A composite foil material for improving the safety of lithium-ion batteries, and its preparation method and use

By designing a composite foil structure, the aluminum foil layer melts to provide a safety net, while the polymer layer wraps around the needle, solving the safety issues of lithium-ion batteries in the high-energy/high-power field. This achieves protection against needle puncture and reduces short-circuit current, improving safety and reducing production costs.

CN112366323BActive Publication Date: 2024-11-08SVOLT ENERGY TECH (WUXI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011194224.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-30
Publication Date
2024-11-08
Estimated Expiration
2040-10-30

AI Technical Summary

Technical Problem

The safety issues of existing lithium-ion batteries in the high-energy/high-power field have not been effectively resolved, especially the management and control of thermal runaway under abuse conditions. Liquid electrolytes are prone to leakage, flammability and explosion, and existing protection measures are irreversible and costly.

Method used

The composite foil structure includes a substrate layer, a polymer layer, and an aluminum foil layer. The aluminum foil layer melts during needle puncture to provide a safety net, while the polymer layer wraps around the needle to increase insulation, reduce debris, prevent short circuits, and reduce short circuit current.

Benefits of technology

It significantly improves the puncture resistance and safety of lithium-ion batteries, reduces production costs, and prevents battery fires and explosions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112366323B_ABST
    Figure CN112366323B_ABST
Patent Text Reader

Abstract

The present invention provides a composite foil material for improving the safety of lithium-ion batteries, a preparation method and use thereof, wherein the composite foil material comprises a substrate layer, a polymer layer and an aluminum foil layer which are stacked in sequence. The preparation method comprises: coating a polymer solution on the surface of the substrate layer, forming a polymer layer after drying, and depositing an aluminum foil layer on the surface of the polymer layer to obtain the composite foil material. The composite foil material provided by the present invention is mainly used to improve the safety of batteries, and replaces the copper foil and aluminum foil commonly used in lithium-ion batteries with stainless steel foil materials, thereby reducing production costs. At the same time, by redesigning the foil material, the safety of the battery cell is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ions, and relates to a composite foil material for improving the safety of lithium ion batteries, a preparation method and application thereof. Background Art

[0002] Lithium-ion secondary batteries have the advantages of high energy density, high power density, and long battery life. They are now widely used in automotive power batteries. With the large-scale application of batteries, safety is becoming more and more prominent. Safety is still a key factor restricting the application of lithium-ion batteries in high-energy / high-power fields. The potential safety issues of lithium-ion batteries have greatly affected the promotion of new energy vehicles.

[0003] Lithium-ion batteries have been widely used in various industries. With the promotion of application fields and the increasing requirements for user experience, end customers have higher and higher requirements for the safety performance of lithium batteries. At present, there are no fully mature products in the industry that can improve the safety performance of lithium-ion batteries. Although the specific cause of the mobile phone explosion incident has not been clearly investigated, the industry analysis is that it is likely that the safety factor of the high-energy-density lithium battery used does not meet the requirements of relevant international certification.

[0004] Lithium-ion batteries have been developing rapidly in recent years due to their advantages such as high specific energy and no memory effect. In particular, with the gradual application of lithium-ion batteries in EV pure electric vehicles, low-speed electric vehicles and other fields, the safety performance and cycle performance of lithium-ion batteries have always attracted much attention. Therefore, the management and control of thermal runaway of power lithium-ion batteries under abuse conditions has always been the focus of research and attention in the industry. Liquid lithium-ion batteries use organic carbonate liquid electrolytes, which are easy to leak, burn, and explode. They are not safe and cannot be punctured. After puncture, the battery is prone to fire and explosion.

[0005] Normally, the process of thermal runaway of lithium-ion batteries is as follows: when a short circuit occurs in the battery cell, the instantaneous short-circuit large current generates heat through the anode and cathode electrodes. First, the anode SEI begins to self-decompose and release heat when it reaches a certain temperature. As the heat accumulates, the charged graphite anode reacts with the electrolyte to release heat, and at the same time, the heat is accumulated to increase the temperature of the battery cell. When the temperature of the battery cell rises to a certain level, the charged cathode structure collapses and releases free highly reactive oxygen atoms. The released oxygen atoms react with the binder in the electrode material, the conductive auxiliary material and the electrolyte in the battery cell, instantly releasing a large amount of heat, and the battery burns or explodes.

[0006] At present, the safety protection measures to prevent thermal runaway of the battery cells in lithium-ion batteries are mainly as follows: (1) The shutdown function of the diaphragm is used to organize the current flow to reduce the risk of thermal runaway. The main drawback of this method is that after the diaphragm is shut down, the battery cell is also scrapped and can no longer be used. In addition, since the diaphragm used in lithium-ion batteries is a porous polyolefin membrane, its shutdown mechanism is mainly to shut down the current by melting polyethylene at a temperature of 130°C. When a short circuit occurs in a lithium-ion battery, the internal temperature distribution is usually uneven. Therefore, some parts will reach the shutdown temperature while others will not. In this way, the current of the entire battery cell cannot be cut off; (2) Safety protection is provided by the CID pressure relief safety valve. When the gas pressure generated by the violent reaction or other forms of reaction of the battery cell reaches the CID rupture threshold, the battery cell CID ruptures to protect the battery cell. This form of protection is similar to the diaphragm shutdown. After the protection occurs, the battery cell can no longer be used. It is an irreversible protection.

[0007] CN106848383A discloses a lithium-ion battery, comprising a negative electrode sheet and a positive electrode sheet, wherein the negative electrode sheet is coated with a chemically inert organic polymer coating, the organic polymer coating is insoluble in water, and the melting point of the organic polymer coating is 90-110°C. When thermal runaway occurs in the lithium-ion battery, the organic polymer coating melts to form a coating layer on the surface of the negative electrode sheet, isolating the contact short circuit between the positive electrode sheet and the negative electrode sheet.

[0008] CN104347892A discloses a lithium battery with high safety, which can solve the safety problems of external puncture of lithium battery or internal short circuit of lithium battery and reduce the internal heat and battery deformation of lithium battery without affecting the chemical properties of single-pack lithium battery sheets. It includes a lithium battery body, which includes a plurality of single-pack lithium battery sheets, which are connected in series in sequence, and circuit breakers are respectively connected in series on the connecting lines of two adjacent layers of single-pack lithium battery sheets; a heat-insulating sealing cloth layer is wrapped on the outer surface of the single-pack lithium battery sheet, a No. 1 protective mesh layer is wrapped on the outer surface of the heat-insulating sealing cloth layer, and main glue is sealed in each mesh of the No. 1 protective mesh layer; a No. 2 protective mesh layer is wrapped on the outer surface of the No. 1 protective mesh layer, and auxiliary glue is sealed in each mesh of the No. 2 protective mesh layer.

[0009] CN106299204A discloses a high-safety lithium battery separator, which comprises a base film and an aluminum oxide coating coated on one or both sides of the base film, wherein the aluminum oxide coating has a thickness of 1 to 4 μm.

[0010] In response to the safety issues of lithium batteries, most current battery cell manufacturers have improved safety by coating the diaphragm with a ceramic layer, adding nickel, manganese and other metal materials to the positive electrode for doping, coating the copper foil / aluminum foil surface, and using graphene and lithium titanate. The above methods have their own characteristics and have also played a certain role in improving safety. However, the safety performance of the battery still cannot meet the demand, so there is an urgent need for a lithium-ion battery with high safety performance. Summary of the invention

[0011] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a composite foil material for improving the safety of lithium-ion batteries, a preparation method and uses thereof. The present invention further improves the safety of the battery cell by redesigning the composite foil material structure.

[0012] To achieve this object, the present invention adopts the following technical solutions:

[0013] In a first aspect, the present invention provides a composite foil material for improving the safety of lithium-ion batteries. The composite foil material comprises a substrate layer, a polymer layer and an aluminum foil layer stacked in sequence.

[0014] The composite foil provided by the present invention is mainly used to improve the safety of batteries. Through the redesign of the foil, after the composite foil is used in lithium-ion batteries, when the lithium-ion batteries are punctured, first the current of the aluminum foil layer is too large, the aluminum foil layer fuses, and a first layer of safety net is provided; because the diameter of the needle is larger than the aperture of the polymer layer, when the needle penetrates the aluminum foil layer and the polymer layer, the polymer can wrap the needle head to increase insulation, and at the same time the polymer layer is closely attached to the stainless steel layer, which can reduce debris, prevent short circuit, reduce short circuit current, and greatly improve the anti-puncture safety of the battery.

[0015] As a preferred technical solution of the present invention, the substrate layer is a stainless steel layer.

[0016] The present invention replaces the copper foil and aluminum foil commonly used in the substrate layer with stainless steel foil, thereby reducing production costs.

[0017] Preferably, the polymer layer comprises a polymer.

[0018] Preferably, the polymer comprises one or a combination of at least two of poly(ethylene glycol acrylate), poly(divinyl sulfide), poly(vinylidene fluoride), polyacrylonitrile, poly(vinylidene fluoride-hexafluoropropylene), polyethylene oxide, poly(methyl methacrylate), polytetrafluoroethylene, poly(propylene carbonate), poly(ethylene carbonate) or poly(vinyl acetate).

[0019] As a preferred technical solution of the present invention, the pore size of the polymer layer is 0.3-0.8 mm, for example, it can be 0.3 mm, 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, 0.55 mm, 0.6 mm, 0.65 mm, 0.7 mm, 0.75 mm or 0.8 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the thickness of the polymer layer is 3 to 5 μm, for example, it can be 3.0 μm, 3.2 μm, 3.4 μm, 3.6 μm, 3.8 μm, 4.0 μm, 4.2 μm, 4.4 μm, 4.6 μm, 4.8 μm or 5.0 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the thickness of the aluminum foil layer is 1 to 2 μm, for example, it can be 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm or 2.0 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] In a second aspect, the present invention provides a method for preparing the composite foil according to the first aspect, the preparation method comprising:

[0023] The polymer solution is coated on the surface of the substrate layer, and after drying, a polymer layer is formed, and an aluminum foil layer is deposited on the surface of the polymer layer to obtain the composite foil material.

[0024] As a preferred technical solution of the present invention, the polymer solution is prepared by the following method:

[0025] In an environment with a dew point of ≤-40° C., a polymer is added to an organic solvent, and the polymer solution is obtained after mixing.

[0026] Preferably, the polymer comprises one or a combination of at least two of poly(ethylene glycol acrylate), poly(divinyl sulfide), poly(vinylidene fluoride), polyacrylonitrile, poly(vinylidene fluoride-hexafluoropropylene), polyethylene oxide, poly(methyl methacrylate), polytetrafluoroethylene, poly(propylene carbonate), poly(ethylene carbonate) or poly(vinyl acetate).

[0027] Preferably, the organic solvent comprises one or a combination of at least two of dimethylacetamide, dimethyl sulfoxide, tetrahydrofuran, acetonitrile or N-methylpyrrolidone.

[0028] Preferably, the polymer accounts for 30-50wt% of the polymer solution, for example, it can be 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt%, 42wt%, 44wt%, 46wt%, 48wt% or 50wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] As a preferred technical solution of the present invention, the drying temperature is 80-90°C, for example, it can be 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the drying time is 20 to 30 hours, for example, it can be 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours or 30 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] As a preferred technical solution of the present invention, the deposition method is evaporation.

[0032] Preferably, the evaporation process comprises: in a vacuum environment, heating and melting solid aluminum until it evaporates to form gaseous aluminum, the gaseous aluminum is deposited on the surface of the polymer layer, and after cooling and reduction, an aluminum foil layer is obtained.

[0033] Preferably, the vacuum degree is 1.3×10 -2 ~1.3×10 -3 Pa, for example, can be 0.0013Pa, 0.002Pa, 0.003Pa, 0.004Pa, 0.005Pa, 0.006Pa, 0.007Pa, 0.008Pa, 0.009Pa, 0.01Pa, 0.012Pa or 0.013Pa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the solid aluminum is heated to 1200-1400°C, for example, it can be 1200°C, 1220°C, 1240°C, 1260°C, 1280°C, 1300°C, 1320°C, 1340°C, 1360°C, 1380°C or 1400°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the cooling temperature is -18 to -15°C, for example, it can be -18°C, -17.5°C, -17°C, -16.5°C, -16°C, -15.5°C or -15°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] In a third aspect, the present invention provides an electrode sheet, comprising the composite foil material as described in the first aspect, and a positive electrode material layer or a negative electrode material layer disposed on a surface of the composite foil material.

[0037] In a fourth aspect, the present invention provides a method for preparing the electrode sheet according to the third aspect, the method comprising:

[0038] The positive electrode slurry or the negative electrode slurry is coated on the surface of the composite foil material in the first aspect, and then the composite foil material is dried, rolled and sliced ​​in sequence to obtain the electrode sheet.

[0039] In a fifth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery uses the electrode sheet described in the third aspect as an electrode.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The composite foil provided by the present invention is mainly used to improve the safety of batteries. The copper foil and aluminum foil commonly used in lithium-ion batteries are replaced with stainless steel foil, thereby reducing production costs. At the same time, by redesigning the foil, after the composite foil is used in lithium-ion batteries, when the lithium-ion batteries are punctured, first the current in the aluminum foil layer is too large, and the aluminum foil layer fuses, providing a first layer of safety net; because the diameter of the needle is larger than the pore size of the polymer layer, when the needle penetrates the aluminum foil layer and the polymer layer, the polymer can wrap the needle head to increase insulation, and at the same time the polymer layer is closely attached to the stainless steel layer, which can reduce debris, prevent short circuits, and reduce short-circuit currents, thereby greatly improving the battery's anti-puncture safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a schematic diagram of the structure of the composite foil provided in Example 1 of the present invention.

[0043] Among them, 1-aluminum foil layer; 2-polymer layer; 3-stainless steel layer. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0045] Example 1

[0046] This embodiment provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0047] (1) in an environment with a dew point of ≤-40° C., adding a polymer poly(ethylene glycol acrylate) to an organic solvent dimethylacetamide, and mixing under ultrasonic conditions to obtain a polymer solution with a concentration of 30 wt %;

[0048] (2) coating the surface of the stainless steel layer 1 with a polymer solution to a coating thickness of 3 μm, and drying at 80° C. for 30 h to form a polymer layer 2, wherein the average pore size of the polymer layer 2 is 0.3 mm;

[0049] (3) In a vacuum environment of 0.0013 Pa, solid aluminum is heated and melted at 1200°C until it evaporates to form gaseous aluminum, which is deposited on the surface of the polymer layer 2 and then cooled and reduced at -15°C to form a 1 μm aluminum foil layer 1, and finally the following is obtained: Figure 1 The composite foil material.

[0050] Example 2

[0051] This embodiment provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0052] (1) adding a polymer polydivinyl sulfide to an organic solvent dimethyl sulfoxide in an environment with a dew point of ≤-40° C., and mixing under ultrasonic conditions to obtain a polymer solution with a concentration of 34 wt %;

[0053] (2) coating the surface of the stainless steel layer 1 with a polymer solution to a coating thickness of 3.4 μm, and drying at 82° C. for 28 h to form a polymer layer 2, wherein the average pore size of the polymer layer 2 is 0.35 mm;

[0054] (3) In a vacuum environment of 0.003 Pa, solid aluminum is heated and melted at 1240° C. until it evaporates to form gaseous aluminum, which is deposited on the surface of the polymer layer 2. After cooling and reduction at -15.6° C., a 1.2 μm aluminum foil layer 1 is formed, thereby finally obtaining the composite foil material.

[0055] Example 3

[0056] This embodiment provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0057] (1) adding a polymer polyvinylidene fluoride to an organic solvent N-methylpyrrolidone in an environment with a dew point of ≤-40° C., and mixing under ultrasonic conditions to obtain a polymer solution with a concentration of 38 wt %;

[0058] (2) coating the surface of the stainless steel layer 1 with a polymer solution to a coating thickness of 3.8 μm, and drying at 84° C. for 26 h to form a polymer layer 2, wherein the average pore size of the polymer layer 2 is 0.56 mm;

[0059] (3) In a vacuum environment of 0.006 Pa, solid aluminum is heated and melted at 1280° C. until it evaporates to form gaseous aluminum, which is deposited on the surface of the polymer layer 2. After cooling and reduction at -16.2° C., a 1.4 μm aluminum foil layer 1 is formed, thereby finally obtaining the composite foil material.

[0060] Example 4

[0061] This embodiment provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0062] (1) adding a polymer polymethyl methacrylate to an organic solvent tetrahydrofuran in an environment with a dew point of ≤-40° C., and mixing under ultrasonic conditions to obtain a polymer solution with a concentration of 42 wt %;

[0063] (2) coating the surface of the stainless steel layer 1 with a polymer solution to a coating thickness of 4.2 μm, and drying at 86° C. for 24 h to form a polymer layer 2, wherein the average pore size of the polymer layer 2 is 0.67 mm;

[0064] (3) In a vacuum environment of 0.008 Pa, solid aluminum is heated and melted at 1320° C. until it evaporates to form gaseous aluminum, which is deposited on the surface of the polymer layer 2. After cooling and reduction at -16.8° C., a 1.6 μm aluminum foil layer 1 is formed, thereby finally obtaining the composite foil material.

[0065] Example 5

[0066] This embodiment provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0067] (1) adding a polymer polyvinyl acetate to an organic solvent acetonitrile in an environment with a dew point of ≤-40° C., and mixing under ultrasonic conditions to obtain a polymer solution with a concentration of 46 wt %;

[0068] (2) coating the surface of the stainless steel layer 1 with a polymer solution to a coating thickness of 4.6 μm, and drying at 88° C. for 22 h to form a polymer layer 2, wherein the average pore size of the polymer layer 2 is 0.74 mm;

[0069] (3) In a vacuum environment of 0.01 Pa, solid aluminum is heated and melted at 1360° C. until it evaporates to form gaseous aluminum, which is deposited on the surface of the polymer layer 2. After cooling and reduction at -17.4° C., a 1.8 μm aluminum foil layer 1 is formed, thereby finally obtaining the composite foil material.

[0070] Example 6

[0071] This embodiment provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0072] (1) adding a polymer polytetrafluoroethylene to an organic solvent N-methylpyrrolidone in an environment with a dew point of ≤-40° C., and mixing under ultrasonic conditions to obtain a polymer solution with a concentration of 50 wt %;

[0073] (2) coating the surface of the stainless steel layer 1 with a polymer solution to a coating thickness of 5 μm, and drying at 90° C. for 20 h to form a polymer layer 2, wherein the average pore size of the polymer layer 2 is 0.8 mm;

[0074] (3) In a vacuum environment of 0.013 Pa, solid aluminum is heated and melted at 1400° C. until it evaporates to form gaseous aluminum, which is deposited on the surface of the polymer layer 2 and cooled and reduced at -18° C. to form a 2 μm aluminum foil layer 1, thereby finally obtaining the composite foil material.

[0075] Comparative Example 1

[0076] This comparative example provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0077] In a vacuum environment of 0.0013 Pa, solid aluminum is heated and melted at 1200°C until it evaporates to form gaseous aluminum, which is deposited on the surface of the stainless steel layer 1 and then cooled and reduced at -15°C to form a 1 μm aluminum foil layer 1, thereby finally obtaining the composite foil.

[0078] The composite foil prepared in this comparative example only includes a stainless steel layer 1 and an aluminum foil layer 1. Compared with Example 1, the intermediate polymer layer 2 is missing. The operating steps and process conditions used in the deposition process of the aluminum foil layer 1 are exactly the same as those in Example 1.

[0079] Comparative Example 2

[0080] This comparative example provides a method for preparing a composite foil, and the preparation method comprises the following steps:

[0081] (1) in an environment with a dew point of ≤-40° C., adding a polymer poly(ethylene glycol acrylate) to an organic solvent dimethylacetamide, and mixing under ultrasonic conditions to obtain a polymer solution with a concentration of 30 wt %;

[0082] (2) A polymer solution is coated on the surface of the stainless steel layer 1 with a coating thickness of 3 μm. After drying at 80° C. for 30 h, a polymer layer 2 is formed. The average pore size of the polymer layer 2 is 0.3 mm.

[0083] The composite foil prepared in this comparative example only includes a stainless steel layer 1 and a polymer layer 2. Compared with Example 1, the outermost aluminum foil layer 1 is missing. The operating steps and process conditions used in the coating process of the polymer layer 2 are exactly the same as those in Example 1.

[0084] The composite foil prepared in Examples 1-5 and Comparative Examples 1-2 was used as an electrode sheet substrate. After the positive electrode slurry was coated on the surface of the composite foil, the positive electrode sheet was obtained by drying, rolling and slicing. After the negative electrode slurry was coated on the surface of another composite foil, the negative electrode sheet was obtained by drying, rolling and slicing. The positive electrode sheet and the negative electrode sheet were used as the positive electrode and the negative electrode of the battery respectively, and the sulfide solid electrolyte layer was used as a separator to assemble and obtain a lithium battery cell.

[0085] The above lithium-ion battery cells are subjected to the following safety performance tests:

[0086] (1) Narrow surface compression test: 10 battery cells were taken from each embodiment and comparative example. After being fully charged, the battery cells were placed upright on their sides between two parallel plates. The pressure was gradually increased to 17.2 MPa. The pressure was maintained for 1 min, then released and observed for 1 h. The battery cells were considered to have passed the test if they did not catch fire or explode.

[0087] (2) Overcharge test: Take 10 battery cells from each embodiment and comparative example, place the battery cells at 23±5°C, discharge the battery cells to 3.0V, charge them to 5V with a current of 3C, and allow the current to drop to nearly 0A at a certain voltage. Monitor the battery temperature change. When the temperature drops to about 10°C lower than the peak value, stop the experiment and observe the battery cell status. If the battery cells do not catch fire or explode, the test is considered to have passed.

[0088] (3) 150°C hot box test: Take 10 battery cells from each example and comparative example, and after fully charging, place the battery cells in a hot box. Heat the temperature to 150±2°C at a rate of 5±2°C / min and keep the temperature for 10 min. Record the surface temperature of the battery and observe the state of the battery cells. If the battery cells do not catch fire or explode, the test is considered to have passed.

[0089] (4) Anti-puncture test: 10 battery cells were taken from each embodiment and comparative example. After fully charged, the battery cells were pierced with a 3 mm needle at a puncture speed of 50 mm / s. The battery surface temperature was recorded and the battery cell status was observed. The battery cells were deemed to have passed the test if they did not catch fire or explode.

[0090] (5) Short-circuit test: 10 battery cells were taken from each embodiment and comparative example. After fully charging, the positive electrode of the battery cell was converted to nickel. The positive and negative electrodes were connected using wires with different internal resistances of 30 mΩ and 45 mΩ. The temperature change of the battery was monitored. When the temperature dropped to about 10°C lower than the peak value, the experiment was stopped and the battery cell status was observed. The battery cell was considered to have passed the test if it did not catch fire or explode.

[0091] The above test methods were used to test one by one, and the safety performance test results obtained are shown in Table 1.

[0092]

[0093]

[0094] It can be seen from the test results provided in Table 1 that compared with the comparative example, all the safety performance tests of Examples 1-6 passed, which indicates that the safety performance of the battery cell prepared by the method provided by the present invention is significantly improved. The reason is that the present invention designs a three-layer composite foil as an electrode sheet substrate. The role of the aluminum foil layer 1 is that during needle puncture, the current of the aluminum foil layer 1 is too large and the aluminum foil layer 1 is melted; the role of the polymer layer 2 is that, since the diameter of the needle is larger than the pore size of the polymer layer 2, when the needle penetrates the aluminum foil layer 1 and the polymer layer 2, the polymer can wrap the needle tip to increase insulation. At the same time, the polymer layer 2 is close to the stainless steel layer 1, which can reduce debris, prevent short circuits, and reduce short-circuit current, thereby greatly improving the battery's anti-puncture safety.

[0095] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a composite foil material for improving the safety of lithium-ion batteries, characterized in that: The composite foil material comprises a substrate layer, a polymer layer and an aluminum foil layer which are stacked in sequence; The preparation method comprises: A polymer solution is coated on the surface of the substrate layer to form a polymer layer after drying, and an aluminum foil layer is deposited on the surface of the polymer layer to obtain the composite foil material; The polymer solution is prepared by the following method: In an environment with a dew point of ≤-40°C, a polymer is added to an organic solvent, and the polymer solution is obtained after mixing; the polymer accounts for 30-50wt% of the polymer solution; The pore size of the polymer layer is 0.3-0.8 mm; The substrate layer is a stainless steel layer; The thickness of the aluminum foil layer is 1.2-2 μm.

2. The preparation method according to claim 1, characterized in that: The polymer layer includes a polymer.

3. The preparation method according to claim 1, characterized in that: The polymer includes one or a combination of at least two of poly(ethylene glycol acrylate), poly(divinyl sulfide), poly(vinylidene fluoride), polyacrylonitrile, poly(vinylidene fluoride-hexafluoropropylene), polyethylene oxide, poly(methyl methacrylate), polytetrafluoroethylene, poly(propylene carbonate), poly(ethylene carbonate) or poly(vinyl acetate).

4. The preparation method according to claim 1, characterized in that: The thickness of the polymer layer is 3-5 μm.

5. The preparation method according to claim 1, characterized in that: The organic solvent includes one or a combination of at least two of dimethylacetamide, dimethyl sulfoxide, tetrahydrofuran, acetonitrile or N-methylpyrrolidone.

6. The preparation method according to claim 1, characterized in that: The drying temperature is 80-90°C.

7. The preparation method according to claim 1, characterized in that: The drying time is 20 to 30 hours.

8. The preparation method according to claim 1, characterized in that: The deposition method is evaporation.

9. The preparation method according to claim 8, characterized in that: The evaporation process includes: in a vacuum environment, heating and melting solid aluminum to evaporate and form gaseous aluminum, the gaseous aluminum is deposited on the surface of the polymer layer, and the aluminum foil layer is obtained after cooling and reduction.

10. The preparation method according to claim 1, characterized in that: The vacuum degree is 1.3×10 -2 ~1.3×10 -3 Pa.

11. The preparation method according to claim 1, characterized in that: The solid aluminum is heated to 1200-1400°C.

12. The preparation method according to claim 1, characterized in that: The cooling temperature is -18~-15℃.

13. An electrode sheet, characterized in that: The electrode sheet comprises a composite foil prepared by the preparation method according to any one of claims 1 to 12, and a positive electrode material layer or a negative electrode material layer arranged on the surface of the composite foil.

14. A method for preparing the electrode sheet according to claim 13, characterized in that: The preparation method comprises: The surface of the composite foil prepared by the preparation method according to any one of claims 1 to 12 is coated with positive electrode slurry or negative electrode slurry, and then dried, rolled and sliced ​​in sequence to obtain the electrode sheet.

15. A lithium ion battery, characterized in that: The lithium-ion battery adopts the electrode sheet described in claim 14 as an electrode.