Battery and method for manufacturing battery

The carbon segregation layer is formed by segregating the binder on the surface of the solid electrolyte layer of the all-solid-state battery, which solves the problem of the solid electrolyte layer becoming hard and brittle after being pressurized and the risk of short circuit, and achieves high strength and high ionic conductivity. Battery design.

CN112930611BActive Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980070725.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-28
Filing Date
2019-11-29
Publication Date
2024-10-11
Estimated Expiration
2039-11-29

AI Technical Summary

Technical Problem

The solid electrolyte layer of existing all-solid-state batteries easily becomes hard and brittle after being pressurized, leading to an increased risk of short circuits, and the uniform distribution of the adhesive will affect ionic conductivity and reduce battery characteristics.

Method used

By segregating the adhesive on the surface of the solid electrolyte layer, a carbon segregated layer is formed. The convection and heating conditions in the drying process are used to concentrate the adhesive on the surface to form a carbon-rich layer, which improves the strength and collapse resistance of the solid electrolyte layer. capability while maintaining high ionic conductivity.

Benefits of technology

The high strength and low risk of short circuit of the solid electrolyte layer is achieved, ensuring the high reliability and ionic conductivity of the battery, and reducing the risk of collapse of the solid electrolyte layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112930611B_ABST
    Figure CN112930611B_ABST
Patent Text Reader

Abstract

The battery disclosed in the present invention comprises a first electrode, a second electrode and a solid electrolyte layer arranged between the first electrode and the second electrode, wherein the solid electrolyte layer contains at least a solid electrolyte and carbon atoms, and contains a carbon segregation layer, wherein the concentration of the carbon atoms in the carbon segregation layer is higher than the concentration of the carbon atoms in a region of the solid electrolyte layer excluding the carbon segregation layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a battery and a method for manufacturing the battery. Background Art

[0002] Patent Documents 1 and 2 both describe an all-solid-state battery including a layer containing carbon in a solid electrolyte layer.

[0003] Prior Art Literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2006-128014

[0006] Patent Document 2: Japanese Patent Application Publication No. 2011-086554 Summary of the invention

[0007] In the prior art, it is desired to obtain a battery with high reliability.

[0008] A battery involved in one embodiment of the present invention comprises a first electrode, a second electrode and a solid electrolyte layer arranged between the first electrode and the second electrode, wherein the solid electrolyte layer contains at least a solid electrolyte and carbon atoms, and contains a carbon segregation layer, and the concentration of the carbon atoms in the carbon segregation layer is higher than the concentration of the carbon atoms in a region of the solid electrolyte layer excluding the carbon segregation layer.

[0009] According to one embodiment of the present disclosure, it is possible to realize a highly reliable battery capable of reducing the risk of short circuit, for example. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is a schematic cross-sectional view of an all-solid-state battery as an example of the battery in Embodiment 1.

[0011] Figure 2 This is a flowchart of a first example of the method for manufacturing a battery in the second embodiment.

[0012] Figure 3 This is a flowchart of a second example of the method for manufacturing a battery in the second embodiment.

[0013] Figure 4A Shown are scanning electron microscope (SEM) images of cross sections of batteries produced in Examples and carbon mapping analysis results.

[0014] Figure 4B Shown are SEM images of cross sections of batteries produced in Examples and results of carbon mapping analysis.

[0015] Figure 5AThe graph shows the results of carbon mapping analysis of the cross section of the battery produced in the example and the carbon mapping intensity converted into numerical values.

[0016] Figure 5B The graph shows the results of carbon mapping analysis of a cross section of a battery produced in Example and quantified carbon mapping intensity. DETAILED DESCRIPTION

[0017] (Insights that form the basis of this disclosure)

[0018] For the reason that it is more advantageous from the viewpoint of large-area, continuous and mass production, the application of the coating process to the manufacture of all-solid-state batteries has been studied. In the coating process, first, the powder is dispersed in a solvent to make a slurry. Then, using the slurry, a coating film is formed on a substrate by a method such as screen printing or die coating. The solvent in the resulting coating film is volatilized by a thermal process such as heating in a drying furnace. A dry film is thus obtained. Generally, in order to obtain a slurry with a certain degree of viscosity suitable for the coating process, in addition, in order to ensure the strength of the dry film and the adhesion of the dry film to the substrate, a binder is added to the slurry when making the slurry.

[0019] It can be considered that the binder is not an indispensable substance for the battery characteristics of the all-solid-state battery. However, it is a necessary substance when a coating process is used for film formation. When a coating process is used, the powder is dispersed in a solvent to make a slurry, and the slurry is applied. In order to have both good coating properties and film quality, it is important to keep the slurry at a certain viscosity. In order to keep the slurry viscous, a dispersion process is used to make the slurry also contain a binder. At this time, by controlling the dispersion process, the binder can be evenly dispersed in the slurry together with the powder. Therefore, by controlling the dispersion process, the content of the binder in the slurry can also be controlled and limited to a minimum.

[0020] For example, in the case of making a solid electrolyte layer of an all-solid battery by a coating process, a solid electrolyte slurry is made by dispersing a powder of a solid electrolyte in a solvent. Using the solid electrolyte slurry, a coating film is formed on an electrode (i.e., a positive electrode and a negative electrode) as a substrate by a coating process. The electrode, for example, can be composed of a collector and an electrode layer (i.e., a positive electrode layer and a negative electrode layer) disposed on the collector. The electrode layer can also be made by a coating process. In order to improve battery performance, the dry film of the electrode layer obtained by the coating process can be pressed before applying the solid electrolyte slurry.

[0021] In the state of slurry, the binder contained in the solid electrolyte layer is uniformly dispersed in the solvent together with the solid electrolyte particles. In the state of a dry film obtained by drying the coating of the slurry applied on the electrode layer, the binder exists between the solid electrolyte particles and the particles are bonded to each other, thereby ensuring the strength as a film. Furthermore, the binder contained in the solid electrolyte layer is usually an organic binder. Therefore, the solid electrolyte layer made by the coating process usually contains carbon atoms derived from the organic compound constituting the binder.

[0022] After forming solid electrolyte layers on the positive electrode and the negative electrode respectively by a coating process, the solid electrolyte layer on the positive electrode and the solid electrolyte layer on the negative electrode are overlapped relative to each other, and the obtained stack is pressed in the stacking direction. Thus, the solid electrolyte layer on the positive electrode and the solid electrolyte layer on the negative electrode are joined to produce a full solid-state battery. At this time, the surface of the solid electrolyte layer formed on the positive electrode layer and the surface of the solid electrolyte layer formed on the negative electrode layer form the bonding interface. By pressing, the filling rate of the solid electrolyte layer is increased and densified, but at the same time it becomes hard and brittle. Therefore, in the case of rebound during pressing and / or impact from the outside, it is possible that the solid electrolyte layer cracks and so on, so that part of the solid electrolyte layer collapses. If a part of the solid electrolyte layer is missing, the solid electrolyte layer cracks, etc., the insulation function between the positive and negative electrodes is reduced, so that a short circuit is possible.

[0023] In the case of making a solid electrolyte layer of an all-solid battery by a coating process, as described above, the solid electrolyte layer is sometimes pressurized in order to bond with an electrode, in order to bond with each other by the solid electrolyte layer, and / or in order to increase the filling rate. The pressurized solid electrolyte layer has an increased filling rate, but sometimes becomes hard and brittle. The solid electrolyte layer is responsible for insulating the positive electrode from the negative electrode. Therefore, in the case of cracks in the solid electrolyte layer due to pressurization, defects at the ends of the solid electrolyte layer, etc., the risk of short circuit increases. Therefore, ensuring the strength of the joint of the solid electrolyte layer becomes a problem.

[0024] The inventors have conducted in-depth research on the above-mentioned issues and have newly discovered that when there is a layer in which the bonding force between the powders is strengthened by a binder near the bonding interface of the solid electrolyte layer, the membrane strength is maintained high even after the solid electrolyte layer is densified by pressurization, which can reduce the risk of short circuits.

[0025] Furthermore, if a layer reinforced by an adhesive is formed at the bonding interface, it is also conceivable to apply a slurry containing an adhesive as another layer on the solid electrolyte layer to use it as an adhesive layer. However, in the case of making it using such a method, it can be considered that the layer containing an adhesive becomes a layer formed by uniformly connecting the components of the adhesive to each other. That is, it can be considered that a continuous carbon-containing layer extending two-dimensionally is formed in the solid electrolyte layer by uniformly connecting the components of the adhesive to each other. Furthermore, the carbon atoms in the carbon-containing layer are carbon atoms derived from the organic compounds that constitute the adhesive. Such a carbon-containing layer becomes a resistance to the conduction of ions (such as lithium ions), thereby causing a reduction in battery characteristics. In addition, in the case of applying a slurry containing an adhesive as another layer on the solid electrolyte layer, the distribution of the adhesive is only on the outermost surface of the solid electrolyte layer formed on the electrode layer. Therefore, it is estimated that the improvement in strength is limited to the bonding interface of the solid electrolyte layer.

[0026] As a result of further repeated and in-depth research, the inventors succeeded in making the binder concentrate on the surface of the solid electrolyte layer in the drying process after the solid electrolyte layer is applied to the electrode layer. Specifically, the binder is concentrated on the surface of the solid electrolyte layer by utilizing the convection in the thickness direction of the solid electrolyte layer during drying. It is known that by using various heating methods such as hot plate heating and far infrared heating, vacuum drying, and changing the conditions such as drying time and heating rate, the convection state in the thickness direction of the solid electrolyte layer can be changed, so that the binder is concentrated near the surface.

[0027] The segregation state of the binder can be confirmed by, for example, cutting the all-solid battery after bonding and pressing with a cutter, grinding the cut surface with a cross-section polisher (CP), and performing carbon mapping analysis of the cross section of the solid electrolyte layer using an electron beam microanalyzer (EPMA). The segregation state of the binder in the solid electrolyte layer produced using the above-mentioned method of segregating the binder on the surface of the solid electrolyte layer in the drying process can be confirmed by, for example, the solid electrolyte layer of the embodiment described later. Figure 4A and 4B Shown are SEM images of cross sections of batteries produced in Examples and carbon mapping (C map) analysis results. Figure 5A and 5B The graph shows the results of carbon mapping analysis of a cross section of a battery produced in Example and quantified carbon mapping intensity.

[0028] Depend on Figure 4A and 4B as well as Figure 5A and 5BIt can be seen that a carbon segregation layer as a carbon segregation area exists in the solid electrolyte layer at a position away from the electrode layer and near the center in the thickness direction. It can be seen that the carbon segregation layer is not a continuous layer in which the binder components are evenly connected to each other, but is composed of a region in which multiple carbon segregation parts with diameters of several μm to tens of μm are two-dimensionally assembled. A carbon segregation layer of such a structure will not greatly hinder the conduction of ions (such as lithium ions). Therefore, according to a solid electrolyte layer including a carbon segregation layer of such a structure, it is possible to achieve high strength of the solid electrolyte layer produced by a coating process without greatly reducing the ion conductivity.

[0029] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0030] (Implementation Method 1)

[0031] The battery in embodiment 1 comprises a first electrode, a second electrode and a solid electrolyte layer disposed between the first electrode and the second electrode. The solid electrolyte layer comprises at least a solid electrolyte and carbon atoms, and comprises a carbon segregation layer. The concentration of carbon atoms in the carbon segregation layer is higher than the concentration of carbon atoms in the region of the solid electrolyte layer excluding the carbon segregation layer. Furthermore, the carbon segregation layer, in other words, is a carbon-rich layer (carbon-rich layer) composed of a region with a high concentration of carbon atoms.

[0032] In the battery in embodiment 1, the solid electrolyte layer includes the above-mentioned carbon segregation layer. The carbon segregation layer is difficult to collapse even after processes such as pressurization, and can have high strength. That is, the carbon segregation layer can have high collapse resistance. Therefore, by including the carbon segregation layer, even if the solid electrolyte layer is produced by a coating process, for example, the solid electrolyte layer can have high strength. As a result, the battery in embodiment 1, for example, has a reduced risk of short circuit and can achieve high reliability.

[0033] In the battery in Embodiment 1, the carbon atoms contained in the solid electrolyte layer and the carbon segregation layer are derived from, for example, an organic binder used when the solid electrolyte layer is made by a coating process. That is, in this case, the carbon atoms contained in the solid electrolyte layer and the carbon segregation layer are not amorphous carbon, but carbon constituting an organic compound, for example, which can be bonded to a hydrogen atom.

[0034] In the battery in Embodiment 1, the carbon segregation layer is composed of, for example, a region in which a plurality of segregation portions where carbon atoms are segregated are two-dimensionally assembled in the solid electrolyte layer. According to this structure, the battery in Embodiment 1 can achieve high reliability, and can suppress the reduction of ion conductivity caused by the carbon segregation layer to a small extent, and can ensure high ion conductivity.

[0035] In the battery in Embodiment 1, the carbon segregation layer may not be in contact with the first electrode and the second electrode. With this configuration, the battery in Embodiment 1 can achieve higher reliability.

[0036] In the battery in Embodiment 1, the carbon segregation layer can be exposed on the side of the solid electrolyte layer. In this configuration, the carbon segregation layer that can have high collapse resistance is exposed on the side of the solid electrolyte layer. Therefore, according to this configuration, the battery in Embodiment 1 can more reliably suppress collapse generated from the side of the solid electrolyte, and thus can achieve higher reliability.

[0037] In the battery of Embodiment 1, the thickness of the carbon segregation layer may be 10 μm or more and 50 μm or less. With this configuration, the battery of Embodiment 1 can further reduce the decrease in ion conductivity caused by the carbon segregation layer and can ensure higher ion conductivity.

[0038] In the battery in Embodiment 1, the first electrode may include a first electrode layer, the first electrode layer includes a first electrode active material, and the second electrode may include a second electrode layer, the second electrode layer includes a second electrode active material. In this case, the thickness of the carbon segregation layer may be greater than 0.1 times and less than 0.5 times the distance between the first electrode layer and the second electrode layer. According to this configuration, the battery in Embodiment 1 can effectively achieve both high reliability and high ion conductivity.

[0039] In the battery in embodiment 1, the concentration of carbon atoms in the carbon segregation layer can be more than 1.5 times and less than 10 times the concentration of carbon atoms in the region of the solid electrolyte layer excluding the carbon segregation layer, or more than 2 times and less than 5 times. According to this structure, the battery in embodiment 1 can effectively achieve both high reliability and high ion conductivity. Furthermore, in embodiment 1, the concentration of carbon atoms in the carbon segregation layer can be obtained by the following method: first, the battery in embodiment 1 is cut in the thickness direction, the cut surface is ground with CP, etc., and the carbon mapping analysis of the cut surface is performed using EPMA, and the obtained carbon mapping intensity is digitized. Furthermore, the concentration of carbon atoms in the region of the solid electrolyte layer excluding the carbon segregation layer is based on the lowest carbon concentration among the carbon concentrations in the region of the solid electrolyte layer that is not the carbon segregation layer.

[0040] In the battery in Embodiment 1, the carbon segregation layer may contain the solid electrolyte contained in the solid electrolyte layer in addition to carbon atoms. Since the carbon segregation layer contains not only carbon atoms but also the solid electrolyte, the battery in Embodiment 1 can achieve higher ion conductivity.

[0041] In the battery of Embodiment 1, the carbon segregation layer may further contain Li atoms. According to this configuration, the conduction of Li ions is not inhibited.

[0042] In the battery in embodiment 1, the first electrode may be a positive electrode and the second electrode may be a negative electrode, or the first electrode may be a negative electrode and the second electrode may be a positive electrode. The first electrode and the second electrode may be applied to, for example, a positive electrode or a negative electrode used in a known all-solid battery (e.g., a lithium ion battery). The first electrode and the second electrode may include a first electrode layer and a second electrode layer, respectively. That is, the first electrode may have a configuration in which a first electrode layer including a first electrode active material is configured on a current collector. In addition, the second electrode may have a configuration in which a second electrode layer including a second electrode active material is configured on a current collector.

[0043] The solid electrolyte contained in the solid electrolyte layer can be, for example, a solid electrolyte used in the solid electrolyte layer of a known all-solid battery (e.g., a lithium-ion battery). The solid electrolyte can be appropriately selected from solid electrolytes generally used in lithium-ion batteries, for example. Examples include sulfide-based solid electrolyte materials, oxide-based solid electrolyte materials, other inorganic solid electrolyte materials, and organic solid electrolyte materials. The solid electrolyte can be used alone or in combination of two or more. The shape and size are not particularly limited, but examples include microparticles. When the solid electrolyte is in the form of microparticles, the average particle size of the solid electrolyte can be 0.01 to 15 μm, or 0.2 to 10 μm. The average particle size is D50 (i.e., the median particle size of the volume distribution) evaluated by a laser diffraction scattering particle size distribution measuring device.

[0044] The carbon atoms contained in the solid electrolyte layer are derived from, for example, an organic binder used when the solid electrolyte layer is made by a coating process. For example, the organic binder can use a thermoplastic resin, but is not particularly limited, and can be appropriately selected from the organic binders used in known all-solid batteries (such as lithium ion batteries). Examples include thermoplastic elastomers of styrene-ethylene-butadiene copolymers. In addition, ethyl cellulose and polyvinylidene fluoride can also be used. In addition, polyethylene, polypropylene, polyisobutylene, polystyrene, polyvinyl chloride, polyvinyl acetate, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polydimethylsiloxane, cis-1,4-polybutadiene, polyisoprene, nylon-6, nylon-6,6, polyethylene terephthalate, and polyvinyl alcohol can also be used. The binder can be used alone or in combination of two or more.

[0045] A specific example of the battery in Embodiment 1 is shown. Figure 1This is a schematic cross-sectional view of an all-solid-state battery as an example of a battery in Embodiment 1. The all-solid-state battery comprises a current collector 1, a positive electrode layer 2, a negative electrode layer 3 and a solid electrolyte layer 4. The positive electrode layer 2 and the negative electrode layer 3 are arranged opposite to each other with the solid electrolyte layer 4 interposed therebetween. The solid electrolyte layer 4 contains at least a solid electrolyte and carbon atoms. Moreover, the solid electrolyte layer 4 contains a carbon segregation layer 5. In the all-solid-state battery, the first electrode is constituted by the current collector 1 and the positive electrode layer 2. The second electrode is constituted by the current collector 1 and the negative electrode layer 3. Furthermore, the current collector 1 is not particularly limited and can be appropriately selected from the current collectors used in known all-solid-state batteries (e.g., lithium-ion batteries).

[0046] (Implementation Method 2)

[0047] The method for manufacturing a battery in Embodiment 2 includes:

[0048] Step A, forming a first solid electrolyte layer on one side of the first electrode, and forming a second solid electrolyte layer on one side of the second electrode;

[0049] Step B, forming a first carbon segregation layer having a higher carbon atom concentration in a surface region of the first solid electrolyte layer than a carbon atom concentration in a region of the first solid electrolyte layer excluding the surface region; and

[0050] In step C, the first carbon segregation layer in the first solid electrolyte layer and the second solid electrolyte layer are bonded to each other.

[0051] The manufacturing method of the battery in embodiment 2 may: in the step B, form a second carbon segregation layer in the surface region of the second solid electrolyte layer, wherein the concentration of carbon atoms is higher than the concentration of carbon atoms in the region of the second solid electrolyte layer excluding the surface region; and in the step C, join the first carbon segregation layer in the first solid electrolyte layer and the second carbon segregation layer in the second solid electrolyte layer to each other.

[0052] Figure 2 A flowchart of a first example of a method for manufacturing a battery in Embodiment 2 is shown. Figure 3 A flow chart showing a second example of the method for manufacturing a battery in the second embodiment.

[0053] In the first example of the method for manufacturing a battery in the second embodiment, Figure 2 As shown, first, a first solid electrolyte layer is formed on one side of a first electrode, and a second solid electrolyte layer is formed on one side of a second electrode (S1). Next, a first carbon segregation layer is formed on the surface region of the first solid electrolyte layer (S2). Next, the first carbon segregation layer in the first solid electrolyte layer and the second solid electrolyte layer are bonded to each other (S3).

[0054] In the second example of the method for manufacturing a battery in the second embodiment, Figure 3 As shown, first, a first solid electrolyte layer is formed on one side of a first electrode, and a second solid electrolyte layer is formed on one side of a second electrode (S11). Next, a first carbon segregation layer is formed on the surface region of the first solid electrolyte layer, and a second carbon segregation layer is formed on the surface region of the second solid electrolyte layer (S12). Next, the first carbon segregation layer in the first solid electrolyte layer and the second carbon segregation layer in the second solid electrolyte layer are bonded to each other (S13).

[0055] According to the manufacturing method in embodiment 2, for example, the battery in embodiment 1 can be manufactured. That is, the battery that can be manufactured by the manufacturing method in embodiment 2 comprises a first electrode, a second electrode, and a solid electrolyte layer disposed between the first electrode and the second electrode. The solid electrolyte layer contains at least a solid electrolyte and carbon atoms, and contains a carbon segregation layer. Here, the solid electrolyte layer is formed by joining the first solid electrolyte layer and the second solid electrolyte layer. In addition, the carbon segregation layer is formed only by the first carbon segregation layer, or by the first carbon segregation layer and the second carbon segregation layer. The concentration of carbon atoms in the carbon segregation layer is higher than the concentration of carbon atoms in the region of the solid electrolyte layer excluding the carbon segregation layer.

[0056] As described in the first embodiment, the battery that can be manufactured by the manufacturing method in the second embodiment includes a carbon segregation layer, so that, for example, the risk of short circuit is reduced and high reliability can be achieved.

[0057] The manufacturing method in Embodiment 2 is described in more detail below. Figure 1 Specifically, a method for manufacturing a battery in which the first electrode is a positive electrode and is composed of a current collector and an electrode layer (i.e., a positive electrode layer), and the second electrode is a negative electrode and is composed of a current collector and an electrode layer (i.e., a negative electrode layer) is described.

[0058] The method for producing the electrode layer is not particularly limited, and a known technique can be used. The electrode layer is usually formed on a current collector.

[0059] The current collector is not particularly limited, and a current collector generally used in lithium ion batteries can be used, such as copper foil, copper alloy foil, aluminum foil, aluminum alloy foil, stainless steel foil, etc.

[0060] The active material used in the electrode layer is not particularly limited and can be selected according to the required function. Generally, the electrode layer can be produced using a mixture of the active material and, if necessary, a conductive material, a solid electrolyte, and / or a binder.

[0061] Active materials generally include positive electrode active materials and negative electrode active materials, and can be selected according to the functions required of each.

[0062] As positive electrode active materials, for example, lithium-containing transition metal oxides, vanadium oxides, chromium oxides, and lithium-containing transition metal sulfides can be cited. As lithium-containing transition metal oxides, lithium nickel oxide, lithium manganate, and lithium cobalt oxide can be cited. As examples of lithium-containing transition metal oxides, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNiCoMnO2, LiNiCoO2, LiCoMnO2, LiNiMnO2, LiNiCoMnO4, LiMnNiO4, LiMnCoO4, LiNiCoAlO2, LiNiPO4, LiCoPO4, LiMnPO4, LiFePO4, Li2NiSiO4, Li2CoSiO4, Li2MnSiO4, Li2FeSiO4, LiNiBO3, LiCoBO3, LiMnBO3, and LiFeBO3 can be cited. As examples of lithium-containing transition metal sulfides, LiTiS2, Li2TiS3, and Li3NbS4 can be cited. One or more kinds selected from these positive electrode active materials can be used.

[0063] Examples of negative electrode active materials include carbon materials, lithium alloys, metal oxides, lithium nitride (Li3N), metallic lithium, and metallic indium. Examples of carbon materials include artificial graphite, graphite, non-graphitizable carbon, and easily graphitizable carbon. Examples of lithium alloys include alloys of lithium and at least one metal selected from Al, Si, Pb, Sn, Zn, and Cd. Examples of metal oxides include LiFe2O3, WO2, MoO2, SiO, and CuO. A mixture or a composite of multiple materials may also be used as a negative electrode active material.

[0064] These positive electrode active materials or negative electrode active materials can be used alone or in combination of two or more. The shape and size are not particularly limited, but examples thereof include microparticles. When the active material is in microparticle form, the average particle size can be 0.5 to 20 μm, or 1 to 15 μm. The average particle size is D50 (i.e., the median particle size of the volume distribution) evaluated by the volume particle size distribution measured using a laser diffraction scattering particle size distribution measuring device. When the particle size distribution cannot be measured, the average particle size of the particles can be calculated by the following method. Observe the particle group with an electron microscope, and calculate the area of ​​specific particles in the electron microscope image by image processing. When it is not possible to directly observe the particle group alone, observe the structure containing the particles with an electron microscope, and calculate the area of ​​specific particles in the electron microscope image by image processing. The diameter of a circle having an area equal to the calculated area is regarded as the diameter of the specific particle. Calculate the diameter of any number of particles (for example, 10), and regard their average as the average particle size of the particles.

[0065] The conductive material is not particularly limited and can be appropriately selected from conductive materials generally used in lithium ion batteries. Examples thereof include graphite, carbon black, conductive fibers, conductive metal oxides, and organic conductive materials. These conductive materials can be used alone or in combination of two or more.

[0066] The solid electrolyte is not particularly limited and can be appropriately selected from solid electrolytes commonly used in lithium-ion batteries according to the type and purpose of the active material. Examples include sulfide-based solid electrolyte materials, oxide-based solid electrolyte materials, other inorganic solid electrolyte materials, organic solid electrolyte materials, and the like. The solid electrolyte can be used alone or in combination of two or more. The shape and size are not particularly limited, but examples include particulates. When the solid electrolyte is particulate, the average particle size can be 0.01 to 15 μm, and can be 0.2 to 10 μm. The average particle size is D50 (i.e., the median particle size of the volume distribution) evaluated by the volume particle size distribution measured using a laser diffraction scattering particle size distribution measuring device.

[0067] Binders can use, for example, thermoplastic resins, but are not particularly limited and can be appropriately selected from thermoplastic resins commonly used in lithium ion batteries. Examples include thermoplastic elastomers of styrene-ethylene-butadiene copolymers. In addition, ethyl cellulose and polyvinylidene fluoride can be used. In addition, polyethylene, polypropylene, polyisobutylene, polystyrene, polyvinyl chloride, polyvinyl acetate, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polydimethylsiloxane, cis-1,4-polybutadiene, polyisoprene, nylon-6, nylon-6,6, polyethylene terephthalate, and polyvinyl alcohol can also be used. Binders can be used alone or in combination of two or more.

[0068] The method for making the electrode layer is not particularly limited, and a known method can be used. A conductive material, a solid electrolyte, and / or a binder are mixed into the positive electrode active material or the negative electrode active material using a mixer as needed. The mixing ratio of each material can be appropriately determined according to the use of the battery, etc. The mixer is not particularly limited, and for example, a known mixer such as a planetary mixer and a ball mill can be used and mixed according to a known method.

[0069] The obtained mixture containing the active material is attached to the current collector so as to have a predetermined thickness.

[0070] In addition, as another forming method, the following method can be cited: prepare a slurry in which a mixture containing an active material is dispersed in an appropriate solvent, apply the slurry to a collector and dry it. As a coating method for the slurry, a general method can be used, for example, screen printing, die coating, spray coating, and scraper method can be cited.

[0071] The method for preparing the first solid electrolyte layer can be, for example, the following method: prepare a slurry in which a solid electrolyte and a binder are dispersed in an appropriate solvent, apply the slurry to one side of the first electrode (here, on the positive electrode layer), and dry the resulting coating. As a method for applying the slurry, general methods can be used, such as screen printing, die coating, spraying, and scraper methods. In addition, other methods such as the following method can also be used to form: apply the slurry on a supporting material, dry the resulting coating, thereby obtaining a solid electrolyte sheet, and transfer the solid electrolyte sheet to one side of the first electrode (here, on the positive electrode layer). The second solid electrolyte layer can also be formed on one side of the second electrode (here, on the negative electrode layer) in the same way as the first fixed electrolyte layer.

[0072] The adhesive can be segregated in the surface area of ​​the first solid electrolyte layer in the drying process after the first solid electrolyte layer is applied to the electrode layer. Thus, a first carbon segregation layer can be formed in the surface area of ​​the first solid electrolyte layer, in which the concentration of carbon atoms is higher than the concentration of carbon atoms in the area of ​​the first solid electrolyte layer excluding the surface area. Specifically, by utilizing the convection in the thickness direction of the first solid electrolyte layer during drying, the adhesive can be segregated in the surface area. For example, by various heating methods such as hot plate heating, far infrared heating and heating using radiation, vacuum drying, and changing the conditions such as drying time and heating rate, the convection condition in the thickness direction of the first solid electrolyte layer can be changed, so that the adhesive is segregated near the surface. In addition to the above-mentioned heating methods, rollers, conveyor belts or walking beams can also be used for continuous heating treatment. In order to improve the dryness, air inlet and outlet ports can also be set in the drying furnace to generate air flow. In the case where the heating treatment is an intermittent treatment, it is also possible to use a pump to combine vacuum drying as described above. In the above-mentioned various drying methods, the film quality of the dried film can be controlled by changing the conditions such as drying temperature, time, heating rate, gas flow rate, etc.

[0073] When forming the second carbon segregation layer in the surface region of the second solid electrolyte layer as in the manufacturing method of the second example, the same method as the method of forming the first carbon segregation layer can be used.

[0074] The first solid electrolyte layer and the second solid electrolyte layer can be joined by overlapping the first carbon segregation layer of the first solid electrolyte layer and the surface of the second solid electrolyte layer or the second carbon segregation layer of the second solid electrolyte layer opposite to each other and pressing. By adopting this pressing, the filling rate of the solid electrolyte is increased, and the contact interface between the particles of the active material and the solid electrolyte is increased, thereby improving the battery performance.

[0075] In the battery manufactured by the manufacturing method of Embodiment 2, since there is a carbon segregation layer near the bonding interface between the first solid electrolyte layer and the second solid electrolyte layer, the binder present between the particles further strengthens the bonding force between the particles, thereby suppressing the collapse of the solid electrolyte at the end and the occurrence of cracks in the film at the bonding interface. Therefore, the battery manufactured by the manufacturing method of Embodiment 2 is a highly reliable battery with a high strength of the solid electrolyte layer and a low risk of short circuit.

[0076] A method for manufacturing a battery, comprising:

[0077] Step a, forming a solid electrolyte layer on one side of the first electrode;

[0078] Step b, forming a carbon segregation layer having a higher concentration of carbon atoms in a surface region of the solid electrolyte layer formed on the one side of the first electrode than in a region of the solid electrolyte layer excluding the surface region; and

[0079] Step c: bonding the carbon segregation layer in the solid electrolyte layer and a second electrode to each other.

[0080] Furthermore, regarding the above-mentioned manufacturing method, the first electrode can be a positive electrode or a negative electrode. In addition, in the case of such a method of joining a solid electrolyte layer and an electrode, for example, a solid electrolyte layer comprising an adhesive is formed on at least one of the positive electrode and the negative electrode, and when the bonding is pressed oppositely, in order to improve bonding, it is also possible to heat. At this time, the temperature of the heating is preferably higher than the transition temperature of the adhesive contained in the electrode layer and / or the solid electrolyte layer. The transition temperature of the adhesive can be measured using thermomechanical analysis (TMA), dynamic viscoelasticity measurement (DMA), differential scanning calorimetry (DSC), differential scanning calorimeter thermal analysis (DTA), etc.

[0081] Example

[0082] In this embodiment, a mixture of sulfide solid electrolytes Li2S and P2S5 is used as a solid electrolyte. As a binder, a styrene-based thermoplastic elastomer is used. As a styrene-based thermoplastic elastomer, "Taftec M1913" manufactured by Asahi Kasei Corporation is used. As a solvent for slurry preparation, 1,2,3,4-tetralin is used. They are mixed to obtain a solid electrolyte layer slurry. Using a printing method using a metal mask, the solid electrolyte slurry is applied to a square electrode layer with a single side of 20 mm in thickness to a thickness of about 100 μm.

[0083] The obtained coating film is dried by intermittent drying using a drying furnace equipped with a sheath heater on the side. The temperature is raised to 100°C in 20 minutes, and after being kept for 10 minutes, the dried sample is taken out. Moreover, during the drying process, the drying furnace is continuously vented by a vacuum pump to form a reduced pressure atmosphere. Through this drying process, the convection in the thickness direction of the solid electrolyte layer during drying is utilized to cause the binder to be concentrated on the surface of the solid electrolyte layer. Furthermore, the binder is respectively concentrated on the surfaces of the solid electrolyte layer on the positive electrode and the solid electrolyte layer on the negative electrode.

[0084] The solid electrolyte layer on the positive electrode layer and the solid electrolyte layer on the negative electrode layer were stacked facing each other, and the obtained stack was heated to 120° C. at a speed of 5 t / cm in the stacking direction. 2 The all-solid-state battery is thus produced.

[0085] In order to confirm the segregation state of the binder, the all-solid-state battery after bonding and pressing was cut with a cutter, the cut surface was ground with CP, and carbon mapping analysis of the cross section of the solid electrolyte layer was performed with EPMA. The analysis was performed on two arbitrary locations of the battery. Figure 4A and 4B Shown are SEM images of cross sections of batteries produced in Examples and results of carbon mapping analysis. Figure 5A and 5B The graph shows the results of carbon mapping analysis of a cross section of a battery produced in Example and quantified carbon mapping intensity.

[0086] exist Figure 4A and Figure 4B In the carbon mapping analysis results shown in , the darker colored portion at the top is the carbon used in the negative electrode. Figure 4A and Figure 4B In the carbon mapping analysis results shown in , the dark-colored region of particles gathered in a band in the center of the solid electrolyte layer represents a concentrated area of ​​carbon. Figure 5A and Figure 5B In the carbon mapping analysis results shown in , the darker colored portion on the left is the carbon used in the negative electrode. Figure 5A and Figure 5B In the carbon mapping analysis results shown in , a dark-colored region in the form of particles gathered in a band in the central portion of the solid electrolyte layer represents a concentrated portion where carbon is concentrated.

[0087] Depend on Figure 4A and 4B as well as Figure 5A and 5B The results shown show that in the all-solid-state battery of this embodiment, a carbon segregation layer exists in the solid electrolyte layer at a position far from the electrode layer and near the center in the thickness direction. This segregation layer is not a uniformly connected layer, but a collection of segregation parts with a size of several μm to tens of μm. Therefore, the conduction of lithium ions is not greatly hindered. Furthermore, in Figure 5A and 5B In the graph showing the numerical carbon mapping intensity shown in , the portion with high intensity at the end of the graph is the negative electrode using carbon. Figure 5A and 5B It can be seen from the figure that in this embodiment, the carbon concentration in the carbon segregation layer in the solid electrolyte layer is at least twice that of the non-segregation part. These values ​​are obtained by integrating the numerical detection intensity in the thickness direction. Here, the so-called non-segregation part refers to the part with the lowest carbon concentration in the area within the solid electrolyte layer that is not a carbon segregation layer.

[0088] It was also found that, when the thickness of the solid electrolyte layer between the positive electrode layer and the negative electrode layer is assumed to be 100%, the carbon segregated layer has a thickness of approximately 30%.

[0089] It is also known that the carbon segregation layer contains not only carbon but also a solid electrolyte.

[0090] In addition, if you can Figure 4A and 4B As confirmed by the SEM image of , no collapse or cracking of the solid electrolyte was confirmed in the all-solid battery of this embodiment obtained by pressing. Therefore, it was confirmed that the battery of the present disclosure having a solid electrolyte layer including a carbon segregation layer has high reliability.

[0091] Industrial Applicability

[0092] The battery disclosed herein is a highly reliable battery and can be used as a secondary battery for various electronic devices and automobiles.

[0093] Description of Reference Numerals

[0094] 1. Current Collector

[0095] 2 Electrode layer (positive electrode layer)

[0096] 3 Electrode layer (negative electrode layer)

[0097] 4 Solid electrolyte layer

[0098] 5 Carbon segregation layer

Claims

1. A battery having: a first electrode; a second electrode; and a solid electrolyte layer disposed between the first electrode and the second electrode, The solid electrolyte layer contains at least a solid electrolyte and carbon atoms, and contains a carbon segregation layer, The carbon segregation layer is composed of a region in the solid electrolyte layer where a plurality of segregation portions where the carbon atoms are segregated are two-dimensionally aggregated. The thickness of the carbon segregation layer is greater than or equal to 10 μm and less than or equal to 50 μm. The concentration of the carbon atoms in the carbon segregation layer is 1.5 times or more and 10 times or less the concentration of the carbon atoms in a region of the solid electrolyte layer excluding the carbon segregation layer. The carbon atoms are derived from an organic binder used in manufacturing the solid electrolyte layer.

2. The battery according to claim 1, The carbon segregation layer is not in contact with the first electrode and the second electrode.

3. The battery according to claim 1 or 2, The carbon segregation layer is exposed on a side surface of the solid electrolyte layer.

4. The battery according to claim 1 or 2, The first electrode comprises a first electrode layer, and the first electrode layer comprises a first electrode active material. The second electrode comprises a second electrode layer, and the second electrode layer comprises a second electrode active material. The thickness of the carbon segregation layer is greater than or equal to 0.1 times and less than or equal to 0.5 times the distance between the first electrode layer and the second electrode layer.

5. The battery according to claim 1 or 2, The concentration of the carbon atoms in the carbon segregation layer is 2 times or more and 5 times or less the concentration of the carbon atoms in the region of the solid electrolyte layer excluding the carbon segregation layer.

6. The battery according to claim 1 or 2, The carbon segregation layer includes the solid electrolyte and the carbon atoms.

7. The battery according to claim 6, The carbon segregation layer further comprises Li atoms.

8. A method for manufacturing a battery, include: Step A, forming a first solid electrolyte layer on one side of the first electrode, and forming a second solid electrolyte layer on one side of the second electrode; Step B, forming a first carbon segregation layer in the surface region of the first solid electrolyte layer, wherein the concentration of carbon atoms in the first carbon segregation layer is higher than the concentration of carbon atoms in a region of the first solid electrolyte layer excluding the surface region; and Step C, joining the first carbon segregation layer in the first solid electrolyte layer and the second solid electrolyte layer to each other, the first solid electrolyte layer and the second solid electrolyte layer include a binder, In the step B, the first solid electrolyte layer is dried to cause the binder contained in the first solid electrolyte layer to be segregated in the surface region of the first solid electrolyte layer, thereby forming the first carbon segregated layer.

9. The method for manufacturing a battery according to claim 8, In the step B, the second solid electrolyte layer is dried so that the binder contained in the second solid electrolyte layer is segregated in the surface region of the second solid electrolyte layer, thereby forming a second carbon segregation layer in the surface region of the second solid electrolyte layer, and the concentration of carbon atoms in the second carbon segregation layer is higher than the concentration of carbon atoms in the region of the second solid electrolyte layer excluding the surface region. In the step C, the first carbon segregation layer in the first solid electrolyte layer and the second carbon segregation layer in the second solid electrolyte layer are bonded to each other.

10. A method for manufacturing a battery, include: Step a, forming a solid electrolyte layer on one side of the first electrode; Step b, forming a carbon segregation layer in the surface region of the solid electrolyte layer formed on the one side of the first electrode, wherein the concentration of carbon atoms in the carbon segregation layer is higher than the concentration of carbon atoms in the region of the solid electrolyte layer excluding the surface region; and Step c, joining the carbon segregation layer in the solid electrolyte layer and the second electrode to each other, The solid electrolyte layer comprises a binder, In the step b, the solid electrolyte layer is dried to cause the binder to be segregated in the surface region of the solid electrolyte layer, thereby forming the carbon segregated layer.