A method for preparing a super-wetting coating suitable for the inner surface of a stainless steel pipe

Through the coaxial dynamic electrochemical etching and anodizing method of coating the cathode, a micron-scale rough structure is constructed on the inner surface of the stainless steel tube and a nanostructure is formed, which solves the short circuit problem in the preparation of the superwetting coating on the inner surface of the small inner diameter stainless steel tube and achieves It has the characteristics of easy operation, simple equipment and low cost.

CN112593281BActive Publication Date: 2024-10-29CHONGQING UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202011324739.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-23
Publication Date
2024-10-29
Estimated Expiration
2040-11-23

AI Technical Summary

Technical Problem

It is difficult to uniformly prepare a superwetting coating on the inner surface of stainless steel tubes with the existing technology, especially in capillary tubes with an inner diameter less than 3.0 mm, because short circuits are prone to occur, resulting in the inability of the electrochemical reaction to continue.

Method used

The two-step method of coaxial dynamic electrochemical etching and anodizing of coated cathodes is used to construct micron-scale micron-scale microstructures on the inner surface of stainless steel tubes through cleaning, drying, coating with polymer solution, electrochemical etching and anodizing. Rough structure and further forming nanostructure, solving the short circuit problem.

Benefits of technology

The preparation of a uniform super-wetting coating on the inner surface of the stainless steel pipe is achieved, which is easy to operate, simple in equipment, safe, efficient, and low-cost, and the inner surface of the stainless steel pipe is in a super-hydrophobic state.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112593281B_ABST
    Figure CN112593281B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of super-wetting modification of metal material surfaces, and specifically to a method for preparing a super-wetting coating suitable for the inner surface of a stainless steel tube. The present invention utilizes a dynamic coaxial method of a polymer-coated cathode to construct a coating with a micro / nano secondary structure on the inner surface of a stainless steel tube through electrochemical etching and electrochemical anodization. The inner surface of the obtained stainless steel tube presents a super-hydrophilic state with a contact angle close to 0°. After being modified with a low surface energy material, the inner surface presents a super-hydrophobic state with a contact angle of 155°. This method solves the problem that the positive and negative electrodes are easily short-circuited during the coaxial electrochemical etching and anodization process on the inner surface of a capillary tube, and has the characteristics of simple operation, low cost, and wide applicability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of super-wetting modification of metal material surfaces, in particular to a method for preparing a super-wetting coating (super-hydrophilic and super-hydrophobic) suitable for the inner surface of a stainless steel pipe. Background Art

[0002] As an important metal material, stainless steel pipes are widely used in various fields such as chemical industry, petroleum, electronics, medical treatment, aerospace, pharmaceuticals, water supply equipment, etc. Stainless steel pipes have low production costs and are the most widely used metal and alloy pipes. However, in some special occasions, due to the hydrophilicity of their surface, their application effects and scenarios are limited. By preparing a super-wetting surface on the surface of stainless steel, its application performance can be improved, such as corrosion resistance, fluid resistance reduction, anti-icing, and droplet lossless transfer. At present, domestic and foreign scholars have studied the super-wetting modification treatment of stainless steel surfaces, but due to the shape and size restrictions of stainless steel pipes, for stainless steel pipes, especially stainless steel capillaries with an inner diameter of less than 3.0 mm, there are few reports on super-wetting modification methods of the inner surface. In the electrochemical etching and anodizing processes of stainless steel pipes, the premise for ensuring the uniformity of the super-wetting coating is to ensure the uniformity of the anode electric field strength, which requires that only the coaxial method can be used for electrochemical etching and anodizing. However, the coaxial method requires that the cathode wire must be placed inside the anode stainless steel capillary. When the inner diameter of the stainless steel is small, it is easy to short-circuit, so that the electrochemical reaction cannot continue. Therefore, it is urgent to develop a method for preparing a super-wetting coating on the inner surface of stainless steel that prevents short circuits, is easy to operate, requires simple equipment, is safe and efficient, and has low cost. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing a super-wetting coating suitable for the inner surface of a stainless steel pipe, characterized in that it comprises the following steps:

[0004] 1〕Cleaning stainless steel tube and cathode wire;

[0005] 2) Drying the stainless steel tube, sealed stainless steel tube and cathode wire treated in step 1);

[0006] 3) Coating a polymer solution on the surface of the cathode wire;

[0007] 4) Drying the cathode wire coated with the high molecular polymer solution;

[0008] 5〕 Insert the cathode wire into the stainless steel tube and fix the cathode wire at the axis of the stainless steel tube as the cathode; connect one end of the stainless steel tube to the dynamic solution supply device;

[0009] 6) The stainless steel pipe is connected to the positive electrode of the power supply, and the cathode wire is connected to the negative electrode of the power supply; after power is turned on, the dynamic solution supply device injects etching electrolyte into the stainless steel pipe to perform electrochemical etching;

[0010] 7) After the electrochemical etching is completed, the etching electrolyte is replaced and an anodizing electrolyte is introduced to perform electrochemical anodizing to obtain a stainless steel tube with a super-hydrophobic coating on the inner surface.

[0011] It is worth noting that the two-step method of coaxial dynamic electrochemical etching of the coated cathode and anodic oxidation for preparing a uniform superwetting coating on the inner surface of a stainless steel tube provided by the present invention solves the problem that the prior art cannot uniformly prepare a superwetting coating on the inner surface of a stainless steel tube.

[0012] Furthermore, both ends of the stainless steel tube are sealed by concentric plugs; the two concentric plugs are made of elastic material, and have a central through hole in the center for the cathode wire to pass through; the two concentric plugs also have through holes for the solution to flow into and out of the stainless steel tube.

[0013] Furthermore, in step 1), the stainless steel tube and the cathode wire are cleaned by ultrasonic vibration in a detergent, alcohol, and deionized water respectively, and the cleaning time is 0.5 to 4 hours;

[0014] In step 2], the stainless steel tube and cathode wire in step 1] are blown dry with a nitrogen spray gun; the stainless steel tube, the stainless steel tube and the cathode wire are then dried at a temperature of 50 to 80° C. for a drying time of 0.5 to 8 hours.

[0015] Furthermore, in step 3), the cathode filament dried in step 2 is used as a substrate, and a polymer solution is repeatedly coated on its surface; the solvent of the polymer solution is one of N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF), the solute is one of polymer materials such as polylactic acid (PLA), polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), etc., the concentration of the polymer solution is 10 to 100 g / L, and the number of coatings is 2 to 30 times.

[0016] The polymer solution solvent is one of N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF), the solute is one of the polymer materials such as polylactic acid (PLA), polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), etc., the polymer solution concentration is 10-100g / L, and the number of coatings is 2-30 times

[0017] Further, in step 5), the relative positions of the cathode wire and the stainless steel tube are fixed;

[0018] Further, in step 5), the stainless steel tube is fixed vertically, and its lower end is connected to a dynamic solution supply device;

[0019] Further, in step 6), the etching electrolyte is transported by a peristaltic pump; the solvent of the electrochemical etching solution is one or more of commonly used solvents such as water, ethylene glycol, and glycerol; the solute is one of halogen compounds such as sodium chloride, potassium chloride, calcium chloride, copper chloride, ferric chloride, sodium bromide, calcium bromide, potassium bromide, copper bromide, and ferric bromide, and the solution concentration is 0.05-3 mol / L; the electrochemical etching voltage is 5-40 V, and the electrochemical etching time is 0.5-120 min.

[0020] Further, in step 7), the electrochemical anodizing solution is delivered by a peristaltic pump, the solvent of the electrochemical anodizing solution is one or more of commonly used solvents such as water, ethylene glycol, glycerol, etc.; the solute is one of fluorides such as sodium fluoride, potassium fluoride, calcium fluoride, copper fluoride, iron fluoride, ammonium fluoride, etc.; the solution concentration is 0.05-0.5 mol / L; the voltage of the electrochemical anodizing solution is 10-80 V, and the electrochemical etching time is 5-300 min.

[0021] Further, after the electrochemical anodizing described in step 7 is completed, the stainless steel tube is subjected to the following treatment:

[0022] Further, 8) the stainless steel tube is cleaned and then dried;

[0023] Further, 9) the stainless steel tube is subjected to annealing treatment.

[0024] Further, after the annealing treatment described in step 9) is completed, the stainless steel tube is subjected to the following treatments:

[0025] Further, 10) the stainless steel tube is soaked in a low surface energy modifier and then dried;

[0026] Furthermore, 11) the stainless steel tube is subjected to annealing treatment.

[0027] Further, in step 9), the annealing temperature is 350-550°C, the annealing time is 0.5-3h, and the heating rate is 1-10°C / min;

[0028] Further, in step 10), the low surface energy modifier solute is one of stearic acid, lauric acid, and fluorosilane, the solvent is one of ethanol and n-hexane, the solute volume concentration is 0.5-5%, the immersion time is 0.5-2h, the immersion temperature is 20-70°C, the drying temperature is 50-80°C, and the drying time is 1-3h.

[0029] Furthermore, in the step 11), the annealing temperature is 110-150° C., and the annealing time is 0.5-3 h.

[0030] The present invention uses a stainless steel tube as a substrate and applies a cathode coating method to solve the problem of easy short circuit in the coaxial electrochemical etching and anodic oxidation process. The electrochemical etching method is used to construct a micron-level rough structure on the inner surface of the stainless steel tube, and then the electrochemical anodic oxidation method is used to construct a nanostructure on the micron-level rough structure. A uniform super-wetting coating is prepared on the inner surface of the stainless steel capillary. The method for preparing a super-wetting surface of the present invention has the characteristics of simple operation, simple equipment, safety, high efficiency, low cost, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of an electrochemical etching and anodizing device. In the figure, 1, cathode metal wire; 2, high molecular polymer membrane; 3, concentric plug; 4, stainless steel tube; 5, infusion tube; 6, peristaltic pump; 7, etching electrolyte storage tank; 8, anodizing electrolyte storage tank; 9, DC power supply.

[0032] Figure 2 It is a schematic diagram of the process of preparing the super-wettable inner surface of stainless steel.

[0033] Figure 3 This is a scanning electron micrograph of the inner surface of stainless steel after electrochemical etching.

[0034] Figure 4 This is a scanning electron micrograph of the inner surface of stainless steel after electrochemical anodization.

[0035] Figure 5 This is a static water contact angle test chart of the super-wettable inner surface of stainless steel that has not been modified with low surface energy.

[0036] Figure 6 This is a static water contact angle test diagram of the super-wettable inner surface of stainless steel after low surface energy modification. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the embodiments, but it should not be understood that the above subject matter of the present invention is limited to the following embodiments. Without departing from the above technical ideas of the present invention, various substitutions and changes are made according to the common technical knowledge and customary means in the art, which should all be included in the protection scope of the present invention.

[0038] Embodiment 1:

[0039] The device used in this embodiment is as shown in the attached Figure 1As shown in the figure, one end of the infusion tube 5 is connected to the liquid outlet of the peristaltic pump 6, and the other end is connected to the lower inlet of the stainless steel tube 4. Liquid can be supplied to the inside of the stainless steel tube 4 through the peristaltic pump 6. The inlet of the peristaltic pump 6 is connected to the etching electrolyte storage tank 7 and the anodizing electrolyte storage tank 8 through a branch pipeline. The etching electrolyte or the anodizing electrolyte can enter the peristaltic pump 6 by opening and closing the valve, and then be transported to the stainless steel tube 4 by the peristaltic pump 6. After the etching electrolyte or the anodizing electrolyte is transported to the stainless steel tube 4, it overflows from the upper end of the upper end of the stainless steel tube 4 (or the through hole of the concentric plug 3 at the upper end). A collection tank for collecting overflowed liquid is provided below the infusion tube 5. A DC power supply 9 provides power for the reaction.

[0040] In this embodiment, the following steps are included:

[0041] 1) The stainless steel tube (e.g., an extremely fine sampling needle made of stainless steel used for medical testing) and the cathode wire are cleaned by ultrasonic vibration in a detergent, alcohol, and deionized water respectively;

[0042] 2) Dry the stainless steel tube and cathode wire in step 1) with a nitrogen spray gun; dry the stainless steel tube and cathode wire;

[0043] 3) Using the cathode wire dried in step 2) as a substrate, repeatedly coating the surface of the cathode wire with a polymer solution;

[0044] 4) Drying the cathode wire coated with the high molecular polymer solution in step 3);

[0045] 5〕 Insert the cathode wire into the stainless steel tube and fix the cathode wire at the axis of the stainless steel tube as the cathode, and try to ensure that the stainless steel tube and the cathode wire are coaxial. Fix the relative position of the cathode wire and the stainless steel tube; connect one end of the stainless steel tube to the dynamic solution supply device.

[0046] 6) Connect the outer surface of the stainless steel tube in step 5) to the positive electrode of the power supply, connect the cathode wire to the negative electrode of the power supply, turn on the peristaltic pump switch to pass the etching electrolyte and control the flow rate. When the etching electrolyte flows out from the upper end of the stainless steel tube (or the through hole of the concentric plug), turn on the power supply to perform electrochemical etching under constant voltage conditions;

[0047] 7〕After the electrochemical etching is completed, pour out the etching electrolyte between the cathode and cathode, the stainless steel tube and the infusion tube, reconnect the outer surface of the stainless steel tube to the positive electrode of the power supply, connect the cathode wire and the stainless steel tube to the negative electrode of the power supply, turn on the peristaltic pump switch to pass the anodic oxidation electrolyte and control the flow rate. When the anodic oxidation electrolyte flows out from the upper end of the stainless steel tube, turn on the power supply to perform electrochemical anodic oxidation under constant pressure conditions;

[0048] 8〕Clean and dry the stainless steel tube;

[0049] The stainless steel tube is cleaned with deionized water and then dried;

[0050] 9〕The stainless steel tube is annealed.

[0051] 10〕Soak the stainless steel tube in a low surface energy modifier and then dry it;

[0052] 11〕 Anneal the stainless steel tube.

[0053] Example 2

[0054] The main steps of this embodiment are the same as those of Embodiment 1, and further:

[0055] In step 1), the stainless steel tube is made of 316L austenitic stainless steel. The stainless steel tube with an inner diameter of 8 mm and the stainless steel wire (cathode wire) with a diameter of 1.0 mm are ultrasonically cleaned in a detergent, alcohol, and deionized water, respectively, and the cleaning time is 0.5 h.

[0056] In step 3), the dried cathode wire is used as a substrate, and a polymer solution (solute is polyvinylidene fluoride, solvent is N-methylpyrrolidone) is repeatedly coated on its surface, the solution concentration is 10g / L, and the number of coatings is 10 to 20 times;

[0057] In step 6), the outer surface of the sampling needle is connected to the positive electrode of the power supply, and the cathode wire is connected to the negative electrode of the power supply; the peristaltic pump switch is turned on to pass the etching electrolyte (a sodium chloride aqueous solution with a concentration of 0.25 mol / L) and the flow rate is controlled to be 10 mL / min. When the etching electrolyte flows out from the upper end of the stainless steel tube, the power is turned on to perform electrochemical etching under constant voltage conditions, the voltage is 5 V, and the etching time is 10 min.

[0058] In step 7), the etching electrolyte remaining in the stainless steel tube and the system is poured out, the outer surface of the stainless steel tube is reconnected to the positive electrode of the power supply, the cathode wire is connected to the negative electrode of the power supply, the peristaltic pump switch is turned on to pass the anodizing electrolyte (sodium fluoride ethylene glycol solution with a concentration of 0.05 mol / L) and the flow rate is controlled to be 10 mL / min. When the anodizing electrolyte flows out from the upper end of the stainless steel tube, the power is turned on to perform electrochemical anodizing under constant voltage conditions. The anodizing voltage is 70 V and the anodizing time is 25 min.

[0059] In step 8], the stainless steel tube obtained in step 7] is washed with deionized water and dried at a temperature of 50° C. for 2 h;

[0060] In step 9), the annealing temperature of the annealing treatment is 450°C, the annealing time is 1h, and the heating rate is 2.5°C / min;

[0061] In step 10), the stainless steel tube is immersed in an ethanol solution of 1H,1H,2H,2H-perfluorooctyltrichlorosilane with a volume concentration of 1.5% for 1 hour, and then dried at a temperature of 50° C. for 4 hours;

[0062] In step 11, the annealing temperature of the annealing treatment is 110° C. and the annealing time is 2 h.

[0063] The relevant performance data of this embodiment are as follows:

[0064] Compared with the original stainless steel tube, the inner surface of the stainless steel tube after electrochemical etching has a uniform micron-scale rough structure, see Figure 3 Scanning electron microscope morphology. After anodization, a nanostructure of a certain thickness is prepared on the etched microstructure, see Figure 4 Scanning electron microscope morphology. Before low surface energy treatment, the inner surface of stainless steel is super hydrophilic with a contact angle of about 0°, see Figure 5 Static water contact angle measurement diagram. After low surface energy treatment, the inner surface of stainless steel is super hydrophobic with a contact angle of 155°. Figure 6 Static water contact angle measurement diagram.

[0065] Example 3

[0066] The difference from Example 2 is that:

[0067] In step 1), the inner diameter of the stainless steel tube is 0.4 mm, the material is 316 austenitic stainless steel, and the cathode wire is a titanium wire with a diameter of 0.15 mm.

[0068] In step 3), the polymer solute is polylactic acid (PLA), the solvent is N-methylpyrrolidone (NMP), the solution concentration is 20 g / L, and the number of coatings is 10 to 15 times.

[0069] In step 6), the etching electrolyte is an aqueous solution of potassium chloride with a concentration of 0.5 mol / L, the etching time is 2 min, and the flow rate of the electrolyte solution is 5 mL / min.

[0070] In step 7), the anodizing electrolyte is an ethylene glycol solution of ammonium fluoride with a concentration of 0.1 mol / L, the anodizing voltage is 50 V and the time is 40 min, and the flow rate of the electrolyte solution is 5 mL / min.

[0071] Example 4

[0072] The difference from Example 2 is that:

[0073] In step 1), the inner diameter of the stainless steel tube is 1.0 mm, the material is 304 austenitic stainless steel, and the cathode wire is a copper wire with a diameter of 0.3 mm.

[0074] In step 3), the polymer solute is polyvinyl chloride (PVC), the solvent is N-methylpyrrolidone (NMP), the solution concentration is 30 g / L, and the number of coatings is 15 to 30 times.

[0075] In step 6), the etching electrolyte is a 0.1 mol / L sodium chloride propylene glycol solution, the etching time is 20 min, and the electrolyte solution flow rate is 20 mL / min.

[0076] In step 7), the anodizing electrolyte is a glycerol solution of sodium fluoride with a concentration of 0.06 mol / L, the anodizing voltage is 40 V and the time is 25 min, and the flow rate of the electrolyte solution is 20 mL / min.

[0077] Example 5

[0078] The difference from Example 2 is that:

[0079] In step 1), the inner diameter of the stainless steel tube is 3.0 mm, the material is 304L austenitic stainless steel, and the cathode wire is an iron wire with a diameter of 1.0 mm.

[0080] In step 6), the etching electrolyte is an aqueous solution of sodium chloride with a concentration of 2 mol / L, the etching time is 30 min, and the flow rate of the electrolyte solution is 35 mL / min.

[0081] In step 7), the anodic oxidation voltage is 70 V for 120 min, and the flow rate of the electrolyte solution is 35 mL / min.

[0082] In step 10), the low surface energy material is a n-hexane solution of stearic acid with a volume concentration of 3.5%, and the immersion time is 1.5 hours.

[0083] Example 6

[0084] The difference from Example 2 is that:

[0085] In step 1), the inner diameter of the stainless steel tube is 5.0 mm, the material is 409 ferritic stainless steel, and the cathode wire is a copper wire with a diameter of 2.0 mm.

[0086] In step 6), the etching time is 45 min and the flow rate of the electrolyte solution is 55 mL / min.

[0087] In step (7), the anodic oxidation voltage is 65 V for 50 min, and the flow rate of the electrolyte solution is 55 mL / min.

[0088] Example 7

[0089] The difference from Example 2 is that:

[0090] In step (1), the inner diameter of the stainless steel tube is 15 mm, the material is 420 martensitic stainless steel, and the cathode wire is a stainless steel wire with a diameter of 2.5 mm.

[0091] In step (6), the etching electrolyte is an aqueous solution of sodium chloride with a concentration of 3 mol / L, the etching time is 60 min, and the electrolyte solution flow rate is 80 mL / min.

[0092] In step (7), the anodic oxidation voltage is 50 V for 60 min, and the flow rate of the electrolyte solution is 80 mL / min.

[0093] In step (10), the low surface energy material is an ethanol solution of lauric acid with a volume concentration of 3.5%, and the immersion time is 0.5 h.

[0094] Example 8

[0095] In step (1), the inner diameter of the stainless steel tube is 30 mm, the material is 410 martensitic stainless steel, and the cathode wire is a stainless steel wire with a diameter of 3.0 mm.

[0096] In step (6), the etching electrolyte is an ethylene glycol solution of sodium chloride with a concentration of 1.5 mol / L, the etching time is 30 min, and the electrolyte solution flow rate is 120 mL / min.

[0097] In step (7), the anodic oxidation voltage is 15 V for 80 min, and the flow rate of the electrolyte solution is 120 mL / min.

[0098] The results of the examples show that the present invention utilizes a dynamic coaxial method of coating the cathode with a polymer, and after electrochemical etching and electrochemical anodization, a coating with a micro / nano secondary structure is constructed on the inner surface of a stainless steel tube. The inner surface coating of the stainless steel tube prepared by the present invention presents a superhydrophilic state with a contact angle close to 0°, and after being modified with a low surface energy material, the inner surface presents a superhydrophobic state with a contact angle of 155°. The method for preparing a superwetting coating on the outer surface of a stainless steel tube provided by the present invention has the characteristics of simple operation, low cost, wide applicability, etc., and can be widely used in the field of preparing a superwetting coating on the inner surface of a stainless steel tube.

Claims

1. A method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe, characterized in that: The following steps are involved: 1〕Cleaning stainless steel tubes and cathode wires; the inner diameter of stainless steel tubes is 0.4mm, 1.0mm, 3.0mm, 5.0mm, 8mm, 15mm or 30mm; 2) Drying the stainless steel tube, sealed stainless steel tube and cathode wire treated in step 1); 3) Coating a polymer solution on the surface of the cathode wire; 4) Drying the cathode wire coated with the high molecular polymer solution; 5〕 Insert the cathode wire into the stainless steel tube and fix the cathode wire at the axis of the stainless steel tube as the cathode; connect one end of the stainless steel tube to the dynamic solution supply device; 6) The stainless steel pipe is connected to the positive electrode of the power supply, and the cathode wire is connected to the negative electrode of the power supply; after power is turned on, the dynamic solution supply device injects etching electrolyte into the stainless steel pipe to perform electrochemical etching; 7) After the electrochemical etching is completed, the etching electrolyte is replaced, and an anodizing electrolyte is introduced to perform electrochemical anodizing to obtain a stainless steel tube with a super-hydrophobic coating inner surface; After the electrochemical anodizing described in step 7 is completed, the stainless steel tube is subjected to the following treatment: 8〕Clean and dry the stainless steel tube; 9) Annealing of stainless steel pipe; After the annealing treatment described in step 9 is completed, the stainless steel tube is subjected to the following treatments: 10〕Soak the stainless steel tube in a low surface energy modifier and then dry it; 11〕 Anneal the stainless steel tube.

2. The method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe according to claim 1, characterized in that: The two ends of the stainless steel tube are sealed by concentric plugs; the two concentric plugs are made of elastic material, and have a central through hole in the center for the cathode wire to pass through; the two concentric plugs also have through holes for the solution to flow into and out of the stainless steel tube.

3. The method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe according to claim 1, characterized in that: In step 1), the stainless steel tube and the cathode wire are cleaned by ultrasonic vibration in a detergent, alcohol, and deionized water respectively, and the cleaning time is 0.5 to 4 hours; In step 2], the stainless steel tube and cathode wire in step 1] are blown dry with a nitrogen spray gun; the stainless steel tube, the stainless steel tube and the cathode wire are then dried at a temperature of 50 to 80° C. for a drying time of 0.5 to 8 hours.

4. The method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe according to claim 1, characterized in that: In step 3), the cathode wire dried in step 2 is used as a substrate, and a high molecular polymer solution is repeatedly coated on its surface.

5. The method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe according to claim 1, characterized in that: In step 5), the relative positions of the cathode wire and the stainless steel tube are fixed; In step 6), the stainless steel tube is fixed vertically, and its lower end is connected to a dynamic solution supply device.

6. The method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe according to claim 1, characterized in that: In step 6), the etching electrolyte is transported by a peristaltic pump; the solvent of the electrochemical etching solution is one or more of common solvents such as water, ethylene glycol, propylene glycol, etc.; the solute is one of halogen compounds such as sodium chloride, potassium chloride, calcium chloride, copper chloride, ferric chloride, sodium bromide, calcium bromide, potassium bromide, copper bromide, ferric bromide, etc., and the solution concentration is 0.05-3 mol / L; the electrochemical etching voltage is 5-60V, and the electrochemical etching time is 0.5-60min.

7. The method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe according to claim 1, characterized in that: In step 7), the electrochemical anodizing solution is delivered by a peristaltic pump, the solvent of the electrochemical anodizing solution is one or more of common solvents such as water, ethylene glycol, glycerol, etc.; the solute is one of fluorides such as sodium fluoride, potassium fluoride, calcium fluoride, copper fluoride, iron fluoride, ammonium fluoride, etc.; the solution concentration is 0.05-0.5 mol / L; the voltage of the electrochemical anodizing solution is 10-70 V, and the electrochemical etching time is 5-360 min.

8. The method for preparing a superwetting coating suitable for the inner surface of a stainless steel pipe according to claim 7, characterized in that: In step 9), the annealing temperature is 350-550°C, the annealing time is 0.5-3h, and the heating rate is 1-10°C / min; In step 10), the low surface energy modifier solute is one of stearic acid, lauric acid, and fluorosilane, the solvent is one of ethanol and n-hexane, the solute volume concentration is 0.5-5%, the soaking time is 0.5-2h, the soaking temperature is 20-70°C, the drying temperature is 40-70°C, and the drying time is 1-4h; In the step 11), the annealing temperature is 110-150° C. and the annealing time is 1-3 hours.

Citation Information

Patent Citations

  • Preparation method of super-wetting coating on inner surface of U-shaped titanium tube

    CN110552042A