A device and method for measuring high temperature conductivity of molten glass
By using a high-temperature crucible and groove-embedded electrode sheet in a high-temperature melt measurement device, combined with a servo motor-controlled pressure gland, a stable conductivity cell is formed, and the problems of inaccurate measurement and easy breakage in the prior art are solved. It realizes high accuracy and wide application of glass melt conductivity measurement.
Patent Information
- Application Number
- CN202110353936.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-03-31
AI Technical Summary
The existing high-temperature molten glass conductivity measurement devices have problems such as inaccurate measurement, poor reproducibility and poor device versatility, especially in glass melt conductivity measurements under different materials and temperatures. The commonly used transparent quartz crucibles are prone to breaking at high temperatures. , increasing the testing cost.
A glass melt high-temperature conductivity measurement device including a high-temperature crucible, groove and pressure gland is designed. The groove is embedded with electrode sheets, and the tight fit between the pressure gland and the groove is controlled by a servo motor to form a stable conductivity cell. , ensure the length and cross-sectional area of the conductivity cell are constant, reduce measurement errors, and use corundum or zirconium oxide materials to improve high temperature resistance.
Accurate conductivity measurement of different types of glass melts at different temperatures is realized, which reduces measurement errors and costs, improves the stability and application range of the device, and can accurately measure within the range of glass softening point to 1600°C.
Smart Images

Figure CN112946028B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass production testing, and in particular relates to a device and method for measuring the high-temperature conductivity of molten glass. The device is suitable for rapid measurement of the conductivity of molten glass with different viscosities. Background Art
[0002] Generally, glass is a good insulator at room temperature. At high temperature, it has a lower resistivity because the mobility of alkali metal ions contained in it is much higher than that at room temperature. However, there is no standard method for measuring the conductivity of high-temperature molten glass in the world.
[0003] In the existing high-temperature molten glass conductivity test device, an observation window is provided on the high-temperature furnace, a scale line is engraved on the pot wall of the transparent quartz crucible, an electrode is connected to each side of the transparent quartz crucible, and both electrodes are connected to the electrochemical workstation. During operation, the height of the molten glass liquid in the transparent quartz crucible at different temperatures is observed through the transparent observation window on the front of the high-temperature furnace, and the accurate height of the glass liquid can be known by observing the position of the glass liquid level at the scale line. The temperature of the furnace body is recorded by a computer, that is, the resistance value of the glass to be tested under various temperature conditions. The conductivity of the glass to be tested under various temperature conditions is calculated using the formula σ=L / RA. σ is the conductivity of the glass to be tested, R is the glass resistance measured by the electrochemical workstation at different temperatures, L is the distance between the two electrode sheets, and A is the relative area between the two electrode sheets, where A=h*b, h is the height of the molten glass liquid in the transparent quartz crucible, and b is the longitudinal width of the transparent quartz crucible.
[0004] The above-mentioned existing technologies have the following deficiencies: (1) the cross-sectional area of the glass melt is obtained through the observation window on the high-temperature furnace and the scale marked on the transparent quartz crucible, which is highly subjective and has certain errors in reading. In addition, the viscosity of glass of different materials and glass melts at different temperatures will also be different, resulting in different fluidity of the glass melt in the transparent quartz crucible, which ultimately makes it difficult to read accurately; (2) some glass melts are opaque and generally have other colors (such as glass melts containing metal ions such as iron and copper). In addition, because glass melts are prone to splashing at high temperatures, the glass melts are prone to splashing. This makes it difficult to accurately determine the position of the glass melt surface, making it impossible to accurately read the reading; (3) The operating temperature of commonly used transparent quartz crucibles generally does not exceed 1100°C. Even high-purity quartz crucibles will crack due to crystal transformation at high temperatures, or crystallization will occur, causing the transparent crucible to turn white, making it impossible to read the reading. When the operating temperature exceeds 1450°C, the quartz crucible is relatively brittle and easy to break; (4) For the high-temperature conductivity measurement technology of glass melts, the test temperature is generally not less than 1200°C. If a specially made transparent crucible is used, the price is generally higher, resulting in increased testing costs.
[0005] In addition, the common methods for measuring the conductivity of molten glass include the direct resistance measurement method using a potential probe and the indirect resistance measurement method using a container coefficient. The former has higher accuracy, but requires a special disposable test container tank, which is costly. The latter can indirectly obtain the conductivity of the glass melt at high temperature through the relationship between the container coefficient and the melt conductivity. However, in the current measurement methods, due to the influence of the viscosity and capillary action of the glass melt, the reproducibility of the glass melt liquid level and the electrode position is generally not high, which affects the accuracy of the measurement results. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a high-temperature conductivity measuring device and method for molten glass, which has a compact structure, simple principle, high accuracy, strong stability, and can realize conductivity testing of different types of molten glass at different temperatures, in order to address the shortcomings of the prior art, such as inaccurate data measurement of the relative area between two electrode sheets, resulting in low precision and poor reproducibility of the conductivity measurement results of molten glass, as well as poor versatility of the measuring device.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] A device for measuring high-temperature conductivity of molten glass comprises: a high-temperature furnace with a furnace temperature control system, a high-temperature resistant and insulated crucible is placed in the high-temperature furnace, a groove for placing a glass sample to be measured is provided at the bottom of the inner side of the crucible, and the volume of the molten glass is greater than the volume of the groove; two opposite sides of the groove are respectively connected to an electrode sheet, and both electrode sheets are electrically connected to an electrochemical workstation; a high-temperature resistant and insulated gland is provided above the groove, and a lifting device is provided above the gland, and the gland is pressed or loosened by the lifting device to achieve the fitting or separation of the gland and the groove, so as to ensure that the closed conductivity cell formed by the groove, the electrode sheet and the gland is filled with molten glass.
[0009] As a further improvement of the present invention, the lifting device includes a screw rod, a connecting rod and a high-temperature resistant and insulating pressure rod, one end of the pressure rod is fixedly connected to the connecting rod, the other end of the pressure rod passes through the top of the high-temperature furnace and is arranged above the pressure cover, the connecting rod is connected to the screw rod, and the screw rod is connected to the servo motor.
[0010] As a further improvement of the present invention, the lifting device further comprises a support rod, the setting direction of the support rod is the same as the setting direction of the screw rod, and driven by the screw rod, the connecting rod moves up and down along the support rod.
[0011] As a further improvement of the present invention, the crucible, the pressure cover and the pressure rod are all made of corundum or zirconium oxide.
[0012] As a further improvement of the present invention, the cross section of the gland is circular, and the cross section of the groove is square; the diameter of the gland is smaller than the diameter of the crucible and larger than the diagonal length of the cross section of the groove.
[0013] As a further improvement of the present invention, the electrode sheet is embedded on the inner side wall of the groove, and the surface area of the electrode sheet is equal to the area of the inner side wall of the groove.
[0014] As a further improvement of the present invention, each of the electrode sheets is connected to the electrochemical workstation via a wire.
[0015] As a further improvement of the present invention, the electrode sheet is a platinum electrode sheet, and the wire is a platinum wire.
[0016] As a general technical concept, the present invention also provides a method for measuring the high-temperature conductivity of a glass melt, comprising the following steps:
[0017] 1) Processing the glass sample to be tested into a required size to ensure that the volume of the glass sample to be tested after melting is larger than the volume of the groove;
[0018] 2) Place the processed glass sample to be tested in the groove at the bottom of the inner side of the crucible, embed an electrode sheet on the two opposite sides of the groove, connect the two electrode sheets to the wires, and place the gland on the glass sample to be tested;
[0019] 3) placing the crucible in a high-temperature furnace, adjusting the pressure rod to be located above the pressure cover, and adjusting the pressure rod to descend and contact the upper surface of the pressure cover through a servo motor;
[0020] 4) Connect the wire to the electrochemical workstation, set the heating program of the high-temperature furnace through the furnace temperature control system, and heat the glass sample to be tested;
[0021] 5) After reaching the preset temperature, continue to keep the temperature to ensure that the glass sample to be tested is completely melted and fills the groove of the crucible; adjust the pressure rod to descend through the servo motor to apply pressure to the pressure cover so that the pressure cover fits tightly with the groove; detect the resistance value of the glass melt through the electrochemical workstation;
[0022] 6) adjusting the pressure rod to rise by the servo motor, removing the pressure on the pressure cover, and making the pressure rod contact the upper surface of the pressure cover; continuing to adjust the temperature in the high-temperature furnace, repeating steps 4) and 5) to obtain the resistance values of the glass melt at different temperatures;
[0023] 7) Substitute the resistance values of the molten glass at different temperatures obtained by the test into the following formula to calculate the conductivity of the molten glass at different temperatures:
[0024]
[0025] In the formula, σ is the conductivity of the glass melt to be measured, R is the resistance of the glass melt to be measured, L is the distance between the two electrodes, and A is the surface area of the electrode.
[0026] As a further improvement of the present invention, in step 5), the insulation time is ≥30 min.
[0027] Compared with the prior art, the advantages of the present invention are:
[0028] 1. The glass melt high temperature conductivity measuring device of the present invention is provided with a groove specially used for placing the glass sample to be measured inside the crucible, and electrode sheets are embedded on the two opposite inner side walls of the groove. The electrode sheets are connected to the electrochemical workstation through wires, so that the resistance value of the glass melt at the corresponding temperature can be quickly measured, and then the conductivity of the glass melt can be obtained. It has the advantages of simple principle and strong operability. At the same time, a gland is also provided above the groove, and the groove, the electrode sheet and the gland together form a closed conductivity cell, so that the glass melt forms a stable conductivity cell at high temperature. The glass melt is affected by temperature and thermal expansion coefficient, and gradually changes from solid to liquid at high temperature, and the volume gradually expands. The gland is tightly attached to the groove by the servo motor control, and the excess glass melt is discharged outside the groove. The overflowed glass melt is still stored in the crucible, which effectively controls the liquid level of the conductivity cell and does not damage the internal components of the high temperature furnace due to the overflow of the glass melt. At the same time, due to the insulating effect of the gland, the length and cross-sectional area of the molten glass contained in the groove are fixed, and a closed conductivity cell is formed with the electrode sheet, which effectively ensures that the length and cross-sectional area of the conductivity cell are always stable, and can eliminate the influence of the viscosity of the molten glass on the test results, greatly reducing the measurement error, so as to accurately determine the conductivity of different types of molten glass at different temperatures. It has the advantages of high precision, strong stability, and a wide range of applications, and can conveniently and accurately measure the conductivity of molten glass in the range from the glass softening point to 1600°C.
[0029] 2. The method for measuring the high-temperature conductivity of glass melt of the present invention is to make the glass sample to be tested into a small sample of the required size and then put it into the groove, and ensure that the volume of the glass melt is greater than the volume of the groove, and squeeze the excess glass melt out of the groove by pressing the cover, so as to ensure that the glass melt forms a stable conductivity cell at high temperature, and the groove plays a good positioning role, ensuring that the shape of the conductivity cell and the distance between the two electrodes remain constant, so that the conductivity of the measured glass melt is only related to the measured conductivity of the glass melt, completely avoiding the detection error caused by manually reading the liquid level data of the conductivity cell, effectively ensuring the accuracy of the measurement result, and well meeting the detection requirements of different types of glass melts. Furthermore, the glass melt overflowed due to thermal expansion at high temperature is stored in the crucible, and the conductivity of the same glass melt at different temperatures can be continuously measured, which not only improves the reliability of the detection result, but also effectively saves the detection cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The figure is a schematic diagram of the structural principle of the device for measuring the high-temperature conductivity of molten glass of the present invention.
[0031] Legend:
[0032] 1. High temperature furnace; 2. Crucible; 21. Groove; 3. Wire; 4. Electrode sheet; 5. Pressure cover; 6. Pressure rod; 7. Support rod; 8. Electrochemical workstation; 9. Screw; 10. Connecting rod. DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0034] Example
[0035] like Figure 1As shown, the glass melt high temperature conductivity measuring device of the present invention comprises: a high temperature furnace 1 with a furnace temperature control system, a high temperature resistant and insulated crucible 2 is placed in the high temperature furnace 1, a groove 21 for placing a glass sample to be measured is provided at the bottom of the inner side of the crucible 2, and the volume of the molten glass melt is greater than the volume of the groove 21. By adjusting the heating rate and the furnace temperature of the high temperature furnace 1, the glass sample to be measured can be heated, and the glass melt at the corresponding temperature can be obtained. An electrode sheet 4 is connected to the opposite sides of the groove 21, and the two electrode sheets 4 are electrically connected to the electrochemical workstation 8. A high temperature resistant and insulated pressure cap 5 is provided above the groove 21, and a lifting device is provided above the pressure cap 5. The lifting device squeezes or releases the pressure cap 5 to achieve the fitting or loosening of the pressure cap 5 and the groove 21, so as to ensure that the closed conductivity cell composed of the groove 21, the electrode sheet 4 and the pressure cap 5 is filled with glass melt. It can be understood that the size of the conductivity cell can be designed according to actual needs. During the measurement process, the excess molten glass is squeezed out of the groove 21 by the gland 5 to ensure that the molten glass always fills the conductivity cell to form a stable conductivity system.
[0036] In this embodiment, the electrode sheet 4 is embedded in the inner wall of the groove 21, and the surface area of the electrode sheet 4 is equal to the inner wall area of the groove 21. The existence of the groove 21 plays a good positioning role, ensuring that the shape of the conductivity cell and the distance between the two electrode sheets 4 remain constant, that is, L and A in the conductivity formula σ=L / RA are not easily changed by external interference, so the conductivity of the measured glass melt is only related to the measured glass melt resistance value R, which greatly improves the accuracy of the test result.
[0037] In this embodiment, each electrode sheet 4 is connected to an electrochemical workstation 8 via a wire 3. The resistance value of the glass melt at the corresponding temperature is detected by the electrochemical workstation 8, and the conductivity of the glass melt at the corresponding temperature can be calculated. Further, to improve the accuracy of the detection, the electrode sheet 4 is a platinum electrode sheet, the wire 3 is a platinum wire, and the diameter of the platinum wire can preferably be 0.3 mm to 1.0 mm.
[0038] In this embodiment, a groove 21 is provided inside the crucible 1 for placing the glass sample to be tested, and an electrode sheet 4 is provided on the two opposite inner side walls of the groove 21. The electrode sheet 4 is electrically connected to the electrochemical workstation to quickly measure the resistance value of the glass melt at the corresponding temperature, and then the conductivity of the glass melt is obtained, which has the advantages of simple principle and strong operability. At the same time, a gland 5 is also provided above the groove 21, and the groove 21, the electrode sheet 4 and the gland 5 together form a closed conductivity cell, so that the glass melt forms a stable conductivity cell at high temperature. The glass melt is affected by temperature and thermal expansion coefficient, and gradually changes from solid to liquid at high temperature, and the volume gradually expands. The gland 5 is controlled by the lifting device to fit tightly on the groove 21, and the excess glass melt is discharged outside the groove 21, and the overflowed glass melt is still stored in the crucible 2, which effectively controls the liquid level of the conductivity cell and does not damage the internal components of the high-temperature furnace 1 due to the overflow of the glass melt. At the same time, due to the insulating effect of the gland 5, the length and cross-sectional area of the glass melt contained in the groove 21 are fixed, and a closed conductivity cell is formed with the electrode sheet 4, which effectively ensures that the length and cross-sectional area of the conductivity cell are always stable, and can eliminate the influence of the viscosity of the glass melt on the test result, greatly reducing the measurement error, so as to accurately measure the conductivity of different types of glass melts at different temperatures. It has the advantages of high precision, strong stability, and a wide range of applications, and can conveniently and accurately measure the conductivity of the glass melt in the range of the glass softening point to 1600°C.
[0039] In this embodiment, the lifting device includes a screw rod 9, a connecting rod 10 and a high temperature resistant and insulated pressure rod 6, one end of the pressure rod 6 is fixedly connected to the connecting rod 10, the other end of the pressure rod 6 passes through the top of the high temperature furnace 1 and is arranged above the pressure cover 5, the connecting rod 10 is connected to the screw rod 9, and the screw rod 9 is connected to a servo motor with a pressure sensor (not shown in the figure). Further, the lifting device also includes a support rod 7, the setting direction of the support rod 7 is the same as the setting direction of the screw rod 9, and the connecting rod 10 moves up and down along the support rod 7 under the drive of the screw rod 9. Through the cooperation of the support rod 7 and the screw rod 9, the stability of the up and down movement of the pressure rod 6 is improved, which also improves the contact stability between the pressure cover 5 and the groove 21, and improves the use stability of the entire measuring device.
[0040] In this embodiment, the crucible 2, the gland 5 and the pressure rod 6 are all made of corundum. Corundum has excellent insulation and high temperature resistance, a small thermal expansion coefficient, and the conductivity cell formed at high temperature does not deform, achieving the effect of easy availability of raw materials and high cost performance. In addition, the crucible 2, the gland 5 and the pressure rod 6 used in this embodiment can also be made of high temperature resistant and insulating materials such as zirconium oxide, so as to facilitate the measurement of glass melt conductivity at higher temperatures and broaden the scope of application of the measurement device of this embodiment.
[0041] In this embodiment, the cross section of the gland 5 is circular, and the cross section of the groove 21 is square; the diameter of the gland 5 is smaller than the diameter of the crucible 2, and larger than the diagonal length of the cross section of the groove 21. The groove 21 is set as a square structure, which is not only conducive to the installation and fixation of the electrode sheet 4, but also ensures that the distance between the two electrode sheets 4 remains constant. The cross-sectional area of the gland 5 is larger than the cross-sectional area of the groove 21 to ensure that the excess glass melt is squeezed out of the groove 21, thereby ensuring the operational stability of the conductivity cell. It can be understood that in this embodiment, the gland 5 is in an unstressed state during the heating process of the glass melt in the groove 21. The glass melt in this process will overflow the groove 21 due to volume expansion, causing the displacement of the gland 5. After reaching the preset temperature and starting the insulation process, and before the conductivity measurement, the gland 5 will be forced to press the groove 21. Therefore, in the present invention, the diameter of the gland 5 is large enough, and even if the gland 5 is not at the center of the groove 21, it can still completely cover the upper surface of the groove 21.
[0042] At the same time, the present invention also provides a method for measuring high-temperature conductivity of a glass melt, comprising the following steps:
[0043] The crucible 2 is selected with an inner diameter of 45mm, an outer diameter of 55mm, and a height of 60mm (30mm hollowed out at the top). The groove 21 is located at the center of the crucible 2 and has a size of 25*20*15mm (length*width*height); the diameter of the gland 5 is 40mm and the thickness is 4mm; the size of the platinum electrode sheet is 20*15*0.3mm, and the diameter of the platinum wire is 0.5mm. From the above parameters, it can be seen that in this embodiment, L / A is 83.3m -1 .
[0044] 1) According to the density of the prepared glass (2.63g / cm -3 ) and the size of the groove 21 (25*20*15mm), weigh 25g of the glass sample, wherein the particle size of a single sample is not less than 5mm.
[0045] 2) Place the processed glass sample to be tested in the groove 21 at the bottom of the inner side of the crucible 2, embed an electrode sheet 4 on the two opposite sides of the groove 21, and both electrode sheets 4 are connected to the wire 3, and place the pressure cover 5 on the glass sample to be tested. The pressure cover 5 is located directly above the groove 21 to ensure that the pressure cover 5 can completely cover the groove 21 after the glass sample to be tested is melted. During the measurement process, the groove 21, the electrode sheet 4 and the pressure cover 5 together form a closed conductivity cell, so that the glass melt forms a stable conductivity cell at high temperature.
[0046] 3) Place the crucible 2 in the high temperature furnace 1, adjust the pressure rod 6 to be located above the gland 5, and adjust the pressure rod 6 to descend and contact the upper surface of the gland 5 through a servo motor (not shown in the figure). It can be understood that in order to improve the accuracy of the measurement, the pressure rod 6 should be located at the center of the gland 5 as much as possible, and at this time the pressure rod 6 is only against the gland 5, and the gland 5 is not in close contact with the groove 21, so that the glass melt expands and overflows the groove 21 during the heating process. At the same time, the gland 5 can be positioned by the pressure rod 6 to avoid the gland 5 from tilting during the heating and expansion of the glass melt, thereby affecting the stability of the conductivity cell. During the test, the pressure applied by the pressure rod 6 to the gland 5 achieves the pressing effect of the gland 5 on the groove 21, and the pressure rod 6 is controlled by a servo motor with a pressure sensor. The pressure on the pressure rod 6 can effectively determine whether the gland 5 is in close contact with the groove 21.
[0047] 4) Connect the wire 3 to the electrochemical workstation 8, set the heating program of the high temperature furnace 1 through the furnace temperature control system, and heat the glass sample to be tested at a rate of 5°C / min. It can be understood that in this embodiment, no special requirements are required for the heating rate during the measurement process, and it is sufficient to meet the heating requirements of the high temperature furnace 1.
[0048] 5) After reaching 1200°C, continue to keep warm for 30 minutes to ensure that the glass sample to be tested is completely melted and fills the groove 21 of the crucible 2; adjust the pressure rod 6 to descend through the servo motor, apply pressure to the pressure cover 5, so that the pressure cover 5 fits tightly with the groove 21, and squeezes the excess glass melt out of the groove 21 to ensure that the glass melt forms a stable conductivity cell in the groove 21; the resistance value of the glass melt is 378.64Ω detected by the electrochemical workstation 8. It can be understood that in order to improve the accuracy of the measurement results and ensure that the test of the conductivity of the glass melt is carried out at the specified temperature, the temperature of the high-temperature furnace 1 should be kept warm for no less than 30 minutes after reaching the preset temperature, and then the conductivity of the glass melt is tested to more accurately reflect the resistivity of the glass melt at this temperature.
[0049] 6) The pressure rod 6 is adjusted to rise by the servo motor to remove the pressure on the pressure cover 5, and the pressure rod 6 contacts the upper surface of the pressure cover 5. It can be understood that at this time, the pressure cover 5 is not in close contact with the groove 21, so that the glass melt continues to expand and overflows the groove 21 during the next heating process; the temperature in the high-temperature furnace 1 is continued to be adjusted, and steps 4) and 5) are repeated to obtain the resistance values of the glass melt at 1300°C and 1400°C, which are 100.36Ω and 12.49Ω respectively.
[0050] 7) Substitute the resistance values of the molten glass at different temperatures obtained by the test into the following formula to calculate the conductivity of the molten glass at different temperatures:
[0051]
[0052] In the formula, σ is the conductivity of the glass melt to be tested, R is the resistance value of the glass melt to be tested, L is the distance between the two electrode sheets 4, that is, the length of the conductivity cell, and A is the surface area of the electrode sheet 4, that is, the area of the conductivity cell. In this embodiment, when the temperature is 1200°C, the conductivity σ of the glass melt is 0.22s / m; when the temperature is 1300°C, the conductivity σ of the glass melt is 0.83s / m; when the temperature is 1400°C, the conductivity σ of the glass melt is 6.67s / m. It can be understood that as the temperature increases, the conductivity of the glass melt changes. By measuring the resistance value of the glass melt, the conductivity of the glass melt can be calculated by the formula; this embodiment can test the conductivity of different types of glass melts at different temperatures, the length and area of the conductivity cell are not easily affected by other factors and change, and the test results are highly accurate and reproducible.
[0053] In this embodiment, the glass sample to be tested is made into a small sample of the required size and then placed in the groove 21, and the volume of the glass melt is ensured to be larger than the volume of the groove 21, and the excess glass melt is squeezed out of the groove 21 by the gland 5, so that the glass melt forms a stable conductivity cell at high temperature, and the groove 21 plays a good positioning role, ensuring that the shape of the conductivity cell and the distance between the two electrodes remain constant, so the conductivity of the measured glass melt is only related to the measured conductivity of the glass melt, completely avoiding the detection error caused by manually reading the liquid level data of the conductivity cell, effectively ensuring the accuracy of the measurement result, and well meeting the detection requirements of different types of glass melts. Further, the glass melt overflowed due to thermal expansion at high temperature is stored in the crucible 2, and the conductivity of the same glass melt at different temperatures can be continuously measured, which not only improves the reliability of the detection result, but also effectively saves the detection cost.
[0054] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any technician familiar with the art can use the above disclosed methods and technical contents to make many possible changes and modifications to the technical solutions of the present invention without departing from the spirit and technical solutions of the present invention, or modify them into equivalent embodiments of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solutions of the present invention still fall within the scope of protection of the technical solutions of the present invention.
Claims
1. A device for measuring high temperature conductivity of glass melt, characterized in that: include: A high temperature furnace (1) with a furnace temperature control system is provided in the high temperature furnace (1). A high temperature resistant and insulated crucible (2) is placed in the high temperature furnace (1). A groove (21) for placing a glass sample to be tested is provided at the bottom of the inner side of the crucible (2). The volume of the molten glass is larger than the volume of the groove (21). Two opposite sides of the groove (21) are respectively connected to an electrode sheet (4). Both electrode sheets (4) are electrically connected to an electrochemical workstation (8). A high temperature resistant and insulated gland (5) is provided above the groove (21). A lifting device is provided above the gland (5). The lifting device is used to squeeze or release the gland (5) to achieve the adhesion or separation of the gland (5) and the groove (21), so as to ensure that the closed conductivity cell formed by the groove (21), the electrode sheet (4) and the gland (5) is filled with the glass melt. The measurement steps are as follows: 1) processing the glass sample to be tested into a desired size to ensure that the volume of the glass sample to be tested after melting is larger than the volume of the groove (21); 2) placing the processed glass sample to be tested in a groove (21) at the bottom of the inner side of the crucible (2), embedding an electrode sheet (4) on two opposite sides of the groove (21), and connecting the two electrode sheets (4) to the wire (3), and placing a pressure cover (5) on the glass sample to be tested; 3) placing the crucible (2) in the high-temperature furnace (1), adjusting the pressure rod (6) to be located above the pressure cover (5), and adjusting the pressure rod (6) by the servo motor to descend and contact the upper surface of the pressure cover (5); 4) connecting the wire (3) to the electrochemical workstation (8), setting the heating program of the high temperature furnace (1) through the furnace temperature control system, and heating the glass sample to be tested; 5) After reaching the preset temperature, continue to keep the temperature for ≥30 minutes to ensure that the glass sample to be tested is completely melted and fills the groove (21) of the crucible (2); adjust the pressure rod (6) to descend by the servo motor to apply pressure to the pressure cover (5) so that the pressure cover (5) and the groove (21) are tightly fitted; and detect the resistance value of the glass melt by the electrochemical workstation (8); 6) adjusting the pressure rod (6) to rise by means of a servo motor, removing the pressure on the pressure cover (5), and keeping the pressure rod (6) in contact with the upper surface of the pressure cover (5); continuing to adjust the temperature in the high-temperature furnace (1), repeating steps 4) and 5), and obtaining the resistance values of the glass melt at different temperatures; 7) Substitute the resistance values of the glass melt at different temperatures into the following formula to calculate the conductivity of the glass melt at different temperatures: In the formula, is the electrical conductivity of the glass melt to be measured, R is the resistance of the glass melt to be measured, L is the distance between the two electrode sheets (4), and A is the surface area of the electrode sheet (4).
2. The device for measuring high temperature electrical conductivity of molten glass according to claim 1, characterized in that: The lifting device comprises a screw rod (9), a connecting rod (10) and a high temperature resistant and insulating pressure rod (6), one end of the pressure rod (6) is fixedly connected to the connecting rod (10), the other end of the pressure rod (6) passes through the top of the high temperature furnace (1) and is arranged above the pressure cover (5), the connecting rod (10) is connected to the screw rod (9), and the screw rod (9) is connected to a servo motor.
3. The device for measuring high temperature electrical conductivity of glass melt according to claim 2, characterized in that: The lifting device further comprises a support rod (7), wherein the setting direction of the support rod (7) is the same as the setting direction of the screw rod (9), and driven by the screw rod (9), the connecting rod (10) moves up and down along the support rod (7).
4. The device for measuring high temperature electrical conductivity of glass melt according to claim 2, characterized in that: The crucible (2), the pressure cover (5) and the pressure rod (6) are all made of corundum or zirconium oxide.
5. The device for measuring high temperature conductivity of glass melt according to claim 2, characterized in that: The cross section of the pressure cover (5) is circular, and the cross section of the groove (21) is square; the diameter of the pressure cover (5) is smaller than the diameter of the crucible (2) and larger than the diagonal length of the cross section of the groove (21).
6. The device for measuring high temperature electrical conductivity of molten glass according to any one of claims 1 to 5, characterized in that: The electrode sheet (4) is embedded in the inner wall of the groove (21), and the surface area of the electrode sheet (4) is equal to the area of the inner wall of the groove (21).
7. The device for measuring high temperature electrical conductivity of molten glass according to claim 6, characterized in that: Each of the electrode sheets (4) is connected to the electrochemical workstation (8) via a wire (3).
8. The device for measuring high temperature conductivity of glass melt according to claim 7, characterized in that: The electrode sheet (4) is a platinum electrode sheet, and the wire (3) is a platinum wire.
9. A method for measuring high temperature conductivity of glass melt, characterized in that: The following steps are involved: 1) processing the glass sample to be tested into a desired size to ensure that the volume of the glass sample to be tested after melting is larger than the volume of the groove (21); 2) placing the processed glass sample to be tested in a groove (21) at the bottom of the inner side of the crucible (2), embedding an electrode sheet (4) on two opposite sides of the groove (21), and connecting the two electrode sheets (4) to the wire (3), and placing a pressure cover (5) on the glass sample to be tested; 3) placing the crucible (2) in the high-temperature furnace (1), adjusting the pressure rod (6) to be located above the pressure cover (5), and adjusting the pressure rod (6) by the servo motor to descend and contact the upper surface of the pressure cover (5); 4) connecting the wire (3) to the electrochemical workstation (8), setting the heating program of the high temperature furnace (1) through the furnace temperature control system, and heating the glass sample to be tested; 5) After reaching the preset temperature, continue to keep the temperature to ensure that the glass sample to be tested is completely melted and fills the groove (21) of the crucible (2); adjust the pressure rod (6) to descend by the servo motor to apply pressure to the pressure cover (5) so that the pressure cover (5) and the groove (21) are tightly fitted; and detect the resistance value of the glass melt by the electrochemical workstation (8); 6) adjusting the pressure rod (6) to rise by means of a servo motor, removing the pressure on the pressure cover (5), and keeping the pressure rod (6) in contact with the upper surface of the pressure cover (5); continuing to adjust the temperature in the high-temperature furnace (1), repeating steps 4) and 5), and obtaining the resistance values of the glass melt at different temperatures; 7) Substitute the resistance values of the glass melt at different temperatures into the following formula to calculate the conductivity of the glass melt at different temperatures: In the formula, is the electrical conductivity of the glass melt to be measured, R is the resistance of the glass melt to be measured, L is the distance between the two electrode sheets (4), and A is the surface area of the electrode sheet (4).
10. The method for measuring high temperature electrical conductivity of glass melt according to claim 9, characterized in that: In the step 5), the insulation time is ≥30 min.
Citation Information
Patent Citations
Testing device for electrical conductivity of high-temperature molten glass
CN106443197A
Formula for initiator material applied to in-situ glass solidification of contaminated soil
CN111995248A
Glass melt high-temperature conductivity measuring device
CN214622429U
Improvements relating to apparatus for measuring the properties of liquids the electrical conductivity of which varies with said properties
GB388897A