Method for etching structures for semiconductor applications

Through multi-step etching process and gas mixture control, the problem of insufficient etching selectivity between different materials in semiconductor manufacturing is solved, efficient and precise conductive layer etching is achieved, and the service life of semiconductor devices is extended.

CN112640065BActive Publication Date: 2024-10-01APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980057814.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-30
Filing Date
2019-10-16
Publication Date
2024-10-01
Estimated Expiration
2039-10-16

AI Technical Summary

Technical Problem

In semiconductor manufacturing, it is difficult to achieve high etching selectivity between different materials with the existing technology, leading to problems such as structural profile deformation, dimensional inaccuracies and early performance failure.

Method used

Using a multi-step etching process, including residue removal, main etching and post-annealing processes, an etching gas mixture containing chlorine gas is used to efficiently etch the conductive layer by controlling gas flow and pressure, ensuring selectivity and precision.

Benefits of technology

It achieves efficient etching of conductive layers of different materials in the film stack, avoids structural deformation and dimensional errors, and extends the service life of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112640065B_ABST
    Figure CN112640065B_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure provide methods and apparatus for forming and patterning features in a film stack disposed on a substrate. In one embodiment, a method for patterning a conductive layer on a substrate comprises the following steps: supplying a first gas mixture comprising a chlorine-containing gas at a first flow rate to etch a first conductive layer disposed on the substrate; reducing the chlorine-containing gas in the first gas mixture to a second flow rate lower than the first flow rate to continue etching the first conductive layer; and increasing the chlorine-containing gas in the first gas mixture to a third flow rate greater than the second flow rate to remove the first conductive layer from the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Examples of the present disclosure generally relate to deposition and etching processes for forming structures in film stacks. In particular, embodiments of the present disclosure provide methods for multiple etching processes for forming features in film stacks having different materials in semiconductor applications. Background Art

[0002] When manufacturing integrated circuits (ICs) or chips, chip designers create patterns that represent different chip layers. A series of reusable masks or photomasks are generated from these patterns to transfer the design of each chip layer to a semiconductor substrate during the manufacturing process. The mask pattern generation system uses a precise laser or electron beam to image the design of each chip layer onto a corresponding mask. The mask is then used to transfer the circuit pattern of each layer to a semiconductor substrate, much like a photographic film. These layers are built using a series of processes and are converted into tiny transistors and circuits that make up each complete chip. Therefore, any defects in the mask may be transferred to the chip, which may adversely affect performance. Sufficiently severe defects may render the mask completely useless. Generally speaking, a set of 15 to 100 masks are used to construct chips and can be reused.

[0003] As critical dimensions (CD) shrink, current photolithography approaches the technical limit of the 45 nanometer (nm) technology node. Next-generation lithography (NGL) is expected to replace conventional photolithography, for example, in the 20 nm technology node and beyond. The image of the patterned mask is projected onto the substrate surface, which is coated with a layer of photoresist, by a high-precision optical system. The pattern is then formed on the substrate surface after complex chemical reactions and subsequent manufacturing steps such as development, post-exposure bake, and wet or dry etching.

[0004] A variety of deposition and etching processes have been widely used to form structures with different materials on substrates to enhance feature density and accuracy. However, as electrical performance requirements are constantly pushed to the limit, different materials with different properties are usually used in the structure to meet performance requirements. However, it is usually difficult to achieve high etching selectivity between different materials. Poor etching selectivity usually causes deformed profiles, height loss, or other defects caused by the etching process. Such deformation of the profile has significantly affected the critical dimension (CD) control and the feature transfer of the target material in the device structure. As a result, the undesirable structural profile and inaccurate generated size lead to early failure of device performance.

[0005] Therefore, there is a need for apparatus and methods for performing an etching process with high selectivity between different materials in a film stack to form structures on a substrate. Summary of the invention

[0006] Embodiments of the present disclosure provide methods and apparatus for etching structures having different materials for semiconductor applications. In one embodiment, a method for patterning a conductive layer on a substrate comprises the following steps: supplying a first gas mixture including a chlorine-containing gas at a first flow rate to etch a first conductive layer disposed on the substrate; reducing the chlorine-containing gas in the first gas mixture to a second flow rate lower than the first flow rate to continue etching the first conductive layer; and increasing the chlorine-containing gas in the first gas mixture to a third flow rate greater than the second flow rate to remove the first conductive layer from the substrate.

[0007] In another embodiment, a method for patterning a conductive layer on a substrate comprises the following steps: performing a hydrogen treatment process on the substrate to remove residues on the substrate; performing an etching process by the following steps: supplying an etching gas mixture including a chlorine-containing gas to etch a first conductive layer on the substrate until a second conductive layer is exposed on the substrate; and performing a post-annealing process at a process pressure between approximately 5 bar and 100 bar.

[0008] In yet another embodiment, a method for patterning a conductive layer on a substrate comprises the following steps: removing residues from the substrate by a hydrogen treatment process, wherein the residues include organic materials, wherein the substrate includes a first conductive layer disposed on a second conductive layer; etching the first conductive layer by the following steps: supplying an etching gas mixture including a chlorine-containing gas until the second conductive layer is exposed on the substrate, wherein while etching the first conductive layer, the chlorine-containing gas in the etching gas mixture is maintained from a first flow rate to a second flow rate and further to a third flow rate; and performing a post-annealing process at a process pressure between approximately 5 bar and 100 bar to thermally treat the second conductive layer on the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] A more detailed description of the disclosure briefly summarized above, as well as the above-recited features of the disclosure and the manner in which they can be understood in detail, can be obtained by reference to the embodiments of the disclosure, which are illustrated in the accompanying drawings.

[0010] Figure 1 is a schematic cross-sectional view of a processing chamber configured to perform an etching process according to one or more embodiments of the present disclosure;

[0011] Figure 2 is a simplified front cross-sectional view of a processing chamber according to some embodiments;

[0012] Figure 3 is a flow chart of a method for patterning a material layer on a substrate according to one or more embodiments of the present disclosure; and

[0013] Figures 4A-4B , 5A-5B, 6A-6B, 7A-7B, 8A-8B, 9A-9B, and 10A-10B are shown in Figure 3 Perspective and cross-sectional views of structures formed on a substrate during an etching process.

[0014] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.

[0015] It is to be noted, however, that the appended drawings illustrate only exemplary embodiments of this disclosure and are therefore not to be considered limiting of its scope, for the disclosure may admit to other equally effective embodiments. DETAILED DESCRIPTION

[0016] Methods for patterning features and manufacturing nanostructures with desired small sizes in film stacks are provided. These methods utilize an etching process with high etching selectivity to etch certain materials in the film stack without substantially damaging other materials in the film stack. In one example, the etching process includes several procedures or steps. For example, a three-step process including a residue removal process, a main etching process, and a post-annealing process is performed to etch a conductive layer in the film stack. In addition, the main etching process further includes a breaking-through process, a bulk etching process, and a residue cleaning process. These multiple processes can efficiently etch a target material (such as a conductive layer) in a film stack without substantially corroding other materials in the film stack.

[0017] As used herein, the term "substrate" refers to a material layer that serves as a base for subsequent processing operations, and includes a surface to be cleaned. For example, the substrate may include one or more materials, the one or more materials comprising silicon-containing materials, containing IV or III-V compounds, such as Si, polycrystalline silicon, amorphous silicon, silicon nitride, silicon oxynitride, silicon oxide, Ge, SiGe, GaAs, InP, InAs, GaAs, GaP, InGaAs, InGaAsP, GaSb, InSb and the like, or a combination of the above items. In addition, the substrate may also include dielectric materials, such as silicon dioxide, organic silicates, and carbon-doped silicon oxide. The substrate may also include one or more conductive metals, such as nickel, titanium, platinum, molybdenum, rhenium, osmium, chromium, iron, aluminum, copper, tungsten, or a combination of the above items. Further, depending on the application, the substrate may include any other material, such as metal nitrides, metal oxides, and metal alloys. In one or more embodiments, the substrate may form a contact structure, a metal silicide layer, or a gate structure including a gate dielectric layer and a gate electrode layer to facilitate connection with interconnect features (such as plugs, vias, contacts, wires, and conductors) subsequently formed on the substrate, or suitable structures utilized in a semiconductor device.

[0018] In addition, the substrate is not limited to any particular size or shape. The substrate can be a circular wafer with a diameter of 200 mm, a diameter of 300 mm, a diameter of 450 mm, or other diameters. The substrate can also be any polygonal, square, rectangular, curved or other non-circular workpiece, such as a polygonal glass or plastic substrate used to manufacture a flat panel display.

[0019] Figure 1 is a simplified cross-sectional view of an exemplary processing chamber 100 suitable for etching a material layer disposed on a substrate 400 in the processing chamber 100. The exemplary processing chamber 100 is suitable for performing a patterning process. One example of a processing chamber 100 that may be adapted to benefit from the present disclosure is available from Applied Materials, Inc. located in Santa Clara, California. Etch Process Chamber. It is contemplated that other process chambers, including those from other manufacturers, may be adapted to practice embodiments of the present disclosure.

[0020] The plasma processing chamber 100 includes a chamber body 105 having a chamber volume 101 defined therein. The chamber body 105 has sidewalls 112 and a bottom 118 coupled to a ground 126. The sidewalls 112 have liners 115 to protect the sidewalls 112 and extend the time between maintenance cycles of the plasma processing chamber 100. The size of the chamber body 105 and related components of the plasma processing chamber 100 is not limited and is generally proportionally larger than the size of the substrate 400 to be processed therein. Examples of substrate sizes include 200 mm diameter, 250 mm diameter, 300 mm diameter, and 450 mm diameter, among others.

[0021] The chamber body 105 supports a chamber lid assembly 110 to enclose the chamber volume 101. The chamber body 105 may be fabricated from aluminum or other suitable materials. A substrate access port 113 is formed through a sidewall 112 of the chamber body 105 to facilitate transferring a substrate 400 into and out of the plasma processing chamber 100. The access port 113 may be coupled to a transfer chamber and / or other chambers of a substrate processing system (not shown).

[0022] A pumping port 145 is formed through the sidewall 112 of the chamber body 105 and is connected to the chamber volume 101. A pumping device (not shown) is coupled to the chamber volume 101 through the pumping port 145 to vent and control the pressure therein. The pumping device may include one or more pumps and throttle valves.

[0023] The gas panel 160 is coupled to the chamber body 105 via a gas line 167 to supply process gases into the chamber volume 101. The gas panel 160 may include one or more process gas sources 161, 162, 163, 164, and may additionally include inert gases, non-reactive gases, and reactive gases as desired. Examples of process gases that may be provided by the gas panel 160 include, but are not limited to, hydrocarbon-containing gases (including methane (CH4)), sulfur hexafluoride (SF6), silicon chloride (SiCl4), carbon tetrafluoride (CF4), hydrogen bromide (HBr), hydrocarbon-containing gases, argon (Ar), chlorine (Cl2), nitrogen (N2), helium (He), and oxygen (O2). In addition, the process gas may also include nitrogen-containing, chlorine-containing, fluorine-containing, oxygen-containing and hydrogen-containing gases, such as BCl3, C2F4, C4F8, C4F6, CHF3, CH2F2, CH3F, NF3, NH3, CO2, SO2, CO, N2, NO2, N2O, and H2, etc.

[0024] Valve 166 controls the flow of process gases from gas panel 160 and from sources 161, 162, 163, 164 and is managed by controller 165. The flow of gases supplied from gas panel 160 to chamber body 105 may include a combination of gases.

[0025] The lid assembly 110 may include a nozzle 114. The nozzle 114 has one or more ports for introducing process gases from sources 161, 162, 164, 163 of a gas panel 160 into the chamber volume 101. After the process gases are introduced into the plasma processing chamber 100, the gases are energized to form a plasma. An antenna 148, such as one or more inductive coils, may be provided proximate the plasma processing chamber 100. An antenna power supply 142 may power the antenna 148 through a matching circuit 141 to inductively couple energy, such as RF energy, to the process gases to sustain a plasma formed by the process gases in the chamber volume 101 of the plasma processing chamber 100. Alternatively or in addition to the antenna power supply 142, a process electrode below the substrate 400 and / or above the substrate 400 may be used to capacitively couple RF power to the process gases to sustain a plasma within the chamber volume 101. The operation of the power supply 142 may be controlled by a controller, such as the controller 165 , which also controls the operation of other components in the plasma processing chamber 100 .

[0026] A substrate support pedestal 135 is disposed in the chamber volume 101 to support a substrate 400 during processing. The substrate support pedestal 135 may include an electrostatic chuck 122 for holding the substrate 400 during processing. The electrostatic chuck (ESC) 122 uses electrostatic attraction to hold the substrate 400 to the substrate support pedestal 135. The ESC 122 is powered by an RF power supply 125 integrated with a matching circuit 124. The ESC 122 includes an electrode 121 embedded in a dielectric body. The electrode 121 is coupled to the RF power supply 125 and provides a bias that attracts plasma ions formed by the process gas in the chamber volume 101 to the ESC 122 and the substrate 400 positioned thereon. The RF power supply 125 may be cycled on and off, or pulsed, during processing of the substrate 400. The ESC 122 has an insulator 128 for the purpose of making the sidewalls of the ESC 122 less attractive to plasma to extend the maintenance life cycle of the ESC 122. In addition, the substrate support pedestal 135 may have a cathode liner 136 to protect the sidewalls of the substrate support pedestal 135 from the plasma gases and extend the time between maintenance of the plasma processing chamber 100.

[0027] In addition, the electrode 121 is coupled to a power supply 150. The power supply 150 provides a chucking voltage of about 200 volts to about 2000 volts to the electrode 121. The power supply 150 may also include a system controller for controlling the operation of the electrode 121 for chucking and unclamping the substrate 400 by directing a DC current to the electrode 121.

[0028] The ESC 122 may include a heater disposed in the ESC and connected to a power source (not shown) for heating the substrate, and a cooling base 129 supporting the ESC 122 may include conduits for circulating a heat transfer fluid to maintain the temperature of the ESC 122 and the substrate 400 disposed on the ESC. The ESC 122 is configured to perform within a temperature range required by the thermal budget of the device being fabricated on the substrate 400. For example, the ESC 122 may be configured to maintain the substrate 400 at a temperature of about -25 degrees Celsius to about 500 degrees Celsius for certain embodiments.

[0029] A cooling base 129 is provided to help control the temperature of the substrate 400. To mitigate process drift and time, the temperature of the substrate 400 may be maintained substantially constant throughout the time the substrate 400 is in the cleaning chamber by the cooling base 129. In one embodiment, the temperature of the substrate 400 is maintained at about 30 degrees Celsius to 120 degrees Celsius throughout the subsequent cleaning process.

[0030] The cover ring 130 is disposed on the ESC 122 and along the perimeter of the substrate support pedestal 135. The cover ring 130 is configured to confine the etching gas to a desired portion of the exposed top surface of the substrate 400 while shielding the top surface of the substrate support pedestal 135 from the plasma environment inside the plasma processing chamber 100. Lift pins (not shown) selectively move through the substrate support pedestal 135 to lift the substrate 400 above the substrate support pedestal 135 to facilitate access to the substrate 400 by a transfer robot (not shown) or other suitable transport mechanism.

[0031] The process sequence may be controlled using controller 165 to adjust the gas flow and other process parameters from gas panel 160 into plasma processing chamber 100. The software program, when executed by the CPU, converts the CPU into a dedicated computer (controller) that controls plasma processing chamber 100 so that processes are performed according to the present disclosure. The software program may also be stored and / or executed by a second controller (not shown) juxtaposed with plasma processing chamber 100.

[0032] Figure 2 2 is a simplified front cross-sectional view of a single substrate processing chamber 200 for a high pressure annealing process of a single substrate 400. The single substrate processing chamber 200 has a body 210 having an outer surface 212 and an inner surface 213 enclosing an inner volume 215. Figure 2In some embodiments, the body 210 has a circular cross-section, while in other embodiments, the cross-section of the body 210 can be rectangular or any closed shape. The outer surface 212 of the body 210 can be made of corrosion resistant steel (CRS) (such as but not limited to stainless steel). One or more heat shields 225 are provided on the inner surface 213 of the body 210, and the heat shields 225 prevent heat loss from the single substrate processing chamber 200 to the external environment. The inner surface 213 of the body 210 and the heat shield 225 can be made of a nickel-based steel alloy that exhibits high corrosion resistance, such as but not limited to and

[0033] The substrate support 230 is disposed within the interior volume 215. The substrate support 230 has a stem 234 and a substrate support member 232 held by the stem 234. The stem 234 passes through a passage 222 formed through the chamber body 210. A rod 239 connected to an actuator 238 passes through a second passage 223 formed through the chamber body 210. The rod 239 is coupled to a plate 235 having a hole 236 that receives the stem 234 of the substrate support 230. A lift pin 237 is connected to the substrate support member 232. The actuator 238 actuates the rod 239 so that the plate 235 moves up and down to connect and disconnect with the lift pin 237. As the lift pin 237 is raised or lowered, the substrate support member 232 is raised or lowered within the interior volume 215 of the chamber 200. The substrate support member 232 has a resistive heating element 231 embedded in the center. The power source 233 is configured to supply power to the resistive heating element 231. The operation of the power source 233 and the actuator 238 is controlled by the controller 280.

[0034] The single substrate processing chamber 200 has an opening 211 on the body 210 through which one or more substrates 400 can be loaded and unloaded to and from a substrate support 230 disposed in the interior volume 215. The opening 211 forms a tunnel 221 on the body 210. The slit valve 228 is configured to sealably close the tunnel 221 so that access to the opening 211 and the interior volume 215 is possible only when the slit valve 228 is open. A high pressure seal 227 is used to seal the slit valve 228 to the body 210 to seal the interior volume 215 for processing. The high pressure seal 227 can be made of a polymer, such as a fluoropolymer, such as, but not limited to, perfluoroelastomer and polytetrafluoroethylene (PTFE). The high pressure seal 227 can further include a spring member for biasing the seal to improve sealing performance. A cooling channel 224 is provided on the tunnel 221 and adjacent the high pressure seal 227 to maintain the high pressure seal 227 below the maximum safe operating temperature of the high pressure seal 227 during processing. A coolant from a cooling fluid source 226, such as but not limited to inert, dielectric, and high performance heat transfer fluids, may be circulated within the cooling channel 224. The flow of the coolant from the cooling fluid source 226 is controlled by a controller 280 via feedback received from a temperature sensor 216 or a flow sensor (not shown). An annular thermal choke 229 is formed around the tunnel 221 to prevent heat from the interior volume 215 from flowing through the opening 211 when the slit valve 228 is open.

[0035] The single substrate processing chamber 200 has a port 217 through the body 210, which is fluidly connected to a fluid circuit 290, which connects the gas panel 250, the condenser 260, and the port 217. The fluid circuit 290 has a gas conduit 292, a source conduit 257, an inlet isolation valve 255, an exhaust conduit 263, and an outlet isolation valve 265. A number of heaters 296, 258, 252, 254, 264, 266 interface with different parts of the fluid circuit 290. A number of temperature sensors 251, 253, 219, 267, and 269 are also placed at different parts of the fluid circuit 290 to intercept temperature measurements and send information to the controller 280. The controller 280 uses the temperature measurement information to control the operation of the heaters 252 , 254 , 258 , 296 , 264 , and 266 so that the temperature of the fluid circuit 290 is maintained above the condensation point of the process fluid disposed in the fluid circuit 290 and the interior volume 215 .

[0036] The gas panel 250 is configured to provide a process fluid at a pressure within the interior volume 215. The pressure of the process fluid introduced into the interior volume 215 is monitored by a pressure sensor 214 coupled to the body 210. The condenser 260 is fluidly coupled to a cooling fluid source (not shown) and is configured to condense the gas phase process fluid exiting the interior volume 215 through the gas conduit 292. The condensed process fluid is then removed by a pump 276. One or more heaters 240 are disposed on the body 210 and are configured to heat the interior volume 215 within the single substrate processing chamber 200. The heaters 240, 252, 254, 258, 296, 264, and 266 maintain the process fluid within the fluid circuit 290 in a gas phase while the outlet isolation valve 265 to the condenser 260 is open to prevent condensation within the fluid circuit.

[0037] The controller 280 controls the operation of the single substrate processing chamber 200. The controller 280 controls the operation of the gas panel 250, the condenser 260, the pump 270, the inlet isolation valve 255, the outlet isolation valve 265, and the power supplies 233 and 245. The controller 280 is also communicatively connected to the temperature sensor 216, the pressure sensor 214, the actuator 238, the cooling fluid source 226, and the temperature reading devices 256 and 262.

[0038] The processing fluid may include an oxygen-containing and / or nitrogen-containing gas, and / or a chalcogenide or telluride (such as S, Se, Te) gas or vapor, such as oxygen, dry steam, water, hydrogen peroxide, ammonia, S vapor, Se vapor, H2S, H2, Se, etc. The processing fluid may react with the metal material on the substrate to form a metal nitride oxide, a metal oxide, a metal oxychalcogenide, or a metal chalcogenide. Instead of or in addition to the oxygen-containing and / or nitrogen-containing gas, the processing fluid may include a silicon-containing gas. Examples of silicon-containing gases include organosilicon, tetraalkyl orthosilicate gas, and disiloxane. Organosilicon gas includes a gas having at least one carbon-silicon bonded organic compound. Tetraalkyl orthosilicate gas includes a gas composed of a silicon-containing compound attached to SiO4. 4-ions. In more detail, the one or more gases may be (dimethylsilyl)(trimethylsilyl)methane ((Me)3SiCH2SiH(Me)2), hexamethyldisilane ((Me)3SiSi(Me)3), trimethylsilane ((Me)3SiH), trimethylsilyl chloride ((Me)3SiCl), tetramethylsilane ((Me)4Si), tetraethoxysilane ((EtO)4Si), tetramethylsilane ((MeO)4Si), tetrakis(trimethylsilyl)silane ((Me3Si)4Si), (dimethylamino) )dimethylsilane ((Me2N)SiHMe2), dimethyldiethoxysilane ((EtO)2Si(Me)2), dimethyldimethoxysilane ((MeO)2Si(Me)2), methyltrimethoxysilane ((MeO)3Si(Me)), dimethoxytetramethyldisiloxane (((Me)2Si(OMe))2O), tris(dimethylamino)silane ((Me2N)3SiH), bis(dimethylamino)methylsilane ((Me2N)2CH3SiH), disiloxane ((SiH3)2O), and combinations of the foregoing.

[0039] During the processing of substrate 400, the environment of internal volume 215 is maintained at a temperature and pressure that maintains the processing fluid in the high pressure region in the gas phase. Such pressure and temperature are selected based on the composition of the processing fluid. In the case of steam, temperature and pressure are maintained under the condition that the steam is maintained in a dry steam state. In one example, the internal volume 215 is pressurized to a pressure greater than atmospheric pressure, for example, greater than about 2 bar. In another example, the internal volume 215 is pressurized to a pressure between about 10 and about 50 bar (such as between about 20 and about 50 bar). In another example, the internal volume 215 is pressurized to a pressure of up to about 100 bar. During the processing, the internal volume 215 is also maintained at a high temperature, for example, a temperature exceeding 225 degrees Celsius (limited by the thermal budget of the substrate 400 disposed on the substrate support member 132), such as between about 300 degrees Celsius and about 500 degrees Celsius.

[0040] Figure 3 3 is a flow chart of an example of a method 300 for an etching process for etching a material layer (or conductive layer) in a film stack used to form a structure on a substrate. The material layer may have different film properties than adjacent materials disposed in the film stack. Figures 4A-4B, 5A-5B, 6A-6B, 7A-7B, 8A-8B, 9A-9B, and 10A-10B are perspective and cross-sectional views of a portion of a substrate 400 having a film stack 450 formed thereon corresponding to various stages of the method 300. The figures ending with an "A" designation depict perspective views of various processing scenarios. The figures ending with a "B" designation depict cross-sectional views corresponding to section AA' of various processing scenarios. In some of the figures, some reference numerals for components or features depicted therein may be omitted to avoid obscuring other components or features; this is for ease of depiction of the drawings. The method 300 may be used to form back-end structures for advanced semiconductor applications, such as dual damascene structures.

[0041] The method 300 begins at operation 302 by providing a substrate 400 having a film stack 450 formed thereon. The film stack 450 includes an interface layer 402 disposed between the substrate 400 and the film stack 450. In one embodiment, the interface layer 402 can be any suitable material that can bridge the film stack 450 and the substrate 400. In some examples, the interface layer 402 can include different structures formed thereon, such as front-end structures, back-end structures, contact structures, metal conductive structures, insulating structures, or the like formed therein as desired. The interface layer 402 can be a conductive layer or a dielectric layer as desired. In some embodiments where the film stack 450 has good interfacial adhesion to the substrate 400, the interface layer 402 can be eliminated.

[0042] Film stack 450 includes a first conductive layer 404, a second conductive layer 406, a third conductive layer 408, and a fourth conductive layer 410. First conductive layer 404 and third conductive layer 408 may be made of similar or identical materials, and second conductive layer 406 and fourth conductive layer 410 may be made of similar or identical materials. In other words, third conductive layer 408 and fourth conductive layer 410 are a repeating pair of first conductive layer 404 and second conductive layer 406. Although Figures 4A-4B Only two pairs of conductive layers are shown in FIG. 4 , but it is noted that pairs of conductive layers 404, 406 or 408, 410 may also be formed in any number as desired. In one example, the first conductive layer 404 and the third conductive layer 408 are Ru-containing layers, Mo-containing layers, NiSi-containing layers, and the like, and the second conductive layer 406 and the fourth conductive layer 410 are Ti-containing layers, Ta-containing layers, TiN-containing layers, TaN-containing layers, TiON-containing layers, TaON-containing layers, TiO-containing layers, and the like. The conductive layers 404, 406, 408, 410 may be formed by MOCVD processes, PECVD, flowable CVD, PVD, ALD, or any suitable deposition technique.

[0043] Then, a dielectric layer 412 is formed on the fourth conductive layer 410. The dielectric layer 412 may be silicon oxide, silicon nitride, silicon oxynitride (SiON), silicon oxycarbide (SiOC), or an amorphous carbon material as required. Then, a first sacrificial layer 414 and a patterned photoresist layer 416 are formed on the dielectric layer 412. The first sacrificial layer 414 may be an organic polymer material that is spin-coated onto the dielectric layer 412. The first sacrificial layer 414 may be an organic polymer material composed of hydrocarbons. The monomer or polymer material may have a formula C x H y O z , where x, y, and z are integers.

[0044] The first sacrificial layer 414 may be spin-coated onto the uneven substrate surface with sufficient thickness to produce a substantially flat top surface for the first sacrificial layer 414. Figures 4A-4B In the embodiment depicted in , the first sacrificial layer 414 is spin-coated onto the substantially flat surface of the dielectric layer 412 in preparation for patterning. Suitable examples of the first sacrificial layer 414 include photoresist materials, spin-coated glass (SOG) materials, and the like. In one example, the photoresist material can be a positive photoresist, a negative photoresist, a UV photoresist, an I-line photoresist, a G-line photoresist, an electron beam resist (e.g., a chemically amplified resist (CAR)), or other suitable photoresists. It is believed that the organic polymeric material provided for the first sacrificial layer 414 can have a self-leveling planarization property so as to be coated onto the dielectric layer 412 to evenly cover the uneven topography (topography) (if any) of the structure formed on the substrate. Thereby, the uneven topographic surface from the substrate 400 can be covered with a flattened or flattened top surface to facilitate subsequent photolithography processes so as to transfer features to the film stack 450 on the substrate 400 with accurate and precise dimensional control.

[0045] In one embodiment, the first sacrificial layer 414 can be spin-coated onto the substrate surface. In another embodiment, the first sacrificial layer 414 can also be applied to the substrate using injection, spray deposition system, aerosol deposition (AD) process, air jet (aerojet), nanoparticle spraying from solution, spray CVD, inkjet, meniscus coating, dip coating, electroplating, spraying, electrospraying, screen printing, or other suitable techniques as needed.

[0046] The patterned photoresist layer 416 includes an organic resist layer. The patterned photoresist layer 416 may be used for extreme ultraviolet (EUV) applications as desired.

[0047] At operation 304, a first etching process is performed to pattern the film stack 450 using the patterned photoresist layer 416 as an etching mask. The first etching process is performed to etch the film stack 450 until the second conductive layer 406 is exposed (eg, Figure 5A and 5B ), thereby forming an open region 430 in the film stack 450 between the patterned structures 432 (further shown as 432a, 432b). The substrate 400 may be transported to an etching process chamber (such as Figure 1 4. The etching process is performed in a processing chamber 100 as depicted in FIG. 4. The first etching process can have a variety of different etching precursors during different stages of the etching process so as to etch the first sacrificial layer 414, the dielectric layer 412, the fourth conductive layer 410, and the third conductive layer 408 in an efficient manner. In one example, the etching precursor used to etch the film stack 450 includes a halogen-containing gas and the like. Suitable examples of etching precursors include CH4, C2H6, C4H8, C4F6, C4F8, C2F2, CF4, CHF3, C2F6, C4F6, C5F8, CH2F2, SF6, NF3, C12, HBr, HCl, HF, and the like. Other reactive gases (such as O2, H2, N2, H2O, O3, CO2, and the like) may also be supplied during the etching process as needed.

[0048] After etching the predetermined portion of the film stack 450 (eg, the open area 430), a second sacrificial layer 422 and a second patterned photoresist layer 438 are then formed on the film stack 450, as shown in FIG. Figure 6A-6B The second patterned photoresist layer 438 is formed on the patterned structure 432 and is vertically aligned with both ends of the patterned structure 432. The second patterned photoresist layer 438 exposes a central portion 440 of the patterned structure 432 (the central portion will be further illustrated in FIG. Figure 7A-7B and 8A-8B), the central portion is to be patterned for a subsequent etching process.

[0049] The second sacrificial layer 422 is similar or identical to the first sacrificial layer 414. The second sacrificial layer 422 is formed on the uneven substrate surface with sufficient thickness to produce a substantially flat top surface for the second sacrificial layer 422. Figure 5A-5BAs shown in , after the etching process, the open area 430 is formed between the patterned structures 432 (further shown as 432a, 432b), thereby generating an uneven surface. Therefore, the second sacrificial layer 422 has a self-leveling capability so as to be coated onto the uneven surface of the etched film stack 450 to evenly cover the uneven topography. Thereby, the uneven topographic surface from the open area 430 between the patterned structures 432 can be covered with a flattened or flattened top surface to facilitate the subsequent photolithography process.

[0050] After forming the second sacrificial layer 422, a second etching process is performed to etch the film stack 450 through the open area 430 and the center portion 440 defined between the second patterned photoresist layer 438 formed on the substrate 400. The second etching process is continuously performed until the surfaces 441a, 441b of the fourth conductive layer 410 are exposed. Figure 7A-7B As shown in . Note that the surfaces 441a, 441b of the fourth conductive layer 410 are aligned with the central portion 440 defined by the second patterned photoresist layer 438, so that after the second etching process, the surfaces 441a, 441b of the fourth conductive layer 410 exposed by the central portion 440 are then exposed. The patterned structures 432a, 432b are then further etched from the central portion 440 to include the surfaces 441a, 441b, respectively, thereby forming corner structures 432c, 432d, 432e, 432f connected by the surfaces 441a, 441b. In Figure 7A-7B In the structure depicted in , the sidewall 445 of the dielectric layer 412 is exposed, and the sidewalls 442a, 442b of the third conductive layer 408 and the fourth conductive layer 410 at the center portion 440 are exposed.

[0051] At operation 306, a residue removal process is performed to remove the remaining second sacrificial layer 422 from the substrate 400, thereby exposing the second conductive layer 406 in the open area 430, as shown in FIG. Figures 8A-8B . A residue removal process is performed to remove the residual second sacrificial layer 422 from the substrate 400. The residual second sacrificial layer 422 on the fourth conductive layer 410 and the second conductive layer 406 in the central portion 440 and in the open area 430 may adversely affect the etching performance subsequently performed to remove the fourth conductive layer 410 and the second conductive layer 406. Therefore, the residue removal process is performed before removing the second conductive layer 406 and the fourth conductive layer 410.

[0052] In one example, the residue removal process is a hydrogen treatment process. The residue removal process is performed by supplying a residue removal gas mixture including a hydrogen-containing gas to the substrate 400 to remove the residual second sacrificial layer 422 (eg, Figure 7A-7B), until the central portion 440 and the open area 430 of the second conductive layer 406 and the fourth conductive layer 410 are exposed, as shown in Figures 8A-8B As shown in . The residue removal gas mixture includes a hydrogen-containing gas and optionally an inert gas. Suitable examples of hydrogen-containing gases include H2, H2O, H2O2, NH3 and the like.

[0053] While performing the residue removal process, some of the exposed surfaces having different materials (such as Figure 7A-7B The surfaces 441a, 441b of the center portion 440 of the fourth conductive layer 410 shown in the figure, the sidewalls 442a, 442b of the third conductive layer 408, and the sidewalls 445 of the dielectric layer 412 are also exposed to the reactive species from the residue removal gas mixture. Therefore, the reactive species used to perform the residue removal process is selected to have high selectivity among these materials, so that the reactive species can selectively remove the residual second sacrificial layer 422 without substantially corroding the exposed fourth conductive layer 410, the third conductive layer 408, and the dielectric layer 412. In one embodiment, a hydrogen-containing gas supplied from a remote plasma source is provided to selectively remove the residual second sacrificial layer 422. A nitrogen-containing gas (such as N2, N2O, NO2, NH3) may also be optionally supplied in the residue removal gas mixture. In a specific example, the residue removal gas mixture includes H2 and N2.

[0054] During the residue removal process, several process parameters can also be adjusted. In an exemplary embodiment, the process pressure in the processing chamber 100 is adjusted between about 10 mTorr and about 5000 mTorr, such as between about 10 mTorr and about 200 mTorr. Remote plasma sources and / or optional RF bias power can be utilized in the residue removal process. The power supplied to the remote plasma source can be between 1000 watts and about 20,000 watts, such as about 5000 watts. In an example, RF bias power is not applied while supplying the residue removal gas mixture. Eliminating RF bias power while performing the residue removal process can assist in distributing the reactive species in the plasma generated by the residue removal gas mixture more evenly across the substrate surface with relatively soft and non-specific directional power.

[0055] The hydrogen-containing gas from the residue removal gas mixture may be flowed into the chamber at a volume flow rate between about 500 sccm and about 2000 sccm, and the nitrogen-containing gas may be supplied at a volume flow rate between about 500 sccm and about 2000 sccm. The hydroxyl-containing gas and the nitrogen-containing gas from the residue removal gas mixture may be supplied to the processing chamber simultaneously, or alternately or sequentially as desired.

[0056] The substrate temperature is maintained at greater than 100 degrees Celsius, such as between about 120 degrees Celsius and about 400 degrees Celsius, such as between about 150 degrees Celsius and about 350 degrees Celsius, for example, between about 200 degrees Celsius and about 300 degrees Celsius. It is believed that high temperature control of the substrate 400 during the residue removal process can assist and evaporate the polymeric material from the residual second sacrificial layer 422 to enhance the removal efficiency without damaging other materials on the substrate 400.

[0057] At operation 308, a main etching process is performed to simultaneously etch the exposed fourth conductive layer 410 and the second conductive layer 406 until the underlying third conductive layer 408 and the first conductive layer 404 are exposed. Figures 9A-9B The main etching process is performed by the following steps: Figure 1 ) supplies a main etching gas mixture to etch the exposed fourth conductive layer 410 and the second conductive layer 406.

[0058] The main etching process further includes three steps, which include a punch-through process, a bulk etching process, and a residue cleaning process. The main etching process as performed is highly selective, so that the reactive species from the main etching process can mainly etch the fourth conductive layer 410 and the second conductive layer 406 without substantially corroding the dielectric layer 412 and the underlying third conductive layer 408 and the first conductive layer 404 when exposed. In the example where the fourth conductive layer 410 and the second conductive layer 406 are titanium (Ti) containing materials, the reactive species from the main etching gas mixture can mainly react with the titanium (Ti) containing material without substantially reacting with the oxide material from the dielectric layer 412, thereby providing a selective etching process. The selective etching process can preferentially etch the target material (such as the titanium (Ti) containing material in this example) without corroding or damaging the adjacent material (such as the oxide containing material from the dielectric layer 412 in this example).

[0059] In one example, the main etching gas mixture includes a halogen-containing gas, such as a chlorine-containing gas. Inert gas can also be supplied in the main etching gas mixture. Suitable examples of chlorine-containing gases include Cl2, HCl and the like. It is believed that the chlorine-containing gas can react mainly with Ti or Ta elements from the fourth conductive layer 410 and the second conductive layer 406 to keep oxide damage or oxide loss from the dielectric layer 412 to be minimal. In one example, the main etching gas mixture includes a chlorine-containing gas (such as Cl2 gas) and Ar gas.

[0060] In one example, the ratio of Cl2 gas to Ar gas supplied in the main etching gas mixture may be varied, adjusted, altered, or changed while etching the titanium (Ti)-containing material. Because the upper surface of the titanium (Ti)-containing material generally includes TiOx , so a relatively high ratio of Cl2 gas (e.g., a higher chlorine gas flow rate) is used in the main etching gas mixture to penetrate the surface oxide (if any) from the surface of the titanium (Ti)-containing material from the fourth conductive layer 410 and the second conductive layer 406. In one example, the thickness of the upper TiOx can be about 3% to about 20% of the total thickness of the fourth conductive layer 410 and the second conductive layer 406. In one example, the Cl2 gas supplied in the main etching gas mixture has a high ratio relative to the Ar gas supplied in the main etching gas mixture during the punch-through process. In one example, the Cl2 gas and the Ar gas supplied in the main etching gas mixture are controlled at a ratio greater than 10:1 (Cl2 gas:Ar gas), such as between about 10:1 and about 50:1. The Cl2 gas in the main gas mixture is supplied at a first flow rate.

[0061] After the titanium (Ti)-containing material is punched through, relatively similar amounts of Cl2 gas and Ar gas (e.g., a lower chlorine gas flow rate or flow ratio) are then used in the main etching gas mixture to etch the bulk of the titanium (Ti)-containing material from the fourth conductive layer 410 and the second conductive layer 406 (e.g., or referred to as a bulk etching process). In the bulk titanium (Ti)-containing material etching process, the Cl2 gas and Ar gas supplied in the main etching gas mixture are controlled at a ratio between about 1:4 and about 2:1 (Cl2 gas:Ar gas). In this example, the thickness of the fourth conductive layer 410 and the second conductive layer 406 can be etched to about 5% to about 98% of the total thickness of the fourth conductive layer 410 and the second conductive layer 406, such as between about 50% and about 98%. The Cl2 gas in the main gas mixture is supplied at a second flow rate lower than the first flow rate in the bulk etching process.

[0062] Finally, a relatively high ratio of Cl2 gas relative to Ar gas (similar to the punch-through process) is used to remove residual titanium (Ti)-containing material from the fourth conductive layer 410 and the second conductive layer 406 (e.g., or referred to as a residue cleaning process) and to remove oxide residues (if any) from the dielectric layer 412. The Cl2 gas in the main gas mixture in the residue cleaning process is at a third flow rate, which is less than the second flow rate but similar to or the same as the first flow rate. In one example, the Cl2 gas and the Ar gas supplied in the main etching gas mixture in the residue cleaning process are controlled at a ratio of approximately greater than 10:1 (Cl2 gas:Ar gas), such as between approximately 10:1 and approximately 20:1. Note that the ratio of Cl2 gas to Ar gas in the main etching gas mixture for the residue cleaning process and the punch-through process can be similar or the same.

[0063] Note that the main etching gas mixture supplied for etching the fourth conductive layer 410 and the second conductive layer 406 may be gradually adjusted, changed, or varied to meet different process requirements during the punch-through process, the bulk etching process, and the residue cleaning process.

[0064] During the main etching process (including punch-through process, main etching process and residue cleaning process), several process parameters can also be adjusted. In an exemplary embodiment, the process pressure in the processing chamber 100 is adjusted between about 10 millitorr and about 5000 millitorr, such as between about 10 millitorr and about 200 millitorr. RF source and / or bias power can be utilized while performing a flash etching process (flashetching process). RF source and RF bias power can be applied to the processing chamber in a continuous mode or in a pulsed mode. In an example, RF bias power is applied while supplying the main etching gas mixture.

[0065] The RF bias power applied while supplying the main etching gas mixture assists in forming the reaction exposed surfaces 440a, 440b, 430 of the fourth conductive layer 410 and the second conductive layer 406 for etching. In one example, an RF source power at a frequency of about 13 MHz may be applied to maintain a plasma in the deposition gas mixture. For example, an RF source power of about 100 watts to about 1000 watts may be applied to maintain a plasma inside the processing chamber 100. An RF bias power of about 300 watts to about 700 watts may be applied while supplying the main etching gas mixture.

[0066] The substrate temperature is maintained between about 10 degrees Celsius and about 300 degrees Celsius, such as between about 20 degrees Celsius and about 80 degrees Celsius, for example between about 30 degrees Celsius and about 50 degrees Celsius.

[0067] At operation 310, a post annealing process is performed. The post annealing process is a high pressure annealing process performed at a high process pressure (such as greater than 2 bar but less than 70 bar). The high pressure annealing process can assist in repairing vacancies and etching byproducts and / or residues after the main etching process, and smoothing surface roughness that may be caused by the main etching process in the exposed third conductive layer 408 and the first conductive layer 404 and the dielectric layer 412. In some examples, the high process pressure can be as high as 70 bar. The post annealing process can be performed in a processing chamber (such as Figure 2 The high pressure annealing process is performed in a processing chamber 200 (depicted in FIG. 2 ) or other suitable processing chambers, including those that process one substrate at a time.

[0068] The high pressure annealing process performed at operation 310 maintains the process pressure at the high pressure region in a gas phase (e.g., a dry vapor phase substantially free of droplets). The process pressure and temperature are controlled to densify the film structure so as to repair film defects, thereby driving off impurities and smoothing surface roughness. In one example, the internal volume 215 (e.g., Figure 2 ) is pressurized to a pressure greater than atmospheric pressure, such as greater than about 2 bar. In another example, the internal volume 215 is pressurized to a pressure from about 5 bar to about 70 bar, such as from about 5 bar to about 50 bar, such as between about 25 bar and about 55 bar. Because high pressure can efficiently assist in densifying the film structure, relatively low processing temperatures (such as less than 500 degrees Celsius) reduce the possibility of thermal cycling damaging the substrate 400.

[0069] During processing, the interior volume 215 is maintained at a relatively low temperature by the heater 240, for example, a temperature less than 500 degrees Celsius, such as between about 150 degrees Celsius and about 350 degrees Celsius. Thus, a low substrate thermal budget may be achieved by utilizing a high pressure annealing process and a low temperature regime.

[0070] It is believed that the high pressure process can provide a driving force to drive off dangling bonds in the exposed third conductive layer 408, the first conductive layer 404, and the dielectric layer 412, thus repairing the residues during the annealing process and smoothing the surface roughness in the exposed third conductive layer 408, the first conductive layer 404, and the dielectric layer 412. In one example, a hydrogen-containing gas or a nitrogen-containing gas (such as H2, H2O, H2O2, N2O, NO2, NH3) and dry steam can be supplied during the annealing process. An inert gas (such as He and Ar) can also be supplied during the annealing process.

[0071] In an exemplary embodiment, the process pressure is adjusted at a pressure greater than 2 bar, such as between 5 bar and 70 bar, such as between 20 bar and about 50 bar. The process temperature can be controlled at greater than 150 degrees Celsius but less than 500 degrees Celsius, such as between about 150 degrees Celsius and about 380 degrees Celsius, such as between about 180 degrees Celsius and about 400 degrees Celsius.

[0072] After the annealing process under high pressure, the third conductive layer 408, the first conductive layer 404, and the dielectric layer 412 have a high-purity repaired film structure, a large grain structure with a smooth surface roughness, which provides a relatively strong film structure, and the relatively strong film structure provides a higher film density and obtains a low film resistivity. In the example where the third conductive layer 408 and the first conductive layer 404 are Ru-containing materials, after the high-pressure annealing process, the film resistivity of the Ru-containing material from the third conductive layer 408 and the first conductive layer 404 can be reduced to between about 3% and about 7%.

[0073] At operation 312, after the third conductive layer 408 and the first conductive layer 404 are exposed, a further etching process may be performed to remove the third conductive layer 408 and the first conductive layer 404 (eg, Figures 9A-9B and then an additional etching process is performed) until the desired structure 460 is formed on the substrate 400, as shown in Figures 10A-10B As shown in . The structure 460 formed on the substrate 400 may be a dual subtractive structure utilized in a back-end structure of a semiconductor application. It should also be noted that the structure 460 may also be used to form any suitable structure on the substrate 400 as desired.

[0074] Therefore, methods for etching features in film stacks are provided. These methods utilize a three-step process including a residue removal process, a main etching process, and a high pressure annealing process to etch metal-containing materials in the film stack. In addition, the main etching process further includes a three-step process, the three-step process including a punch-through process, a bulk etching process, and a residue cleaning process. The process can efficiently etch a target material (such as a conductive layer) in the film stack without substantially corroding other materials in the film stack.

[0075] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope thereof, the scope of which is determined by the claims that follow.

Claims

1. A method for patterning a conductive layer on a substrate, the method comprising the following three steps: supplying a first gas mixture including a chlorine-containing gas at a first flow rate during a punch-through process to etch a first conductive layer disposed on the substrate, wherein the first conductive layer is a metal-containing layer; During the bulk etching process, reducing the chlorine-containing gas in the first gas mixture to a second flow rate lower than the first flow rate to continue etching the first conductive layer; and During a residue cleaning process, the chlorine-containing gas in the first gas mixture is increased to a third flow rate greater than the second flow rate to remove the first conductive layer from the substrate. 2 . The method of claim 1 , wherein the first conductive layer is a Ti-containing layer or a Ta-containing layer. The method of claim 1 , wherein the first gas mixture further comprises an inert gas.

4. The method of claim 1, wherein the chlorine-containing gas is Cl2 or HCl. The method of claim 1 , wherein the first flow rate is the same as or similar to the third flow rate.

6. The method of claim 1, further comprising the steps of: A hydrogen treatment process is performed before etching the first conductive layer.

7. The method of claim 6, further comprising the steps of: While performing the hydrogen treatment process, the substrate temperature is maintained at greater than 150 degrees Celsius.

8. The method of claim 7, wherein the substrate temperature is between 200 degrees Celsius and 300 degrees Celsius.

9. The method of claim 1, further comprising the steps of: A post annealing process is performed on the substrate after removing the first conductive layer from the substrate.

10. The method of claim 9, wherein the post annealing process further comprises the following steps: The process pressure was maintained between 5 and 100 bar.

11. The method of claim 10, further comprising the steps of: While the post annealing process is performed, an annealing gas mixture including a hydrogen-containing gas or a nitrogen-containing gas is supplied.

12. The method of claim 9, wherein the post-annealing process densifies the second conductive layer exposed on the substrate. The method of claim 12 , wherein the second conductive layer is a Ru-containing material.

14. The method of claim 1, wherein the first gas mixture supplied at the first flow rate removes oxide material from metal-containing material.

15. The method of claim 1, wherein the first gas mixture supplied at the second flow rate removes between 5% and 95% of the first conductive layer.

16. A method for patterning a conductive layer on a substrate, the method comprising the steps of: performing a hydrogen treatment process on a substrate to remove residues on the substrate, wherein the treatment process is performed at a temperature exceeding 100° C. to remove residual material from a first conductive layer, wherein the first conductive layer is a Ti-containing layer or a Ta-containing layer; performing an etching process by a three-step process, the three-step process including a punch-through process, a bulk etching process, and a residue cleaning process, wherein an etching gas mixture including a chlorine-containing gas is supplied to etch the first conductive layer on the substrate until the second conductive layer is exposed on the substrate; and The post annealing process is performed at a process pressure between 5 bar and 100 bar.

17. The method of claim 16, wherein the step of performing the etching process further comprises the following steps: While etching the first conductive layer, the chlorine-containing gas in the etching gas mixture is maintained from a first flow rate to a second flow rate and further to a third flow rate.

18. The method of claim 17, wherein the first flow rate is greater than the second flow rate. The method of claim 16 , wherein the second conductive layer is a Ru-containing layer.

20. A method for patterning a conductive layer on a substrate, the method comprising the steps of: removing residue from a substrate by a hydrogen treatment process, wherein the residue comprises an organic material, wherein the substrate comprises a first conductive layer disposed on a second conductive layer, wherein the first conductive layer is a metal-containing layer; etching the first conductive layer by a three-step process, the three-step process comprising a punch-through process, a bulk etching process, and a residue cleaning process, wherein an etching gas mixture comprising a chlorine-containing gas is supplied until a second conductive layer is exposed on the substrate, wherein while etching the first conductive layer, the chlorine-containing gas in the etching gas mixture is maintained from a first flow rate to a second flow rate and further to a third flow rate, wherein the second flow rate is lower than the first flow rate and the third flow rate is greater than the second flow rate; and A post annealing process is performed at a process pressure between 5 bar and 100 bar to thermally treat the second conductive layer on the substrate.