AlGaN-based deep ultraviolet LED epitaxial wafer and preparation method thereof
By growing nanocolumn structures on sapphire substrates and replacing the traditional multi-layer thin film buffer layer, the lattice mismatch problem of AlGaN-based deep ultraviolet LED epitaxial sheets is solved, and the preparation of high-performance AlGaN-based deep ultraviolet LED epitaxial sheets is realized. Simplifies the process and reduces costs.
Patent Information
- Application Number
- CN202011329853.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-11-24
AI Technical Summary
The existing AlGaN-based deep ultraviolet LED epitaxial sheet has low performance, mainly due to the lattice mismatch between the sapphire substrate and the AlGaN material, which limits the scale of its commercial production application.
The nanocolumn structure is used instead of the traditional multi-layer thin film buffer layer. By growing the SiN layer on the sapphire substrate, the GaN nanocolumn, the AlN nanocolumn shell and the AlGaN nanocolumn shell are then grown, and non-doped layers are grown on it. The hetero AlGaN layer, n-type doped AlGaN layer, AlGaN multi-quantum well layer, electron barrier layer and p-type doped GaN layer reduce lattice mismatch.
The performance of AlGaN-based deep ultraviolet LED is significantly improved, and the high crystal quality epitaxial sheet is obtained, which overcomes lattice mismatch and defect problems, simplifies the preparation process, and reduces costs.
Smart Images

Figure CN112271240B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor devices, and in particular to an AlGaN-based deep ultraviolet LED epitaxial wafer and a preparation method thereof. Background Art
[0002] Deep ultraviolet light has broad application prospects in the fields of national defense technology, information technology, biopharmaceuticals, environmental monitoring, public health, sterilization and disinfection. The traditional ultraviolet light sources currently used are gas lasers and mercury lamps, which have disadvantages such as large size, high energy consumption and pollution. AlGaN-based compound semiconductor ultraviolet light-emitting diodes (LEDs) are a solid-state ultraviolet light source with the advantages of small size, high efficiency, long life, environmental friendliness, low energy consumption and no pollution. High Al component AlGaN material is an irreplaceable material system for the preparation of high-performance deep ultraviolet LEDs. There is a great demand for both civilian and military applications. For example, in the medical and health fields such as sterilization and disinfection, cancer detection, and skin disease treatment, AlGaN-based ultraviolet light sources have many advantages such as no mercury pollution, adjustable wavelength, small size, good integration, low energy consumption, and long life.
[0003] In recent years, the development of AlGaN-based deep ultraviolet LEDs has made some progress, but its performance problems such as low external quantum efficiency and low luminous power still hinder its commercialization, and high-quality epitaxial materials are the basis for preparing high-performance deep ultraviolet LEDs. At present, high-quality AlGaN materials are generally made by heteroepitaxial methods. At present, most sapphire substrates are used as epitaxial substrates for AlGaN-based deep ultraviolet LEDs. However, due to the large lattice mismatch between sapphire and the epitaxially grown AlGaN material, it is generally necessary to use a buffer layer of various structures between the sapphire substrate and AlGaN to reduce the lattice mismatch between the two. Therefore, in order to achieve the growth of high-quality AlGaN materials and high-performance deep ultraviolet LED epitaxial wafers on sapphire substrates, it is still necessary to overcome major defects such as lattice mismatch, crystal dislocation, and stacking faults, which seriously limits the large-scale application of commercial production of ultraviolet LEDs. Summary of the invention
[0004] The purpose of the present invention is an AlGaN-based deep ultraviolet LED epitaxial wafer and a preparation method thereof, aiming to solve the problem in the prior art that the performance of the AlGaN-based deep ultraviolet LED epitaxial wafer needs to be improved.
[0005] An embodiment of the present invention provides an AlGaN-based deep ultraviolet LED epitaxial wafer, which includes: a SiN layer grown on a sapphire substrate, a plurality of GaN nanocolumns grown on the SiN layer, a plurality of AlN nanocolumn shell layers corresponding to outer layers of the plurality of GaN nanocolumns, a plurality of AlGaN nanocolumn shell layers corresponding to outer layers of the plurality of AlN nanocolumn shell layers, an undoped AlGaN layer grown on the plurality of AlGaN nanocolumn shell layers, an n-type doped AlGaN layer grown on the undoped AlGaN layer, an AlGaN multi-quantum well layer grown on the n-type doped AlGaN layer, an electron blocking layer grown on the AlGaN multi-quantum well layer, a p-type doped AlGaN layer grown on the electron blocking layer, and a p-type doped GaN layer grown on the p-type doped AlGaN layer.
[0006] Preferably, the diameter of a single GaN nanocolumn is 50-200 nm, and the height is 300-2000 nm.
[0007] Preferably, the thickness of a single AlN nanocolumn shell layer is 50-150 nm.
[0008] Preferably, the thickness of a single AlGaN nanocolumn shell layer is 50-150 nm.
[0009] Preferably, the thickness of the undoped AlGaN layer is 500-800 nm.
[0010] Preferably, the thickness of the n-type doped AlGaN layer is 3-5 μm.
[0011] Preferably, the AlGaN multi-quantum well layer consists of 7 to 10 periods of Al 0.3 Ga 0.7 N well layer and Al 0.5 Ga 0.5 N barrier layer.
[0012] Preferably, the Al 0.3 Ga 0.7 The thickness of the N well layer is 2 to 3 nm. 0.5 Ga 0.5 The thickness of the N barrier layer is 10 to 13 nm.
[0013] Preferably, the electron blocking layer is Al 0.4 Ga 0.6 N electron blocking layer, the thickness of the electron blocking layer is 20-50 nm.
[0014] The embodiment of the present invention provides a method for preparing the AlGaN-based deep ultraviolet LED epitaxial wafer as described above, which comprises:
[0015] Select a sapphire substrate;
[0016] growing a SiN layer on the sapphire substrate;
[0017] growing a plurality of GaN nanorods on the SiN layer;
[0018] Growing a plurality of AlN nanocolumn shell layers corresponding to the plurality of GaN nanocolumn outer layers;
[0019] Correspondingly growing a plurality of AlGaN nanocolumn shell layers on the plurality of AlN nanocolumn shell layers;
[0020] Growing a non-doped AlGaN layer on the plurality of AlGaN nanocolumn shell layers;
[0021] Growing an n-type doped AlGaN layer on the non-doped AlGaN layer;
[0022] Growing an AlGaN multi-quantum well layer on the n-type doped AlGaN layer;
[0023] Growing an electron blocking layer on the AlGaN multi-quantum well layer;
[0024] growing a p-type doped AlGaN layer on the electron blocking layer;
[0025] A p-type doped GaN layer is grown on the p-type doped AlGaN layer.
[0026] The embodiment of the present invention provides an AlGaN-based deep ultraviolet LED epitaxial wafer and a preparation method thereof, wherein the AlGaN-based deep ultraviolet LED epitaxial wafer comprises: a SiN layer grown on a sapphire substrate, a plurality of GaN nanocolumns grown on the SiN layer, a plurality of AlN nanocolumn shell layers corresponding to the outer layers of the plurality of GaN nanocolumns, a plurality of AlGaN nanocolumn shell layers corresponding to the outer layers of the plurality of AlN nanocolumn shell layers, a non-doped AlGaN layer grown on the plurality of AlGaN nanocolumn shell layers, an n-type doped AlGaN layer grown on the non-doped AlGaN layer, an AlGaN multi-quantum well layer grown on the n-type doped AlGaN layer, an electron blocking layer grown on the AlGaN multi-quantum well layer, a p-type doped AlGaN layer grown on the electron blocking layer, and a p-type doped GaN layer grown on the p-type doped AlGaN layer. The present invention adopts a nanocolumn structure to replace a traditional complex multi-layer thin film buffer layer structure, reduces the lattice mismatch between sapphire and AlGaN, overcomes the deficiencies of the prior art, and obtains a high-performance AlGaN-based deep ultraviolet LED epitaxial wafer. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0028] Figure 1 A schematic diagram of the structure of an AlGaN-based deep ultraviolet LED epitaxial wafer provided in an embodiment of the present invention;
[0029] Figure 2 A schematic flow chart of a method for preparing an AlGaN-based deep ultraviolet LED epitaxial wafer provided in an embodiment of the present invention;
[0030] Figure 3 This is the electroluminescence spectrum of the AlGaN-based deep ultraviolet LED epitaxial wafer prepared in an embodiment of the present invention. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0033] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0034] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0035] The embodiment of the present invention provides an AlGaN-based deep ultraviolet LED epitaxial wafer, such as Figure 1As shown, it includes: a SiN layer 102 grown on a sapphire substrate 101, a plurality of GaN nanocolumns 103 grown on the SiN layer 102, a plurality of AlN nanocolumn shell layers 104 corresponding to the outer layers of the plurality of GaN nanocolumns 103, a plurality of AlGaN nanocolumn shell layers 105 corresponding to the outer layers of the plurality of AlN nanocolumn shell layers 104, an undoped AlGaN layer 106 grown on the plurality of AlGaN nanocolumn shell layers 105, an n-type doped AlGaN layer 107 grown on the undoped AlGaN layer 106, an AlGaN multi-quantum well layer 108 grown on the n-type doped AlGaN layer 107, an electron blocking layer 109 grown on the AlGaN multi-quantum well layer 108, a p-type doped AlGaN layer 110 grown on the electron blocking layer 109, and a p-type doped GaN layer 111 grown on the p-type doped AlGaN layer 110.
[0036] Since there is a large lattice mismatch between sapphire and AlGaN, the embodiment of the present invention adopts a nano-column structure to replace the traditional complex multi-layer thin film buffer layer structure, thereby reducing the lattice mismatch between sapphire and AlGaN, overcoming the shortcomings of the prior art, and obtaining a high-performance AlGaN-based deep ultraviolet LED.
[0037] Generally speaking, due to the high lattice mismatch between sapphire and AlGaN, a multi-layer and complex buffer layer structure is generally required to epitaxially grow AlGaN materials with high crystal quality on a sapphire substrate. Compared with thin film materials, nanopillars have a high specific surface area. Their high specific surface area allows the lattice strain caused by the lattice mismatch between the nanopillars and the substrate to be effectively relaxed on the side walls of the nanopillars, which can significantly reduce the threading dislocation density and obtain nanopillar materials with high crystal quality.
[0038] Since it is difficult to directly grow high-crystalline quality AlGaN nanocolumn materials on a sapphire substrate, the AlN nanocolumn shell layer 104 and the AlGaN nanocolumn shell layer 105 are continuously grown outside the high-quality GaN nanocolumn 103, thereby obtaining a high-quality AlGaN nanocolumn (i.e., the AlGaN nanocolumn shell layer 105); based on the high-crystalline quality AlGaN nanocolumn shell layer 105, a non-doped AlGaN layer 106 is laterally epitaxially grown on the AlGaN nanocolumn shell layer 105, thereby obtaining a high-crystalline non-doped AlGaN layer 106, which is helpful for preparing high-performance AlGaN-based optoelectronic devices.
[0039] In one embodiment, the SiN layer 102 has a thickness of 2-10 nm.
[0040] In one embodiment, the diameter of a single GaN nanorod 103 is 50-200 nm, and the height is 300-2000 nm. The GaN nanorods 103 may be evenly distributed on the SiN layer. In addition, the distance between adjacent GaN nanorods 103 may be 400-600 nm.
[0041] In one embodiment, the thickness of a single AlN nanocolumn shell layer 104 is 50-150 nm. This thickness refers to the thickness covering a single GaN nanocolumn 103, and this thickness refers to both the side surface thickness and the top surface thickness.
[0042] In one embodiment, the thickness of a single AlGaN nanocolumn shell layer 105 is 50-150 nm. This thickness refers to the thickness covering a single AlN nanocolumn shell layer 104, and this thickness refers to both the side surface thickness and the top surface thickness.
[0043] In one embodiment, the thickness of the undoped AlGaN layer 106 is 500-800 nm.
[0044] In one embodiment, the thickness of the n-type doped AlGaN layer 107 is 3-5 μm. The n-type doped AlGaN layer 107 is doped with Si, and the Si doping concentration is 1×10 17 ~1×10 20 cm -3 .
[0045] In one embodiment, the AlGaN multi-quantum well layer 108 is composed of 7 to 10 periods of Al 0.3 Ga 0.7 N well layer and Al 0.5 Ga 0.5 N barrier layer. That is to say, the AlGaN multi-quantum well layer 108 is a layer of Al 0.3 Ga 0.7 N well layer and an Al 0.5 Ga 0.5 N barrier layers constitute a unit, and such a unit is repeated continuously, and a total of 7 to 10 units are set.
[0046] In one embodiment, the Al 0.3 Ga 0.7 The thickness of the N well layer is 2 to 3 nm. 0.5 Ga 0.5 The thickness of the N barrier layer is 10-13 nm. The above thickness refers to the thickness of each layer, that is, each Al 0.3 Ga 0.7 The thickness of the N-well layer is 2 to 3 nm. 0.5 Ga 0.5 The thickness of the N barrier layer is 10 to 13 nm.
[0047] In one embodiment, the electron blocking layer 109 is Al 0.4 Ga 0.6 N electron blocking layer, the thickness of the electron blocking layer 109 is 20-50 nm. In order to prevent the injected electrons from being unable to efficiently perform radiation recombination in the active region, the electron blocking layer 109 is provided in the embodiment of the present invention.
[0048] In one embodiment, the thickness of the p-type doped AlGaN layer 110 is 300-350 nm. The electron blocking layer 109 is an AlGaN layer with an Al component of 0.4, which has a large lattice mismatch with GaN. In order to reduce the Al 0.4 Ga 0.6 Since there is a lattice mismatch between the N electron blocking layer 109 and the p-type doped GaN layer 111 , a p-type doped AlGaN layer 110 is inserted between the two.
[0049] In one embodiment, the thickness of the p-type doped GaN layer 111 is 300-350 nm. In order to obtain a p-type contact layer material with high doping concentration and high crystal quality, GaN is used as the p-type layer material.
[0050] The present invention also provides a method for preparing the AlGaN-based deep ultraviolet LED epitaxial wafer as described above, Figure 2 As shown, it includes:
[0051] S201, selecting a sapphire substrate;
[0052] S202, growing a SiN layer on the sapphire substrate;
[0053] S203, growing a plurality of GaN nanorods on the SiN layer;
[0054] S204, growing a plurality of AlN nanocolumn shell layers corresponding to the outer layers of the plurality of GaN nanocolumns;
[0055] S205, growing a plurality of AlGaN nanocolumn shell layers correspondingly on the plurality of AlN nanocolumn shell layers;
[0056] S206, growing a non-doped AlGaN layer on the plurality of AlGaN nanocolumn shell layers;
[0057] S207, growing an n-type doped AlGaN layer on the non-doped AlGaN layer;
[0058] S208, growing an AlGaN multi-quantum well layer on the n-type doped AlGaN layer;
[0059] S209, growing an electron blocking layer on the AlGaN multi-quantum well layer;
[0060] S210, growing a p-type doped AlGaN layer on the electron blocking layer;
[0061] S211 , growing a p-type doped GaN layer on the p-type doped AlGaN layer.
[0062] In the step S201, a commercially available sapphire substrate may be selected.
[0063] In the step S202, in the SiN layer growth step, the SiN layer is grown by metal organic chemical vapor deposition, and the process conditions are: the reaction chamber pressure is 50-300 torr, and the substrate temperature is 1000-1160°C.
[0064] In the step S203, in the step of growing GaN nanocolumns, GaN nanocolumns are grown on the SiN layer by metal organic chemical vapor deposition, and the process conditions are: the reaction chamber pressure is 50-300torr, the substrate temperature is 1000-1260°C, the beam ratio V / III is 10-50, and the growth rate is 1-2μm / h. Since the thickness of the SiN layer grown on sapphire is very thin, a dense SiN layer cannot be formed, resulting in a part of the sapphire area being exposed on the surface of the SiN layer, and GaN cannot nucleate and grow on the surface of the SiN layer, which is equivalent to using a thin SiN layer to make a mask on the sapphire substrate. Under low V / III ratio conditions (V / III is 10-50), GaN nanocolumns can be grown; similarly, using low V / III ratio conditions (V / III is 10-50), two layers of nanocolumns (i.e., AlN nanocolumn shell layer and AlGaN nanocolumn shell layer) are continuously wrapped on the GaN nanocolumn.
[0065] In the step S204, in the AlN nanocolumn shell growth step, a metal organic chemical vapor deposition method is used to grow an AlN nanocolumn shell on the GaN nanocolumn, and the process conditions are: a reaction chamber pressure of 50 to 300 torr, a substrate temperature of 1000 to 1260° C., a beam ratio V / III of 10 to 50, and a growth rate of 1 to 2 μm / h.
[0066] In the step S205, in the AlGaN nanocolumn shell growth step, the AlGaN nanocolumn shell is grown on the AlN nanocolumn by metal organic chemical vapor deposition, and the process conditions are: the reaction chamber pressure is 50-300 torr, the substrate temperature is 1000-1260°C, the beam ratio V / III is 10-50, and the growth rate is 1-2 μm / h.
[0067] In the step S206, in the step of epitaxial growth of the non-doped AlGaN layer, a metal organic chemical vapor deposition method is used to grow the non-doped AlGaN layer on the AlGaN nanocolumn, and the process conditions are: the reaction chamber pressure is 50 to 300 torr, the substrate temperature is 1000 to 1260° C., the beam ratio V / III is 3000 to 5000, and the growth rate is 2 to 4 μm / h.
[0068] In the step S207, in the step of epitaxial growth of the n-type doped AlGaN layer, an n-type doped AlGaN layer is grown on the non-doped AlGaN layer by metal organic chemical vapor deposition, and the process conditions are: a reaction chamber pressure of 50 to 300 torr, a substrate temperature of 1000 to 1260° C., a beam ratio V / III of 3000 to 5000, and a growth rate of 2 to 4 μm / h; the n-type doped AlGaN layer is doped with Si, and the Si doping concentration is 1×10 17 ~1×10 20 cm -3 .
[0069] In the step S208, in the AlGaN multi-quantum well layer epitaxial growth step, 7 to 10 periods of Al are grown on the n-type doped AlGaN layer using a metal organic chemical vapor deposition method. 0.3 Ga 0.7 N well layer / Al 0.5 Ga 0.5 N barrier layer, the process conditions are: reaction chamber pressure of 50 ~ 300torr, substrate temperature of 1000 ~ 1260 ℃, beam ratio V / III of 3000 ~ 5000, growth rate of 2 ~ 4μm / h.
[0070] In the step S209, in the step of epitaxially growing the electron blocking layer, Al is grown on the AlGaN multi-quantum well layer by metal organic chemical vapor deposition. 0.4 Ga 0.6 N electron blocking layer, the process conditions are: reaction chamber pressure of 50-300 torr, substrate temperature of 1000-1260°C, beam ratio V / III of 3000-5000, and growth rate of 2-4 μm / h.
[0071] In the step S210, in the epitaxial growth step of the p-type doped AlGaN layer, a metal organic chemical vapor deposition method is used to grow a p-type doped AlGaN layer on the electron blocking layer, and the process conditions are: the reaction chamber pressure is 50 to 300 torr, the Si substrate temperature is 1000 to 1260° C., the beam ratio V / III is 3000 to 5000, and the growth rate is 2 to 4 μm / h.
[0072] In the step S211, in the epitaxial growth step of the p-type doped GaN layer, a p-type doped GaN layer is grown on the p-type doped AlGaN layer by metal organic chemical vapor deposition, and the process conditions are: the reaction chamber pressure is 50 to 300 torr, the Si substrate temperature is 1000 to 1060° C., the beam ratio V / III is 3000 to 5000, and the growth rate is 2 to 4 μm / h.
[0073] The AlGaN-based deep ultraviolet LED epitaxial wafer finally prepared in the embodiment of the present invention has an electroluminescence spectrum as shown in FIG. Figure 3 shown.
[0074] The embodiment of the present invention uses core-shell structured nanocolumns as a buffer layer to replace the traditional multi-layer thin film buffer layer structure. The core-shell structured nanocolumns are beneficial to alleviating the stress generated during the growth of the epitaxial layer and the defect density in the thin film, thereby achieving the growth of high-crystalline quality AlGaN thin films and AlGaN-based deep ultraviolet LED epitaxial wafers. In the preparation method of the embodiment of the present invention, in order to obtain high-crystalline quality AlGaN materials, core-shell structured nanocolumns are used as a buffer layer, and then the AlGaN thin film is continued to grow on the nanocolumns by changing the epitaxial growth mode, so as to obtain a high-quality epitaxial layer film with a smooth interface, and then prepare a high-performance, high-luminous efficiency deep ultraviolet LED. This method is simple, easy to implement, effective and low-cost.
[0075] The various embodiments in the specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same or similar parts between the various embodiments can be referred to each other. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principle of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0076] It should also be noted that, in this specification, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the statement "comprising a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element.
Claims
1. An AlGaN-based deep ultraviolet LED epitaxial wafer, characterized in that: include: A SiN layer grown on a sapphire substrate, a plurality of GaN nanocolumns grown on the SiN layer, a plurality of AlN nanocolumn shell layers corresponding to the outer layers of the plurality of GaN nanocolumns, a plurality of AlGaN nanocolumn shell layers corresponding to the outer layers of the plurality of AlN nanocolumn shell layers, an undoped AlGaN layer grown on the plurality of AlGaN nanocolumn shell layers, an n-type doped AlGaN layer grown on the undoped AlGaN layer, an AlGaN multi-quantum well layer grown on the n-type doped AlGaN layer, an electron blocking layer grown on the AlGaN multi-quantum well layer, a p-type doped AlGaN layer grown on the electron blocking layer, and a p-type doped GaN layer grown on the p-type doped AlGaN layer; The diameter of a single GaN nanocolumn is 50-200 nm, and the height is 300-2000 nm; The thickness of a single AlN nanocolumn shell layer is 50 to 150 nm; The thickness of a single AlGaN nanocolumn shell layer is 50-150 nm.
2. The AlGaN-based deep ultraviolet LED epitaxial wafer according to claim 1, characterized in that: The thickness of the non-doped AlGaN layer is 500-800 nm.
3. The AlGaN-based deep ultraviolet LED epitaxial wafer according to claim 1, characterized in that: The thickness of the n-type doped AlGaN layer is 3-5 μm.
4. The AlGaN-based deep ultraviolet LED epitaxial wafer according to claim 1, characterized in that: The AlGaN multi-quantum well layer is composed of 7 to 10 periods of Al 0.3 Ga 0.7 N well layer and Al 0.5 Ga 0.5 N barrier layer.
5. The AlGaN-based deep ultraviolet LED epitaxial wafer according to claim 4, characterized in that: The Al 0.3 Ga 0.7 The thickness of the N well layer is 2 to 3 nm. 0.5 Ga 0.5 The thickness of the N barrier layer is 10 to 13 nm.
6. The AlGaN-based deep ultraviolet LED epitaxial wafer according to claim 1, characterized in that: The electron blocking layer is Al 0.4 Ga 0.6 N electron blocking layer, the thickness of the electron blocking layer is 20-50 nm.
7. A method for preparing an AlGaN-based deep ultraviolet LED epitaxial wafer as claimed in any one of claims 1 to 6, characterized in that: include: Select a sapphire substrate; growing a SiN layer on the sapphire substrate; growing a plurality of GaN nanorods on the SiN layer; Growing a plurality of AlN nanocolumn shell layers corresponding to the plurality of GaN nanocolumn outer layers; Correspondingly growing a plurality of AlGaN nanocolumn shell layers on the plurality of AlN nanocolumn shell layers; Growing a non-doped AlGaN layer on the plurality of AlGaN nanocolumn shell layers; Growing an n-type doped AlGaN layer on the non-doped AlGaN layer; Growing an AlGaN multi-quantum well layer on the n-type doped AlGaN layer; Growing an electron blocking layer on the AlGaN multi-quantum well layer; growing a p-type doped AlGaN layer on the electron blocking layer; A p-type doped GaN layer is grown on the p-type doped AlGaN layer.