Dianhydride Derivative Y5 of Trimellitic Anhydride Derivative of TFMB

[0137] The 6FDA in Synthesis Example 1 was replaced by the bis-trimellitic anhydride derivative of TFMB (structural formula as follows), and other conditions remained unchanged to obtain the dianhydride derivative Y5 of the bis-trimellitic anhydride derivative of TFMB.

[0138]

[0139] Synthesis Example 6 Synthesis of CBDA Dianhydride Derivative Y6

[0140] The dianhydride derivative Y6 of CBDA was obtained by replacing 6FDA in Synthesis Example 1 with CBDA while keeping other conditions unchanged.

[0141] Synthesis Example 7

[0142] Synthesis of Alkali Soluble Resin A1

[0143] Under a dry nitrogen flow, 6FDA (0.020 mol) and Y1 (0.020 mol) were dissolved in NMP (100 g), and then ODA (0.008 mol), SiDA (0.002 mol), 3,5-diaminobenzoic acid (0.010 mol), 6FAP (0.018 mol), and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 2 h. Then 3-aminophenol (0.004 mol) was added, and the mixture was reacted at 25°C for 24 h; the mixture was then heated to 40°C for 2 h, and then heated to 60°C for 2 h. The mixture was precipitated in a solvent of 2L ethanol: water = 2:1 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 2:1 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of the alkali-soluble resin A1, and the infrared absorption spectrum was measured, and the imide rate was 45.1%.

[0144] Synthesis example 8

[0145] Synthesis of Alkali Soluble Resin A2

[0146] Under a dry nitrogen stream, bis(4-aminophenyl)hexafluoropropane (0.016 mol), 6FAP (0.016 mol), and SiDA (0.002 mol) were dissolved in NMP (100 g). Y2 (0.020 mol), CBDA (0.020 mol), and 40 g NMP were then added thereto, and the mixture was reacted at 25°C for 2 h. 4-aminosalicylic acid (0.012 mol) was then added, and the mixture was reacted at 25°C for 48 h, and then the mixture was heated to 60°C for 6 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A2, and the infrared absorption spectrum was measured, and the imide rate was 49.0%.

[0147] Synthesis example 9

[0148] Synthesis of Alkali Soluble Resin A3

[0149] Under a dry nitrogen flow, 6FAP-derived diamine (structural formula as follows) (0.032 mol) and SiDA (0.002 mol) were dissolved in NMP (100 g). BPDA (0.020 mol), Y3 (0.020 mol), and NMP (40 g) were then added thereto, reacted at 25°C for 2 h, and then 3-aminophenol (0.012 mol) was added, reacted at 25°C for 48 h, and then heated to 60°C for 4 h; precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, filtered the precipitate, washed the filter cake several times with ethanol: water = 1:3 (volume ratio), and dried the filter cake in vacuum at 50°C for 72 h to obtain a powder of alkali-soluble resin A3, and measured the infrared absorption spectrum, with an imide rate of 47.2%.

[0150]

[0151] Synthesis example 10

[0152] Synthesis of Alkali Soluble Resin A4

[0153] Under a dry nitrogen flow, the diamine (0.028 mol), ODA (0.008 mol), and SiDA (0.002 mol) shown in the following formula were dissolved in NMP (100 g). Subsequently, 6FDA (0.020 mol), Y4 (0.020 mol), and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 2 h. 3-aminophenol (0.004 mol) was then added, and the mixture was reacted at 25°C for 48 h. The mixture was then heated to 60°C for 2 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate. The precipitate was filtered, and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of the alkali-soluble resin A4. The infrared absorption spectrum was measured, and the imide rate was 49.4%.

[0154]

[0155] Synthesis example 11

[0156] Synthesis of Alkali Soluble Resin A5

[0157] Under a dry nitrogen flow, the diamine (0.034 mol) and SiDA (0.002 mol) in the following formula were dissolved in NMP (100 g). Then 6FDA (0.020 mol), Y5 (0.020 mol), and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 2 h. 3-aminophenol (0.008 mol) was added, and the mixture was reacted at 25°C for 48 h, and then the mixture was heated to 60°C for 6 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A5. The infrared absorption spectrum was measured, and the imide rate was 48.9%.

[0158]

[0159] Synthesis example 12

[0160] Synthesis of Alkali Soluble Resin A6

[0161] Under a dry nitrogen stream, 4,4'-diaminotetrafluorodiphenyl ether (0.034 mol) and SiDA (0.003 mol) were dissolved in NMP (100 g); then 6FAP-derived dianhydride (structural formula below) (0.020 mol), Y6 (0.020 mol), and 40 g NMP were added thereto, and the mixture was reacted at 25°C for 2 h, and then 3-aminophenol (0.060 mol) was added, and the mixture was reacted at 25°C for 48 h, and then the mixture was heated to 60°C for 6 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered, and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A6, and the infrared absorption spectrum was measured, and the imide rate was 47.6%.

[0162]

[0163] Synthesis example 13

[0164] Synthesis of Alkali Soluble Resin A7

[0165] Under a dry nitrogen flow, the derivative diamine of 6FAP (structural formula as follows) (0.035 mol) and SiDA (0.002 mol) were dissolved in NMP (100 g). BPDA (0.025 mol), Y2 (0.015 mol), and NMP (40 g) were then added thereto and reacted at 25°C for 2 h. 3-Aminophenol (0.006 mol) was then added and reacted at 25°C for 48 h, and then the temperature was raised to 60°C for 6 h. A white precipitate was obtained by precipitation in a solvent of 2L ethanol: water = 1:3 (volume ratio). The precipitate was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A7. The infrared absorption spectrum was measured and the imide rate was 37.1%.

[0166]

[0167] Synthesis example 14

[0168] Synthesis of Alkali Soluble Resin A8

[0169] Under a dry nitrogen flow, bis(4-aminophenyl)hexafluoropropane (0.016 mol), 6FAP (0.016 mol), and SiDA (0.002 mol) were dissolved in NMP (100 g). Y2 (0.016 mol), ODPA (0.024 mol), and NMP (40 g) were then added thereto, and the mixture was reacted at 25°C for 2 h. 4-aminosalicylic acid (0.012 mol) was then added, and the mixture was reacted at 25°C for 48 h, and then the mixture was heated to 60°C for 4 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A13. The infrared absorption spectrum was measured, and the imide rate was 39.2%.

[0170] Synthesis Example 15

[0171] Synthesis of Alkali Soluble Resin A9

[0172] Under a dry nitrogen flow, bis(4-aminophenyl)hexafluoropropane (0.025 mol), ODA (0.014 mol), and SiDA (0.001 mol) were dissolved in NMP (100 g). Then, Y2 (0.012 mol), 6FAP derivative dianhydride (structural formula as follows) (0.025 mol), and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 2 h. Phthalic anhydride (0.006 mol) was then added, and the mixture was reacted at 25°C for 48 h, and then the mixture was heated to 60°C for 4 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered, and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A9. The infrared absorption spectrum was measured, and the imide rate was 29.6%.

[0173]

[0174] Synthesis example 16

[0175] Synthesis of Alkali Soluble Resin A10

[0176] Under a dry nitrogen flow, the diamine (0.014 mol), TFMB (0.018 mol), and SiDA (0.003 mol) in the following formula were dissolved in NMP (100 g); Y2 (0.014 mol), ODPA (0.026 mol), and NMP (40 g) were then added thereto, and the mixture was reacted at 25° C. for 2 h; 3-aminophenol (0.010 mol) was then added, and the mixture was reacted at 25° C. for 48 h, and then the mixture was heated to 60° C. for 4 h; the mixture was precipitated in a solvent of 2 L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50° C. for 72 h to obtain a powder of alkali-soluble resin A10, and the infrared absorption spectrum was measured, and the imide rate was 34.8%.

[0177]

[0178] Synthesis Example 17

[0179] Synthesis of Alkali Soluble Resin A11

[0180] Under a dry nitrogen stream, ODA (0.015 mol), SiDA (0.004 mol), 6FAP (0.020 mol), and 3-aminophenol (0.002 mol) were dissolved in NMP (100 g). 6FDA (0.030 mol), Y2 (0.010 mol), and NMP (40 g) were then added thereto, and the mixture was reacted at 25°C for 48 h; the mixture was then heated to 40°C for 6 h; the mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of the alkali-soluble resin A11, and the infrared absorption spectrum was measured, with an imide rate of 24.4%.

[0181] Synthesis Example 18

[0182] Synthesis of Alkali Soluble Resin A12

[0183] Under a dry nitrogen flow, the diamine (0.014 mol), TFMB (0.018 mol), and SiDA (0.003 mol) in the following formula were dissolved in NMP (100 g). Subsequently, ODPA (0.040 mol) and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 2 h. 3-aminophenol (0.010 mol) was then added, and the mixture was reacted at 25°C for 48 h. The mixture was then heated to 60°C for 4 h. The mixture was precipitated in 2 L of water to obtain a white precipitate. The precipitate was filtered, and the filter cake was washed with water several times. The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of the alkali-soluble resin A12. The infrared absorption spectrum was measured, and the imide rate was 3%.

[0184]

[0185] Synthesis example 19

[0186] Synthesis of Alkali Soluble Resin A13

[0187] Under a dry nitrogen flow, the derivative diamine of 6FAP (structural formula as follows) (0.035 mol) and SiDA (0.002 mol) were dissolved in NMP (100 g). BPDA (0.025 mol), ODPA (0.015 mol), and NMP (40 g) were then added thereto, and the mixture was reacted at 25°C for 20 h. 3-aminophenol (0.006 mol) was then added, and the mixture was reacted at 25°C for 2 h. The mixture was then heated to 60°C for 2 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate. The precipitate was filtered, and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A13. The infrared absorption spectrum was measured, and the imide rate was 13%.

[0188] Synthesis example 20

[0189] Synthesis of Alkali Soluble Resin A14

[0190] Under a dry nitrogen flow, TFMB (0.025 mol), ODA (0.010 mol), and SiDA (0.002 mol) were dissolved in NMP (100 g). Subsequently, 2,2',3,3'-benzophenonetetracarboxylic dianhydride (0.015 mol), Y2 (0.025 mol), and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 2 h. Then, 3-aminobenzoic acid (0.006 mol) was added, and the mixture was reacted at 25°C for 48 h. The mixture was then heated to 60°C for 6 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate. The precipitate was filtered, and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A14. The infrared absorption spectrum was measured, and the imide rate was 59.6%.

[0191]

[0192] Synthesis Example 21

[0193] Synthesis of Alkali Soluble Resin A15

[0194] Under a dry nitrogen flow, 6FODA (0.010 mol), 6FAP (0.027 mol), and SiDA (0.002 mol) were dissolved in NMP (100 g); CBDA (0.017 mol), ODPA (0.015 mol), Y2 (0.008 mol), and NMP (40 g) were then added thereto, and the mixture was reacted at 25° C. for 2 h, and 4-aminophenol (0.002 mol) was then added, and the mixture was reacted at 25° C. for 48 h, and then the mixture was heated to 60° C. and reacted for 6 h; the mixture was precipitated in a solvent of 2 L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio), and the filter cake was vacuum dried at 50° C. for 72 h to obtain a powder of alkali-soluble resin A15, and the infrared absorption spectrum was measured, and the imide rate was 19.2%.

[0195] Synthesis example 22

[0196] Synthesis of Alkali Soluble Resin A16

[0197] Under a dry nitrogen stream, 4,4'-diaminotetrafluorodiphenyl ether (0.034 mol) and SiDA (0.003 mol) were dissolved in NMP (100 g). Subsequently, 6FAP-derived dianhydride (structural formula shown below) (0.025 mol), Y6 (0.015 mol), and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 2 h. 3-aminophenol (0.060 mol) was then added, and the mixture was reacted at 40°C for 2 h. Pyridine (5 g) was then diluted with xylene (30 g) and added to the solution. A condenser was installed, and water and xylene were removed from the system together by azeotropy. The temperature of the solution was raised to 150°C and the mixture was reacted for 4 h, and then raised to 180°C and the mixture was reacted for 2 h. The temperature of the solution was lowered to room temperature and precipitated in 2 L of water to obtain a white precipitate. The precipitate was filtered and the filter cake was washed with water several times. The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A16. The infrared absorption spectrum was measured and the imide rate was 93%.

[0198]

[0199] Synthesis example 23

[0200] Synthesis of Alkali Soluble Resin A17

[0201] Under a dry nitrogen flow, ODA (0.015 mol), SiDA (0.004 mol), 6FAP (0.020 mol), and 3-aminophenol (0.002 mol) were dissolved in NMP (100 g). Subsequently, 6FDA (0.020 mol), Y1 (0.020 mol), and NMP (40 g) were added thereto, and the mixture was reacted at 25°C for 48 h, and then the mixture was heated to 60°C for 6 h. The mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A17. The infrared absorption spectrum was measured, and the imide rate was 49.9%.

[0202] Synthesis example 24

[0203] Synthesis of Alkali Soluble Resin A18

[0204] Under a dry nitrogen flow, ODA (0.025 mol), SiDA (0.004 mol), 3,5-diaminobenzoic acid (0.010 mol), and 3-aminophenol (0.002 mol) were dissolved in NMP (100 g); ODPA (0.020 mol), Y2 (0.020 mol), and NMP (40 g) were then added thereto, and the mixture was reacted at 25°C for 48 h, and then the temperature was raised to 60°C for 6 h; the mixture was precipitated in a solvent of 2L ethanol: water = 1:3 (volume ratio) to obtain a white precipitate, which was filtered and the filter cake was washed several times with ethanol: water = 1:3 (volume ratio). The filter cake was vacuum dried at 50°C for 72 h to obtain a powder of alkali-soluble resin A17, and the infrared absorption spectrum was measured, and the imide rate was 45.5%.

[0205] Example 1

[0206] The present embodiment provides a positive photosensitive resin composition, and the preparation method thereof is as follows: 10 g of alkali-soluble resin A1 is taken, and photoacid generators: 0.6 g of PAC-1 and 0.6 g of PAC-7 are added thereto, crosslinking agents: 1.5 g of HMOM-TPHAP (manufactured by Honshu Chemical Industry Co., Ltd.) and 2.5 g of EXA-4880 (manufactured by Dainippon Ink & Chemicals Co., Ltd.) are added thereto, and a solvent: 10 g of γ-butyrolactone is added thereto to prepare a varnish.

[0207] The varnish was applied to a silicon substrate using a spin coater and dried at 80°C for 8 minutes to form a film, which was then exposed using a small developer for photolithography (AC3000; manufactured by Takizawa Sangyo Co., Ltd.). After exposure, the film was developed for 55 seconds using a 2.38 mass % tetramethylammonium hydroxide aqueous solution and rinsed with water for 30 seconds. After development and rinsing, the film was thermally cured at 230°C using a high-temperature inert gas oven (INH-9CD-S; manufactured by Koyo Thermo Systems Co., Ltd.) to produce a cured film with a film thickness of about 1.5 μm. The thermal curing conditions were thermal curing at 230°C for 60 minutes in a nitrogen atmosphere. The positive photosensitive resin composition of the present invention was then evaluated.

[0208] Embodiments 2 to 13

[0209] Examples 2 to 11 respectively provide a positive photosensitive resin composition, and the preparation method thereof is substantially the same as that in Example 1, except that the alkali-soluble resin A1 in Example 1 is replaced with alkali-soluble resins A2 to A11, A14, and A15 in sequence, and other conditions remain unchanged.

[0210] Comparative Examples 1 to 5

[0211] Comparative Examples 1 to 5 respectively provide a positive photosensitive resin composition, and the preparation method thereof is substantially the same as that in Example 1, except that the alkali-soluble resin A1 in Example 1 is replaced by alkali-soluble resins A12, A13, A16, A17, and A18, respectively, while other conditions remain unchanged.

[0212] Comparative Example 6

[0213] Comparative Example 6 provides a positive photosensitive resin composition, and its preparation method is substantially the same as that in Example 1, except that the alkali-soluble resin A1:10 g in Example 1 is replaced by alkali-soluble resins A12:5 g and A16:5 g, respectively, and other conditions remain unchanged.

[0214] The evaluation results of the above examples and comparative examples are shown in Table 1.

[0215] Table 1 - Performance evaluation results of Examples 1-13 and Comparative Examples 1-6

[0216]

[0217] According to the present invention, a film can be developed with an alkaline aqueous solution, has excellent sensitivity and resolution, a clear pattern, and a high residual film rate in the unexposed portion, and is suitable for use as a semiconductor element protective film, a planarization layer, an interlayer insulating film, an insulating film for a display, an insulating layer from an organic field to a light-emitting element, an insulating layer for a thin film transistor TFT, etc.

Claims

1. A positive photosensitive resin composition, characterized in that: Contains the following ingredients: (a) 100 parts by weight of an alkali-soluble resin, wherein the main chain structure of the alkali-soluble resin comprises a structural unit having a structural formula (a1) and a structural unit having a structural formula (a2); (b) a photoacid generator, 10-30 parts by weight; (c) thermal crosslinking agent, 20-60 parts by weight; (d) organic solvents; In the above structural formula (a1) and structural formula (a2), X represents a reaction residue of a tetraacid, and P and Q represent reaction residues of a diamine; at least one of the groups X, Y, P, and Q contains a fluorine atom, and the mass ratio of the fluorine atom to the alkali-soluble resin (a) is 5-25%, and at least one of the groups X, Y, P, and Q also contains one or more of a hydroxyl group, a carboxyl group, and a sulfonic acid group; The structural formula (a2) is prepared from a methylene derivative of a dianhydride having a structural formula (a3); In the methylene derivative of the dianhydride, R1 represents a reaction residue of a dianhydride containing the following structures: 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, fluoropyromellitic dianhydride, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, cyclobutane tetracarboxylic dianhydride; The structural unit of the structural formula (a1) accounts for 20-80 mol% of the alkali-soluble resin (a), the structural unit of the structural formula (a2) accounts for 10-80 mol% of the alkali-soluble resin (a), 10 mol%-25 mol% of the alkali-soluble resin (a) is derived from the structural formula (a3), and the imidization rate of the alkali-soluble resin (a) is 20-50%; The tetraacid is prepared by reacting one or more of the following dianhydride compounds: 2,2-bis(3,4-dicarboxylic acid phenyl)hexafluoropropane dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, cyclobutane tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride and dianhydrides of the following structures; The diamine comprises one or more combinations of the following compounds: 4,4'-diaminodiphenyl ether, bis(4-aminophenyl)hexafluoropropane, 3,5-diaminobenzoic acid, bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 4,4'-diaminotetrafluorodiphenyl ether, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 1,1,3,3-tetramethyl-1,3-bis(3-aminopropyl)disiloxane, and diamines of the following structures; 2. A positive photosensitive resin composition according to claim 1, characterized in that: In the methylene derivative of the dianhydride, R1 represents a reaction residue of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride.

3. A positive photosensitive resin composition according to claim 1, characterized in that: The structural unit of the structural formula (a3) ​​reacts with diamine at low temperature, and the reaction temperature is 20-120°C.

4. A positive photosensitive resin composition according to claim 1, characterized in that: The end-capping groups of the main chain structure of the alkali-soluble resin (a) have the structure shown in general formula (1) and / or (2), A is derived from a primary monoamine, and B is derived from a dianhydride:

5. A positive photosensitive resin composition according to any one of claims 1 to 4, characterized in that: The X and Y are one or more of an aromatic structure or an aliphatic structure, and the P and Q are one or more of an aromatic structure, an aliphatic structure, and a silicon-containing structure.

6. A cured film obtained by curing the positive photosensitive resin composition according to any one of claims 1 to 5.

7. A method for patterning a cured film, comprising the following steps: i) coating the positive photosensitive resin composition according to any one of claims 1 to 5 on a substrate, and drying at 40 to 120° C. for 1 to 10 min to form a positive photosensitive resin composition film; ii) exposing the film under a mask; iii) removing the exposed portion of the film using an alkaline developer, developing and washing; iiii) The developed film is cured and dried at 100-400° C. to obtain a cured film having a desired pattern.