Compound, solid electrolyte, electrochemical cell, method for preparing compound and protected positive electrode active material
By developing the compound LixM1vPSyM2wM3z with a sulfide-germanite crystal structure for use in solid electrolytes, the problem of insufficient lithium ion conductivity and stability in solid lithium batteries has been solved, and efficient lithium ion conduction and battery cycle characteristics have been improved.
Patent Information
- Application Number
- CN202011180766.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-09
- Filing Date
- 2020-10-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-29
AI Technical Summary
The solid electrolyte material of existing solid lithium batteries is not stable enough, and the lithium ion conductivity is lower than that of liquid alternatives, so there is a need for improvement.
A compound LixM1vPSyM2wM3z with a sulfide-germanite crystal structure was developed to prepare efficient solid electrolytes and improve lithium ion conductivity and stability by using it as the electrolyte layer of electrochemical cells.
It achieves high lithium ion conductivity at room temperature and improved oxidation stability and atmospheric stability, reducing the internal resistance of the battery and improving the cycle characteristics of the battery.
Smart Images

Figure CN112777625B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefits of Korean Patent Application No. 10-2019-0138765 filed in the Korean Intellectual Property Office on November 1, 2019, and Korean Patent Application No. 10-2020-0115523 filed in the Korean Intellectual Property Office on September 9, 2020, and all rights and interests arising therefrom, the contents of which are incorporated herein by reference in their entirety. Technical Field
[0003] The present disclosure relates to a solid ion conductor, a solid electrolyte including the solid ion conductor, a lithium battery including the solid ion conductor, and a method of preparing the solid ion conductor. Background Art
[0004] All-solid lithium batteries include solid electrolytes. All-solid batteries can avoid the use of flammable organic solvents and thus can provide improved safety and stability.
[0005] Solid electrolyte materials are not sufficiently stable relative to lithium metal. Moreover, the lithium ion conductivity of solid electrolytes is lower than that of liquid alternatives. Therefore, there is still a need for improved solid electrolytes. Summary of the invention
[0006] Compounds having improved lithium ion conductivity, oxidative stability, and atmospheric stability in the solid state are provided.
[0007] A solid electrolyte including the compound is provided.
[0008] An electrochemical cell comprising the compound is provided.
[0009] Methods for preparing the compounds are provided.
[0010] Additional aspects will be set forth in part in the description which follows and, in part, will be apparent from the description.
[0011] According to an aspect of one embodiment, there is disclosed
[0012] A compound represented by Formula 1 and having an argyrodite-type crystal structure:
[0013] Formula 1
[0014] Li x M1 v PS y M2 w M3 z
[0015] Among them, in formula 1,
[0016] M1 is at least one metal element of Groups 1 to 15 of the periodic table other than Li,
[0017] M2 is SO n ;
[0018] M3 is at least one element of Group 17 of the periodic table, and
[0019] 4 ≤ x ≤ 8, 0 ≤ v < 1, 3 ≤ y ≤ 7, 0 < w < 2, 0 ≤ z ≤ 2, and 1.5 ≤ n ≤ 5.
[0020] According to an aspect of another embodiment,
[0021] The solid electrolyte includes a layer containing the compound.
[0022] According to an aspect of another embodiment, an electrochemical cell includes
[0023] A positive electrode layer including a positive electrode active material layer;
[0024] A negative electrode layer including a negative electrode active material layer; and
[0025] An electrolyte layer disposed between the positive electrode layer and the negative electrode layer,
[0026] Wherein at least one of the positive electrode active material layer and the electrolyte layer includes the compound.
[0027] According to an aspect of another embodiment, a method for preparing a compound includes:
[0028] Contacting a compound containing lithium, a compound including a metal element of Groups 1 to 15 of the periodic table other than Li, a compound containing P, a compound containing SO where 1.5 ≤ n ≤ 5 n ; and optionally a compound containing an element of Group 17 of the periodic table to prepare a mixture; and
[0029] Heat-treating the mixture in an inert atmosphere to prepare the compound.
[0030] A protected positive electrode active material is also disclosed, which includes: a lithium transition metal oxide, a transition metal sulfide, or a combination thereof; and the compound on the surface of the lithium transition metal oxide or the transition metal sulfide. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The above and other aspects, features, and advantages of some embodiments of the present disclosure will become clearer from the following description when considered in conjunction with the accompanying drawings, where:
[0032] Figure 1Ais a graph of intensity (arbitrary unit, au) versus diffraction angle (degrees, 2θ), which shows the results of powder X-ray diffraction (XRD) analysis of the solid ion conductor compounds prepared in Examples 1-3 and Reference Example 1;
[0033] Figure 1B for Figure 1A An enlarged view of a portion of
[0034] Figure 1C for Figure 1B An enlarged view of a portion of
[0035] Figure 2 is a schematic diagram of an all-solid secondary battery according to one embodiment;
[0036] Figure 3 is a schematic diagram of an all-solid secondary battery according to another embodiment; and
[0037] Figure 4 is a schematic diagram of an all-solid secondary battery according to another embodiment. DETAILED DESCRIPTION
[0038] Embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings, wherein the same reference numerals refer to the same elements throughout. In this regard, the embodiments may have different forms and should not be construed as being limited to the descriptions set forth herein. Therefore, embodiments are described below only by reference to the accompanying drawings to illustrate aspects.
[0039] Various example embodiments are more fully described herein with reference to the accompanying drawings. However, the inventive concept may be embodied in many different forms and should not be construed as being limited to the exemplary embodiments set forth herein. Rather, these embodiments are provided so that the disclosure will be thorough and complete and will fully convey the scope of the inventive concept to those of ordinary skill in the art. The same reference numerals in the accompanying drawings represent the same elements.
[0040] It will be understood that when a component is referred to as being "on" another component, the component may be directly on the other component or an intervening component may exist therebetween. Conversely, when a component is referred to as being "directly on" another component, there are no intervening components therebetween.
[0041] Although terms such as "first", "second", "third" and the like may be used to describe various elements, components (parts), regions, layers and / or parts, such elements, components (parts), regions, layers and / or parts are not necessarily limited by the above terms. The above terms are only used to distinguish one element, component (part), region, layer or part from another element, component (part), region, layer or part. Therefore, without departing from the teachings of this specification, the first element, component (part), region, layer or part described below may be referred to as a second element, component (part), region, layer or part.
[0042] The terms used in this specification are only used to describe specific embodiments, and are not intended to limit the inventive concept. As used herein, "one (kind) (indefinite article) (a, an)", "said (the)" and "at least one (kind)" do not represent the limitation of quantity, and are intended to cover both the singular and the plural, unless the context clearly states otherwise. For example, "(individual (kind)) element" has the same meaning as "at least one (kind) element", unless the context clearly states otherwise. Statements such as "at least one (kind)" modify the entire list of elements and do not modify the individual elements of the list when before or after the list of elements. As used herein, the term "and / or" includes any and all combinations of one or more of the related enumerated items. It will be further understood that the terms "include" and / or "comprising" when used in this specification indicate that there are stated features, regions, wholes, steps, operations, elements and / or components (parts), but do not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components (parts), and / or their sets.
[0043] As used herein, "about" or "approximately" is inclusive of the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±30%, 20%, 10%, or 5% relative to the stated value.
[0044] For ease of description, spatially relative terms such as "bottom", "below", "lower", "below", "above", "top", and "upper" may be used herein to describe the relationship of one element or feature to another element or feature as shown in the figure. It will be understood that in addition to the orientation shown in the figure, the spatially relative terms are intended to cover different orientations of the device in operation or use. For example, if the device in the figure is turned over, the elements described as "below" or "beneath" other elements or features will be oriented "above" the other elements or features. Therefore, terms such as "below" can cover both above and below. The device can be oriented in other ways (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein can be interpreted accordingly.
[0045] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. It will be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and will not be interpreted in an idealized or overly formal sense unless clearly so defined herein.
[0046] Example embodiments are described herein with reference to cross-sectional views that are schematic diagrams of idealized example embodiments. As such, deviations from the shapes of the figures as a result of, for example, manufacturing techniques and / or tolerances are to be expected. Therefore, example embodiments should not be construed as limited to the specific shapes of the regions as illustrated herein, but rather include deviations in shape caused by, for example, manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. Moreover, corners illustrated as sharp may be rounded. Therefore, the regions illustrated in the figures are schematic in nature and their shapes are not intended to illustrate the actual shapes of the regions and are not intended to limit the scope of this specification.
[0047] As used herein, the term "Group" refers to a Group of the Periodic Table of the Elements according to the International Union of Pure and Applied Chemistry ("IUPAC") 1-18 Group classification system.
[0048] Although specific embodiments have been described, substitutions, modifications, variations, improvements, and substantial equivalents that are currently unforeseeable or unexpected may or may occur to the applicant or those skilled in the art. Therefore, the appended claims, as filed and as they may be amended, are intended to cover all such substitutions, modifications, variations, improvements, and substantial equivalents.
[0049] As used herein, "argyrodite", "argyrodite structure", or "argyrodite-type structure" means that the compound has a crystal structure isomorphous with argyrodite Ag 8 GeS 6 . As used herein, the term "metal element" includes both metals and metalloids.
[0050] Hereinafter, according to one or more embodiments, solid ion conductor compounds, solid electrolytes including the solid ion conductor compounds, electrochemical cells including the solid ion conductor compounds, and methods for preparing the solid ion conductor compounds will be described in detail.
[0051] Solid ion conductor compounds
[0052] Compounds having ionic conduction properties, i.e., solid ion conductor compounds, are disclosed. The solid ion conductor compounds according to embodiments are represented by Formula 1 and have an argyrodite-type crystal structure:
[0053] Formula 1
[0054] Li x M1 v PS y M2 w M3 z
[0055] In Formula 1, M1 is at least one metal element of Groups 1 to 15 of the periodic table other than Li; M2 is SO n ; M3 is at least one element of Group 17 of the periodic table; and 4 ≤ x ≤ 8, 0 ≤ v < 1, 3 ≤ y ≤ 7, 0 < w < 2, 0 ≤ z ≤ 2, and 1.5 ≤ n ≤ 5. For example, 5 ≤ x ≤ 8, 0 ≤ v < 1, 4 ≤ y ≤ 7, 0 < w < 2, 0 ≤ z ≤ 2, and 1.5 ≤ n ≤ 5, or 5 < x < 8, 0 < v < 1, 4 < y < 7, 0 < w < 2, 0 < z < 2, and 1.5 < n < 5. For example, 5 ≤ x ≤ 7, 0 ≤ v < 1, 4 ≤ y ≤ 6, 0 < w < 2, 0 ≤ z ≤ 2, and 1.5 ≤ n ≤ 5. For example, 5.4 ≤ x ≤ 7, 0 ≤ v < 1, 4.5 ≤ y ≤ 6, 0 < w < 2, 0.2 ≤ z ≤ 1.8, and 1.5 ≤ n ≤ 5, or 5.4 < x < 7, 0 < v < 1, 4.5 < y < 6, 0 < w < 2, 0.2 < z < 1.8, and 1.5 < n < 5.
[0056] The compound represented by Formula 1 can be a crystalline compound having an argyrodite-type crystal structure and, due to including SO substituted at some of the sulfur (S) sites in the crystal structure 4, the compound may have improved ionic conductivity of lithium ions and reduced activation energy. In one aspect, and without wishing to be bound by theory, it is understood that the lattice volume may increase because in the solid ion conductor compound represented by Formula 1, ions having an ionic radius larger than that of a sulfide ion are placed in some of the sulfur sites. When the lattice volume increases, the migration of lithium ions in the lattice can be promoted. Moreover, when in the solid ion conductor compound represented by Formula 1, those including oxygen atoms having a greater oxidation stability and / or atmospheric stability relative to the oxidation stability and / or atmospheric stability of sulfur atoms, such as SO 4 are placed in some of the sulfur (S) sites, the structural stability of the compound can be improved.
[0057] Moreover, when the compound represented by Formula 1 includes a metal or metalloid substituted in some of the lithium sites in the crystal structure, the compound may have improved ionic conductivity of lithium ions and reduced activation energy. For example, and without wishing to be bound by theory, it is understood that since in the solid ion conductor compound represented by Formula 1, ions having an ionic radius larger than that of a lithium ion and having the same oxidation number as that of lithium are placed in some of the lithium sites, the lattice volume may increase. When the lattice volume increases, the migration of lithium ions in the lattice can be promoted. For example, when in the solid ion conductor compound represented by Formula 1, ions having an oxidation number of at least 2 (which is larger than the oxidation number of a lithium ion) are placed in the lithium sites, some of the lithium sites may be vacancy sites, for example, for charge neutrality. When vacancy sites exist in the lattice, the migration of lithium ions in the lattice can be promoted.
[0058] In the solid ion conductor compound represented by Formula 1, for example, v, w, x, and y may satisfy 0 ≤ v / (x + v) < 0.2 and 0 < w / (y + w) < 0.2; 0 ≤ v / (x + v) < 0.15 and 0 < w / (y + w) < 0.15; or 0 ≤ v / (x + v) < 0.1 and 0 < w / (y + w) < 0.1.
[0059] In the solid ion conductor compound represented by Formula 1, for example, v, w, x, y, and z may satisfy 0 ≤ v / (x + v) < 0.2 and 0 < w / (y + w + z) < 0.2; 0 ≤ v / (x + v) < 0.15 and 0 < w / (y + w + z) < 0.15; or 0 ≤ v / (x + v) < 0.1 and 0 < w / (y + w + z) < 0.1.
[0060] In the solid ion conductor compound represented by Formula 1, for example, SO n may be S 4 O 6 、S 3 O 6 、S 2 O 3 、S2 O 4 、 S 2 O 5 、 S 2 O 6 、 S 2 O 7 、 S 2 O 8 、 SO 4 、 SO 5 、 or a combination thereof. SO n may be, for example, a monovalent anion or a divalent anion. SO n 2- may be, for example, S 4 O 6 2- 、 S 3 O 6 2- 、 S 2 O 3 2- 、 S 2 O 4 2- 、 S 2 O 5 2- 、 S 2 O 6 2- 、 S 2 O 7 2- 、 S 2 O 8 2- 、 SO 4 2- 、 SO 5 2- 、 or a combination thereof.
[0061] In the solid ion conductor compound represented by Formula 1, for example, v, w, x, and y may satisfy 0 ≤ v / (x + v) < 0.08 and 0 < w / (y + w) < 0.08, and the compound may include SO 4 .
[0062] In the solid ion conductor compound represented by Formula 1, for example, v, w, x, y, and z may satisfy 0 ≤ v / (x + v) < 0.08 and 0 < w / (y + w + z) < 0.08, and the compound may include SO 4 .
[0063] In the solid ion conductor compound represented by Formula 1, for example, M1 may include Na, K, Mg, Ag, Cu, Hf, In, Ti, Pb, Sb, Fe, Zr, Zn, Cr, B, Sn, Ge, Si, Ta, Nb, V, Ga, Al, As, or a combination thereof.
[0064] In the solid ion conductor compound represented by Formula 1, for example, M1 may include Na, K, Mg, Ag, Cu, or a combination thereof.
[0065] In the solid ion conductor compound represented by Formula 1, for example, M3 may include F, Cl, Br, I, or a combination thereof.
[0066] The solid ion conductor compound represented by Formula 1 may be, for example, the solid ion conductor compound represented by Formula 2:
[0067] Formula 2
[0068] Li 7-m×v-z M1 v PS 6-w-z M2 w M3 z
[0069] In Formula 2, M1 is at least one metal element of Groups 1-15 of the periodic table other than Li; m is the oxidation number of M1; M2 is SO n ; M3 is an element of Group 17 of the periodic table; and 0 ≤ v < 1, 0 < w < 2, 0 ≤ z ≤ 2, 1.5 ≤ n ≤ 5, and 1 ≤ m ≤ 2. For example, m is 1 or 2.
[0070] Suitable monovalent cations of Groups 1-11 of the periodic table may be, for example, Na, K, Rb, Cs, Cu, or Ag.
[0071] The solid ion conductor compound represented by Formula 1 may be, for example, the solid ion conductor compound represented by at least one of Formula 3 or Formula 4:
[0072] Formula 3
[0073] (Li 1-d M1 d ) a P(S 1-e M2 e ) b M3 c
[0074] Formula 4
[0075] (Li 1-d M1 d ) a Li fc P(S 1+fc-e M2 e ) b (M3 1-f M2 f ) c
[0076] In Formulas 3 and 4, M1 is Na, K, Mg, Ag, Cu, Hf, In, Ti, Pb, Sb, Fe, Zr, Zn, Cr, B, Sn, Ge, Si, Ta, Nb, V, Ga, Al, As, or a combination thereof; M2 is SO 4 ; M3 is at least one element of Group 17 of the periodic table; 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < d ≤ 0.08, 0 < e ≤ 0.08, 0 < f ≤ 0.08, and 0 < e + f ≤ 0.08. In one aspect, the solid ion conductor compound is one of Formulas 3 or 4. In one aspect, M3 is a single element of Group 17.
[0077] In the solid ion conductor compound represented by Formula 4, for example, since M2 substitutes at the S site, some chlorine atoms may precipitate as LiCl.
[0078] The solid ion conductor compound represented by Formula 1 may be, for example, a solid ion conductor compound represented by at least one of Formulas 5 or 6.
[0079] Formula 5
[0080] (Li 1-d M1 d ) a P(S 1-e (SO 4 ) e ) b M3 c
[0081] Formula 6
[0082] (Li 1-d M1 d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (M3 1-f (SO 4 ) f ) c
[0083] In Formulas 5 and 6, M1 is Na, K, Mg, Ag, Cu, or a combination thereof; M3 is at least one element of Group 17 of the periodic table; 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < d < 0.08, 0 < e < 0.08, 0 < f < 0.08, and 0 < e + f < 0.08. In one aspect, M3 is a single element of Group 17.
[0084] In the solid ion conductor compound represented by Formula 6, for example, due to SO 4Substituted in the S site, some chlorine atoms are precipitated as LiCl.
[0085] The solid ion conductor compound represented by Formula 1 may be, for example, a solid ion conductor compound represented by at least one of Formulae 5a to 6e:
[0086] Formula 5a
[0087] (Li 1-d Na d ) a P(S 1-e (SO 4 ) e ) b M3 c
[0088] Formula 5b
[0089] (Li 1-d K d ) a P(S 1-e (SO 4 ) e ) b M3 c
[0090] Formula 5c
[0091] (Li 1-d Mg d ) a P(S 1-e (SO 4 ) e ) b M3 c
[0092] Formula 5d
[0093] (Li 1-d Ag d ) a P(S 1-e (SO 4 ) e ) b M3 c
[0094] Formula 5e
[0095] (Li 1-d Cu d ) a P(S 1-e (SO 4 ) e ) b M3 c
[0096] Formula 6a
[0097] (Li 1-d Na d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (M3 1-f (SO 4 ) f ) c
[0098] Formula 6b
[0099] (Li 1-d K d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (M3 1-f (SO 4 ) f ) c
[0100] Formula 6c
[0101] (Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (M3 1-f (SO 4 ) f ) c
[0102] Formula 6d
[0103] (Li 1-d Ag d ) a Li fc P(S 1-e (SO 4 ) e ) b (M3 1-f (SO 4 ) f ) c
[0104] Formula 6e
[0105] (Li 1-d Cu d )a Li fc P(S 1+fc-e (SO 4 ) e ) b (M3 1-f (SO 4 ) f ) c
[0106] In Formulas 5a to 6e, M3 is at least one element of Group 17 of the periodic table; 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < d ≤ 0.06, 0 < e ≤ 0.06, 0 < f ≤ 0.06, and 0 < e + f ≤ 0.06. In one aspect, M3 is a single element of Group 17.
[0107] In the solid ion conductor compound represented by one of Formulas 6a to 6e, for example, due to SO 4 substituting at the S site, some chlorine atoms may precipitate as LiCl.
[0108] The solid ion conductor compound represented by Formula 1 may be, for example, a solid ion conductor compound represented by at least one of the following:
[0109] (Li 1-d Cu d ) a P(S 1-e (SO 4 ) e ) b F c , (Li 1-d Cu d ) a P(S 1-e (SO 4 ) e ) b Cl c , (Li 1-d Cu d ) a P(S 1-e (SO 4 ) e ) b Br c , (Li 1-d Cu d ) a P(S 1-e (SO 4 ) e ) b I c ,
[0110] (Li 1-d Cu d) a Li fc P(S 1+fc-e (SO 4 ) e ) b (F 1-f (SO 4 ) f ) c (Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Cl 1-f (SO 4 ) f ) c (Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Br 1-f (SO 4 ) f ) c (Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (I 1-f (SO 4 ) f ) c ,
[0111] (Li 1-d So d ) a P(S 1-e (SO 4 ) e ) b F c (Li 1-d So d ) a P(S 1-e (SO 4 ) e ) b Cl c (Li 1-d So d ) aP(S 1-e (SO 4 ) e ) b Br c ,(Li 1-d Na d ) a P(S 1-e (SO 4 ) e ) b I c ,
[0112] (Li 1-d Na d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (F 1-f (SO 4 ) f ) c ,(Li 1-d Na d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Cl 1-f (SO 4 ) f ) c ,(Li 1-d Na d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Br 1-f (SO 4 ) f ) c ,(Li 1-d Na d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (I 1-f (SO 4 ) f ) c ,
[0113] (Li 1-d K d )a P(S 1-e (SO 4 ) e ) b F c ,(Li 1-d K d ) a P(S 1-e (SO 4 ) e ) b Cl c ,(Li 1-d K d ) a P(S 1-e (SO 4 ) e ) b Br c ,(Li 1-d K d ) a P(S 1-e (SO 4 ) e ) b I c ,
[0114] (Li 1-d K d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (F 1-f (SO 4 ) f ) c ,(Li 1-d K d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Cl 1-f (SO 4 ) f ) c ,(Li 1-d K d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Br 1-f (SO 4 ) f )c ,(Li 1-d K d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (I 1-f (SO 4 ) f ) c ,
[0115] (Li 1-d Mg d ) a P(S 1-e (SO 4 ) e ) b F c ,(Li 1-d Mg d ) a P(S 1-e (SO 4 ) e ) b Cl c ,(Li 1-d Mg d ) a P(S 1-e (SO 4 ) e ) b Br c ,(Li 1-d Mg d ) a P(S 1-e (SO 4 ) e ) b I c ,
[0116] (Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (F 1-f (SO 4 ) f ) c ,(Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO 4 )e ) b (Cl 1-f (SO 4 ) f ) c ,(Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Br 1-f (SO 4 ) f ) c ,(Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (I 1-f (SO 4 ) f ) c ,
[0117] (Li 1-d Ag d ) a P(S 1-e (SO 4 ) e ) b F c ,(Li 1-d Ag d ) a P(S 1-e (SO 4 ) e ) b Cl c ,(Li 1-d Ag d ) a P(S 1-e (SO 4 ) e ) b Br c ,(Li 1-d Ag d ) a P(S 1-e (SO 4 ) e ) b I c ,
[0118] (Li 1-d Agd ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (F 1-f (SO 4 ) f ) c ,(Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Cl 1-f (SO 4 ) f ) c ,(Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (Br 1-f (SO 4 ) f ) c ,或者(Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO 4 ) e ) b (I 1-f (SO 4 ) f ) c 。Combinations of at least two including the foregoing may be used.
[0119] In the above formula, each of a, b, c, d, e, and f can be independently selected, and 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < d ≤ 0.06, 0 < e < 0.06, 0 < f < 0.06, and 0 < e + f < 0.06.
[0120] The solid ion conductor compound represented by Formula 1 can be, for example, the solid ion conductor compound represented by Formula 7:
[0121] Formula 7
[0122] Li 7-p×v-u-z M4 v M5 u PS6-w-z M2 w M3 z
[0123] In formula 7, M4 is a metal element of Groups 2-15 of the periodic table; p is the oxidation number of M4, and M2 is SO n ; M3 is an element of Group 17 of the periodic table; M5 is a metal element of Group 1 of the periodic table other than Li and is a monovalent cation; and 0 ≤ v < 1, 0 ≤ u < 1, 0 < w < 2, 0 ≤ z ≤ 2, 1.5 ≤ n ≤ 5, and 1 ≤ p ≤ 2. For example, p is 1 or 2. In one aspect, M4 is at least one element of Groups 2-15. In one aspect, M3 is at least one element of Group 17.
[0124] In the solid ion conductor compound represented by formula 7, for example, M4 may include Cu, Ag, Mg, Hf, In, Ti, Pb, Sb, Fe, Zr, Zn, Cr, B, Sn, Ge, Si, Ta, Nb, V, Ga, Al, As, or a combination thereof. In the solid ion conductor compound represented by formula 7, for example, M5 may include Na, K, Rb, Cs, or a combination thereof.
[0125] Suitable monovalent cations of Groups 2-11 of the periodic table may be, for example, Cu or Ag. Suitable divalent cations selected from Groups 2-11 of the periodic table may be, for example, Ca, Zn, Mg, or Fe.
[0126] The solid ion conductor compound represented by formula 1 may be, for example, the solid ion conductor compound represented by formula 8:
[0127] Formula 8
[0128] Li 7-z PS 6-w-z M2 w M3 z
[0129] In formula 8, M2 is SO n ; M3 is an element of Group 17 of the periodic table; and 0 < w < 2, 0 ≤ z ≤ 2, and 1.5 ≤ n ≤ 5. In one aspect, M3 is at least one element of Group 17.
[0130] The solid ion conductor compound represented by formula 1 may be, for example, one of the solid ion conductor compounds represented by formula 9 or 10:
[0131] Formula 9
[0132] Li a+fc P(S 1+fc-e M2 e ) b (M3 1-f M2f ) c
[0133] Formula 10
[0134] Li a P(S 1-e M2 e ) b M3 c
[0135] In Formulas 9 and 10, M2 is SO 4 ; M3 is at least one element of Group 17 of the periodic table; 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < e ≤ 0.08, 0 < f ≤ 0.08, and 0 < e + f ≤ 0.08. In one aspect, M3 is a single element of Group 17.
[0136] In the solid ion conductor compound represented by Formula 9, for example, since M2 substitutes at the S site, some chlorine atoms may precipitate as LiCl.
[0137] The solid ion conductor compound represented by Formula 1 may be, for example, the solid ion conductor compound represented by Formula 11 or 12:
[0138] Formula 11
[0139] Li a+fc P(S 1+fc-e (SO 4 ) e ) b (M3 1-f (SO 4 ) f ) c
[0140] Formula 12
[0141] Li a P(S 1-e (SO 4 ) e ) b M3 c
[0142] In Formula 11 or 12, M3 is an element of Group 17 of the periodic table; 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < e < 0.08, 0 < f < 0.08, and 0 < e + f < 0.08. In one aspect, M3 is at least one element of Group 17. In one aspect, M3 is a single element of Group 17.
[0143] In the solid ion conductor compound represented by Formula 11, for example, since SO 4 substitutes at the S site, some chlorine atoms may precipitate as LiCl.
[0144] The solid ion conductor compound represented by Formula 1 may be a solid ion conductor compound represented by one of the following: Li a+fc P(S 1+fc-e (SO 4 ) e ) b (F 1-f (SO 4 ) f ) c , Li a+fc P(S 1+fc-e (SO 4 ) e ) b (Cl 1-f (SO 4 ) f ) c , Li a+fc P(S 1+fc-e (SO 4 ) e ) b (Br 1-f (SO 4 ) f ) c , Li a+fc P(S 1+fc-e (SO 4 ) e ) b (I 1-f (SO 4 ) f ) c , Li a P(S 1-e (SO 4 ) e ) b F c , Li a P(S 1-e (SO 4 ) e ) b Cl c , Li a P(S 1-e (SO 4 ) e ) b Br c , or Li a P(S 1-e (SO 4 ) e ) b I c .
[0145] In the above formula, a, b, c, e, and f are each independently selected, and 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < e < 0.06, 0 < f < 0.06, and 0 < e + f < 0.06.
[0146] The solid ion conductor compound represented by Formula 1 provides improved lithium ion conductivity. The solid ion conductor compound represented by Formula 1 provides the following improved lithium ion conductivity at room temperature, for example, at about 25 °C: about 1 millisiemens per centimeter (mS / cm) or greater, about 1.5 mS / cm or greater, about 2.0 mS / cm or greater, about 2.5 mS / cm or greater, about 3.0 mS / cm or greater, about 3.5 mS / cm or greater, about 4.0 mS / cm or greater, or about 5.0 mS / cm or greater. The solid ion conductor compound represented by Formula 1 provides an ion conductivity in the following ranges at room temperature, for example, at about 25 °C: about 1.0 mS / cm - about 500 mS / cm, about 1.5 mS / cm - about 400 mS / cm, about 2.0 mS / cm - about 300 mS / cm, about 2.5 mS / cm - about 200 mS / cm, about 3.0 mS / cm - about 150 mS / cm, about 3.5 mS / cm - about 100 mS / cm, about 4.0 mS / cm - about 100 mS / cm, or about 5.0 mS / cm - about 100 mS / cm. Therefore, in an electrochemical cell including a positive electrode, a negative electrode, and the solid ion conductor compound represented by Formula 1 disposed between the positive electrode and the negative electrode, ion transport between the positive electrode and the negative electrode can be effectively performed, and thus the internal resistance between the positive electrode and the negative electrode can be reduced. The ion conductivity can be measured by using a direct current (DC) polarization method. In an embodiment, the ion conductivity can be measured using a complex impedance method.
[0147] After 10 days under dry conditions in an air atmosphere having a dew point below about -60 °C, the solid ion conductor compound represented by Formula 1 can have, for example, an ion conductivity retention of about 70% or greater, about 75% or greater, or about 80% or greater, for example, about 70% - about 99.9%, or about 80% - about 99%. The ion conductivity retention can be defined, for example, as shown in Equation 1. In Equation 1, the initial ion conductivity of the solid ion conductor compound represents the ion conductivity of the solid ion conductor compound before storage under dry conditions. The ion conductivity retention can be measured by using the method described in Evaluation Example 3.
[0148] Equation 1
[0149] Ion conductivity retention = [Ion conductivity of the solid ion conductor compound after 10 days / Initial ion conductivity of the solid ion conductor compound] × 100%
[0150] The solid ion conductor compound represented by Formula 1 may belong to, for example, a cubic system, or more specifically, to a F-43m space group. Also, the solid ion conductor compound represented by Formula 1 may be an argyrodite-type sulfide having an argyrodite-type crystal structure. As some sulfur (S) sites are replaced by SO 4 2- The solid ion conductor compound represented by Formula 1 includes oxygen atoms and thus can simultaneously provide improved lithium ion conductivity and improved oxidation resistance and atmospheric stability. Moreover, when some lithium sites in the argyrodite crystal structure are selected from M1 + Cationic elements, M1 2+ Cationic elements, and M1 3+ When substituted with at least one element of the cationic element, the solid ion conductor compound represented by Formula 1 can simultaneously provide improved lithium ion conductivity and improved electrochemical stability relative to lithium metal.
[0151] Reference Figure 1C , the solid ion conductor compound represented by Formula 1 has, for example, a first peak at a diffraction angle of 30.1°2θ±0.5°2θ and a second peak at a diffraction angle of 31.5°2θ±0.5°2θ when analyzed by X-ray diffraction using CuKα radiation, and a compound having the same composition as that of the solid ion conductor compound represented by Formula 1 except that M2 is changed to S has, when analyzed by X-ray diffraction using CuKα radiation, a third peak at a diffraction angle of 30.1°2θ±0.5°2θ and a fourth peak at a diffraction angle of 31.5°2θ±0.5°2θ, wherein the positions of the first peak and the second peak may be shifted downward by about 0.01° or more, about 0.02° or more, about 0.03° or more, or about 0.04° or more, for example, from about 0.01° to about 0.5°, or from about 0.05° to about 0.1°, compared with the positions of the third peak and the fourth peak, respectively. The downward shift of the peak is due to the substitution of SO with an ionic radius larger than that of sulfur (S). 4 The solid ion conductor compound having an increased distance between the planes of the crystal lattice can provide improved oxidation resistance and atmospheric stability.
[0152] Reference Figure 1B , when analyzed by X-ray diffraction using CuKα radiation, the solid ion conductor compound represented by Formula 1 may also have, for example, an additional peak corresponding to LiM3 reprecipitated due to M2 at a diffraction angle of 35.0°2θ±1.0°2θ. LiM3 may be, for example, LiCl. The solid ion conductor compound having the additional peak may provide improved oxidation resistance and atmospheric stability.
[0153] In one aspect, the disclosed compounds of Formula 1 can be used to provide a protected cathode active material. The cathode active material can include a lithium transition metal oxide, a transition metal sulfide, a lithium transition metal sulfide, or a combination thereof. The compound of Formula 1 can be on the surface of the cathode active material. For example, the compound of Formula 1 can be in the form of a layer on the surface of the cathode active material. The thickness of the layer can be from about 1 nanometer (nm) to about 1000 nm, or from about 10 nm to about 100 nm.
[0154] Solid electrolyte
[0155] A solid electrolyte according to another embodiment includes a solid ion conductor compound represented by Formula 1. The solid electrolyte can be in the form of including the compound of Formula 1, for example, a layer composed of the compound of Formula 1. The layer can be between the cathode and the anode, or the layer can be on the cathode active material, or on the anode active material. Due to including the solid ion conductor compound, the solid electrolyte can have high ionic conductivity and high chemical stability. A solid electrolyte including a solid ion conductor compound represented by Formula 1 can provide improved stability with respect to air and electrochemical stability with respect to lithium metal. Therefore, the solid ion conductor compound represented by Formula 1 can be used as, for example, a solid electrolyte of an electrochemical cell.
[0156] In addition to the solid ion conductor compound represented by Formula 1, the solid electrolyte can further include a second solid electrolyte. For example, the solid electrolyte can further include a sulfide-based solid electrolyte and / or an oxide-based solid electrolyte. Examples of the second solid electrolyte further included in the solid electrolyte can include Li 2 O - Al 2 O 3 -TiO 2 -P 2 O 5 (LATP), lithium superionic conductor (LISICON), Li 3-y PO 4-x N x (LIPON, where 0 < y < 3 and 0 < x < 4), Li 3.25 Ge 0.25 P 0.75 S 4 (Thio-LISICON), Li 2 S, Li 2 S - P 2 S 5 、Li 2 S - SiS 2 、Li 2 S - GeS 2 、Li 2SB 2 S 3 , or Li 2 S-Al 2 S 3 , but the embodiment is not limited thereto, and any suitable material that can be used as a solid ion conductor compound in the art may be used.
[0157] The solid electrolyte may be in a powder form or a monolithic form. The monolithic form of the solid electrolyte may be in the form of, for example, a sheet (wafer), a sheet, or a film, but the embodiment is not limited thereto, and the solid electrolyte may be in various forms according to its purpose of use.
[0158] Electrochemical Cells
[0159] An electrochemical cell according to another embodiment includes: a positive electrode layer including a positive electrode active material layer; a negative electrode layer including a negative electrode active material layer; and an electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode active material layer and / or the electrolyte layer includes a solid ion conductor compound represented by Formula 1. When the electrochemical cell includes the solid ion conductor compound represented by Formula 1, lithium ion conductivity and stability relative to lithium metal of the electrochemical cell are improved.
[0160] The electrochemical battery may be, for example, an all-solid secondary battery, a secondary battery containing a liquid electrolyte, or a lithium air battery, but the embodiment is not limited thereto, and any suitable material usable as an electrochemical battery in the art may be used.
[0161] Hereinafter, the all-solid secondary battery will be described in further detail.
[0162] All-solid-state secondary battery: Type I
[0163] The all-solid secondary battery may include a solid ion conductor compound represented by Formula 1.
[0164] The all-solid secondary battery may include, for example, a positive electrode layer including a positive electrode active material layer; a negative electrode layer including a negative electrode active material layer; and an electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode active material layer and / or the electrolyte layer may include a solid ion conductor compound represented by Formula 1.
[0165] An all-solid secondary battery according to another embodiment may be prepared as follows.
[0166] Solid electrolyte layer
[0167] The solid electrolyte layer may be prepared by mixing a solid ion conductor compound represented by Formula 1 and a binder and drying the mixture, or by rolling powder of the solid ion conductor compound represented by Formula 1 into a regular shape by applying a pressure in the range of about 1 ton to about 10 tons. The solid ion conductor compound represented by Formula 1 may be used as a solid electrolyte.
[0168] The particle size of the solid electrolyte may be, for example, in the range of about 0.5 micrometers (μm) to about 20 μm, or about 0.5 μm to about 15 μm, or about 1 μm to about 10 μm. When the particle size of the solid electrolyte is within this range, the bonding properties during the formation of the sintered body are improved, and thus the ionic conductivity and life characteristics of the solid electrolyte can be improved.
[0169] The thickness of the solid electrolyte layer may be in the range of about 10 μm to about 200 μm, or about 20 μm to about 150 μm, or about 30 μm to about 100 μm. When the thickness of the solid electrolyte layer is within this range, sufficient migration rate of lithium ions can be ensured, which can lead to high ion conductivity.
[0170] The solid electrolyte layer may further include a solid electrolyte other than the solid ion conductor compound represented by Formula 1, for example, a sulfide-based (ie, containing sulfide) solid electrolyte and / or an oxide-based solid electrolyte.
[0171] Examples of the sulfide-based solid electrolyte may include lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. Examples of the sulfide-based solid electrolyte may include Li 2 S.P. 2 S 5 、SiS 2 ,GeS 2 , B 2 S 3 , or a combination thereof. Examples of the sulfide-based solid electrolyte may include Li 2 S or P 2 S 5 The sulfide-based solid electrolyte is known to have a higher lithium ion conductivity than other inorganic compounds. Examples of the sulfide-based solid electrolyte may include Li 2 S and / or P 2 S 5 When the sulfide-based solid electrolyte material constituting the sulfide-based solid electrolyte includes Li 2 SP 2 S 5 When Li 2 S vs. P 2 S5 The mixing molar ratio can be, for example, in the range of about 50:50 to about 90:10. Moreover, an inorganic solid electrolyte prepared as follows can be used as the sulfide-based solid electrolyte: Li 3 PO 4 , a halogen compound, Li 2+2x Zn 1-x GeO 4 (LISICON, where 0 < x < 1), Li 3+y PO 4-x N x (LIPON, where 0 < y < 3 and 0 < x < 4), Li 3.25 Ge 0.25 P 0.75 S 4 (Thio-LISICON), and Li 2 O - Al 2 O 3 -TiO 2 -P 2 O 5 (LATP) are added to Li 2 S - P 2 S 5 , SiS 2 , GeS 2 , B 2 S 3 , or a combination thereof. Examples of the sulfide-based solid electrolyte material can include Li 2 S - P 2 S 5 ; Li 2 S - P 2 S 5 -LiX (where X is a halogen element); Li 2 S - P 2 S 5 -Li 2 O; Li 2 S - P 2 S 5 -Li 2 O - LiI; Li 2 S - SiS 2 ; Li 2 S - SiS 2 -LiI; Li 2 S - SiS 2 -LiBr; Li 2 S - SiS 2 -LiCl; Li 2 S - SiS 2 -B 2 S3 -LiI; Li 2 S-SiS 2 -P 2 S 5 -LiI; Li 2 SB 2 S 3 ;Li 2 SP 2 S 5 -Z m S n (wherein m and n are each a positive integer, and Z is Ge, Zn, or Ga); Li 2 S-GeS 2 ;Li 2 S-SiS 2 -Li 3 PO 4 and Li 2 S-SiS 2 -Li p MO q (wherein p and q are each a positive integer, and M is P, Si, Ge, B, Al, Ga, or In). In this regard, the sulfide-based solid electrolyte material may be prepared by: reacting a starting material of the sulfide-based solid electrolyte material (e.g., Li 2 S or P 2 S 5 ) is processed by a melt quenching method or a mechanical grinding method. Moreover, a calcination process may be performed after the treatment.
[0172] Examples of the binder included in the solid electrolyte layer may include styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, and polyvinyl alcohol, but the embodiment is not limited thereto, and any suitable material that can be used as a binder in the art can be used. The binder of the solid electrolyte layer may be the same as or different from the binder of the positive electrode layer and the negative electrode layer.
[0173] Positive electrode layer
[0174] The positive electrode layer may be prepared by forming a positive electrode active material layer including a positive electrode active material on a current collector. The average particle size of the positive electrode active material may be, for example, in the range of about 2 μm to about 10 μm.
[0175] The positive electrode active material may be any suitable material that can be used as a positive electrode active material in a secondary battery in the art. Examples of the positive electrode active material may include lithium transition metal oxides, transition metal sulfides, and lithium transition metal sulfides. For example, the positive electrode active material may be at least one composite oxide of lithium and Co, Mn, Ni, or a combination thereof. In some embodiments, the positive electrode active material may be a compound represented by:
[0176] Li a A 1-b B' b D 2 (where 0.90≤a≤1.8 and 0≤b≤0.5); Li a E 1-b B' b O 2-c D c (where 0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05); LiE 2-b B' b O 4-c D c (where 0≤b≤0.5 and 0≤c≤0.05); Li a Ni 1-b- c Co b B' c D α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Co b B' c O 2-α F' α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Co b B' c O 2-α F' 2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c D α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Mn b B' c O2-α F' α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c O 2-α F' 2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni b E c G d O 2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, and 0.001≤d≤0.1); Li a Ni b Co c Mn d G e O 2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0.001≤e≤0.1); Li a NeG b O 2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a CoG b O 2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a MnG b O 2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a Mn 2 G b O 4 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); QO 2 ;QS 2 ;LiQS 2 ; V 2 O 5 ;LiV 2 O 2 ;LiI'O 2 ;LiNiVO 4 ;Li (3-f) J 2 (PO 4 ) 3 (where 0≤f≤2); Li (3-f) Fe 2 (PO4 ) 3 (where 0≤f≤2); or LiFePO 4 In the above formula, A may include nickel (Ni), cobalt (Co), manganese (Mn), or a combination thereof; B' may include aluminum (Al), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), iron (Fe), magnesium (Mg), strontium (Sr), vanadium (V), rare earth elements, or a combination thereof; D may include oxygen (O), fluorine (F), sulfur (S), phosphorus (P), or a combination thereof; E may include cobalt (Co), manganese (Mn), or a combination thereof; F' may include fluorine (F), sulfur (S), phosphorus (P), or a combination thereof alloy; G may include aluminum (Al), chromium (Cr), manganese (Mn), iron (Fe), magnesium (Mg), lanthanum (La), cerium (Ce), strontium (Sr), vanadium (V), or a combination thereof; Q may include titanium (Ti), molybdenum (Mo), manganese (Mn), or a combination thereof; I' may include chromium (Cr), vanadium (V), iron (Fe), scandium (Sc), yttrium (Y), or a combination thereof; and J may include vanadium (V), chromium (Cr), manganese (Mn), cobalt (Co), nickel (Ni), copper (Cu), or a combination thereof.
[0177] In some embodiments, the positive electrode active material may be LiCoO 2 、LiMn x O 2x (where x is 1 or 2), LiNi 1-x Mn x O 2 (where 0 <x<1)、LiNi 1-x-y Co x Mn y O 2 (where 0≤x≤0.5 and 0≤y≤0.5), LiNi 1-x- y Co x Al y O 2 (where 0≤x≤0.5 and 0≤y≤0.5), LiFePO 4 、TiS 2 , FeS 2 、TiS 3 , or FeS 3In the compound, A may be Ni, Co, Mn, or a combination thereof; B may be Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D may be O, F, S, P, or a combination thereof; E may be Co, Mn, or a combination thereof; F may be F, S, P, or a combination thereof; G may be Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q may be Ti, Mo, Mn, or a combination thereof; I may be Cr, V, Fe, Sc, Y, or a combination thereof; and J may be V, Cr, Mn, Co, Ni, Cu, or a combination thereof.
[0178] The compounds listed above as positive electrode active materials may have a surface coating layer (hereinafter, also referred to as "coating layer"). Alternatively, a mixture of a compound without a coating layer and a compound with a coating layer may be used, the compound being selected from the compounds listed above. In some embodiments, the coating layer may include, for example, a coating element compound such as an oxide, hydroxide, oxyhydroxide, oxycarbonate, or hydroxycarbonate of a coating element. In some embodiments, the compound used for the coating layer may be amorphous or crystalline. In some embodiments, the coating element used for the coating layer may be magnesium (Mg), aluminum (Al), cobalt (Co), potassium (K), sodium (Na), calcium (Ca), silicon (Si), titanium (Ti), vanadium (V), tin (Sn), germanium (Ge), gallium (Ga), boron (B), arsenic (As), zirconium (Zr), or a mixture thereof. In some embodiments, the coating layer may be formed using any method that does not adversely affect the physical properties of the positive electrode active material. For example, the coating layer may be formed using a spraying method or an impregnation method. The coating method may be well understood by those of ordinary skill in the art, and thus a detailed description thereof will be omitted.
[0179] The positive electrode active material may include, for example, a lithium salt of a transition metal oxide having a layered rock salt structure among examples of lithium transition metal oxides. For example, the "layered rock salt structure" refers to a structure in which <111> The oxygen atomic layers and the metal atomic layers are arranged alternately and regularly in the direction, wherein the atomic layers each form a two-dimensional plane. "Cubic rock salt type structure" refers to a sodium chloride (NaCl) type structure as one of the crystal structures, in particular a structure in which the face-centered cubic (fcc) lattice formed by anions and cations, respectively, is offset by only half of the ridge of each unit lattice. Examples of lithium transition metal oxides having a layered rock salt type structure may include LiNi x Co y Al z O 2 (NCA) or LiNi x Co y Mnz O 2 A ternary lithium transition metal oxide of (NCM) (where 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z = 1). When the positive electrode active material includes a ternary lithium transition metal oxide having a layered rock salt structure, the energy density and thermal stability of the all-solid-state secondary battery can be further improved.
[0180] As described above, the positive electrode active material may be covered with a coating layer. The coating layer may include any suitable material that can be used as a coating layer for the positive electrode active material of an all-solid-state secondary battery in the art. The coating layer may be, for example, Li 2 O-ZrO 2 (LZO).
[0181] When the positive electrode active material includes nickel (Ni) as a ternary lithium transition metal oxide such as NCA or NCM, the capacity density of the all-solid-state secondary battery increases, and thus the elution of metal from the positive electrode active material in the charged state can be reduced. As a result, the cycle characteristics of the all-solid-state secondary battery are improved.
[0182] The shape of the positive electrode active material may be, for example, a particulate shape such as a true spherical shape or an ellipsoidal shape. The particle size of the positive electrode active material is not particularly limited and may be within the range applicable to the positive electrode active material of an all-solid-state secondary battery. The amount of the positive electrode active material in the positive electrode layer is not particularly limited and may be within the range applicable to the positive electrode layer of an all-solid-state secondary battery. In the positive electrode active material layer, the amount of the positive electrode active material may be, for example, in the range of about 50 wt% - about 95 wt%.
[0183] The positive electrode active material layer may further include a solid ion conductor compound represented by Formula 1.
[0184] The positive electrode active material layer may include a binder. Examples of the binder may include styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene.
[0185] The positive electrode active material layer may include a conductive agent. Examples of the conductive agent may include graphite, carbon black, acetylene black, Ketjen black, carbon fiber, and metal powder.
[0186] In addition to the positive electrode active material, solid electrolyte, binder, and conductive agent, the positive electrode active material layer may further include additives such as fillers, coating agents, dispersants, and ion conductors.
[0187] The fillers, dispersants, and ion conductors that can be added to the positive electrode active material layer may be materials commonly used in the electrodes of all-solid-state secondary batteries.
[0188] The positive electrode current collector may be a plate or foil formed of, for example, aluminum (Al), indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector may be omitted.
[0189] The positive electrode current collector may further include a carbon layer disposed on one or both surfaces of the metal substrate. When the carbon layer is additionally disposed on the metal substrate, the metal of the metal substrate can be prevented from being corroded by the solid electrolyte in the positive electrode layer, and the interface resistance between the positive electrode active material layer and the positive electrode current collector can be reduced. The thickness of the carbon layer may, for example, be in the range of about 1 μm to about 5 μm. When the thickness of the carbon layer is too thin, the contact between the metal substrate and the solid electrolyte may not be completely prevented. When the thickness of the carbon layer is too thick, the energy density of the all-solid secondary battery may deteriorate. The carbon layer may include amorphous carbon and crystalline carbon.
[0190] Negative electrode layer
[0191] The negative electrode layer may be prepared in the same manner as the positive electrode layer except that a negative electrode active material is used instead of a positive electrode active material. The negative electrode layer may be prepared by forming a negative electrode active material layer including a negative electrode active material on a negative electrode current collector.
[0192] The negative active material layer may further include a solid ion conductor compound represented by Formula 1.
[0193] The negative electrode active material may be lithium metal, lithium metal alloy, or a combination thereof.
[0194] The negative electrode active material layer may further include a negative electrode active material other than lithium metal, a lithium metal alloy, or a combination thereof. Examples of the negative electrode active material may include at least one of the following: a metal / metalloid capable of alloying with lithium, a transition metal oxide, a non-transition metal oxide, or a carbonaceous material. Examples of the metal / metalloid capable of alloying with lithium may be Ag, Si, Sn, Al, Ge, Pb, Bi, Sb, a Si-Y' alloy (where Y' is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, or a combination thereof, and Y' is not Si), and a Sn-Y' alloy (where Y' is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, or a combination thereof, and Y' is not Sn). In some embodiments, Y' may be magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), rutherfordium (Rf), vanadium (V), niobium (Nb), tantalum (Ta), (Db), chromium (Cr), molybdenum (Mo), tungsten (W), (Sg), technetium (Tc), rhenium (Re), (Bh), iron (Fe), lead (Pb), ruthenium (Ru), osmium (Os), (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), boron (B), aluminum (Al), gallium (Ga), tin (Sn), indium (In), thallium (Tl), germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po), or a combination thereof. Examples of the transition metal oxide may include lithium titanium oxide, vanadium oxide, and lithium vanadium oxide. Examples of the non-transition metal oxide may include SnO 2 and SiO x (where 0 < x < 2). Examples of the carbonaceous material may include crystalline carbon, amorphous carbon, or a mixture thereof. Examples of the crystalline carbon are graphite in the form of shapeless, plates, flakes, spheres, or fibers such as natural graphite or artificial graphite. Examples of the amorphous carbon are soft carbon (carbon sintered at low temperature), hard carbon, mesophase pitch carbonized product, and sintered coke.
[0195] Refer to Figure 2, the all-solid secondary battery 40 according to the embodiment includes a solid electrolyte layer 30, a positive electrode layer 10 provided on one surface of the solid electrolyte layer 30, and a negative electrode layer 20 provided on the other surface of the solid electrolyte layer 30. The positive electrode layer 10 includes a positive electrode active material layer 12 in contact with the solid electrolyte layer 30, and a positive electrode collector 11 in contact with the positive electrode active material layer 12, and the negative electrode layer 20 includes a negative electrode active material layer 22 in contact with the solid electrolyte layer 30, and a negative electrode collector 21 in contact with the negative electrode active material layer 22. The all-solid secondary battery 40 can be completed, for example, by forming the positive electrode active material layer 12 and the negative electrode active material layer 22 on both surfaces of the solid electrolyte layer 30; and forming the positive electrode collector 11 and the negative electrode collector 21 on the positive electrode active material layer 12 and the negative electrode active material layer 22, respectively. In some embodiments, the all-solid secondary battery 40 may be completed by, for example, sequentially stacking the negative electrode active material layer 22 , the solid electrolyte layer 30 , the positive electrode active material layer 12 , and the positive electrode collector 11 on the negative electrode collector 21 .
[0196] All-solid-state secondary battery: Type II
[0197] Reference Figure 3 and 4 The all-solid secondary battery 1 may include, for example, a positive electrode layer 10 including a positive electrode active material layer 12 disposed on a positive electrode current collector 11; a negative electrode layer 20 including a negative electrode active material layer 22 disposed on a negative electrode current collector 21; and an electrolyte layer 30 disposed between the positive electrode layer 10 and the negative electrode layer 20, wherein the positive electrode active material layer 12 and / or the electrolyte layer 30 may include a solid ion conductor compound represented by Formula 1.
[0198] The all-solid secondary battery 1 according to another embodiment may be prepared as follows.
[0199] The positive electrode layer 10 and the solid electrolyte layer 30 are prepared in the same manner as in the above-described all-solid secondary battery according to the embodiment.
[0200] Negative electrode layer
[0201] Next, the negative electrode layer 20 is prepared.
[0202] Reference Figure 3 and 4 The negative electrode layer 20 may include a negative electrode collector 21 and a negative electrode active material layer 22 disposed on the negative electrode collector 21 , and the negative electrode active material layer 22 may include, for example, a negative electrode active material and a binder.
[0203] The negative electrode active material included in the negative electrode active material layer 22 may be, for example, in the form of particles. The average particle size of the negative electrode active material in particle form may be, for example, about 4 μm or less, about 3 μm or less, about 2 μm or less, about 1 μm or less, or about 900 nm or less. The average particle size of the negative electrode active material in particle form may be, for example, in the range of about 10 nm to about 4 μm or less, about 10 nm to about 3 μm or less, about 10 nm to about 2 μm or less, about 10 nm to about 1 μm or less, or about 10 nm to about 900 nm or less. When the average particle size of the negative electrode active material is within these ranges, the reversible absorption and / or desorption of lithium during charge / discharge may be further promoted. The average particle size of the negative electrode active material may be, for example, a median diameter (D50) measured by using a laser diffraction particle size distribution instrument.
[0204] The negative electrode active material in the negative electrode active material layer 22 may include, for example, at least one of a carbonaceous negative electrode active material, a metal or a metalloid negative electrode active material.
[0205] The carbonaceous negative electrode active material may be, for example, particularly amorphous carbon. Examples of the amorphous carbon may include carbon black (CB), acetylene black (AB), furnace black (FB), Ketjen black (KB), and graphene, but embodiments are not limited thereto, and any suitable material that can be used as amorphous carbon in the art may be used. Amorphous carbon refers to carbon that has no crystallinity or has very low crystallinity, which may be different from crystalline carbon or graphite carbon.
[0206] For example, the metal or metalloid negative electrode active material may include at least one of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), or zinc (Zn), but the embodiment is not limited thereto, and any suitable material that can be used as a metal negative electrode active material or a metalloid negative electrode active material that can form an alloy or compound with lithium can be used in the art. For example, nickel (Ni) does not form an alloy with lithium and is therefore not a metal negative electrode active material.
[0207] The negative electrode active material layer 22 may include at least one of these negative electrode active materials, for example, a mixture of a plurality of different negative electrode active materials. For example, the negative electrode active material layer 22 may include only amorphous carbon or may include at least one of the following: gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), or zinc (Zn). In some embodiments, the negative electrode active material layer 22 may include a mixture containing at least one of the following and amorphous carbon: gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), or zinc (Zn). The mixing ratio of the amorphous carbon to gold or the like may be a weight ratio in the range of about 10: 1-about 1: 2, about 5: 1-about 1: 1, or about 4: 1-about 2: 1, but the embodiment is not limited thereto, and the mixing ratio may be selected according to the characteristics of the all-solid secondary battery 1. When the negative electrode active material has the composition, the cycle characteristics of the all-solid secondary battery 1 can be further improved.
[0208] The negative electrode active material in the negative electrode active material layer 22 may include, for example, a mixture of first particles formed of amorphous carbon and second particles formed of metal or metalloid. Examples of the metal or metalloid may include gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), or zinc (Zn). In some embodiments, the metalloid may be a semiconductor. Based on the total weight of the mixture, the amount of the second particle may be in the range of about 8 wt % to about 60 wt %, about 10 wt % to about 50 wt %, about 15 wt % to about 40 wt %, or about 20 wt % to about 30 wt %. When the amount of the second particle is within these ranges, for example, the cycle characteristics of the all-solid secondary battery 1 may be further improved.
[0209] Examples of the binder in the negative electrode active material layer 22 may include styrene-butadiene rubber (SBR), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile (PAN), and polymethyl methacrylate (PMMA), but the embodiment is not limited thereto, and any suitable material that can be used as a binder in the art may be used. The binder may be formed of one of the examples of the binder alone or of a plurality of different binders.
[0210] When the negative electrode active material layer 22 includes the binder, the negative electrode active material layer 22 is stabilized on the negative electrode collector 21. Moreover, despite the volume change and / or relative position change of the negative electrode active material layer 22 during charge / discharge, cracking of the negative electrode active material layer 22 can be suppressed. For example, when the negative electrode active material layer 22 does not include the binder, the negative electrode active material layer 22 can be easily separated from the negative electrode collector 21. When the negative electrode active material layer 22 is separated from the negative electrode collector 21, the possibility of short circuit occurrence can increase because the negative electrode collector 21 contacts the solid electrolyte layer 30 at the exposed portion of the negative electrode collector 21. The negative electrode active material layer 22 can be prepared by, for example, applying a slurry in which a material forming the negative electrode active material layer 22 is dispersed on the negative electrode collector 21 and drying. When the binder is included in the negative electrode active material layer 22, the negative electrode active material can be stably dispersed in the slurry. For example, when the slurry is coated on the negative electrode collector 21 by using a screen printing method, clogging of the screen (eg, clogging by aggregates of the negative electrode active material) may be suppressed.
[0211] The negative electrode active material layer 22 may further include additives used in all-solid secondary batteries such as a filler, a coating agent, a dispersant, and an ion conductive agent.
[0212] The thickness of the negative electrode active material layer 22 may be, for example, about 50% or less, about 40% or less, about 30% or less, about 20% or less, about 10% or less, or about 5% or less of the thickness of the positive electrode active material layer 12. For example, the thickness of the negative electrode active material layer 22 may be in the range of about 1 μm to about 20 μm, about 2 μm to about 10 μm, or about 3 μm to about 7 μm. When the thickness of the negative electrode active material layer 22 is too thin, lithium dendrites formed between the negative electrode active material layer 22 and the negative electrode current collector 21 destroy the negative electrode active material layer 22, and thus the cycle characteristics of the all-solid secondary battery 1 may be difficult to improve. When the thickness of the negative electrode active material layer 22 is too thick, the energy density of the all-solid secondary battery 1 deteriorates, and the internal resistance of the all-solid secondary battery 1 caused by the negative electrode active material layer 22 increases, and thus the cycle characteristics of the all-solid secondary battery 1 may be difficult to improve.
[0213] For example, when the thickness of the negative active material layer 22 decreases, the charge (charging) capacity of the negative active material layer 22 decreases. The charge capacity of the negative active material layer 22 may be, for example, about 50% or less, about 40% or less, about 30% or less, about 20% or less, about 10% or less, about 5% or less, or about 2% or less of the charge capacity of the positive active material layer 12. The charge capacity of the negative active material layer 22 may be, for example, in the range of about 0.1% to about 50%, about 0.1% to about 40%, about 0.1% to about 30%, about 0.1% to about 20%, about 0.1% to about 10%, about 0.1% to about 5%, or about 0.1% to about 2% of the charge capacity of the positive active material layer 12. When the charge capacity of the negative electrode active material layer 22 is too low, the thickness of the negative electrode active material layer 22 is too thin, lithium dendrites formed between the negative electrode active material layer 22 and the negative electrode current collector 21 during repeated charge / discharge processes destroy the negative electrode active material layer 22, and thus the cycle characteristics of the all-solid secondary battery 1 may not be improved. When the charge capacity of the negative electrode active material layer 22 is too high, the energy density of the all-solid secondary battery 1 deteriorates and the internal resistance of the all-solid secondary battery 1 caused by the negative electrode active material layer 22 increases, and thus the cycle characteristics of the all-solid secondary battery 1 may not be improved.
[0214] The charge capacity of the positive electrode active material layer 12 is obtained by multiplying the weight of the positive electrode active material in the positive electrode active material layer 12 by the specific charge capacity (milliampere hour / gram; mAh / g) of the positive electrode active material. When multiple types of materials are used as the positive electrode active material, the values of the specific charge capacity x weight of each of the positive electrode active materials are calculated, and the sum of these values is the charge capacity of the positive electrode active material layer 12. The charge capacity of the negative electrode active material layer 22 can be calculated in the same manner. That is, the charge capacity of the negative electrode active material layer 22 is obtained by multiplying the weight of the negative electrode active material in the negative electrode active material layer 22 by the specific charge capacity (mAh / g) of the negative electrode active material. When multiple types of materials are used as the negative electrode active material, the values of the specific charge capacity x weight of each of the negative electrode active materials are calculated, and the sum of these values is the charge capacity of the negative electrode active material layer 22. Here, the specific charge capacity of the positive electrode active material and the negative electrode active material is a capacity estimated by using an all-solid half-cell in which lithium metal is used as a reference electrode. The specific charge capacity of the positive active material layer 12 and the negative active material layer 22 is directly measured by measuring the charge (charging) capacity using an all-solid half-cell. When the measured charge capacity is divided by the weight of each of the active materials, the specific charge capacity can be obtained. In some embodiments, the charge capacity of the positive active material layer 12 and the negative active material layer 22 may be the initial charge capacity measured in the first charging cycle.
[0215] Reference Figure 4 , the all-solid secondary battery 1a may further include, for example, a metal layer 23 disposed between the negative electrode current collector 21 and the negative electrode active material layer 22. The metal layer 23 may include lithium or a lithium alloy. Therefore, the metal layer 23 may, for example, act as a lithium reservoir. Examples of the lithium alloy may include Li-Al alloys, Li-Sn alloys, Li-In alloys, Li-Ag alloys, Li-Au alloys, Li-Zn alloys, Li-Ge alloys, or Li-Si alloys, but embodiments are not limited thereto, and any suitable material that can be used as a lithium alloy in the art may be used. The metal layer 23 may include one of these alloys or lithium or may be formed of a lithium alloy.
[0216] The thickness of the metal layer 23 may be, for example, in the range of about 1 μm to about 1000 μm, about 1 μm to about 500 μm, about 1 μm to about 200 μm, about 1 μm to about 150 μm, about 1 μm to about 100 μm, or about 1 μm to about 50 μm, but embodiments are not limited thereto. When the thickness of the metal layer 23 is too thin, the metal layer 23 may be difficult to act as a lithium reservoir. When the thickness of the metal layer 23 is too thick, the weight and volume of the all-solid secondary battery 1a increase and the cycle characteristics may deteriorate. The metal layer 23 may be, for example, a metal foil having a thickness within these ranges.
[0217] In the all-solid secondary battery 1a, the metal layer 23 may be disposed between the negative electrode current collector 21 and the negative electrode active material layer 22 before assembling the all-solid secondary battery 1a, or may be deposited between the negative electrode current collector 21 and the negative electrode active material layer 22 after assembling the all-solid secondary battery 1a. When the metal layer 23 is disposed between the negative electrode current collector 21 and the negative electrode active material layer 22 before assembling the all-solid secondary battery 1a, the metal layer 23 includes lithium and thus can act as a lithium reservoir. For example, a lithium foil is disposed between the negative electrode current collector 21 and the negative electrode active material layer 22 before assembling the all-solid secondary battery 1a. In this regard, the cycle characteristics of the all-solid secondary battery 1a including the metal layer 23 can be further improved. When the metal layer 23 is deposited by charging after assembling the all-solid secondary battery 1a, the energy density of the all-solid secondary battery 1a is increased because the metal layer 23 is not included during assembling the all-solid secondary battery 1a. For example, the all-solid secondary battery 1a can be charged to exceed the charge capacity of the negative electrode active material layer 22. That is, the negative electrode active material layer 22 is overcharged. At the start of charging, lithium is absorbed in the negative electrode active material layer 22. The negative electrode active material in the negative electrode active material layer 22 may form an alloy or a compound with lithium ions migrated from the positive electrode layer 10.
[0218] When the negative electrode active material layer is charged beyond its capacity, for example, lithium is deposited on the back side of the negative electrode active material layer 22 between the negative electrode current collector 21 and the negative electrode active material layer 22, and a metal layer corresponding to the metal layer 23 can be formed by the deposited lithium. The metal layer 23 is a metal layer mainly formed of lithium (ie, metallic lithium). This is due to, for example, the following: the negative electrode active material in the negative electrode active material layer 22 is formed of a material capable of forming an alloy or compound with lithium. During discharge, the lithium of the negative electrode active material layer 22 and the lithium of the metal layer 23 are ionized and migrate in a direction toward the positive electrode layer 10. Therefore, lithium can be used as a negative electrode active material in the all-solid secondary battery 1a. Moreover, since the negative electrode active material layer 22 covers the metal layer 23, the negative electrode active material layer 22 acts as a protective layer for the metal layer 23 and simultaneously suppresses the deposition and growth of lithium dendrites. Therefore, the short circuit and capacity deterioration of the all-solid secondary battery 1a can be suppressed, and as a result, the cycle characteristics of the all-solid secondary battery 1a can be improved. Moreover, when the metal layer 23 is formed by charging after assembling the all-solid secondary battery 1a, in the initial state or the discharged state of the all-solid secondary battery 1a, the negative electrode collector 21, the negative electrode active material layer 22, and the area therebetween are, for example, Li-free areas that do not include lithium.
[0219] The negative electrode current collector 21 may be formed of, for example, a material that does not react with lithium, i.e., does not form both an alloy and a compound. Examples of materials forming the negative electrode current collector 21 may include copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), or nickel (Ni), but the embodiment is not limited thereto, and any suitable material that can be used as an electrode current collector in the art may be used. The negative electrode current collector 21 may be formed of one of the examples of the metal or of an alloy or a covering material of at least two metals. The negative electrode current collector 21 may be, for example, in the form of a plate or foil.
[0220] The all-solid secondary battery 1 may further include, for example, a thin film including an element that can be alloyed with lithium on the negative electrode current collector 21. The thin film is disposed between the negative electrode current collector 21 and the negative electrode active material layer 22. The thin film includes, for example, an element that can be alloyed with lithium. Examples of the element that can be alloyed with lithium may include gold, silver, zinc, tin, indium, silicon, aluminum, or bismuth, but the embodiment is not limited thereto, and any suitable element that can be alloyed with lithium in the art may be used. The thin film is formed of an alloy of any one or more of these metals. When the thin film is disposed on the negative electrode current collector 21, for example, the metal layer 23 in the form of a deposition deposited between the thin film and the negative electrode active material layer 22 can be further flattened, and thus the cycle characteristics of the all-solid secondary battery 1 can be further improved.
[0221] The thickness of the film may be, for example, in the range of about 1nm-about 800nm, about 10nm-about 700nm, about 50nm-about 600nm, or about 100nm-about 500nm. When the thickness of the film is less than 1nm, the function of the film may not be present. When the thickness of the film is too thick, the film itself absorbs lithium, and the amount of lithium deposited in the negative electrode may be reduced, which leads to the deterioration of the energy density of the all-solid battery, and therefore the cycle characteristics of the all-solid secondary battery 1 may be deteriorated. The film may be arranged on the negative electrode current collector 21 using, for example, vacuum vapor deposition, sputtering, or plating, but the embodiment is not limited thereto, and any method capable of forming a film in the art may be used.
[0222] According to another embodiment, a method for preparing a solid ion conductor compound may include: mixing a compound containing lithium, a compound containing a metal element selected from Groups 1 to 15 of the periodic table other than Li, a compound containing phosphorus (P), a compound containing SO n (wherein 1.5≤n≤5) and a compound containing a Group 17 element to prepare a mixture; and heat-treating the mixture in an inert atmosphere to prepare a solid ion conductor compound. The solid ion conductor compound may be, for example, a solid ion conductor compound represented by Formula 1.
[0223] The compound containing lithium may include a sulfide containing lithium. For example, lithium sulfide is prepared.
[0224] The compound containing a metal element selected from Groups 1 to 15 of the periodic table except Li includes a sulfide containing an element selected from Groups 1 to 15 of the periodic table except Li. Examples of the sulfide may include copper sulfide, silver sulfide, sodium sulfide (Na 2 S), magnesium sulfide, and potassium sulfide (K 2 S).
[0225] The compound containing phosphorus (P) includes a sulfide containing phosphorus. Examples of the sulfide containing phosphorus may include P 2 S 5 A compound containing sulfur (S) may be further added to the mixture.
[0226] The SO n Examples of compounds (wherein 1.5≤n≤5) include SO n The lithium salt containing SO n Examples of compounds (wherein 1.5≤n≤5) may include Li 2 S 4 O 6 , Li 2 S 3 O 6, Li 2 S 2 O 3 , Li 2 S 2 O 4 , Li 2 S 2 O 5 , Li 2 S 2 O 6 , Li 2 S 2 O 7 , Li 2 S 2 O 8 , Li 2 SO 4 , and Li 2 SO 5 .
[0227] Examples of the compound including the Group 17 element may include a lithium salt including the Group 17 element. Examples of the lithium salt including the Group 17 element may include LiCl, LiF, LiBr, or LiI.
[0228] The compound can be prepared by contacting the starting materials in suitable amounts, such as stoichiometric amounts, to form a mixture and heat treating the mixture. The contacting may include, for example, grinding, such as ball milling, or pulverizing.
[0229] A mixture of precursors mixed in stoichiometric composition may be heat treated in an inert atmosphere to prepare a solid ion conductor compound.
[0230] The heat treatment may be performed at a temperature in the range of, for example, about 400°C to about 700°C, about 400°C to about 650°C, about 400°C to about 600°C, about 400°C to about 550°C, or about 400°C to about 500°C. The heat treatment may be performed, for example, at about 1 hour to about 36 hours, about 2 hours to about 30 hours, about 4 hours to about 24 hours, about 10 hours to about 24 hours, or about 16 hours to about 24 hours. The inert atmosphere is an atmosphere including an inert gas. Examples of the inert gas may include nitrogen and argon, but embodiments are not limited thereto, and any gas that can be used as an inert gas in the art may be used.
[0231] One or more embodiments will now be described in more detail with reference to the following examples and comparative examples. However, these examples are for illustrative purposes only and are not intended to limit the scope of one or more embodiments.
[0232] Example
[0233] Preparation of solid ion conductor compounds
[0234] Embodiment 1: (Li 5.69 Cu 0.06 )P(S 4.70 (SO 4 ) 0.05 )Cl 1.25 Preparation
[0235] In a glove box with Ar atmosphere, Li 2 S, P as a phosphorus (P) precursor 2 S 5 , LiCl as a chlorine (Cl) precursor, Cu as a copper (Cu) precursor 2 S, and as SO 4 Precursor Li 2 SO 4 To obtain (Li 5.69 Cu 0.06 )P(S 4.70 (SO 4 ) 0.05 )Cl 1.25 The stoichiometric ratio of the desired composition is mixed, and the resultant is crushed and mixed at 100 rpm in an Ar atmosphere in a planetary ball mill including zirconium oxide (YSZ) balls for 1 hour, and then crushed and mixed at 800 rpm for 30 minutes to obtain a mixture. The obtained mixture is pressed by uniaxial pressure to prepare a disc having a thickness of about 10 mm and a diameter of about 13 mm. The disc thus obtained is coated with a gold film and placed in a carbon furnace, and the carbon furnace is vacuum sealed by using a quartz glass tube. The temperature of the vacuum-sealed disc is increased from room temperature to 500°C at a rate of 1.0°C / minute (°C / min) using an electric furnace, heat treated at 500°C for 12 hours, and then cooled to room temperature at a rate of 1.0°C / min to prepare a solid ion conductor compound.
[0236] The composition of the solid ion conductor compound prepared in this way is (Li 5.69 Cu 0.06 )P(S 4.70 (SO 4 ) 0.05 )Cl 1.25 (where the ratio of the substituted cation (Cu) is 0.01, and the substituted anion (SO 4 ) is 0.01).
[0237] Example 2: ((Li 5.69+b Cu 0.06 )P(S 4.75+b-a (SO 4 ) a )(Cl 1.25-b (SO4 ) b ),(SO 4 ) a+b =(SO 4 ) 0.15 ,(where 0.05 < a < 0.15, 0 < b < 0.15, and a + b = 0.15)) preparation
[0238] The solid ion conductor compound was prepared in the same manner as in Example 1, except as follows: The stoichiometric ratio of the starting materials was changed to satisfy (Li 5.69+b Cu 0.06 )P(S 4.75+b-a (SO 4 ) a )(Cl 1.25-b (SO 4 ) b ) composition.
[0239] As Figure 1B shown, since some of the Cl in the composition re-precipitated in the form of LiCl, a solid ion conductor compound with the following composition was obtained.
[0240] The composition of the obtained solid ion conductor compound is (Li 5.69+b Cu 0.06 )P(S 4.75+b-a (SO 4 ) a )(Cl 1.25-b (SO 4 ) b ),(SO 4 ) a+b =(SO 4 ) 0.15 ,(0.05 < a < 0.15, 0 < b < 0.15, a + b = 0.15).
[0241] Example 3: (Li 5.72 Cu 0.03 )P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 preparation
[0242] The solid ion conductor compound was prepared in the same manner as in Example 1, except as follows: The stoichiometric ratio of the starting materials was changed to satisfy (Li 5.72 Cu 0.03 )P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 desired composition.
[0243] The composition of the solid ion conductor compound is (Li 5.72 Cu 0.03 )PS 4.725 (SO 4 ) 0.025 Cl 1.25 (where the ratio of the substituted cation (Cu) is 0.005 and the substituted anion (SO 4 ) is 0.005).
[0244] Embodiment 4: (Li 5.72 Na 0.03 )P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 Preparation
[0245] A solid ion conductor compound was prepared in the same manner as in Example 1, except that Na was used as a sodium (Na) precursor. 2 S replaces the copper precursor and changes the stoichiometric ratio of the starting materials to meet (Li 5.72 Na 0.03 )P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 expected composition.
[0246] The composition of the solid ion conductor compound is (Li 5.72 Na 0.03 )P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 (where the ratio of the substituted cation (Na) is 0.005 and the substituted anion (SO 4 ) is 0.005).
[0247] Example 5: Li 5.75 P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 Preparation
[0248] A solid ion conductor compound was prepared in the same manner as in Example 1, except that: 2 S, the stoichiometric ratio of the starting materials was changed to meet the requirements of Li 5.75 P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 expected composition.
[0249] The solid ion conductor compound is composed of Li 5.75 P(S 4.725 (SO 4 ) 0.025 )Cl 1.25 (where the substituted anion (SO 4 ) is 0.005).
[0250] Comparative Example 1: Li 5.75 PS 4.75 Cl 1.25 Preparation
[0251] A solid ion conductor compound was prepared in the same manner as in Example 1, except that: 2 S and Li 2 SO 4 In the case of changing the stoichiometric ratio of the starting materials to meet the requirements of Li 5.75 PS 4.75 Cl 1.25 expected composition.
[0252] The solid ion conductor compound is composed of Li 5.75 PS 4.75 Cl 1.25 .
[0253] Comparative Example 2: Li 5.75 P(S 4.72 O 0.03 )Cl 1.25 Preparation
[0254] A solid ion conductor compound was prepared in the same manner as in Example 1, except that Li 2 O, and without adding Cu 2 S and Li 2 SO 4 In the case of changing the stoichiometric ratio of the starting materials to meet the requirements of Li 5.75 P(S 4.72 O 0.03 )Cl 1.25 expected composition.
[0255] The solid ion conductor compound is composed of Li 5.75 P(S 4.72 O 0.03 )Cl 1.25 (wherein the ratio of substituted anions (O) is 0.006).
[0256] Reference Example 1: (Li 5.69 Cu 0.06 )PS 4.75 Cl1.25 Preparation
[0257] A solid ion conductor compound was prepared in the same manner as in Example 1, except that: 2 SO 4 In the case of changing the stoichiometric ratio of the starting materials to meet (Li 5.69 Cu 0.06 )PS 4.75 Cl 1.25 expected composition.
[0258] The composition of the solid ion conductor compound is (Li 5.69 Cu 0.06 )PS 4.75 Cl 1.25 (wherein the ratio of the substituted cation (Cu) is 0.01).
[0259] Reference Example 2: (Li 5.72 Cu 0.03 )PS 4.75 Cl 1.25 Preparation
[0260] A solid ion conductor compound was prepared in the same manner as in Example 1, except that: 2 SO 4 In the case of changing the stoichiometric ratio of the starting materials to meet (Li 5.72 Cu 0.03 )PS 4.75 Cl 1.25 expected composition.
[0261] The composition of the solid ion conductor compound is (Li 5.72 Cu 0.03 )PS 4.75 Cl 1.25 (wherein the ratio of the substituted cation (Cu) is 0.005).
[0262] Example 6: Preparation of all-solid secondary battery
[0263] Preparation of positive electrode layer
[0264] Preparation of LiNi 0.8 Co 0.15 Al 0.05 O 2 (NCA) was used as a positive electrode active material. The sulfide-based solid electrolyte powder obtained in Example 1 was prepared as a solid electrolyte. Nanofibers (CNF) were prepared as a conductive agent. These materials were mixed in a weight ratio of 60:35:5 = positive electrode active material: solid electrolyte: conductive agent to prepare a positive electrode mixture.
[0265] Preparation of solid electrolyte powder
[0266] The sulfide-based solid ion conductor compound prepared in Example 1 was pulverized by using an agate mortar to prepare a solid electrolyte powder.
[0267] Preparation of negative electrode layer
[0268] A metal lithium foil having a thickness of 30 μm was prepared as a negative electrode.
[0269] Preparation of all-solid-state secondary batteries
[0270] The negative electrode layer, 150 mg of the solid electrolyte powder, and 15 mg of the positive electrode mixture were sequentially stacked on the SUS lower electrode in the order stated, and a SUS upper electrode was placed on the positive electrode mixture to prepare a stack. Then, the stack was heated at 4 tons / cm 2 The stack was pressed at a pressure of 200 N·m for 2 minutes. Subsequently, the pressed stack was pressed at a torque of 4 N·m by using a torque wrench to prepare an all-solid secondary battery.
[0271] Examples 7-10
[0272] An all-solid secondary battery was prepared in the same manner as in Example 6, except that the solid electrolyte powders prepared in Examples 2 to 5 were each used instead of the solid electrolyte powder prepared in Example 1.
[0273] Comparative Example 3
[0274] An all-solid secondary battery was prepared in the same manner as in Example 6, except that the solid electrolyte powder prepared in Comparative Example 1 was used instead of the solid electrolyte powder prepared in Example 1.
[0275] Evaluation Example 1: X-ray diffraction test
[0276] The solid ion conductor compounds prepared in Examples 1 to 5 and Reference Examples 1 and 2 were pulverized by using an agate mortar to prepare powders, and the powder XRD of each of the powders was measured and a part of the results is shown in FIG. Figures 1A-1C CuKα radiation was used in the XRD measurement. It was confirmed that the solid ion conductor compounds of Examples 1 to 5 and Reference Example 1 belonged to the F-43m space group, had a structure belonging to the cubic system, and were argyrodite-type sulfides having an argyrodite-type crystal structure. Figure 1B for Figure 1A an enlarged view of a portion of Figure 1C for Figure 1B : is an enlarged view of a portion of and is a view in which the positions of the peaks of the solid ion conductor compounds of Example 2 and Reference Example 1 are compared.
[0277] exist Figure 1A and 1B The solid ion conductor compound of Example 2 has a peak corresponding to the LiCl phase at a diffraction angle 2θ of 35°. Furthermore, no peaks due to the inclusion of SO 4 Peaks caused by impurities.
[0278] Therefore, the peak due to the LiCl phase is considered to be a peak due to some of the Cl reprecipitated in the form of LiCl as follows: In addition to the tetrahedral PS in the argyrodite type crystal structure 4 In addition to the P(4b) site and S(16c) site of the group, in the solid ion conductor compound of Example 2, SO 4 Therefore, it is confirmed that the S(4c) site and / or the Cl(4a) site in the solid ion conductor compound of Example 2 is replaced by SO 4 A Cl(4a) site is a site where S is present prior to substitution by Cl.
[0279] like Figure 1C As shown in , the solid ion conductor compound of Example 2 has a first peak at a diffraction angle of 30.14° 2θ and a second peak at a diffraction angle of 31.52° 2θ.
[0280] Moreover, if Figure 1C As shown in FIG. 1 , the solid ion conductor compound of Reference Example 1 (having the same composition as the solid ion conductor compound of Example 2, except that SO 4 The solid ion conductor compound of Example 2 has a third peak at a diffraction angle of 30.18°2θ and a fourth peak at a diffraction angle of 31.56°2θ. Therefore, it is confirmed that the first peak and the second peak of the solid ion conductor compound of Example 2 are shifted downward by 0.04° toward a lower angle compared to the third peak and the fourth peak of the solid conductor compound of Reference Example 1.
[0281] The downward shift is considered to be caused by the following: some of the S in the solid ion conductor compound of Example 2 is replaced by SO having an ion diameter larger than that of S. 4 Instead, the distance between adjacent faces of the lattice (eg, the d-spacing) increases.
[0282] Evaluation Example 2: Ion conductivity measurement
[0283] The solid ion conductor compounds prepared in Examples 1 to 5 and Comparative Examples 1 and 2 were pulverized by using an agate mortar to prepare powders, and 200 mg of each powder was pulverized at 4 tons / cm 2The wafer was pressed at a pressure of 200 μm for 2 minutes to prepare a disc sample having a thickness of about 100 μm and a diameter of about 13 mm. An indium (In) electrode having a thickness of about 50 μm and a diameter of about 13 mm was disposed on each of the two surfaces of the disc sample to prepare a symmetrical unit cell. The preparation of the symmetrical unit cell was carried out in a glove box with an Ar atmosphere.
[0284] For a sample having indium electrodes on both surfaces thereof, the impedance of the disc was measured by a 2-probe method using an impedance analyzer (Material Mates 7260 impedance analyzer). The frequency range was in the range of about 0.1 Hz to about 1 MHz, and the amplitude voltage was about 10 mV. The measurement was performed in an Ar atmosphere at about 25° C. The ionic conductivity was calculated as follows: the resistance was obtained from the arc of the Nyquist plot on the impedance measurement result, and the area and thickness of the sample were taken into account.
[0285] The results are shown in Table 1.
[0286] Table 1
[0287] Room temperature (25°C) ionic conductivity [mS / cm] Example 1 4.2 Example 2 2.3 Example 3 2.8 Example 4 3.2 Example 5 3.7 Comparative Example 1 2.2 Comparative Example 2 2.8
[0288] As shown in Table 1, the solid ion conductor compounds of Examples 1 to 5 have high ion conductivity of about 2.3 mS / cm or more at room temperature.
[0289] Compared to the ionic conductivity of the solid ionic conductor compound of Comparative Example 1, the solid ionic conductor compounds of Examples 1 to 5 have improved ionic conductivity.
[0290] having a composition corresponding to that of the solid ion conductor compound of Example 5 and wherein O is substituted for SO 4 The solid ion conductor compound of Example 5 has improved ion conductivity compared to the solid ion conductor compound of Comparative Example 2. It is believed that the improved ion conductivity is provided as follows: due to the substitution of oxygen ions (O 2- , 0.140 nm) compared to the sulfate ion (SO 4 2- , ionic radius of 0.147nm), the crystal structure is distorted.
[0291] The ionic conductivity of the solid ion conductor compound of Example 2 is lower than that of the solid ion conductor of Comparative Example 2, but the lowered ionic conductivity is believed to be due to the addition of SO 4 For example, with low Cu and SO 4The solid ion conductor compounds of Examples 1 and 3 having a content of 200 Å and 80 Å have ion conductivities equal to or higher than that of the solid ion conductor compound of Comparative Example 2.
[0292] Evaluation Example 3: Atmospheric Stability Evaluation
[0293] The solid ion conductor compounds prepared in Examples 1 and 2 and Comparative Example 1 were pulverized using an agate mortar to prepare powders, and the powders were stored in a drying chamber with an air atmosphere having a dew point of less than -60°C for 10 days. The powders were removed from the drying chamber, and the changes in the ionic conductivity of each of the powders were measured. The changes in ionic conductivity were calculated by using the ionic conductivity retention of Equation 1. The results of the measurements are shown in Table 2. The initial ionic conductivity is the ionic conductivity of the powder before storage in the drying chamber. The ionic conductivity measurement was performed in the same manner as in Evaluation Example 2.
[0294] Equation 1
[0295] Ion conductivity retention = [Ion conductivity of solid ion conductor compound after 10 days / initial ion conductivity of solid ion conductor compound] × 100%
[0296] Table 2
[0297] Ion conductivity retention [%] Example 1 81.2 Example 2 83.2 Comparative Example 1 65.6
[0298] As shown in Table 2, the solid ion conductor compounds of Examples 1 and 2 have improved ion conductivity retention compared to that of the solid ion conductor compound of Comparative Example 1.
[0299] The solid ion conductor compounds of Examples 1 and 2 have improved atmospheric stability or oxidative stability compared to the atmospheric stability or oxidative stability of the solid ion conductor compound of Comparative Example 1. Evaluation Example 4: Charge / Discharge Test and Interface Stability Evaluation
[0300] The charge / discharge characteristics of the all-solid secondary batteries prepared in Examples 6 and 7 and Comparative Example 3 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid secondary batteries in a chamber at 45°C.
[0301] In the first cycle, the battery was charged with a constant current of 0.1 C until the battery voltage reached 4.25 V, and then charged with a constant voltage of 4.25 V until the current reached 0.05 C. Then, the battery was discharged with a constant current of 0.1 C until the battery voltage reached 2.5 V.
[0302] The discharge capacity at the first cycle was used as the standard capacity.
[0303] The C rate refers to the current that discharges the battery in 1 hour, for example, a battery with a discharge capacity of 1.6 ampere hours would have a C rate of 1.6 amperes.
[0304] In the second cycle, the battery was charged with a constant current of 0.1 C until the battery voltage reached 4.25 V, and then charged for 50 hours at a constant voltage of 4.25 V. Then, the battery was discharged with a constant current of 0.1 C until the battery voltage reached 2.5 V. The constant voltage charging step corresponds to the step of storage at high temperature.
[0305] The discharge capacity at the second cycle was used as the retention capacity.
[0306] In the third cycle, the battery was charged with a constant current of 0.1 C until the battery voltage reached 4.25 V, and then charged with a constant voltage of 4.25 V until the current reached 0.05 C. Then, the battery was discharged with a constant current of 0.1 C until the battery voltage reached 2.5 V.
[0307] The discharge capacity of the 3rd cycle was used as the recovery capacity. A dwell time of 10 minutes was set after each charge / discharge cycle.
[0308] The capacity recovery and capacity retention of the all-solid secondary batteries prepared in Examples 6 and 7 and Comparative Example 3 after storage at high temperature are shown in Table 3.
[0309] The capacity retention and capacity recovery after storage at high temperature are defined as shown in Equations 2 and 3.
[0310] Equation 2
[0311] Capacity retention (%) = [retention capacity / standard capacity] × 100%
[0312] Equation 3
[0313] Capacity recovery (%) = [recovery capacity / standard capacity] × 100%
[0314] Table 3
[0315] Capacity retention [%] Capacity recovery [%] Example 6 91.4 80.7 Example 7 88.8 73.1 Comparative Example 3 86.9 69.7
[0316] As shown in Table 3, the all-solid secondary batteries of Examples 6 and 7 had improved capacity retention after storing the battery at high temperature for a long time in a charged state and improved capacity recovery compared with those of the all-solid secondary battery of Comparative Example 3.
[0317] Compared to the all-solid secondary battery of Comparative Example 3, the all-solid secondary batteries of Examples 6 and 7 have improved stability (eg, oxidation resistance) with respect to lithium metal.
[0318] As described above, according to one or more embodiments, an electrochemical battery having improved stability and cycle characteristics may be provided by including a solid ion conductor compound having improved lithium ion conductivity and stability relative to lithium metal.
[0319] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for limiting purposes. The description of features or aspects in each embodiment should be considered to be applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the accompanying drawings, it will be understood by those of ordinary skill in the art that various changes in form and detail may be made therein without departing from the spirit and scope as defined by the appended claims.
Claims
1. A compound represented by Formula 1 and having a stannite-type crystal structure: Formula 1 <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> M1<h2 style=";text-align:left;direction:ltr"> v <h2 style=";text-align:left;direction:ltr"> PS<h2 style=";text-align:left;direction:ltr"> y <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> w <h2 style=";text-align:left;direction:ltr"> M3<h2 style=";text-align:left;direction:ltr"> z in, In Formula 1, M1 is at least one metal element of Groups 1 to 15 of the periodic table other than Li, M2 is SO n , M3 is at least one element of Group 17 of the periodic table, and 4 ≤ x ≤ 8, 0 ≤ v < 1, 3 ≤ y ≤ 7, 0 < w < 2, 0 ≤ z ≤ 2, and 1.5 ≤ n ≤ 5, M2 is substituted at the S site.
2. The compound according to claim 1, wherein 0 ≤ v / (x + v) < 0.2 and 0 < w / (y + w) < 0.
2.
3. The compound as claimed in claim 1, wherein SO n It is S4O6, S3O6, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, SO4, SO5, or a combination thereof.
4. The compound according to claim 1, wherein 0 ≤ v / (x + v) < 0.08 and 0 < w / (y + w) < 0.
08.
5. The compound according to claim 1, wherein M1 includes Na, K, Mg, Ag, Cu, Hf, In, Ti, Pb, Sb, Fe, Zr, Zn, Cr, B, Sn, Ge, Si, Ta, Nb, V, Ga, Al, As, or a combination thereof.
6. The compound according to claim 1, wherein M1 includes Na, K, Mg, Ag, Cu, or a combination thereof.
7. The compound according to claim 1, wherein M3 includes F, Cl, Br, I, or a combination thereof.
8. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by Formula 2: Formula 2 <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 7-m×v-z <h2 style=";text-align:left;direction:ltr"> M1<h2 style=";text-align:left;direction:ltr"> v <h2 style=";text-align:left;direction:ltr"> PS<h2 style=";text-align:left;direction:ltr"> 6-w-z <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> w <h2 style=";text-align:left;direction:ltr"> M3<h2 style=";text-align:left;direction:ltr"> z in, In Formula 2, M1 is at least one metal element of Groups 1-15 of the periodic table other than Li, and m is the oxidation number of M1, M2 is SO n , M3 is at least one element of Group 17 of the periodic table, and 0 ≤ v < 1, 0 < w < 2, 0 ≤ z ≤ 2, 1.5 ≤ n ≤ 5, and 1 ≤ m ≤ 2.
9. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by one of Formula 3 or Formula 4: Formula 3 <h2 style=";text-align:left;direction:ltr">(Li<h2 style=";text-align:left;direction:ltr"> 1-d <h2 style=";text-align:left;direction:ltr"> M1<h2 style=";text-align:left;direction:ltr"> d <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> P(S<h2 style=";text-align:left;direction:ltr"> 1-e <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> e <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> M3<h2 style=";text-align:left;direction:ltr"> c Formula 4 <h2 style=";text-align:left;direction:ltr">(Li<h2 style=";text-align:left;direction:ltr"> 1-d <h2 style=";text-align:left;direction:ltr"> M1<h2 style=";text-align:left;direction:ltr"> d <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> Li<h2 style=";text-align:left;direction:ltr"> fc <h2 style=";text-align:left;direction:ltr"> P(S<h2 style=";text-align:left;direction:ltr"> 1+fc-e <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> e <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> (M3<h2 style=";text-align:left;direction:ltr"> 1-f <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> f <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> c in, In Formulas 3 and 4, M1 is Na, K, Mg, Ag, Cu, Hf, In, Ti, Pb, Sb, Fe, Zr, Zn, Cr, B, Sn, Ge, Si, Ta, Nb, V, Ga, Al, As, or a combination thereof, M2 is SO4, M3 is at least one element of Group 17 of the periodic table; 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2, and 0 < d ≤ 0.08, 0 < e ≤ 0.08, 0 < f ≤ 0.08, and 0 < e + f ≤ 0.
08.
10. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by Formula 5 or Formula 6, Formula 5 (Li 1-d M1 d ) a P(S 1-e (SO4) e ) b M3 c ,or Formula 6 (Li 1-d M1 d ) a Li fc P(S 1+fc-e (SO4) e ) b (M3 1-f (SO4) f ) c , in, In Formulas 5 and 6, M1 is Na, K, Mg, Ag, Cu, or a combination thereof; M3 is at least one element of Group 17 of the periodic table; 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2, and 0 < d < 0.08, 0 < e < 0.08, 0 < f < 0.08, and 0 < e + f < 0.
08.
11. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by one of Formula 5a, Formula 5b, Formula 5c, Formula 5d, Formula 5e, Formula 6a, Formula 6b, Formula 6c, Formula 6d, or Formula 6e, Formula 5a (Li 1-d Na d ) a P(S 1-e (SO4) e ) b M3 c , Formula 5b (Li 1-d K d ) a P(S 1-e (SO4) e ) b M3 c , Formula 5c (Li 1-d Mg d ) a P(S 1-e (SO4) e ) b M3 c , Formula 5d <h2 style=";text-align:left;direction:ltr">(Li<h2 style=";text-align:left;direction:ltr"> 1-d <h2 style=";text-align:left;direction:ltr"> Ag<h2 style=";text-align:left;direction:ltr"> d <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> P(S<h2 style=";text-align:left;direction:ltr"> 1-e <h2 style=";text-align:left;direction:ltr"> (SO4)<h2 style=";text-align:left;direction:ltr"> e <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> M3<h2 style=";text-align:left;direction:ltr"> c <h2 style=";text-align:left;direction:ltr"> , Formula 5e (Li 1-d With d ) a P(S 1-e (SO4) e ) b M3 c , Formula 6a (Li 1-d Na d ) a Li fc P(S 1+fc-e (SO4) e ) b (M3 1-f (SO4) f ) c , Formula 6b (Li 1-d K d ) a Li fc P(S 1+fc-e (SO4) e ) b (M3 1-f (SO4) f ) c , Formula 6c (Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO4) e ) b (M3 1-f (SO4) f ) c , Formula 6d (Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO4) e ) b (M3 1-f (SO4) f ) c , or Formula 6e (Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO4) e ) b (M3 1-f (SO4) f ) c , in, In Formulas 5a, 5b, 5c, 5d, 5e, 6a, 6b, 6c, 6d, and 6e, each M3 is independently selected and is an element of Group 17 of the periodic table, a, b, and c are each independently selected, and 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2, and d, e, and f are each independently selected, and 0 < d ≤ 0.06, 0 < e ≤ 0.06, 0 < f ≤ 0.06, and 0 < e + f ≤ 0.
06.
12. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by: (Li 1-d With d ) a P(S 1-e (SO4) e ) b F c ,(Li 1-d With d ) a P(S 1-e (SO4) e ) b Cl c ,(Li 1-d With d ) a P(S 1-e (SO4) e ) b Br c ,(Li 1-d With d ) a P(S 1-e (SO4) e ) b and c , (Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO4) e ) b (F 1-f (SO4) f ) c ,(Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO4) e ) b (Cl 1-f (SO4) f ) c ,(Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO4) e ) b (Br 1-f (SO4) f ) c ,(Li 1-d Cu d ) a Li fc P(S 1+fc-e (SO4) e ) b (I 1-f (SO4) f ) c , (Li 1-d Na d ) a P(S 1-e (SO4) e ) b F c ,(Li 1-d Na d ) a P(S 1-e (SO4) e ) b Cl c ,(Li 1-d Na d ) a P(S 1-e (SO4) e ) b Br c ,(Li 1-d Na d ) a P(S 1-e (SO4) e ) b I c , (Li 1-d Na d ) a Li fc P(S 1+fc-e (SO4) e ) b (F 1-f (SO4) f ) c ,(Li 1-d Na d ) a Li fc P(S 1+fc-e (SO4) e ) b (Cl 1-f (SO4) f ) c ,(Li 1-d Na d ) a Li fc P(S 1+fc-e (SO4) e ) b (Br 1-f (SO4) f ) c ,(Li 1-d Na d ) a Li fc P(S 1+fc-e (SO4) e ) b (I 1-f (SO4) f ) c , (Li 1-d K d ) a P(S 1-e (SO4) e ) b F c ,(Li 1-d K d ) a P(S 1-e (SO4) e ) b Cl c ,(Li 1-d K d ) a P(S 1-e (SO4) e ) b Br c ,(Li 1-d K d ) a P(S 1-e (SO4) e ) b I c , (Li 1-d K d ) a Li fc P(S 1+fc-e (SO4) e ) b (F 1-f (SO4) f ) c ,(Li 1-d K d ) a Li fc P(S 1+fc-e (SO4) e ) b (Cl 1-f (SO4) f ) c ,(Li 1-d K d ) a Li fc P(S 1+fc-e (SO4) e ) b (Br 1-f (SO4) f ) c ,(Li 1-d K d ) a Li fc P(S 1+fc-e (SO4) e ) b (I 1-f (SO4) f ) c , (Li 1-d Mg d ) a P(S 1-e (SO4) e ) b F c ,(Li 1-d Mg d ) a P(S 1-e (SO4) e ) b Cl c ,(Li 1-d Mg d ) a P(S 1-e (SO4) e ) b Br c ,(Li 1-d Mg d ) a P(S 1-e (SO4) e ) b I c , (Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO4) e ) b (F 1-f (SO4) f ) c ,(Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO4) e ) b (Cl 1-f (SO4) f ) c ,(Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO4) e ) b (Br 1-f (SO4) f ) c ,(Li 1-d Mg d ) a Li fc P(S 1+fc-e (SO4) e ) b (I 1-f (SO4) f ) c , (Li 1-d Ag d ) a P(S 1-e (SO4) e ) b F c ,(Li 1-d Ag d ) a P(S 1-e (SO4) e ) b Cl c ,(Li 1-d Ag d ) a P(S 1-e (SO4) e ) b Br c ,(Li 1-d Ag d ) a P(S 1-e (SO4) e ) b I c , (Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO4) e ) b (F 1-f (SO4) f ) c ,(Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO4) e ) b (Cl 1-f (SO4) f ) c ,(Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO4) e ) b (Br 1-f (SO4) f ) c , or (Li 1-d Ag d ) a Li fc P(S 1+fc-e (SO4) e ) b (I 1-f (SO4) f ) c , in, each a, b, c, d, e, and f is independently selected, and 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, 0 ≤ c ≤ 2, 0 < d ≤ 0.06, 0 < e < 0.06, 0 < f < 0.06, and 0 < e + f < 0.
06.
13. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by Formula 7, Formula 7 <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 7-p×v-u-z <h2 style=";text-align:left;direction:ltr"> M4<h2 style=";text-align:left;direction:ltr"> v <h2 style=";text-align:left;direction:ltr"> M5<h2 style=";text-align:left;direction:ltr"> u <h2 style=";text-align:left;direction:ltr"> PS<h2 style=";text-align:left;direction:ltr"> 6-w-z <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> w <h2 style=";text-align:left;direction:ltr"> M3<h2 style=";text-align:left;direction:ltr"> z in, In Formula 7, M4 is at least one metal element of Groups 2-15 of the periodic table, and p is the oxidation number of M4; M5 is at least one metal element of Group 1 of the periodic table other than Li and is a monovalent cation, M2 is SO n , M3 is at least one element of Group 17 of the periodic table; and 0 ≤ v < 1, 0 ≤ u < 1, 0 < w < 2, 0 ≤ z ≤ 2, 1.5 ≤ n ≤ 5, and 1 ≤ p ≤ 2.
14. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by Formula 8: Formula 8 <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 7-z <h2 style=";text-align:left;direction:ltr"> PS<h2 style=";text-align:left;direction:ltr"> 6-w-z <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> w <h2 style=";text-align:left;direction:ltr"> M3<h2 style=";text-align:left;direction:ltr"> z in, In Formula 8, M2 is SO n , M3 is at least one element of Group 17 of the periodic table, and 0 < w < 2, 0 ≤ z ≤ 2, and 1.5 ≤ n ≤ 5.
15. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by Formula 9 or Formula 10: Formula 9 Li a+fc P(S 1+fc-e M2 e ) b (M3 1-f M2 f ) c or Formula 10 <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> a <h2 style=";text-align:left;direction:ltr"> P(S<h2 style=";text-align:left;direction:ltr"> 1-e <h2 style=";text-align:left;direction:ltr"> M2<h2 style=";text-align:left;direction:ltr"> e <h2 style=";text-align:left;direction:ltr"> )<h2 style=";text-align:left;direction:ltr"> b <h2 style=";text-align:left;direction:ltr"> M3<h2 style=";text-align:left;direction:ltr"> c <h2 style=";text-align:left;direction:ltr"> , in, In Formulas 9 and 10, M2 is SO4, M3 is an element of Group 17 of the periodic table, 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2, and 0 < e ≤ 0.08, 0 < f ≤ 0.08, and 0 < e + f ≤ 0.
08.
16. The compound according to claim 1, wherein the compound represented by Formula 1 is represented by Formula 11 or Formula 12, Formula 11 Li a+fc P(S 1+fc-e (SO4) e ) b (M3 1-f (SO4) f ) c ,or Formula 12 Li a P(S 1-e (SO4) e ) b M3 c , in, In Formulas 11 and 12, each M3 is independently selected and is an element of Group 17 of the periodic table, each a, b, and c is independently selected, and 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2, and each e and f is independently selected, and 0 < e < 0.08, 0 < f < 0.08, and 0 < e + f < 0.
08.
17. The compound as claimed in claim 1, wherein the compound represented by Formula 1 is Li a+fc P(S 1+fc-e (SO4) e ) b (F 1-f (SO4) f ) c , Li a+fc P(S 1+fc-e (SO4) e ) b (Cl 1-f (SO4) f ) c , Li a+fc P(S 1+fc-e (SO4) e ) b (Br 1-f (SO4) f ) c , Li a+fc P(S 1+fc-e (SO4) e ) b (I 1-f (SO4) f ) c , Li a P(S 1-e (SO4) e ) b F c , Li a P(S 1-e (SO4) e ) b Cl c , Li a P(S 1-e (SO4) e ) b Br c , or Li a P(S 1-e (SO4) e ) b I c , in, In the said formulas, 5 ≤ a ≤ 7, 4 ≤ b ≤ 6, and 0 ≤ c ≤ 2; and 0 < e < 0.06, 0 < f < 0.06, and 0 < e + f < 0.
06.
18. The compound according to claim 1, wherein the compound represented by Formula 1 has an ionic conductivity of 1 millisiemens / cm or greater at a temperature of 25°C.
19. The compound according to claim 1, wherein when analyzed after 10 days in an air atmosphere having a dew point below -60°C, the compound represented by Formula 1 has an ionic conductivity retention of 70% or greater, wherein the ionic conductivity retention is defined as shown in Equation 1: Equation 1 Ion conductivity retention = [ion conductivity of the compound after 10 days / initial ion conductivity of the compound] x 100%.
20. The compound as claimed in claim 1, wherein the compound represented by Formula 1 belongs to a cubic system.
21. The compound of claim 1, wherein the compound represented by Formula 1 belongs to the F-43m space group.
22. The compound of claim 1, wherein the compound represented by Formula 1 has a first peak at a diffraction angle of 30.1°2θ±0.5°2θ and a second peak at a diffraction angle of 31.5°2θ±0.5°2θ when analyzed by X-ray diffraction using CuKα radiation, and When analyzed by X-ray diffraction using CuKα radiation, the compound having the same composition as that of the compound represented by Formula 1 except that M2 is S has a third peak at a diffraction angle of 30.1°2θ±0.5°2θ and a fourth peak at a diffraction angle of 31.5°2θ±0.5°2θ, and The position of the first peak is at least 0.01° 2θ smaller than the position of the third peak, and the position of the second peak is at least 0.01° 2θ smaller than the position of the fourth peak.
23. The compound of claim 1, wherein the compound represented by Formula 1 further has a peak corresponding to LiM3 at a diffraction angle of 35.0°2θ±1.0°2θ when analyzed by X-ray diffraction using CuKα radiation.
24. A protected positive electrode active material comprising: Lithium transition metal oxides, lithium transition metal sulfides, transition metal sulfides, or combinations thereof; and The compound of any one of claims 1 to 23 on the surface of the lithium transition metal oxide, the transition metal sulfide or the lithium transition metal sulfide.
25. A solid electrolyte comprising the compound according to any one of claims 1 to 23.
26. An electrochemical cell comprising: a positive electrode layer including a positive electrode active material layer; a negative electrode layer including a negative electrode active material layer; as well as An electrolyte layer is provided between the positive electrode layer and the negative electrode layer, At least one of the positive electrode active material layer and the electrolyte layer comprises the compound according to any one of claims 1 to 23.
27. The electrochemical cell of claim 26, wherein the electrochemical cell is an all-solid secondary battery.
28. The electrochemical cell of claim 26, wherein the negative electrode active material layer comprises a negative electrode active material and a binder, wherein the negative electrode active material comprises amorphous carbon, and Au, Pt, Pd, Si, Ag, Al, Bi, Sn, Zn, or a combination thereof.
29. The electrochemical cell of claim 26, wherein the negative electrode layer further comprises a negative electrode current collector, and further comprises a metal layer between the negative electrode current collector and the negative electrode active material layer, wherein the metal layer comprises lithium or a lithium alloy.
30. A method for preparing a compound, the method comprising: The following materials were contacted to prepare a mixture: Compounds containing lithium, A compound containing a metal element of Group 1 to Group 15 of the periodic table other than Li, Compounds containing P, Contains SO n A compound wherein 1.5≤n≤5, and Optionally, a compound comprising an element from Group 17 of the Periodic Table; and The mixture is heat treated in an inert atmosphere to prepare a compound as claimed in any one of claims 1 to 23.
31. The method of claim 30, wherein the heat treatment comprises heat treatment at a temperature of 400°C to 600°C for 1 hour to 36 hours.
Citation Information
Patent Citations
Monitoring method for dressing process and polishing apparatus
KR1020190138765A
How to prevent shoulder belt slipping and slip prevention devices, shoulder belts and bags
KR1020200115523A
Cubic-phase sulfide and preparation method thereof
CN108238616A
Sulfide solid electrolyte based on oxygen doping and preparation method of sulfide solid electrolyt
CN108493479A
Lithium battery cathode with different sulfide type lithium ion conductors