Printed circuit board substrate comprising coated boron nitride
By using coated boron nitride particles and a reinforcing layer in the printed circuit board substrate, the problem of insufficient mechanical properties and adhesion of thermally conductive materials in the printed circuit board substrate is solved, achieving efficient heat dissipation and improved strength, making it suitable for high-frequency and miniaturized electronic devices.
Patent Information
- Application Number
- CN201980065052.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-10-02
- Filing Date
- 2019-10-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The addition of thermally conductive materials to existing printed circuit board substrates results in reduced mechanical properties and peel strength, especially during thermal aging, where effective heat dissipation and insufficient adhesion are difficult to achieve.
Coated boron nitride particles are used, and an atomic layer deposition technique is used to coat the surface of the boron nitride particles with a coating thickness of 0.1 nanometers to 100 nanometers to enhance the adhesion between the particles and the polymer matrix. Combined with a reinforcing layer and an appropriate amount of thermally stable fibers, a printed circuit board substrate is formed.
It significantly improves the Z-direction thermal conductivity and peel strength of printed circuit board substrates while maintaining good mechanical properties and thermal stability, making it suitable for higher frequency and smaller electronic devices.
Smart Images

Figure CN112806103B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Patent Application Serial No. 62 / 740,083, filed on October 2, 2018. The related application is incorporated herein by reference in its entirety. Background Art
[0003] Disclosed herein are printed circuit board substrates and methods for making the same.
[0004] The circuit designs of electronic devices such as televisions, radios, computers, medical instruments, business machines, communication equipment, etc. have become smaller and thinner. The increased power of such electronic components leads to increased heat generation. In addition, smaller electronic components are densely packed in smaller and smaller spaces, resulting in greater heat generation as hot spot temperatures increase. At the same time, temperature-sensitive components in electronic devices may need to be maintained within specified operating temperatures to avoid significant performance degradation or even system failure.
[0005] In this context, printed circuit board substrates have been developed to facilitate efficient heat dissipation. Typically, these printed circuit board substrates are based on composite materials, such as thermosetting polymers containing thermally conductive particles. For example, epoxy resins are some of the most widely used thermosetting polymers in the art due to their good adhesion properties and processability. However, epoxy resins themselves have relatively low thermal conductivity and therefore cannot effectively dissipate the heat generated in advanced microelectronic devices. Therefore, thermally conductive materials such as aluminum nitride (AlN), boron nitride (BN), aluminum oxide (Al2O3) or silicon carbide (SiC) are typically incorporated into polymers to achieve efficient heat dissipation.
[0006] While the addition of such thermally conductive materials has been shown to achieve an increase in thermal conductivity of various printed circuit board substrates, these filler materials typically experience at least one of reduced mechanical properties, reduced peel strength, or long term problems with thermal aging. It would be particularly advantageous to develop a printed circuit board substrate that could be easily processed, had improved mechanical / adhesive properties to current thermal interfaces, or provided improved heat transfer efficiency. Summary of the invention
[0007] Disclosed herein are printed circuit board substrates and methods for making the same.
[0008] In one embodiment, a printed circuit board substrate comprises a polymer matrix; a reinforcement layer; and a plurality of coated boron nitride particles; wherein the plurality of coated boron nitride particles comprises a coating having an average coating thickness of 0.1 nanometers to 100 nanometers.
[0009] The method of making a printed circuit board substrate includes: forming a mixture including a thermosetting composition and a plurality of coated boron nitride particles; and curing the thermosetting composition to form the printed circuit board substrate.
[0010] The above described and other features are exemplified by the following figures, detailed description, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] The following drawings are exemplary embodiments provided to illustrate the present disclosure. The drawings are illustrative of examples and are not intended to limit devices made according to the present disclosure to the materials, conditions, or process parameters set forth herein.
[0012] Figure 1 is a cross-sectional view of one embodiment of a circuit material including a printed circuit board substrate;
[0013] Figure 2 is a diagram of one embodiment of a method of preparing a printed circuit board substrate;
[0014] Figure 3 is a graphical illustration of aluminum concentration versus cycle number for Examples 1 to 6;
[0015] Figure 4 is a graphical illustration of the surface energy of Examples 1 to 6 as a function of cycle number; and
[0016] Figure 5 is a graphical illustration of the dielectric strength of Examples 9 and 11 over time. DETAILED DESCRIPTION
[0017] Although the addition of thermally conductive particles such as boron nitride to polymer composites has been shown to increase thermal conductivity, many of these thermally conductive particles have been shown to cause a significant decrease in copper peel strength with increasing filler loading. This decrease in copper peel strength with increasing filler loading occurs due to the extremely low surface energy of boron nitride, its relatively inert surface chemistry resulting in a lack of chemical bonding sites, and its smooth basal topography resulting in a significant lack of opportunity for chemical bonding or mechanical interlocking sites between the boron nitride and its surrounding matrix. In practice, these features combine to cause adhesion failure between the boron nitride particles and the polymer, which empirically results in the boron nitride acting as a void in the polymer composite.
[0018] It has been found that a printed circuit board substrate comprising a plurality of coated boron nitride particles having an average coating thickness of 0.1 nanometers (nm) to 100 nanometers can produce a printed circuit board substrate with improved peel strength. For example, the peel strength between the printed circuit board substrate and the conductive layer as measured by IPC-TM-650-2.4.8 can be greater than or equal to 3 pounds per linear inch (pli) [0.54 kilograms per linear centimeter (kg / cm)]. The printed circuit board substrate can unexpectedly maintain a minimum of 90%, or 90% to 99% of the Z-direction thermal conductivity compared to other similar printed circuit board substrates prepared from a plurality of boron nitride particles without a coating. "Z-direction thermal conductivity" refers to the thermal conductivity in a direction perpendicular to the plane of the dielectric substrate layer. The disclosed printed circuit board substrate can help overcome thermal management challenges in designing multilayer circuits dedicated to further component miniaturization and integration and higher operating frequencies. The Z-direction thermal conductivity as measured by ASTM D5470-17, TIM Tester 1300 may be at least 0.8 Watts per meter per Kelvin (W / mK). When measured according to ASTM D570-98 (2018), the water absorption of the printed circuit board may be less than or equal to 0.15 wt %, or 0.01 wt % to 0.1 wt %, based on the total weight of the sample.
[0019] Figure 1 4 is a cross-sectional view of a circuit material 40 including a printed circuit board substrate 12 located between a first conductive layer 46 and a second conductive layer 46'. It should be understood that in all embodiments described herein, different layers can completely or partially cover each other, and additional copper foil layers, patterned circuit layers, and substrate layers may also be present. It should also be understood that different layers can be in direct physical contact with adjacent layers (directly on adjacent layers), or layers such as adhesive layers can be located between (on) each layer and adjacent layers. The printed circuit board substrate 12 includes a plurality of coated boron nitride particles 44 and a reinforcement layer 42.
[0020] A plurality of coated boron nitride particles may comprise one or both of a single particle (primary particle) or an agglomerate (secondary particle) containing a plurality of particles. The average particle size of a plurality of coated boron nitride particles (primary particles or agglomerates of particles) may be 0.1 micron to 1000 microns, or 5 microns to 500 microns, or 10 microns to 250 microns, or 25 microns to 150 microns, or 500 nanometers to 100 microns, or 3 microns to 40 microns. A plurality of coated boron nitride particles having an average particle size greater than or equal to 10 microns may include irregularly shaped hexagonal boron nitride flakes. As used herein, "particle size" may refer to an average diameter or equivalent diameter preferably determined by standard laser particle measurement. Particle size may refer to D 50The particle size, which is called the median diameter or median of the particle size distribution; is the value of the particle diameter at which 50% of the cumulative distribution lies.
[0021] The plurality of coated boron nitride particles may be in the form of at least one of a powder (including flakes, platelets, and other shapes), fibers, rods, whiskers, sheets, nanosheets, agglomerates, or boron nitride nanotubes (BNNTs), which may vary with crystal type, shape, or size, and include distributions as described above. The average aspect ratio (ratio of the width or diameter of the particle to the length) of the plurality of coated boron nitride particles may be 1:2 to 1:100000, or 1:5 to 1:1000, or 1:10 to 1:300. Exemplary shapes of particles with particularly high aspect ratios include platelets, rod-shaped particles, fibers, whiskers, and the like. The plurality of coated boron nitride particles may include coated boron nitride platelets. The precise shape of the platelets is not critical. In this regard, the coated boron nitride platelets may have irregular shapes. It should be noted that the term "platelet" as used herein generally describes any thin, flat particle, including a flake. The average aspect ratio of the platelets (ratio of the width to the length of the particles) may be from 4:5 to 1:300, or from 1:2 to 1:300, or from 1:2 to 1:200, or from 3:5 to 1:100, or from 1:25 to 1:100.
[0022] About crystal type, coated boron nitride particles can include at least one structure in hexagonal structure, cubic structure, wurtzite structure, rhombohedral structure or other synthetic structures. Among various structures, hexagonal boron nitride particles (hBN) can obtain excellent thermal conductivity of, for example, 10 watts per meter Calvin (W / mK) to 300 watts per meter Calvin or greater, and particles of cubic structure can obtain extremely high thermal conductivity of up to 1300W / mK. The thermal conductivity of boron nitride particles can be determined according to ASTM E1225-13. Hexagonal boron nitride has a layered structure similar to graphite, wherein the layers are stacked in alignment so that the hexagonal rings in the layers overlap. The positions of N atoms and B atoms are alternated in layers. Multiple coated boron nitride particles can have a hexagonal structure with a crystallization index of at least 0.12, or 0.20 to 0.55, or 0.30 to 0.55. hBN particles can be obtained from various commercial sources.
[0023] Boron nitride particles, crystals or partial crystals can be manufactured by methods known in the art. These include, for example, boron nitride powders produced by the pressing methods disclosed in U.S. Patents No. 5,898,009 and No. 6,048,511, boron nitride agglomerated powders disclosed in U.S. Patent Publication No. 2005 / 0041373 and highly layered boron nitride powders disclosed in U.S. Patent No. 6,951,583. Various boron nitride powders are commercially available, such as the trade name POLARTHERMA boron nitride from Momentive.
[0024] The plurality of coated boron nitride particles comprises a coating. The coating may comprise at least one of carbon, aluminum, silicon, germanium, copper, nickel, palladium, platinum, iridium, cobalt, iron, ruthenium, molybdenum, tungsten, tantalum, zirconium, or titanium, for example in the form of at least one of a carbide, an oxide, a nitride, a sulfide, or a phosphide. The coating may comprise at least one of an inorganic carbide (e.g., aluminum carbide or titanium carbide), an inorganic oxide (e.g., aluminum oxide (Al2O3), magnesium oxide, silicon dioxide (SiO2), titanium dioxide, yttrium oxide, zirconium oxide, or zinc oxide), an inorganic nitride (e.g., aluminum nitride (AlN) or silicon nitride), an inorganic sulfide (e.g., gallium sulfide, molybdenum sulfide, or tungsten sulfide), an inorganic hydroxide (e.g., aluminum hydroxide ... x O y H z ), zinc hydroxide (Zn x O y H z ), or silicon hydroxide (Si x O y H z The coating may include at least one of silicon dioxide or aluminum oxide.
[0025] The coating may include one or more different coatings, which may optionally be alternating layers. For example, the coating may include a first coating comprising aluminum oxide and a second coating comprising aluminum nitride. In another example, the coating may include a first coating comprising aluminum oxide and a second coating comprising silicon dioxide. Before depositing a silicon dioxide layer by atomic layer deposition (ALD), it may be beneficial to first coat a plurality of boron nitride particles with aluminum oxide, because aluminum oxide tends to deposit much more uniformly on the base and edges of the boron nitride particles than silicon dioxide, and may then be used as a seed layer for depositing silicon dioxide.
[0026] The coating may be disposed on 10 area percent (A%) to 100A%, or 50A% to 100A%, or 90A% to 100A% of the surface. The coating may have a thickness of 0.1nm to 100nm, or 0.5nm to 30nm, or 1nm to 20nm, or less than or equal to 5nm. The coating may have a thickness of 0.5nm to 100nm, or 1nm to 10nm. Based on the total weight of the plurality of coated boron nitride particles, the plurality of coated boron nitride particles may include less than 1 weight percent (wt%), or 0.001wt% to 0.9wt%, or 0.001wt% to 0.5wt%, or 0.005wt% to 0.1wt% of the coating.
[0027] The plurality of coated boron nitride particles may be further surface treated with a coupling agent. The coupling agent promotes the formation of covalent bonds that improve the adhesion between the filler and the thermosetting polymer matrix or participates in the covalent bonds that improve the adhesion between the filler and the thermosetting polymer matrix. Exemplary coupling agents include silanes, zirconates, titanates, and the like, such as vinyl trichlorosilane, vinyl trimethoxysilane, trivinyl methoxysilane, vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-glycidoxypropyl triethoxysilane, γ-methacryloxypropyl methyl dimethoxysilane, γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyl diethoxysilane, γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyl diethoxysilane, γ-methacryloxypropyl Oxypropyltriethoxysilane, N-β (aminoethyl) γ-aminopropylmethyldimethoxysilane, N-β (aminoethyl) γ-aminopropyltrimethoxysilane, bis (trimethoxysilylethyl) benzene, bis (triethoxysilyl) ethylene, triethoxysilyl-modified butadiene, styrylethyltrimethoxysilane, N-β (aminoethyl) γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, trimethoxyphenylsilane, perfluorooctyltriethoxysilane, and γ-mercaptopropyltrimethoxysilane.
[0028] The coating can be applied to multiple boron nitride particles via ALD. ALD is a type of chemical vapor deposition in which a thin film is deposited on a substrate using a gas phase chemical precursor that reacts on the substrate surface. For example, a silicon dioxide coating can be deposited by alternately exposing the boron nitride particles to SiCl4 and H2O, and an aluminum oxide coating can be deposited by alternating exposure of Al(CH3)3 and H2O. A convenient method for applying an ultra-thin coating of an inorganic material to multiple boron nitride particles is to form a fluidized bed of particles and then pass various reagents through the fluidized bed in sequence under reaction conditions. Methods for fluidizing particulate materials are well known and typically include supporting particles on a porous plate or screen. The fluidizing gas can then pass upward through the plate or screen, slightly lifting the particles and expanding the volume of the bed. With appropriate expansion, the particles behave like a fluid. A fluid (gas or liquid) reagent can be introduced into the bed to react with the surface of the particles. The method for applying a coating of an inorganic material can include performing a coating reaction in a rotating reactor to evenly distribute individual particles and expose all particles to reactants. If desired, multiple layers of ultra-thin coatings can be deposited on multiple coated boron nitride particles. Multiple layers may be deposited to provide layers with different compositions, for example to provide alternating compositions.
[0029] After forming the inorganic coating, one or more reactions may be performed on the coating thus formed to modify the coating. This technique is useful for forming various types of ultra-thin coatings that are not suitable for deposition using atomic layer deposition techniques. For example, various types of ultra-thin oxide coatings may be formed using the above-mentioned atomic layer deposition techniques, which may then be carburized to convert the oxide into a corresponding carbide or nitrided to convert the oxide into a corresponding nitride.
[0030] Before or after the coating process, the boron nitride particles can be heat treated. The heat treatment can include heating the boron nitride particles at a temperature of 100 degrees Celsius (° C.) to 250° C., or 150° C. to 200° C., for example, for more than 4 hours, or 6 hours to 10 hours. The heat treatment can include heating the boron nitride particles at a temperature of 500° C. to 1500° C., for example, for 4 hours to 18 hours, or 6 hours to 10 hours. The heat treatment can be carried out in the presence of air, in an inert atmosphere, or in a vacuum.
[0031] Based on the total volume of the printed circuit board substrate, the printed circuit board substrate may contain 1 volume percent (volume %) to 85 volume %, or 25 volume % to 80 volume %, or 40 volume % to 60 volume % of a plurality of coated boron nitride particles. Based on the total volume of the printed circuit board substrate, the printed circuit board substrate may contain 1 volume % to 50 volume %, or 5 volume % to 35 volume %, or 10 volume % to 25 volume % of a plurality of coated boron nitride particles. Based on the total volume of the printed circuit board substrate, the printed circuit board substrate may contain 15 volume % to 99 volume %, or 50 volume % to 99 volume %, or 65 volume % to 95 volume %, or 75 volume % to 80 volume % of the thermosetting polymer matrix. The printed circuit board substrate may have no empty space.
[0032] The printed circuit board substrate may optionally include a reinforcement layer, for example, a fiber layer comprising multiple heat-stable fibers. The reinforcement layer may be a fabric reinforcement. The fiber layer may be woven or nonwoven, such as a felt. The reinforcement layer may reduce the shrinkage of the printed circuit board substrate when solidified in the plane of the material. In addition, the use of a reinforcement layer may help impart relatively high mechanical strength to the material. Such materials may be more easily processed by methods in commercial uses such as lamination (including roll-to-roll lamination). The heat-stable fiber may include glass fiber, such as at least one of E glass fiber, S glass fiber, or D glass fiber. The heat-stable fiber may include polymer-based fibers, such as high-temperature polymer fibers. Polymer-based fibers may include liquid crystal polymers, such as VECTRAN commercially available from Kuraray America Inc., Fort Mill, SC. Polymer-based fibers may include at least one of polyetherimide fibers, polyetherketone fibers, polysulfone fibers, polyethersulfone fibers, polycarbonate fibers, or polyester fibers.
[0033] The printed circuit board substrate may include a plurality of uncoated boron nitride particles. The printed circuit board substrate may include a second inorganic filler, particularly a dielectric filler and / or a flame retardant filler, in combination with the coated boron nitride particles. The second inorganic dielectric filler includes titanium dioxide (rutile and anatase), barium titanate, strontium titanate, silicon dioxide including fused amorphous silicon dioxide (particles and hollow spheres), corundum, wollastonite, glass fiber, Ba2Ti9O 20 , glass balls, quartz, boron nitride, aluminum nitride, phosphorus compounds (e.g., phosphorus-containing flame retardant compounds), brominated compounds (e.g., bromine-containing flame retardant compounds), silicon carbide, beryllium oxide, aluminum oxide, magnesium oxide, mica, talc, nanoclay, aluminosilicates (natural and synthetic), and fumed silica (e.g., CAB-O-SIL available from Cabot Corporation). Other second fillers, such as magnesium hydroxide, may be used. Combinations of second dielectric fillers may also be used. More specifically, rutile titanium dioxide and amorphous silica are particularly desirable because these fillers have high dielectric constants and low dielectric constants, respectively, allowing, for example, a wide range of dielectric constants combined with low dielectric loss to be achieved in the final cured product by adjusting the respective amounts of the two second dielectric fillers in the printed circuit board substrate. Specific dielectric fillers include rutile titanium dioxide and amorphous silica. The second filler may be in the form of solid, porous or hollow particles. The second filler, when used, may be present in an amount of 15 volume % to 60 volume %, or 20 volume % to 50 volume %, based on the total volume of the printed circuit board substrate.
[0034] The printed circuit board substrate can include a particle fluoropolymer. Exemplary particle fluoropolymers include, but are not limited to, fluorinated homopolymers such as polytetrafluoroethylene (PTFE), and fluorinated copolymers, such as copolymers of tetrafluoroethylene and hexafluoropropylene or perfluoroalkyl vinyl ether (e.g., perfluorooctyl vinyl ether), or copolymers of tetrafluoroethylene and ethylene. Combinations of fluorinated polymers, copolymers, and terpolymers can also be used. Fluoropolymers can be in the form of fine powders, dispersions, or granules, including: fine powders (or "solidified dispersions") PTFE made by solidifying and drying the dispersed PTFE, usually made to show a particle size of 400 microns to 500 microns; granular PTFE made by suspension polymerization, usually with two different particle size ranges (for standard products, the median particle size is 30 microns to 40 microns, for high bulk density products, the median particle size is 400 microns to 500 microns); and / or granular PTFE, fluorinated ethylene-propylene copolymers (FEP), or copolymers (PFA) with a tetrafluoroethylene backbone and fully fluorinated alkoxy side chains. The particulate fluoropolymer may be cryogenically ground to exhibit a median particle size of less than 100 microns.
[0035] When present, one of ordinary skill in the art can readily determine the effective particulate fluoropolymer content of the printed circuit board substrate, depending on the desired flame retardancy of the composition, the amounts of other components, and other properties desired in the final product. More specifically, the amount of fluoropolymer depends on the amount of coated boron nitride particles, other fillers, and particulate flame retardants in the printed circuit board substrate. Typically, the effective amount is 1 part by weight per 100 parts by weight of the thermosetting polymer matrix (phr) to 90 phr, or 5 phr to 75 phr, or 10 phr to 50 phr.
[0036] The polymer matrix may include at least one of an epoxy resin, a polyphenylene oxide, a polystyrene, an ethylene-propylene dicyclopentadiene copolymer, a polybutadiene, a polyisoprene, a fluoropolymer, a poly(etheretherketone), a polyimide, or a cross-linked matrix comprising at least one of triallyl cyanurate, triallyl isocyanurate, 1,2,4-trivinylcyclohexane, trimethylolpropane triacrylate, or trimethylolpropane trimethacrylate. The thermosetting polymer matrix may include at least one of an epoxy resin, a polybutadiene, or a polyisoprene. The polymer matrix may include a polyphenylene oxide thermosetting resin, such as OPE-2ST 1200 or OPE-2ST 2200 (commercially available from Mitsubishi Gas Chemical Co.) or NORYL SA9000 (commercially available from SABIC Innovative Plastics). The polymer matrix may include an ethylene-propylene dicyclopentadiene copolymer. The thermosetting resin comprises a cross-linked matrix comprising a derivative of a cross-linking agent, such as at least one of triallyl cyanurate, triallyl isocyanurate, 1,2,4-trivinylcyclohexane, trimethylolpropane triacrylate, or trimethylolpropane trimethacrylate. The polymer matrix may comprise a thermoplastic resin, such as a fluoropolymer, a poly(arylene ether ketone) (e.g., poly(ether ether ketone) (PEEK) or poly(ether ketone ketone) (PEKK)), or a polyimide (e.g., polyetherimide (PEI), such as ULTEM commercially available from SABIC Innovative Plastics). The thermosetting resin may comprise an epoxy resin.
[0037] As used herein, "fluoropolymers" include homopolymers and copolymers comprising repeating units derived from fluorinated α-olefin monomers (i.e., α-olefin monomers containing at least one fluorine atom substituent) and optionally non-fluorinated ethylenically unsaturated monomers reacted with the fluorinated α-olefin monomers. Exemplary fluorinated α-olefin monomers include CF2=CF2, CHF=CF2, CH2=CF2, CHCl=CHF, CClF=CF2, CCl2=CF2, CClF=CClF, CHF=CCl2, CH2=CClF, CCl2=CClF, CF3CF=CF2, CF3CF=CHF, CF3CH=CF2, CF3CH=CH2, CHF2CH=CHF, and CF3CH=CH2, as well as perfluoro(C2-8 alkyl)vinyl ethers, such as perfluoromethylvinyl ether, perfluoropropylvinyl ether, and perfluorooctylvinyl ether. In some embodiments, the fluorinated α-olefin monomer includes at least one of tetrafluoroethylene (CF2=CF2), chlorotrifluoroethylene (CClF=CF2), (perfluorobutyl)ethylene, vinylidene fluoride (CH2=CF2), or hexafluoropropylene (CF2=CFCF3). Exemplary non-fluorinated monoethylenically unsaturated monomers include ethylene, propylene, butene, and ethylenically unsaturated aromatic monomers such as styrene and α-methyl-styrene. Exemplary fluoropolymers include poly(chlorotrifluoroethylene) (PCTFE), poly(chlorotrifluoroethylene-propylene), poly(ethylene-tetrafluoroethylene) (ETFE), poly(ethylene-chlorotrifluoroethylene) (ECTFE), poly(hexafluoropropylene), poly(tetrafluoroethylene) (PTFE), poly(tetrafluoroethylene-ethylene-propylene), poly(tetrafluoroethylene-hexafluoropropylene) (also known as fluorinated ethylene-propylene copolymer (FEP)), poly(tetrafluoroethylene-propylene) (also known as fluoroelastomer) (FEPM), poly(tetrafluoroethylene-perfluoropropylene vinyl ether), copolymers having a tetrafluoroethylene backbone and fully fluorinated alkoxy side chains (also known as perfluoroalkoxy polymers (PFA)) (e.g., poly(tetrafluoroethylene-perfluoropropylene vinyl ether)), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-trifluoroethylene), perfluoropolyether, perfluorosulfonic acid, or perfluoropolyoxetane, preferably a perfluoroalkoxy alkane polymer, or a fluorinated ethylene-propylene, more preferably a perfluoroalkoxy alkane polymer. Combinations comprising at least one of the foregoing fluoropolymers can be used. In some embodiments, the fluoropolymer is FEP, PFA, ETFE, or PTFE, which can be fibril-forming or non-fibril-forming.FEP is available from DuPont under the trade name TEFLON FEP or from Daikon as NEOFLON FEP; PFA is available from Daikin under the trade name NEOFLON PFA, from DuPont as TEFLON PFA, or from Solvay Solexis as HYFLON PFA.
[0038] The thermosetting resin may include at least one of a copolymer or homopolymer containing units derived from at least one of butadiene or isoprene. Units derived from other copolymerizable monomers may also be present in the thermosetting polymer, for example, in the main chain of the polymer or in the form of grafting. Copolymerizable monomers include, but are not limited to: vinyl aromatic monomers, for example, substituted and unsubstituted monovinyl aromatic monomers such as styrene, 3-methylstyrene, 3,5-diethylstyrene, 4-n-propylstyrene, α-methylstyrene, α-methylvinyltoluene, p-hydroxystyrene, p-methoxystyrene, α-chlorostyrene, α-bromostyrene, dichlorostyrene, dibromostyrene, tetrachlorostyrene, etc.; and substituted and unsubstituted divinyl aromatic monomers such as divinylbenzene, divinyltoluene, etc. A combination comprising at least one of the aforementioned copolymerizable monomers may also be used. The thermosetting polymer matrix may include, but is not limited to, at least one of an epoxy resin, a butadiene homopolymer, an isoprene homopolymer, a butadiene-vinyl aromatic copolymer (e.g., butadiene-styrene), an isoprene-vinyl aromatic copolymer (e.g., isoprene-styrene copolymer), and the like.
[0039] The polybutadiene and / or polyisoprene may be present in the thermosetting polymer matrix in an amount up to 100 wt%, or up to 75 wt%, or 10 wt% to 70 wt%, or 20 wt% to 60 wt%, or 70 wt%, relative to the total weight of the thermosetting polymer matrix (minus any filler or reinforcement layer). The thermosetting polymer matrix may have at least 90 wt% 1,2 addition based on total repeating units, which upon curing may exhibit greater crosslink density due to the large number of pendant vinyl groups available for crosslinking.
[0040] Other polymers that can be co-cured with thermosetting polymer matrix can be present for specific characteristics or processing modification.For example, in order to improve the dielectric strength of electrical substrate materials and the stability of mechanical properties over time, ethylene-propylene elastomers of lower molecular weight can be used.As used herein, ethylene-propylene elastomers are copolymers (such as terpolymers), or other polymers that mainly comprise ethylene and propylene.Ethylene-propylene elastomers can be further classified as EPM copolymers (that is, copolymers of ethylene monomers and propylene monomers) or EPDM terpolymers (i.e. terpolymers of ethylene monomers, propylene monomers and diene monomers).Especially, ethylene-propylene-diene terpolymer rubbers have saturated main chains, and have available unsaturation for easy crosslinking away from the main chain.Liquid ethylene-propylene-diene terpolymer rubbers can be used, wherein diene is dicyclopentadiene.
[0041] The molecular weight of the ethylene-propylene rubber may be less than or equal to 10,000 grams per mole (g / mol) viscosity average molecular weight (Mv). The weight average molecular weight (Mw) of the ethylene-propylene rubber as measured by gel permeation chromatography based on polycarbonate standards may be less than or equal to 50,000 g / mol. The ethylene-propylene rubber may include an ethylene-propylene rubber having an Mv of 7,200 g / mol, which is available from Lion Copolymer, Baton Rouge, LA under the trade name TRILENE CP80; a liquid ethylene-propylene-dicyclopentadiene terpolymer rubber having an Mv of 7,000 g / mol, which is available from Lion Copolymer under the trade name TRILENE 65; and a liquid ethylene-propylene-ethylidene norbornene terpolymer having an Mv of 7,500 g / mol, which is available from Lion Copolymer under the trade name TRILENE 67.
[0042] Ethylene-propylene rubber can be present in an amount effective to maintain the properties of the substrate material, particularly the stability of dielectric strength and mechanical properties over time. Typically, such an amount is up to 20 wt %, or 4 wt % to 20 wt %, or 6 wt % to 12 wt %, relative to the total weight of the thermosetting polymer matrix.
[0043] Another type of co-curable polymer is an unsaturated polybutadiene or polyisoprene containing elastomer. This component can be a random copolymer or block copolymer of predominantly 1,3-addition butadiene or isoprene with an ethylenically unsaturated monomer such as a vinyl aromatic compound such as styrene or α-methylstyrene, an acrylate or methacrylate such as methyl methacrylate, or acrylonitrile. The elastomer can be a solid thermoplastic elastomer including a linear or grafted block copolymer having a polybutadiene or polyisoprene block and a thermoplastic block that can be derived from a monovinyl aromatic monomer such as styrene or α-methylstyrene. Block copolymers of this type include styrene-butadiene-styrene triblock copolymers, such as those available under the trade designation VECTOR 8508M from Dexco Polymers, Houston, TX, SOL-T-6302 from Enichem Elastomers America, Houston, TX, and CALPRENE 401 from Dynasol Elastomers; styrene-butadiene diblock copolymers and mixed triblock and diblock copolymers comprising styrene and butadiene, such as those available under the trade designation KRATOND 1118 from Kraton Polymers (Houston, TX). KRATOND 1118 is a mixed diblock / triblock copolymer comprising styrene and butadiene that contains 33 wt% styrene based on the total weight of the copolymer.
[0044] The optional polybutadiene or polyisoprene containing elastomer may also include a second block copolymer similar to that described above, except that the polybutadiene or polyisoprene blocks are hydrogenated to form polyethylene blocks (in the case of polybutadiene) or ethylene-propylene copolymer blocks (in the case of polyisoprene). When used in combination with the above copolymers, a material with greater toughness can be produced. An example of this type of second block copolymer is KRATONGX1855 (commercially available from Kraton Polymers), which is believed to be a mixture of a high styrene 1,2-butadiene-styrene block copolymer and a styrene-(ethylene-propylene)-styrene block copolymer.
[0045] The unsaturated polybutadiene or polyisoprene containing elastomeric component may be present in the polymer matrix composition in an amount of 2 wt % to 60 wt %, or 5 wt % to 50 wt %, or 10 wt % to 40 wt %, or 10 wt % to 50 wt %, relative to the total weight of the thermosetting polymer matrix.
[0046] Still other co-curable polymers that may be added for specific properties or processing modifications include, but are not limited to: homopolymers or copolymers of ethylene, such as polyethylene and ethylene oxide copolymers; natural rubber; norbornene polymers such as polydicyclopentadiene; hydrogenated styrene-isoprene-styrene copolymers and butadiene-acrylonitrile copolymers; unsaturated polyesters; etc. The level of these copolymers is generally less than or equal to 50 weight percent of the total weight of the thermosetting polymer matrix.
[0047] Free radical curable monomers for specific properties or processing modifications can also be added, for example to improve the crosslinking density of the cured system. Monomers that can be used as suitable crosslinking agents include, for example, diethylenically unsaturated monomers, triethylenically unsaturated monomers or higher ethylenically unsaturated monomers such as divinylbenzene, trivinylbenzene, triallyl cyanurate, diallyl phthalate and multifunctional acrylate monomers (for example, the SARTOMER polymers available from Sartomer USA, Newtown Square, PA), or combinations thereof, all of which are commercially available. Based on the gross weight of the thermosetting polymer matrix, the crosslinking agent can be present in the polymer matrix composition in an amount up to 20 wt % or 1 wt % to 15 wt % when used.
[0048] Curing agent can be added to thermosetting composition before curing to accelerate the curing reaction of polyene with olefinic reactive sites. Curing agent can include organic peroxide, for example, dicumyl peroxide, tert-butyl perbenzoate, 2,5-dimethyl-2,5-di-(tert-butyl peroxy) hexane, α, α-di-bis-(tert-butyl peroxy) diisopropylbenzene or at least one of 2,5-dimethyl-2,5-di-(tert-butyl peroxy) hexine-3. Carbon-carbon initiator can be used, for example 2,3-dimethyl-2,3 diphenylbutane. Curing agent or initiator can be used alone or in combination. Based on the gross weight of the thermosetting polymer matrix, the amount of curing agent can be 1.5 weight % to 10 weight %.
[0049] Thermosetting polymer matrix can also be modified. For example, the thermosetting polymer matrix can be carboxylate-terminated, hydroxyl-terminated, methacrylate-terminated, etc. Post-reaction polymers can be used, such as epoxy-modified, maleic anhydride-modified, or carbamate-modified polymers of butadiene or isoprene polymers. Thermosetting polymer matrix can also be cross-linked, for example, by divinyl aromatic compounds (such as divinyl benzene), for example, polybutadiene-styrene cross-linked with divinyl benzene. Polymers are broadly classified as "polybutadiene" by their manufacturers, such as Nippon Soda Co., Tokyo, Japan, and Cray Valley Hydrocarbon Specialty Chemicals, Exton, PA. Mixtures of polymers can also be used, for example, mixtures of polybutadiene homopolymers and poly (butadiene-isoprene) copolymers. Combinations comprising syndiotactic polybutadiene can also be useful.
[0050] The thermosetting polymer matrix can be carboxyl functionalized. Functionalization can be accomplished using polyfunctional compounds having (i) a carbon-carbon double bond or a carbon-carbon triple bond and (ii) at least one carboxyl group in the molecule, including carboxylic acids, anhydrides, amides, esters or acyl halides. The specific carboxyl group is a carboxylic acid or ester. Examples of polyfunctional compounds that can provide carboxylic acid functional groups include maleic acid, maleic anhydride, fumaric acid and citric acid. In particular, polybutadiene adducted with maleic anhydride can be used in thermosetting compositions. Suitable maleated polybutadiene polymers can be commercially available from Cray Valley, for example, under the trade names RICON 130MA8, RICON 130MA1 3, RICON 130MA20, RICON 131MA5, RICON 131MA10, RICON 131MA1 7, RICON 131MA20 and RICON156MA1 7. Suitable maleated polybutadiene-styrene copolymers are commercially available, for example, under the trade name RICON 184MA6 from Sartomer (butadiene-styrene copolymer adducted with maleic anhydride, styrene content of 17 to 27% by weight, number average molecular weight (Mn) of 9900 g / mol).
[0051] The relative amounts of various polymers (e.g., polybutadiene or polyisoprene polymers and other polymers) in a thermosetting polymer matrix can depend on considerations such as the desired properties of the specific conductive metal layer, circuit material, and copper-clad laminate used. For example, the use of poly(arylene ether) can provide increased bonding strength for the conductive metal layer (e.g., copper). The use of polybutadiene and / or polyisoprene (e.g., when these polymers are carboxyl functionalized) can improve the high temperature resistance of the laminate. The use of elastomeric block copolymers can be used to make the components of the polymer matrix compatible. Based on the desired properties of a particular application, the appropriate amount of each component can be determined without excessive experimentation.
[0052] Typically, a printed circuit board substrate can be prepared by first mixing all components including, for example, a monomer, coated boron nitride particles, an optional second filler, an optional coupling agent (e.g., such as at least one of a silane, a zirconate, or a titanate), an optional solvent, and an optional curing agent. Mixing can be continued to form a slurry or dispersion in which the individual components are uniformly dispersed throughout the mixture. For those applications in which the mixture is impregnated onto a reinforcement layer to form a prepreg, conventional prepreg manufacturing methods can be employed. Typically, the reinforcement layer is impregnated with the mixture, metered to the correct thickness, and then any solvent is removed to form a prepreg. If the prepreg contains certain thermosetting polymers, it can then optionally be subjected to a B stage to form a partially cured layer before being used to form a circuit assembly.
[0053] The solvent or dispersion medium may optionally be present to adjust the viscosity of the mixture. The solvent may be selected to dissolve or disperse the components of the mixture and have an evaporation rate that is convenient for applying the mixture, for example, on a reinforcing layer and drying the mixture. A non-exclusive list of possible solvents and dispersion mediums includes water, xylene, toluene, methyl ethyl ketone, methyl isobutyl ketone, hexane, or higher liquid linear alkanes (e.g., heptane, octane, nonane, cyclohexane, isophorone), or at least one of various terpene-based solvents. Specific solvents and dispersion mediums for thermosetting compositions may include at least one of xylene, toluene, methyl ethyl ketone, methyl isobutyl ketone, or hexane, and more specifically, may include at least one of xylene or toluene.
[0054] Figure 2 is a diagram of a method for preparing a printed circuit board substrate. Figure 2The reinforcement layer is shown unwinding from the roller 10, passing through the first accumulator 12 ', and entering the coating zone 16. In the coating zone 16, the coating mixture in the groove 20 is raised so that the reinforcement layer passes through the coating mixture to cover the reinforcement layer with the coating mixture. The reinforcement layer then passes through the metering roller 22 to help ensure that the coating mixture is evenly coated on the reinforcement layer. After coating, the reinforcement layer passes through the drying tower 18 to help evaporate any solvent present and at least partially solidify the polymer matrix. Finally, the reinforcement layer traverses around the drive roller 28, passes through the second accumulator 30, and finally surrounds the coating roller 32. It should be understood that many variations on this coating process can be made, and this illustration is provided only as a non-limiting embodiment of the coating method.
[0055] The article may include a printed circuit board substrate. The article may be an adhesive layer, a cover film or a buildup material, and when combined with a conductive layer, the article may provide a circuit laminate, a resin-coated cover layer, or a circuit assembly. The circuit material may include a printed circuit board substrate having a conductive layer disposed on one or two wide surfaces. Useful conductive layers include, for example, at least one of stainless steel, copper, gold, silver, aluminum, zinc, tin, lead, or a transition metal. There are no particular restrictions on the thickness of the conductive layer, nor are there any restrictions on the shape, size, or surface texture of the conductive layer. The thickness of the conductive layer may be 3 microns to 200 microns, or 9 microns to 180 microns. When there are two or more conductive layers, the thickness of the two layers may be the same or different. The conductive layer may include a copper layer. Suitable conductive layers include thin layers of conductive metals, for example, copper foil currently used to form circuits, for example, electro-deposited copper foil. The root mean square (RMS) roughness of the copper foil may be less than or equal to 2 microns, or less than or equal to 0.7 microns, wherein the roughness is measured using a white light interferometer method using a Veeco instrument WYCO optical profiler.
[0056] The conductive layer can be applied by placing the conductive layer in a mold prior to reaction injection molding, laminating the conductive layer on a printed circuit board substrate, direct laser structuring, or adhering the conductive layer to the printed circuit board substrate via an adhesive layer. Other methods known in the art can be used to apply the conductive layer, such as electrodeposition, chemical vapor deposition, etc., where the specific materials and form of the circuit material permit.
[0057] Lamination can cause a multilayer stack including a printed circuit board substrate, a conductive layer, and an optional intermediate layer between the printed circuit board substrate and the conductive layer to be laminated to form a layered structure. The conductive layer can be in direct contact with the printed circuit board substrate without an intermediate layer. The layered structure can then be placed in a press, such as a vacuum press, under a pressure and temperature and duration suitable for combining the layers and forming a laminate. Lamination and optional curing can be by a one-step method, such as using a vacuum press, or can be by a multi-step method. In a one-step method, the layered structure can be placed in a press, raised to a lamination pressure (e.g., 150 pounds per square inch to 2500 pounds per square inch (psi) [1 MPa to 17 MPa]) and heated to a lamination temperature (e.g., 150°C to 390°C). The lamination temperature and pressure can maintain a desired soak time, i.e., 20 minutes, followed by cooling (while still under pressure) to less than or equal to 150°C.
[0058] If present, the intermediate layer may include a polyfluorocarbon film that may be located between the conductive layer and the substrate layer, and an optional microglass reinforced fluorocarbon polymer layer may be located between the polyfluorocarbon film and the conductive layer. The microglass reinforced fluorocarbon polymer layer may improve the adhesion of the conductive layer to the substrate. The microglass may be present in an amount of 4 wt % to 30 wt % based on the total weight of the layer. The longest length scale of the microglass may be less than or equal to 900 microns, or less than or equal to 500 microns. The microglass may be a type of microglass such as that commercially available through Johns-Manville Corporation of Denver, CO. The polyfluorocarbon film includes fluoropolymers such as polytetrafluoroethylene (PTFE), fluorinated ethylene-propylene copolymers such as Teflon FEP, and copolymers having a tetrafluoroethylene backbone and fully fluorinated alkoxy side chains such as Teflon PFA.
[0059] The conductive layer can be applied by laser direct structuring. Here, the printed circuit board substrate can contain a laser direct structuring additive; and the laser direct structuring can include using a laser to irradiate the surface of the substrate, forming a track of the laser direct structuring additive, and applying a conductive metal to the track. The laser direct structuring additive can include metal oxide particles (e.g., titanium oxide and copper chromium oxide). The laser direct structuring additive can include spinel-based inorganic metal oxide particles such as spinel copper. The metal oxide particles can be coated with, for example, a composition comprising tin and antimony (e.g., 50% to 99% by weight of tin and 1% to 50% by weight of antimony based on the total weight of the coating). Based on 100 parts of the corresponding composition, the laser direct structuring additive can include 2 to 20 parts of the additive. The irradiation can be performed with a YAG laser having a wavelength of 1,064 nanometers at an output power of 10 watts, a frequency of 80 kilohertz (kHz), and a rate of 3 meters per second. The conductive metal can be applied using a plating method in a chemical plating bath comprising, for example, copper.
[0060] The conductive layer can be applied by applying the conductive layer adhesively. The conductive layer can be a circuit (a metallized layer of another circuit), such as a flexible circuit. The adhesive layer can be disposed between one or more conductive layers and the substrate. When appropriate, the adhesive layer can include poly (arylene ether); and carboxyl functionalized polybutadiene or polyisoprene polymers, the carboxyl functionalized polybutadiene or polyisoprene polymers comprising butadiene, isoprene, or butadiene and isoprene units, and 0 wt % to 50 wt % of co-curable monomer units. The adhesive layer can be present in an amount of 2 grams per square meter to 15 grams per square meter. Poly (arylene ether) can include carboxyl functionalized poly (arylene ether). Poly (arylene ether) can be a reaction product of poly (arylene ether) and cyclic anhydride, or a reaction product of poly (arylene ether) and maleic anhydride. Carboxyl functionalized polybutadiene or polyisoprene polymers can be carboxyl functionalized butadiene-styrene copolymers. The carboxyl functionalized polybutadiene or polyisoprene polymer may be the reaction product of a polybutadiene or polyisoprene polymer and a cyclic anhydride. The carboxyl functionalized polybutadiene or polyisoprene polymer may be a maleated polybutadiene-styrene or a maleated polyisoprene-styrene copolymer.
[0061] The following examples are provided to illustrate the present disclosure. These examples are merely illustrative and are not intended to limit devices made according to the present disclosure to the materials, conditions, or process parameters described therein.
[0062] Example
[0063] In an embodiment, copper peel strength is measured according to IPC-TM-650-2.4.8 after thermal stress involving exposure to molten solder for 10 seconds at 288°C. Relative dielectric constant and dielectric loss are measured according to IPC-TM-650-2.5.5.5. Dielectric strength is measured according to IPC-TM-650-2.5.6.2. Water absorption is measured according to ASTM D570-98 (2018) using a test sample with a nominal thickness of 1.52 mm after immersion at 50°C for 48 hours. Thermal conductivity is the Z-direction thermal conductivity measured according to ASTM D5470-17, TIMTester1300.
[0064] Examples 1 to 6: Effect of coating thickness on coated hexagonal boron nitride
[0065] Using trimethylaluminum and water as precursors, the surface of hexagonal boron nitride particles is coated with aluminum oxide by atomic layer deposition (ALD). The boron nitride powder used is PBN20, which is a high-density agglomerate of hexagonal boron nitride flakes supplied by ZiboJonye Ceramics Technology Company. PBN20 shows a typical median particle size of 18 to 22 microns, and 6.2 square meters per gram (m 2 / g) of specific surface area. A series of coated powders with different coating thicknesses were produced by gradually changing the number of ALD cycles. The aluminum content of the coated powders was determined by ICP analysis, and the surface energy was measured by Washburn wicking for the contact angles of different probe liquids. The contact angle measurements were combined with Fowkes theory to decompose the surface energy into dispersive and polar components. The results are shown in Table 1. Figure 3 ,and Figure 4 In which mJ / m 2 and mJ / sqm stands for millijoules per square meter, and ppm stands for parts per million by weight based on the total weight of the sample.
[0066]
[0067] Table 1 and Figure 3 It is shown that the amount of aluminum deposition is well controlled by the number of ALD cycles. Without being bound by theory, it is believed that this self-regulation is due to the surface reaction involving trimethylaluminum and water being self-limiting.
[0068] Table 1 and Figure 4 It is shown that the uncoated Example 1 exhibits the lowest total surface energy, dispersed surface energy ( Figure 4 The top curve) and surface polarity ( Figure 4The surface polarity of the uncoated boron nitride is believed to be substantially due to the boron oxide present on the surface. It can be seen that the coating provides a method for modifying the surface polarity of the boron nitride filler. The increase in surface polarity may be due to the hydroxyl groups present on the surface of the coating.
[0069] Example 7: Printed Circuit Board Substrate Comprising Coated Boron Nitride
[0070] A printed circuit board substrate was prepared containing 15 volume % of coated boron nitride and 85 volume % of RO4000 (commercially available from Rogers Corporation), both based on the total volume of the substrate minus the glass fiber reinforcement layer. The coated boron nitride was prepared by coating boron nitride powder (Momentive PT-120) with 10 ALD cycles of aluminum oxide. The thickness of the aluminum oxide coating was 5 nm. Thermal conductivity and peel strength are shown in Table 2.
[0071] Example 8: Printed Circuit Board Substrate Comprising Uncoated Boron Nitride
[0072] A printed circuit board substrate was prepared containing 15 volume % of uncoated boron nitride and 85 volume % of RO4000 (commercially available from Rogers Corporation). The uncoated boron nitride was Momentive PT-100. The thermal conductivity and peel strength are shown in Table 2.
[0073]
[0074] Table 2 shows that the peel strength of the printed circuit board substrate of Example 7 containing coated boron nitride is significantly improved compared to the printed circuit board substrate of Example 8 containing the same amount of boron nitride but not coated.
[0075] Examples 9 to 11: Effect of coated boron nitride in multilayer composites
[0076] Using a conventional solution prepreg process, a dielectric substrate containing 17.3% by volume of PBN20 and 27.6% by volume of fused amorphous silica particles was produced using a 1674 type woven glass fabric. The prepreg material was made with both boron nitride aggregates as is and aggregates coated with alumina using 4 ALD cycles (coating thickness of 0.4 nm). The nominal composition of the prepreg material is shown in Table 3, where the polymer blend includes a mixture of 1,2-polybutadiene (NISSO-PBB-3000), butadiene-styrene block copolymer (KRATON D1118 ET), and EPDM terpolymer (TRILENE 65) in an amount sufficient to become a continuous phase.
[0077]
[0078] Multiple sheets of the resulting prepreg material having a nominal pressed thickness of 0.25 millimeters (mm) (0.010 inches) were stacked and laminated to 1.0 ounces per square foot (305 grams per square meter) of electrodeposited copper foil to produce test panels having nominal core thicknesses of 0.508 mm (0.020 inches) and 1.52 millimeters (0.060 inches). Table 4 shows a summary of the properties of Examples 9 and 10, respectively, containing uncoated boron nitride and coated boron nitride, where kV / cm stands for kilovolts per centimeter.
[0079]
[0080] Table 4 shows that Example 10, which contains coated boron nitride, has greater dielectric breakdown strength and lower water absorption, indicating improved filler for polymer interface. Table 4 also shows lower water absorption relative to Example 9. This low water absorption is particularly important because the printed circuit process involves immersion in a water bath, and the ingress of ionic materials can have a deleterious effect on electrical properties. These benefits are obtained without a significant impact on the Z-direction thermal conductivity.
[0081] In addition to the beneficial effects on dielectric strength and water absorption, the long-term resistance to thermo-oxidative degradation at elevated temperatures can be significantly improved by using coated boron nitride. Figure 5 It is shown that the dielectric substrate comprising coated boron nitride of Example 11 exhibits a 4-fold increase in the half-life of dielectric strength when continuously exposed to 200°C. Specifically, Figure 5 The half-life of Example 9 comprising uncoated boron nitride (lower curve) and Example 11 comprising coated boron nitride at a thickness of 0.51 mm (0.020 inches) (upper curve) are shown to be 980 hours and 4200 hours, respectively.
[0082] Various non-limiting aspects of the present disclosure are set forth below.
[0083] Aspect 1A: A printed circuit board substrate, comprising: a polymer matrix; a reinforcement layer; and a plurality of coated boron nitride particles; wherein the plurality of coated boron nitride particles comprises a coating having an average coating thickness of 0.5 nm to 100 nm, or 1 nm to 100 nm.
[0084] Aspect 1B: A printed circuit board substrate comprising: a polymer matrix, wherein the polymer matrix comprises at least one of an epoxy resin, a polyphenylene ether, a polystyrene, an ethylene-propylene dicyclopentadiene copolymer, a polybutadiene, a polyisoprene, a fluoropolymer, or a cross-linked matrix, the cross-linked matrix comprising at least one of triallyl cyanurate, triallyl isocyanurate, 1,2,4-trivinylcyclohexane, trimethylolpropane triacrylate, or trimethylolpropane trimethacrylate; a reinforcement layer; and a plurality of coated boron nitride particles; wherein the plurality of coated boron nitride particles comprises a coating having an average coating thickness of 0.5 nm to 100 nm, or 1 nm to 100 nm.
[0085] Aspect 1C: A printed circuit board substrate comprising: a thermosetting polymer matrix comprising at least one of an epoxy resin, polybutadiene, or polyisoprene; a reinforcement layer; and a plurality of coated boron nitride particles; wherein the plurality of coated boron nitride particles comprises a coating having an average coating thickness of 0.5 nm to 100 nm, or 1 nm to 100 nm.
[0086] Aspect 2: The printed circuit board substrate of Aspect 1, wherein the average particle size of the plurality of coated boron nitride particles is 0.1 micrometer to 1000 micrometers, or 5 micrometers to 500 micrometers, or 25 micrometers to 150 micrometers, or 3 micrometers to 40 micrometers.
[0087] Aspect 3: The printed circuit board substrate of any one or more of the preceding aspects, wherein the coating comprises at least one of an inorganic carbide, an inorganic oxide, an inorganic nitride, an inorganic sulfide, an inorganic hydroxide, or an inorganic phosphide. The inorganic hydroxide, if present, may include at least one of aluminum hydroxide, zinc hydroxide, or silicon hydroxide.
[0088] Aspect 4: The printed circuit board substrate of any one or more of the preceding aspects, wherein the coating comprises at least one of silicon dioxide or aluminum oxide.
[0089] Aspect 5: The printed circuit board substrate of any one or more of the preceding aspects, wherein the thickness is 0.5 nm to 30 nm, or 1 nm to 20 nm, or less than or equal to 5 nm.
[0090] Aspect 6: The printed circuit board substrate of any one or more of the preceding aspects, wherein the coating is disposed on 10A% to 100A%, or 50A% to 100A%, or 90A% to 100A% of the surface of the plurality of boron nitride particles.
[0091] Aspect 7: The printed circuit board substrate of any one or more of the preceding aspects, wherein the plurality of coated boron nitride particles comprises less than 1 wt%, or 0.001 wt% to 0.9 wt%, or 0.001 wt% to 0.5 wt%, or 0.005 wt% to 0.1 wt% of the coating based on the total weight of the plurality of coated boron nitride particles.
[0092] Aspect 8: The printed circuit board substrate of any one or more of the preceding aspects, wherein the plurality of coated boron nitride particles comprises ALD coated particles.
[0093] Aspect 9: The printed circuit board substrate of any one or more of the preceding aspects, wherein the printed circuit board substrate comprises 1 volume % to 85 volume %, or 1 volume % to 50 volume %, or 5 volume % to 35 volume %, or 10 volume % to 25 volume % of a plurality of coated boron nitride particles based on the total volume of the printed circuit board substrate.
[0094] Aspect 10: The printed circuit board substrate of any one or more of the preceding aspects, wherein the printed circuit board substrate comprises 15 volume % to 99 volume %, or 50 volume % to 99 volume %, or 65 volume % to 95 volume %, or 75 volume % to 80 volume % of the thermosetting polymer matrix based on the total volume of the printed circuit board substrate.
[0095] Aspect 11: The printed circuit board substrate of any one or more of the preceding aspects, wherein the reinforcement layer comprises a plurality of glass fibers.
[0096] Aspect 12: The printed circuit board substrate of any one or more of the preceding aspects, wherein the thermosetting polymer matrix comprises at least one of an epoxy resin, a butadiene homopolymer, an isoprene homopolymer, a butadiene-vinyl aromatic copolymer, or an isoprene-vinyl aromatic copolymer. The thermosetting polymer matrix may comprise an epoxy resin. The thermosetting polymer matrix may comprise polybutadiene. The thermosetting polymer matrix may comprise polyisoprene.
[0097] Aspect 13: The printed circuit board substrate of any one or more of the preceding aspects, wherein the printed circuit board substrate has a peel strength greater than or equal to 3 pli as determined in accordance with IPC-TM-650-2.4.8.
[0098] Aspect 14: A circuit material comprising the printed circuit board substrate of any one or more of the preceding aspects and a conductive layer disposed on at least one surface of the printed circuit board substrate.
[0099] Aspect 15: A method of making a printed circuit board substrate of any one or more of the preceding aspects, comprising: forming a mixture comprising a thermosetting composition and a plurality of coated boron nitride particles; coating a reinforcement layer with the mixture; and curing the thermosetting composition to form the printed circuit board substrate.
[0100] Aspect 16: The method of aspect 15, wherein coating the reinforcement layer comprises at least one of dip coating, knife-on-roll coating, roll-to-roll coating, and the like.
[0101] Aspect 17: The method of Aspect 16, wherein coating the reinforcement layer includes roll-to-roll coating the reinforcement layer with the mixture, which is performed by first unwinding the reinforcement layer from a first roll, passing the reinforcement layer through the mixture, passing the reinforcement layer through a solvent drying zone and at least partially curing the thermosetting mixture, and winding the coated reinforcement layer onto a second roll.
[0102] Aspect 18: The method of any one or more of Aspects 15 to 17, wherein curing comprises partially curing to form a prepreg.
[0103] Aspect 19: The method of any one or more of Aspects 15 to 18, further comprising depositing a conductive layer on at least one surface of the printed circuit board substrate.
[0104] Aspect 20: The method of any one or more of Aspects 15 to 19, further comprising depositing a coating on the plurality of boron nitride coated particles by atomic layer deposition prior to forming the mixture.
[0105] Compositions, methods and articles may alternatively include, consist of, or consist essentially of any suitable material, step or component disclosed herein. Compositions, methods and articles may additionally or alternatively be expressed as being free of or substantially free of any material (or substance), step, or component that is not otherwise necessary to achieve the function or purpose of the composition, method and article.
[0106] As used herein, unless the context clearly indicates otherwise, "one", "a kind of", "said" and "at least one" do not represent quantitative limitations, and are intended to cover the singular and the plural. For example, unless the context clearly indicates otherwise, "element" has the same meaning as "at least one element". Unless the context clearly indicates otherwise, the term "or" means "and / or". References to "aspects", "one embodiment", "another embodiment", "some embodiments" and the like throughout the specification mean that the specific elements (e.g., features, structures, steps or characteristics) described in conjunction with the embodiment are included in at least one embodiment described herein, and may or may not be present in other embodiments. In addition, it should be understood that the described elements can be combined in any suitable manner in multiple embodiments.
[0107] When an element (e.g., layer, film, region, or substrate) is referred to as being "on" another element, it can be directly on the other element or intervening elements may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0108] In general, compositions, methods and articles may alternatively include, consist of, or consist essentially of any ingredients, steps or components disclosed herein. Compositions, methods and articles may additionally or alternatively be expressed, performed, or manufactured to be free of or substantially free of any ingredients, steps, or components that are not necessary to achieve the function or purpose of the claims.
[0109] Unless otherwise specified herein, all test standards are the most recent standards in effect prior to the filing date of this application or, if priority is claimed, prior to the filing date of the earliest priority application in which such test standard appears.
[0110] The endpoints of all ranges involving the same component or property are inclusive, independently combinable, and include all intermediate points and ranges. For example, the range of "up to 25% by weight, or 5% by weight to 20% by weight" includes the endpoints and all intermediate values of the range of "5% by weight to 25% by weight", such as 10% by weight to 23% by weight, etc.
[0111] The term "combination" includes blends, mixtures, alloys, reaction products, etc. Additionally, "at least one" means that the list includes each element individually, as well as combinations of two or more elements in the list, and combinations of at least one element in the list with similar unnamed elements.
[0112] Unless defined otherwise, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0113] All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if a term in the present application contradicts or conflicts with a term in the incorporated reference, the term in the present application takes precedence over the conflicting term in the incorporated reference.
[0114] Although specific embodiments have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently foreseeable or may not currently be foreseeable may occur to applicants or other technical personnel in the art. Therefore, the appended claims as submitted and as they may be amended are intended to cover all such alternatives, modifications, variations, improvements, and substantial equivalents.
Claims
1. A printed circuit board substrate, comprising: A polymer matrix, wherein the polymer matrix comprises at least one of epoxy resin, polyphenylene ether, polystyrene, ethylene-propylene dicyclopentadiene copolymer, polybutadiene, polyisoprene, fluoropolymer, or a cross-linked matrix comprising at least one of triallyl cyanurate, triallyl isocyanurate, 1,2,4-trivinylcyclohexane, trimethylolpropane triacrylate, or trimethylolpropane trimethacrylate; Enhancement layer; and 10% to 50% by volume of a plurality of coated boron nitride particles having an average particle size of 5 micrometers to 500 micrometers based on the total volume of the printed circuit board substrate; wherein the plurality of coated boron nitride particles comprises a coating layer comprising aluminum oxide, wherein the coating layer has an average coating thickness of 0.5 nanometers to 10 nanometers; wherein the peel strength of the printed circuit board substrate determined according to IPC-TM-650-2.4.8 is greater than or equal to 3 pli; and The Z-direction thermal conductivity of the printed circuit board substrate is at least 90% of that of an equivalent printed circuit board substrate comprising boron nitride particles without the coating comprising aluminum oxide. 2 . The printed circuit board substrate of claim 1 , wherein the plurality of coated boron nitride particles have an average particle size of 10 microns to 250 microns.
3. The printed circuit board substrate of claim 1, wherein the coating further comprises silicon dioxide.
4. The printed circuit board substrate of claim 1, wherein the coating is disposed on 10 A% to 100 A% of the total surface area of the plurality of coated boron nitride particles.
5. The printed circuit board substrate of claim 1, wherein the coating is disposed on 50 A% to 100 A% of the total surface area of the plurality of coated boron nitride particles.
6. The printed circuit board substrate of claim 1, wherein the coating is disposed on 90 A% to 100 A% of the total surface area of the plurality of coated boron nitride particles.
7. The printed circuit board substrate of claim 1, wherein the plurality of coated boron nitride particles comprises less than 1 wt% of the coating layer based on the total weight of the plurality of coated boron nitride particles.
8. The printed circuit board substrate of claim 1, wherein the plurality of coated boron nitride particles comprises 0.001 wt% to 0.9 wt% of the coating layer based on the total weight of the plurality of coated boron nitride particles.
9. The printed circuit board substrate of claim 1, wherein the plurality of coated boron nitride particles comprises 0.001 wt% to 0.5 wt% of the coating layer based on the total weight of the plurality of coated boron nitride particles.
10. The printed circuit board substrate of claim 1, wherein the plurality of coated boron nitride particles comprises 0.005 wt% to 0.1 wt% of the coating layer based on the total weight of the plurality of coated boron nitride particles.
11. The printed circuit board substrate of claim 1, wherein the plurality of coated boron nitride particles comprises ALD coated particles.
12. The printed circuit board substrate of claim 1, wherein the printed circuit board substrate comprises 10 volume % to 25 volume % of the plurality of coated boron nitride particles based on the total volume of the printed circuit board substrate.
13. The printed circuit board substrate of claim 1, wherein the printed circuit board substrate comprises 15 volume % to 99 volume % of the thermosetting polymer matrix based on the total volume of the printed circuit board substrate.
14. The printed circuit board substrate of claim 1, wherein the printed circuit board substrate comprises 50 volume % to 99 volume % of the thermosetting polymer matrix based on the total volume of the printed circuit board substrate.
15. The printed circuit board substrate of claim 1, wherein the printed circuit board substrate comprises 65 volume % to 95 volume % of the thermosetting polymer matrix based on the total volume of the printed circuit board substrate.
16. The printed circuit board substrate of claim 1, wherein the printed circuit board substrate comprises 75 volume % to 80 volume % of the thermosetting polymer matrix based on the total volume of the printed circuit board substrate.
17. The printed circuit board substrate of claim 1, wherein the reinforcement layer comprises a plurality of glass fibers.
18. The printed circuit board substrate of any one of claims 13 to 16, wherein the thermosetting polymer matrix comprises at least one of an epoxy resin, a butadiene homopolymer, an isoprene homopolymer, a butadiene-vinyl aromatic copolymer, or an isoprene-vinyl aromatic copolymer.
19. A circuit material comprising the printed circuit board substrate according to any one of claims 1 to 18 and a conductive layer provided on at least one surface of the printed circuit board substrate.
20. A method of manufacturing a printed circuit board substrate according to any one of claims 1 to 18, comprising forming a mixture comprising a thermosetting composition and the plurality of coated boron nitride particles; coating a reinforcement layer with the mixture; as well as The thermosetting composition is cured to form the printed circuit board substrate.
21. The method of claim 20, wherein the reinforcement layer comprises a plurality of glass fibers.
22. The method of claim 21, wherein coating the reinforcement layer comprises roll-to-roll coating the reinforcement layer with the mixture by first unwinding the reinforcement layer from a first roll, passing the reinforcement layer through the mixture, passing the reinforcement layer through a solvent drying zone and at least partially curing the mixture, and winding the coated reinforcement layer onto a second roll.
23. The method of claim 21, wherein the curing comprises partial curing to form a prepreg.
24. The method of claim 21, further comprising depositing a conductive layer on at least one surface of the printed circuit board substrate.
25. The method of claim 21, further comprising depositing the coating on a plurality of boron nitride particles by atomic layer deposition prior to forming the mixture.