Transparent superlattice structure semiconductor nano-electric heating film and its preparation method and application
Through the preparation of the superlattice structure n-type semiconductor nanoelectric heating film, combined with the tunnel furnace electric heating film production system and specific coating equipment, the problems of low light transmittance and unstable electric heating efficiency in the prior art are solved, and the problem of low light transmittance and unstable electric heating efficiency in the existing technology is realized. Highly transparent, efficient and high temperature-resistant electric heating film is suitable for a variety of matrix materials and improves the feasibility of industrial production.
Patent Information
- Application Number
- CN202011027442.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-09-25
AI Technical Summary
The existing nano-semiconductor electrothermal film has low light transmittance and unstable electric heating efficiency. The high-temperature coating process is immature, and large-scale industrial production cannot be achieved. The R&D cost is high, the finished coating is uneven, and the stability is poor.
Using superlattice structure n-type semiconductor nanoelectric electrothermal film, including antimony chloride, tin chloride, stannous chloride, tin oxide, boron oxide and organic solvents, the coating is carried out through the tunnel furnace electric heating film production system, using tracks The mobile spray gun device and the pipe-type defogging device realize the preparation of electric heating films with high transparency and high conductivity.
It has achieved an electric heating film with a transparency of more than 85%, with an electric heating efficiency of up to 98.77%, energy saving of 45% to 60%, high temperature and high strength resistance, suitable for various matrix materials, with good corrosion resistance and hardness, long working life and safety Highly sexual.
Smart Images

Figure CN112291867B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electric heating films, and in particular to a transparent superlattice structure semiconductor nano electric heating film and a preparation method and application thereof. Background Art
[0002] Nano semiconductor electric heating film is a new generation of heating material. Its heating method is different from traditional metal resistance wire. It has zero inductance, pure resistance heating, and improved power factor. And it breaks the traditional linear heating form with surface heating, with good heat transfer effect and high electric heat conversion efficiency: 80% to 97%, which has good energy saving advantages. At present, the formula used in nano semiconductor electric heating film liquid makes the effect of the obtained nano electric heating film unstable.
[0003] In the patent with publication number CN201710399122.6, a nano-electrothermal film liquid formula is disclosed, which adopts a combination of tin tetrachloride, antimony trichloride, graphene, anhydrous ethanol, and cobalt chloride. Its effect on the electrothermal efficiency is unstable. It is suitable for electrical appliances for electric heating of hot water. It has no advantages over nano-ceramics, microcrystalline glass and quartz glass as the matrix material, and the transmittance is affected by graphene and the like, and the transmittance is low.
[0004] At present, the coating spray gun system used in the immature high-temperature coating process is not heat-resistant and cannot overcome the problems of high temperature and corrosion, which makes it impossible to mass-produce industrial products and the R&D cost is high. The finished product coating is uneven and the stability is not high, which easily leads to product damage. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a transparent superlattice structure n-type semiconductor nano-electric heating film, which can be based on a non-metallic material. The electric heating film formed thereon has a transparency of more than 85% and a stable electric heating efficiency.
[0007] Correspondingly, the present invention also provides a method for preparing the above-mentioned transparent superlattice structure n-type semiconductor nano-electric heating film.
[0008] (II) Technical solution
[0009] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0010] The present invention provides a superlattice structure n-type semiconductor nano-electric heating film, which includes the following components by weight:
[0011] Antimony chloride 0.3~0.6 parts,
[0012] Tin chloride 5~10 parts,
[0013] 4-8 parts of stannous chloride,
[0014] Tin oxide 3~9 parts,
[0015] 4-8 parts of tin oxide,
[0016] Boron oxide 0.2~0.5 parts,
[0017] 0.3~0.8 parts of bismuth oxide,
[0018] 5~30 parts of organic solvent
[0019] Further, the antimony chloride is antimony trichloride dihydrate;
[0020] or / and
[0021] Tin chloride is tin tetrachloride pentahydrate;
[0022] or / and
[0023] The organic solvent includes 5 to 15 parts of ethanol, 5 to 9 parts of acetic acid, and 2 to 6 parts of methyl acetate.
[0024] Another aspect of the present invention provides a method for preparing a superlattice structure n-type semiconductor nano-electric heating film, which comprises the following steps:
[0025] S1: adding stannous oxide, tin oxide, tin tetrachloride pentahydrate and an organic solvent into distilled water, stirring them thoroughly, and filtering to obtain a solid and a filtrate;
[0026] S2 adding antimony chloride, hydrochloric acid, stannous chloride, an organic solvent, methyl acetate, boron oxide and bismuth oxide to the filtrate to obtain an electrothermal film treatment solution;
[0027] S3: spreading the obtained electrothermal film treatment liquid on the substrate to obtain an electrothermal film on the surface of the substrate.
[0028] Furthermore, in step S4, a tunnel furnace type electric heating film production system is used for coating, which includes a coating machine, a track type mobile spray gun device and a pipeline type demisting device, and the coating machine includes a high temperature furnace body and a feeding device, and the feeding device is connected to the inlet of the high temperature furnace body;
[0029] The spray gun of the track-type mobile spray gun device can be extended into the furnace chamber of the high-temperature furnace body of the coating machine;
[0030] The pipeline defogger comprises a porous mist extraction pipeline, an exhaust fan, a cooling pipeline, a low-temperature closed chamber and a wastewater treatment pool which are connected in sequence; the porous mist extraction pipeline is connected to the bottom of the furnace body, and the through holes of the porous mist extraction pipeline are connected to the inner cavity of the coating furnace body; atomizing nozzles are provided in the cooling pipeline and the low-temperature closed chamber.
[0031] Furthermore, a condenser tube is wound around the outside of the cooling pipe (13), an air inlet of the low-temperature sealed chamber (14) is arranged at the upper end of the low-temperature sealed chamber (14), and an air outlet is arranged at the lower end of the low-temperature sealed chamber (14).
[0032] Furthermore, the track-type movable spray gun (21) device comprises a main body component and a spray gun (21), and the spray gun (21) can move back and forth relative to the main body component.
[0033] Furthermore, the main body component comprises a fixed base, the spray gun (21) is fixedly connected to a connecting rod (22), the connecting rod (22) and the fixed base are slidably connected, the fixed base comprises a slide rail (232), the slide rail (232) is slidably connected to a slider (233), the slider (233) is fixedly connected to the connecting rod (22), and the slider (233) is driven to slide by the power component.
[0034] Furthermore, the main body component also includes a liquid storage barrel (24) and a liquid extraction pump (25), and the feed port of the spray gun (21) is connected to the liquid storage barrel (24) via the liquid extraction pump (25); a liquid flow controller (27) is provided on the pipeline connecting the spray gun (21) and the liquid extraction pump (25); the feed port of the spray gun (21) is also connected to an air intake channel, and an air pressure controller (28) is provided on the air intake channel.
[0035] Furthermore, the spray gun (21) is made of titanium alloy.
[0036] The invention also provides an application of a superlattice structure n-type semiconductor nano-electric heating film in an electrode.
[0037] (III) Beneficial effects
[0038] The beneficial effects of the present invention are:
[0039] The transparent superlattice structure n-type semiconductor nano-electric heating film of the present invention is a combination of antimony chloride, bismuth oxide, tin chloride, stannous chloride, tin oxide, stannous oxide, boron oxide and organic solvent. The semiconductor nano-electric heating film is a transparent superlattice structure n-type, with a light transmittance of more than 85%, and the surface of the film can generate heat evenly, and light energy will not be converted during the heating process. Its electric heating efficiency is as high as more than 98.77%; it saves 45% to 60% of energy compared with ordinary electric furnace wire;
[0040] Among them, the present invention combines insulating tin oxide with other components to make it have the function of a semiconductor, and the preparation of antimony chloride, bismuth oxide, tin chloride, stannous chloride, stannous oxide, and boron oxide. The addition of boron oxide can increase the resistance value and reduce the temperature coefficient of the electric heating film of the present invention. The addition of bismuth oxide and other components can control the fluctuation of conductivity within a certain range to prevent the conductivity from being too high or too low.
[0041] When it is used in the field of water heating, it can achieve water and electricity separation. When it is used in the field of heating dry burning, people can directly contact it.
[0042] It can be applied to low-temperature electrodes and high-temperature electrodes. The sintering temperatures can be 130~170℃ and 550~620℃ respectively, and the sintering temperature can be controlled at a lower level. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a structural schematic diagram of the pipeline type demisting device of the present invention;
[0044] Figure 2 It is a three-dimensional schematic diagram of the mobile spray gun device of the present invention.
[0045] [Description of Reference Numerals]
[0046] 11: Multi-hole mist extraction pipe;
[0047] 12: Exhaust fan
[0048] 13: Cooling pipe;
[0049] 14: Low temperature sealed room;
[0050] 15: Wastewater treatment pool;
[0051] 16: Bottom of furnace;
[0052] 17: Atomizing nozzle;
[0053] 21: spray gun;
[0054] 22: Connecting rod;
[0055] 231: cushion seat; 232: slide rail; 233: slider;
[0056] 24: Liquid storage tank;
[0057] 25: Liquid pump;
[0058] 261: servo motor; 262: conveyor belt; 263: pulley;
[0059] 27: Liquid flow controller;
[0060] 28: Air pressure controller. DETAILED DESCRIPTION
[0061] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.
[0062] The present invention is to improve the preparation of a superlattice structure n-type semiconductor nano-electric heating film with high light transmittance and high electrical conductivity, which includes the following components by weight:
[0063] Antimony chloride 0.3~0.6 parts,
[0064] Tin chloride 5~10 parts,
[0065] 4-8 parts of stannous chloride,
[0066] Tin oxide 3~9 parts,
[0067] 4-8 parts of tin oxide,
[0068] Boron oxide 0.2~0.5 parts,
[0069] 0.3~0.8 parts of bismuth oxide,
[0070] 5~30 parts of organic solvent
[0071] Wherein, antimony chloride is preferably antimony trichloride dihydrate;
[0072] Wherein, tin chloride is preferably tin tetrachloride pentahydrate;
[0073] The organic solvent includes 5 to 15 parts of ethanol, 5 to 9 parts of acetic acid, and 2 to 6 parts of methyl acetate.
[0074] The above-mentioned antimony chloride, tin chloride, stannous chloride, tin oxide ~9 parts, stannous oxide, boron oxide, bismuth oxide and organic solvent are necessary. The replacement of any one component will reduce the transparency and electrothermal efficiency of the semiconductor nano-electrothermal film.
[0075] The transparent superlattice structure n-type semiconductor nano-electric heating film prepared by the present invention uses high-temperature resistant and high-strength metal materials such as iron, stainless steel, aluminum alloy and non-metal materials such as ceramics, quartz glass, mica, ordinary glass, silicon carbide, silicon nitride, microcrystalline glass as the matrix, and can be sprayed on the matrix by a prepared inorganic material mixed liquid to form a conductive film. The light transmittance can reach 85-90%, the atoms and molecules of the coating layer are at the nanometer level, the film presents a superlattice structure, and the conductive mechanism is the n-type semiconductor conductive mechanism.
[0076] Its resistance range can reach 1~10000Ω, and the maximum operating temperature can reach 1000℃ (maximum operating temperature = maximum temperature × 1.4). The substrate can be made into any shape, and the transparent superlattice structure n-type semiconductor nano-electric heating film can be made into the corresponding power according to the required heating temperature. The power supply is not positive or negative, and both AC and DC can be used. The voltage can be any value between 1~450V, and the electrical appliances that need to be heated in life can be realized within the full voltage range, as recorded in the "A safe voltage heater" (patent number: CN201921786277.6) that our company has applied for. It has great selectivity.
[0077] It has excellent characteristics such as high temperature resistance, corrosion resistance, high hardness, long working life, safety and high electrical strength. Under the condition of continuous high temperature dry burning, the resistance of the film layer will not decay significantly, and the temperature coefficient is close to zero. The film layer will not be oxidized, is corrosion-resistant, and is easy to store. The hardness of the film layer can reach 7.5~8. The film layer must be removed by high-intensity grinding with diamond sand on a grinder. Under normal physical collision or scratch conditions, the film layer will hardly be damaged. The working life meets the standard requirements and is greater than 7000 hours. In terms of safety, the leakage current is 0.013mA, which is much smaller than the standard requirement (0.75mA). The film layer is non-toxic, has no harmful radiation, and has no pollution; the electrical strength meets the requirements, that is, the basic insulation can withstand an AC test voltage of 1500V for 1min without breakdown or flashover.
[0078] The present invention provides the following preparation method for preparing the above-mentioned formula components to obtain a superlattice structure n-type semiconductor nano-electric heating film having the above-mentioned effect, which comprises the following steps:
[0079] S1: adding stannous oxide, tin oxide, tin tetrachloride pentahydrate and an organic solvent into distilled water, stirring them thoroughly, and filtering to obtain a solid and a filtrate;
[0080] S2 adding antimony chloride, hydrochloric acid, stannous chloride, an organic solvent, methyl acetate, boron oxide and bismuth oxide to the filtrate to obtain an electrothermal film treatment solution;
[0081] S3: spreading the obtained electrothermal film treatment liquid on the substrate to obtain an electrothermal film on the surface of the substrate.
[0082] Preferably,
[0083] It includes the following steps:
[0084] S1 first mixed material: obtained by mixing antimony chloride, ethanol, acetic acid and stannous chloride;
[0085] S2 second mixed material: obtained by mixing ethanol, stannous oxide and tin oxide;
[0086] S3 third mixed material: obtained by mixing tin chloride, acetic acid and methyl acetate;
[0087] S4 fourth mixed material: obtained by mixing glycerol, methyl acetate, boron oxide and bismuth oxide;
[0088] S5: putting the second mixed material and the third mixed material into 20-25 parts by weight of distilled water at 30-50° C. and stirring for 20-40 minutes to obtain the precipitated solid and the filtrate after filtering;
[0089] S6: Add the first mixed material and the fourth mixed material to the filtrate, and then add 15-20% by mass of distilled water to fully stir for 15-30 minutes to obtain a transparent superlattice structure n-type semiconductor nano-electric heating film treatment liquid. The well-proportioned treatment liquid can be stored in an environment of 5-15°C. When using, take out the treatment liquid and stir it fully at room temperature until the temperature of the treatment liquid reaches room temperature.
[0090] S7: spreading the obtained electrothermal film treatment liquid on the substrate to obtain an electrothermal film on the surface of the substrate.
[0091] The present invention processes insulating tin oxide to obtain a semiconductor and then mixes it with other materials for reaction to adjust the temperature coefficient and control the conductivity within a stable range.
[0092] The present invention also provides the application of the above-mentioned superlattice structure n-type semiconductor nano-electric heating film in an electrode.
[0093] Preparation of high temperature electrode: After printing the conductive silver paste on the obtained coating substrate through a polyester screen or a stainless steel screen, sintering at a temperature of 550~620℃ for 7~10 minutes to obtain a high temperature electrode. The thickness of the screen printing is 11~12μm.
[0094] The preparation method of the low-temperature electrode is to screen-print the conductive silver paste on the obtained coating substrate through the low-temperature conductive ink, and then dry and sinter at 200~280℃ to obtain the low-temperature electrode.
[0095] Furthermore, in step S7, a tunnel furnace type electric heating film production system is used for coating, and the tunnel furnace type electric heating film production system includes a coating machine, a track type mobile spray gun device and a pipeline type demisting device.
[0096] The coating machine includes a high-temperature furnace body and a feeding device, wherein the feeding device is connected to the inlet of the high-temperature furnace body;
[0097] The pipeline demisting device comprises a porous mist extraction pipeline 11, an exhaust fan 12, a cooling pipeline 13, a low-temperature sealed chamber 14 and a wastewater treatment pool 15 which are connected in sequence; the porous mist extraction pipeline 11 is connected to the bottom 16 of the furnace body, and the through hole of the porous mist extraction pipeline 11 is connected to the inner cavity of the coating furnace body; the cooling pipeline 13 and the low-temperature sealed chamber 14 are both provided with atomizing nozzles 17. It solves the technical problem of high cost of manual removal of waste liquid after coating.
[0098] The spray gun 21 of the track-type movable spray gun device can extend into the furnace chamber of the high-temperature furnace body of the coating machine.
[0099] The track-type mobile spray gun device includes a main body component and a spray gun 21, and the spray gun 21 can move back and forth relative to the main body component. The spray gun 21 can move back and forth relative to the main body component to solve the problem that the spray gun 21 is too close to other components in the spray gun 21 device and cannot be flexibly extended to the position to be sprayed inside the furnace body, especially the problem that the main body component is damaged in a high-temperature furnace body such as a high-temperature and highly corrosive environment.
[0100] It also includes a fixed base, and the spray gun 21 is fixedly connected with a connecting rod 22, and the connecting rod 22 is slidably connected to the fixed base. The connecting rod 22 can flexibly extend the spray gun 21 to the outside of the fixed base through the movable connection with the fixed base, so as to extend to the closed environment to be sprayed.
[0101] The fixed base includes a slide rail 232, the slide rail 232 is slidably connected with a slider 233, the slider 233 is fixedly connected to the connecting rod 22, and the slider 233 is driven to slide by a power assembly. The power assembly drives the slider 233 to slide along the slide rail 232, and drives the connecting rod 22 to slide along the direction of the slide rail 232, thereby realizing the movement of the spray gun 21.
[0102] To realize the movement of the connecting rod 22, the power assembly includes a motor 61 and a conveyor belt 262. The motor 61 drives the conveyor belt 262 to move, and the conveyor belt 262 is fixedly connected to the slider 233. The motor 61 is preferably a servo motor 261.
[0103] The fixed base includes more than one slide rail 232 and a raised seat 231 respectively fixed at both ends of the slide rail 232. The inner side walls of the two raised seats 231 are provided with a fixed rod, and a pulley 263 is provided on the fixed rod. The pulley 263 rotates with the fixed rod as the rotation axis. The pulley 263 is also connected to the output end of the motor 61, and the conveyor belt 262 is wound around the pulley 263. The motor 61 is preferably a servo motor 261. The servo motor 261 drives the pulley 263 to rotate with the rotation axis, thereby driving the belt to move, and the belt drives the sliding block to move. The servo motor 261 can accurately control the rotation speed of the pulley 263, so that the pulley 263 drives the base of the fixed spray gun 21, and then accurately controls the required moving speed of the moving spray gun 21.
[0104] The main assembly further includes a liquid storage barrel 24 and a liquid extraction pump 25, and the feed port of the spray gun 21 is connected to the liquid storage barrel 24 through the liquid extraction pump 25. The liquid extraction pump 25 extracts the liquid in the liquid storage barrel 24 into the spray gun 21.
[0105] In order to accurately control the required liquid flow rate, a liquid flow controller 27 is provided on the pipeline connecting the spray gun 21 and the liquid pump 25 .
[0106] The feed port of the spray gun 21 is also connected to an air inlet channel, on which an air pressure controller 28 is provided. The air pressure controller 28 accurately controls the required air pressure to pass into the spray gun 21.
[0107] The air inlet channel and / or the liquid inlet channel connected to the feed port of the spray gun 21 are sleeved in the connecting rod 22. It can be used to protect the air inlet channel and the liquid inlet channel.
[0108] Since the coating conditions are high temperature, corrosive and harsh, the spray gun 21 is made of titanium alloy to be more suitable for the harsh environment in a closed environment or a high-temperature fireplace.
[0109] Other specific structures of the coating machine may be the patented medium and high temperature nano-electric heating film heating glass coating machine structure with patent number ZL 2019 2 0849259.1.
[0110] In order to better understand the above technical solution, exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a clearer and more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0111] Example 1
[0112] The treatment solution of the superlattice structure n-type semiconductor nano-electric heating film includes the following components in parts by weight:
[0113] First mixed material: 0.6 parts of antimony trichloride dihydrate, 5 parts of ethanol, 2 parts of acetic acid, 8 parts of stannous chloride;
[0114] Second mixture: 5 parts of ethanol, 4 parts of stannous chloride, 9 parts of tin oxide;
[0115] The third mixture: 10 parts of tin tetrachloride pentahydrate, 2 parts of acetic acid, and 3 parts of methyl acetate;
[0116] Fourth mixed material: 0.4 parts of glycerol, 1 part of methyl acetate, 0.5 parts of boron oxide and 0.5 parts of bismuth oxide;
[0117] 6 parts of hydrochloric acid;
[0118] 40 parts of distilled water;
[0119] The purity of the above components is above 99%.
[0120] Its preparation method is:
[0121] S1 first mixed material: obtained by mixing corresponding weight portions of the above antimony trichloride dihydrate, ethanol, acetic acid and stannous chloride;
[0122] S2 second mixed material: obtained by mixing the above-mentioned ethanol, stannous oxide and tin oxide in corresponding weight parts;
[0123] S3 third mixed material: obtained by mixing corresponding weight portions of the above tin chloride, acetic acid and methyl acetate;
[0124] S4 fourth mixed material: obtained by mixing corresponding weight portions of the above glycerol, methyl acetate, boron oxide and bismuth oxide;
[0125] S5: putting the second mixed material and the third mixed material into 25 parts by weight of distilled water at 40° C. and stirring them for 20 minutes to obtain the precipitated solid and the filtrate after filtering;
[0126] S6: Add the first mixed material and the fourth mixed material to the filtrate, and then add 15 parts by weight of distilled water and stir it for 30 minutes to obtain a transparent superlattice structure n-type semiconductor nano-electric heating film treatment liquid. The well-proportioned treatment liquid can be stored in an environment of 10°C. When using, take out the treatment liquid and stir it in a room temperature environment until the temperature of the treatment liquid reaches room temperature.
[0127] S7: spreading the obtained electrothermal film treatment liquid on the substrate to obtain an electrothermal film on the surface of the substrate.
[0128] Example 2
[0129] The treatment solution of the superlattice structure n-type semiconductor nano-electric heating film includes the following components in parts by weight:
[0130] First mixed material: 0.3 parts of antimony trichloride dihydrate, 8 parts of ethanol, 3 parts of acetic acid, 4 parts of stannous chloride;
[0131] Second mixture: 7 parts of ethanol, 5 parts of stannous chloride, 3 parts of tin oxide;
[0132] The third mixture: 10 parts of tin tetrachloride pentahydrate, 5 parts of acetic acid, and 1 part of methyl acetate;
[0133] Fourth mixed material: 0.5 parts of glycerol, 1.5 parts of methyl acetate, 0.2 parts of boron oxide and 0.8 parts of bismuth oxide;
[0134] 10 parts of hydrochloric acid;
[0135] 35 parts of distilled water;
[0136] The purity of the above components is above 99%.
[0137] Its preparation method is:
[0138] S1 first mixed material: obtained by mixing corresponding weight portions of the above antimony trichloride dihydrate, ethanol, acetic acid and stannous chloride;
[0139] S2 second mixed material: obtained by mixing the above-mentioned ethanol, stannous oxide and tin oxide in corresponding weight parts;
[0140] S3 third mixed material: obtained by mixing corresponding weight portions of the above tin chloride, acetic acid and methyl acetate;
[0141] S4 fourth mixed material: obtained by mixing corresponding weight portions of the above glycerol, methyl acetate, boron oxide and bismuth oxide;
[0142] S5: putting the second mixed material and the third mixed material into 20 parts by weight of 50° C. distilled water and stirring them for 30 minutes to obtain the precipitated solid and the filtrate after filtering;
[0143] S6: Add the first mixed material and the fourth mixed material to the filtrate, and then add 15 parts by weight of distilled water and stir it for 15 minutes to obtain a transparent superlattice structure n-type semiconductor nano-electric heating film treatment liquid. The well-proportioned treatment liquid can be stored in an environment of 15°C. When using, take out the treatment liquid and stir it in a room temperature environment until the temperature of the treatment liquid reaches room temperature.
[0144] S7: spreading the obtained electrothermal film treatment liquid on the substrate to obtain an electrothermal film on the surface of the substrate.
[0145] Embodiment 3:
[0146] The treatment solution of the superlattice structure n-type semiconductor nano-electric heating film includes the following components in parts by weight:
[0147] First mixed material: 0.5 parts of antimony trichloride dihydrate, 3 parts of ethanol, 5 parts of acetic acid, and 5 parts of stannous chloride;
[0148] Second mixture: 2 parts of ethanol, 8 parts of stannous chloride, 5 parts of tin oxide;
[0149] The third mixture: 5 parts of tin tetrachloride pentahydrate, 6 parts of acetic acid, and 1.5 parts of methyl acetate;
[0150] Fourth mixed material: 0.1 parts of glycerol, 3 parts of methyl acetate, 0.4 parts of boron oxide and 0.3 parts of bismuth oxide;
[0151] 12 parts of hydrochloric acid;
[0152] 40 parts of distilled water;
[0153] The purity of the above components is above 99%.
[0154] Its preparation method is:
[0155] S1 first mixed material: obtained by mixing corresponding weight portions of the above antimony trichloride dihydrate, ethanol, acetic acid and stannous chloride;
[0156] S2 second mixed material: obtained by mixing the above-mentioned ethanol, stannous oxide and tin oxide in corresponding weight parts;
[0157] S3 third mixed material: obtained by mixing corresponding weight portions of the above tin chloride, acetic acid and methyl acetate;
[0158] S4 fourth mixed material: obtained by mixing corresponding weight portions of the above glycerol, methyl acetate, boron oxide and bismuth oxide;
[0159] S5: putting the second mixed material and the third mixed material into 20 parts by weight of distilled water at 30° C. and stirring them for 40 minutes to obtain the precipitated solid and the filtrate after filtering;
[0160] S6: Add the first mixed material and the fourth mixed material to the filtrate, and then add 20 parts by weight of distilled water and stir it for 20 minutes to obtain a transparent superlattice structure n-type semiconductor nano-electric heating film treatment liquid. The well-proportioned treatment liquid can be stored in an environment of 5°C. When using, take out the treatment liquid and stir it in a room temperature environment until the temperature of the treatment liquid reaches room temperature.
[0161] S7: spreading the obtained electrothermal film treatment liquid on the substrate to obtain an electrothermal film on the surface of the substrate.
[0162] Example 4
[0163] In step S7 of Example 1-3, a tunnel-type electric heating film production system is used for coating, which includes a coating machine, a track-type mobile spray gun device and the above-mentioned pipeline demisting device. The coating machine includes a high-temperature furnace body and a feeding device, and the feeding device is connected to the inlet of the high-temperature furnace body; the spray gun 21 of the track-type mobile spray gun device is arranged at the upper end of the high-temperature furnace body.
[0164] like Figure 2 As shown, the pipeline demisting device comprises a porous mist extraction pipeline 11, an exhaust fan 12, a cooling pipeline 13, a low-temperature sealed chamber 14 and a wastewater treatment pool 15 connected in sequence; the porous mist extraction pipeline 11 is connected to the bottom 16 of the high-temperature furnace body of the coating section, and the through hole of the porous mist extraction pipeline 11 is connected to the inner cavity of the coating furnace body; the cooling pipeline 13 and the low-temperature sealed chamber 14 are both provided with an atomizing nozzle 17. The air inlet of the low-temperature sealed chamber 14 is arranged at the upper end of the low-temperature sealed chamber 14, and the air outlet is arranged at the lower end of the low-temperature sealed chamber 14.
[0165] The track-type mobile spray gun device includes a main body component and a spray gun 21. The spray gun 21 can move relative to the main body.
[0166] The main assembly includes a liquid storage barrel 24, a liquid pump 25, a power assembly and a fixed base;
[0167] The spray gun 21 is made of titanium alloy material, and a connecting rod 22 is fixedly connected to the spray gun 21;
[0168] The fixed base includes two raised seats 231, two slide rails 232 and a slider 233 placed in parallel and longitudinally. The two raised seats 231 are respectively fixed at both ends of the slide rails 232. The slider 233 is slidably connected to the slide rails 232. The slider 233 is provided with two through holes for the slide rails 232 to pass through. The slider 233 is fixedly connected to the connecting rod 22. The inner side walls of the two raised seats 231 are respectively fixed with transversely placed fixing rods.
[0169] The power assembly includes a servo motor 261, a conveyor belt 262 and a pulley 263. Pulleys 263 are respectively provided on the fixed rods of the two raised seats 231. The pulleys 263 rotate with the fixed rods as the rotating axes. The conveyor belt 262 is wound around the two pulleys 263 so that the conveyor belt 262 is arranged parallel to the slide rail 232. The conveyor belt 262 and the slider 233 are fixedly connected. The output end of the servo motor 261 is connected to the pulley 263 to drive the conveyor belt 262 to transmit, drive the slider 233 to slide, and thereby enable the spray gun 21 to move.
[0170] The feed port of the spray gun 21 is connected to the liquid storage barrel 24 through a liquid extraction pump 25 , and a liquid flow controller 7 is provided on the pipeline connecting the spray gun 21 and the liquid extraction pump 25 .
[0171] The feed port of the spray gun 21 is also connected to an air inlet channel, on which an air pressure controller 28 is provided. The air inlet channel and / or the liquid inlet channel connected to the feed port of the spray gun 21 are sleeved in the connecting rod 22.
[0172] The specific usage is:
[0173] The coated substrate is placed on the feeding device and sent into the high-temperature furnace. The furnace temperature is 350~820℃ and the temperature uniformity is ≤2.5%. When the coated substrate is evenly heated to the furnace temperature, the coated substrate is transported to the coating section of the high-temperature furnace by a conveyor chain.
[0174] The liquid pump 25 in the track-type mobile spray gun device is an electronic control device that can strictly control the infusion volume and flow rate. The liquid pump 25 transports the liquid treatment liquid to the spray gun 21 system through the conduit, fully mixes the liquid treatment liquid with 3-8 kg of air pressure and atomizes it through the spray gun 21, so that the fully atomized liquid treatment liquid is evenly plated on the substrate;
[0175] During the coating stage, the excess liquid treatment solution atomized by the spray gun 21 will be sucked into the cooling pipe 13 by the exhaust fan 12. A large number of atomizing nozzles 17 are installed in the pipe. When the excess liquid treatment solution passes through the cooling pipe 13, it is cooled by the cooling water sprayed by the atomizing nozzles 17 in the cooling pipe 13 to be liquefied. The liquid treatment solution smoke that is not completely cooled and liquefied in the cooling pipe 13 is further fully liquefied, and then the completely liquefied liquid treatment solution is sent to the wastewater treatment pool 15 through the pipe. Industrial production without pollution is realized. After the coating is completed, the substrate will be transported to the air cooling device to quickly cool the substrate to about 30 degrees, and the substrate can be directly touched by hand.
[0176] This embodiment uses a mechanized and automatic track-type mobile spray gun device for atomization spray coating, replacing the manual spraying method, and uses a pipeline demisting device to cool and liquefy the excess atomized treatment liquid that is over-sprayed, and finally flows into the wastewater treatment pool through a pipeline, thereby achieving industrial production without pollution. Due to the low equipment failure rate, the production time is greatly shortened, and only personnel need to carry the substrate during the production process.
[0177] Among them, since the spray gun can be extended into the high-temperature furnace body, the problem of high temperature resistance and corrosion caused by components other than the spray gun being too close to the furnace body is prevented, and the spraying mold is further made more uniform and more accurate.
[0178] Experimental data:
[0179] After inspection by the National Infrared and Industrial Electric Heating Product Quality Supervision and Inspection Center, all indicators of the electric heating films obtained in Examples 1-3 of the present invention meet the standard requirements and are higher than the standard requirements.
[0180] The electric heating film is far-infrared surface heating, and its normal total reflectivity is 0.83 (+), with concentrated heat transfer and fast temperature rise. The electrothermal radiation conversion efficiency is 70%, which is nearly 20% higher than the standard requirement, and its electrothermal conversion efficiency is more than 98% (electrothermal conversion efficiency = electrothermal radiation conversion efficiency × 1.4). After the electric heating film is powered on, the relative radiation energy spectrum (infrared radiation wavelength range) is 5~20μm, and the human body has the best absorption of far infrared rays in this band.
[0181] The obtained electric heating film can reach 1000 degrees Celsius, and the electric heating efficiency is as high as 98.77% or more. When working for a short time under constant voltage, the current will drop, resulting in a decrease in power, high energy-saving efficiency, and 45% to 60% energy saving compared to ordinary resistance wire electric heating coils. It also has the characteristics of strong acid and alkali resistance, high temperature non-aging, and zero attenuation. It can be easily installed and set up, and can be cut at will according to needs, with different powers, and flexibly laid on the ground and walls. It can be widely used in homes, villas, offices, hotels, steam rooms, delivery rooms, greenhouses and other places that require heating. It does not occupy any indoor plane space, so that the indoor space can be more flexibly arranged and placed furniture, and enjoy the use of a larger space. In the field of household appliances, it can replace traditional electric furnace wire heaters and is widely used in electric ceramic stoves, ovens, water boilers, water heaters, kettles, etc.
[0182] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0183] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0184] In the present invention, unless otherwise clearly specified and limited, when a first feature is “on” or “below” a second feature, it may be that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, when a first feature is “above”, “above” or “above” a second feature, it may be that the first feature is directly above or obliquely above the second feature, or it may simply mean that the first feature is higher in level than the second feature. When a first feature is “below”, “below” or “below” a second feature, it may be that the first feature is directly below or obliquely below the second feature, or it may simply mean that the first feature is lower in level than the second feature.
[0185] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "embodiment", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0186] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may alter, modify, replace and modify the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a superlattice structure n-type semiconductor nano-electric heating film, characterized in that: Its use includes the following components by weight: Antimony chloride 0.3~0.6 parts, 5-10 parts of tin tetrachloride pentahydrate, 4-8 parts of stannous chloride, Tin oxide 3~9 parts, 4-8 parts of tin oxide, Boron oxide 0.2~0.5 parts, 0.3~0.8 parts of bismuth oxide, 5-30 parts of organic solvent; The method for preparing the superlattice structure n-type semiconductor nano-electric heating film comprises the following steps: S1: adding stannous oxide, tin oxide, tin tetrachloride pentahydrate and an organic solvent into distilled water, stirring them thoroughly, and filtering to obtain a solid and a filtrate; S2 adding antimony chloride, hydrochloric acid, stannous chloride, an organic solvent, boron oxide and bismuth oxide to the filtrate to obtain an electrothermal film treatment solution; S3: coating the obtained electrothermal film treatment liquid on the substrate to obtain an electrothermal film on the surface of the substrate.
2. The method for preparing the superlattice structure n-type semiconductor nano-electric heating film according to claim 1, characterized in that: The antimony chloride is antimony trichloride dihydrate; or / and The organic solvent includes 5 to 15 parts of ethanol, 5 to 9 parts of acetic acid, and 2 to 6 parts of methyl acetate.
3. The method for preparing the superlattice structure n-type semiconductor nano-electric heating film according to claim 1, characterized in that: In step S3, a tunnel furnace type electric heating film production system is used for coating, which includes a coating machine, a track type mobile spray gun (21) device and a pipeline type demisting device, wherein the coating machine includes a high temperature furnace body and a feeding device, wherein the feeding device is connected to the inlet of the high temperature furnace body; The spray gun (21) of the track-type movable spray gun (21) device can extend into the furnace chamber of the high-temperature furnace body of the coating machine; The pipeline demisting device comprises a porous mist extraction pipeline (11), an exhaust fan (12), a cooling pipeline (13), a low-temperature sealed chamber (14) and a wastewater treatment pool (15) which are connected in sequence; the porous mist extraction pipeline (11) is connected to the bottom of the furnace body (16), and the through hole of the porous mist extraction pipeline (11) is connected to the inner cavity of the coating furnace body; and atomizing nozzles (17) are provided in the cooling pipeline (13) and the low-temperature sealed chamber (14).
4. The method for preparing the superlattice structure n-type semiconductor nano-electric heating film according to claim 3, characterized in that: A condenser tube is wound around the outside of the cooling pipe (13); the air inlet of the low-temperature sealed chamber (14) is arranged at the upper end of the low-temperature sealed chamber (14), and the air outlet is arranged at the lower end of the low-temperature sealed chamber (14).
5. The method for preparing the superlattice structure n-type semiconductor nano-electric heating film according to claim 3, characterized in that: The track-type movable spray gun (21) device comprises a main body component and a spray gun (21), and the spray gun (21) can move back and forth relative to the main body component.
6. The method for preparing the superlattice structure n-type semiconductor nano-electric heating film according to claim 5, characterized in that: The main body component comprises a fixed base, the spray gun (21) is fixedly connected to a connecting rod (22), the connecting rod (22) and the fixed base are slidably connected, the fixed base comprises a slide rail (232), the slide rail (232) is slidably connected to a slider (233), the slider (233) is fixedly connected to the connecting rod (22), and the slider (233) is driven to slide by a power component.
7. The method for preparing the superlattice structure n-type semiconductor nano-electric heating film according to claim 6, characterized in that: The main body assembly further comprises a liquid storage barrel (24) and a liquid extraction pump (25), and the feed port of the spray gun (21) is connected to the liquid storage barrel (24) via the liquid extraction pump (25); a liquid flow controller (27) is provided on the pipeline connecting the spray gun (21) and the liquid extraction pump (25); the feed port of the spray gun (21) is also connected to an air intake channel, and an air pressure controller (28) is provided on the air intake channel.
8. The method for preparing the superlattice structure n-type semiconductor nano-electric heating film according to any one of claims 3 to 7, characterized in that: The spray gun (21) is made of titanium alloy.
9. The superlattice structured n-type semiconductor nano-electric heating film prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the superlattice structure n-type semiconductor nano-electric heating film according to claim 9 in an electrode.