A modified carbon material and its preparation method and application

By pore-forming activation of carbon materials and loading nano-barium sulfate and hydrogen evolution inhibitors, the low-temperature discharge capacity and hydrogen evolution problems of lead-carbon batteries are solved, and the low-temperature performance and cycle life of the battery are improved.

CN113036093BActive Publication Date: 2024-10-18DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201911358090.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-25
Publication Date
2024-10-18
Estimated Expiration
2039-12-25

AI Technical Summary

Technical Problem

It is difficult to effectively solve the problems of reduced discharge capacity and hydrogen evolution of lead-carbon batteries under low temperature conditions. The addition of existing carbon materials leads to accelerated sulfation and increased hydrogen evolution.

Method used

By pore-forming and activating the carbon material, and loading nanometer barium sulfate and hydrogen evolution inhibitors on its surface, a modified carbon material is formed, which improves the low-temperature discharge capacity and charge acceptance capability of the battery and reduces hydrogen gas evolution.

Benefits of technology

It significantly improves the discharge capacity and charging ability of lead-carbon batteries at low temperatures, extends the cycle life of the battery, and expands its application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002336483230000191
    Figure BDA0002336483230000191
Patent Text Reader

Abstract

The present invention discloses a modified carbon material and a preparation method and application thereof, wherein the modified carbon material comprises a carbon-based material that has been activated and pore-formed, and the surface of the carbon-based material is loaded with nano-barium sulfate and a hydrogen evolution inhibitor. By loading nano-barium sulfate on the surface of the carbon-based material, the present invention can increase the lead sulfate crystallization site of the negative electrode of the lead-carbon battery, thereby improving the discharge capacity and charging acceptance of the negative electrode of the lead-carbon battery at low temperatures; by loading the hydrogen evolution inhibitor on the surface of the carbon-based material, the hydrogen evolution overpotential of the negative electrode of the lead-carbon battery can be significantly increased, thereby reducing the amount of hydrogen gas released during the charging process of the negative electrode. The lead-carbon battery prepared by incorporating the modified carbon material of the present invention into the negative electrode can still maintain excellent battery performance under low temperature conditions of ‑40°C to 0°C, thereby expanding the application field of the lead-carbon battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery energy storage, and in particular relates to a modified carbon material and a preparation method and application thereof. Background Art

[0002] Over the past 150 years, lead-acid batteries have dominated the low-cost, large-scale secondary energy storage battery market. Lead-acid batteries are widely used around the world due to their mature production technology, high safety, low production cost, and high recycling rate.

[0003] Adding a certain amount of carbon material to the negative electrode of a lead-acid battery forms a lead-carbon battery. The high conductivity of the carbon material can effectively inhibit the sulfation problem of the lead-acid battery, thereby greatly extending the cycle life of the lead-acid battery. However, the addition of carbon material has brought two new prominent problems to the lead-carbon battery: one is the hydrogen evolution problem during the battery charging process, and the other is the significant reduction in the low temperature capacity of the battery.

[0004] The main reason for the low low-temperature capacity of lead-carbon batteries is that under low-temperature conditions, the reduction of electrolyte sulfuric acid concentration will increase its freezing point temperature, thereby reducing the migration speed of electrolyte ions and increasing the concentration polarization of the electrode. The increase in negative electrode concentration polarization will cause the terminal voltage of the lead-carbon battery to reach the discharge termination voltage in advance during the discharge process, causing the amount of electricity released by the battery to decrease. Although increasing the concentration of the electrolyte can improve the low-temperature discharge capacity of the lead-carbon battery to a certain extent, it will accelerate the sulfation of the electrode and significantly reduce the charge and discharge cycle life of the battery. The main reason for hydrogen evolution is that the addition of carbon materials will reduce the hydrogen evolution overpotential of the negative electrode, resulting in increased electrolyte water loss during overcharging and high current charging. Loading a single substance or compound with a high hydrogen evolution overpotential on the surface of the carbon material can reduce the hydrogen evolution of the lead-carbon battery, but the simple mechanical mixing method cannot make the hydrogen evolution inhibitor work well and cannot effectively improve hydrogen evolution. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a carbon material suitable for an internal mixed lead-carbon battery, and specifically proposes a modified carbon material and a preparation method and application thereof. By pore-forming and activating a conventional carbon material and loading a large amount of nano-barium sulfate and a hydrogen evolution inhibitor on its surface, while inhibiting hydrogen evolution during the battery charging process, a large amount of lead sulfate crystallization sites can be provided at the end of the battery discharge, thereby improving the low-temperature discharge capacity of the battery.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] In one aspect, the present invention provides a carbon material for a low-temperature lead-carbon battery. The modified carbon material comprises an activated pore-forming carbon-based material, and the surface of the carbon-based material is loaded with nano-barium sulfate and a hydrogen evolution inhibitor.

[0008] Optionally, the content of nano-barium sulfate is 0.1% to 99% of the total mass of the carbon material.

[0009] Optionally, the particle size of the nano-barium sulfate ranges from 0.1 to 500 nm.

[0010] The amount of the hydrogen evolution inhibitor used is 0.1% to 91% of the total mass of the hydrogen evolution inhibitor and the carbon-based material.

[0011] Specifically, the amount of the hydrogen evolution inhibitor is independently selected from 0.1%, 1%, 20%, 70.3%, 74.7%, 80.6%, 90.8% and 91% of the total mass of the hydrogen evolution inhibitor and the carbon material.

[0012] Optionally, the hydrogen evolution inhibitor is a single substance or compound of an element with high hydrogen evolution overpotential;

[0013] The element with high hydrogen evolution overpotential includes at least one of Zn, Bi, Cd, Pb, In and Sn;

[0014] The compound includes at least one of nitrate, acetate, and alkoxide.

[0015] Optionally, the specific surface area of ​​the carbon-based material is 300 to 2500 m 2 / g.

[0016] In another aspect, the present invention provides a method for preparing a modified carbon material, comprising at least:

[0017] Activating and pore-forming the carbon-based material to obtain an activated carbon material;

[0018] The activated carbon material is immersed and mixed in a solution of a hydrogen evolution inhibitor to obtain a hydrogen evolution inhibiting carbon material;

[0019] The barium salt is subjected to a complexing reaction with a complexing agent to obtain a barium salt complex;

[0020] The barium salt complex is used to modify the hydrogen evolution inhibiting carbon material to obtain a modified carbon material.

[0021] Optionally, the amount of the barium salt is 1% to 65% of the total mass of the barium salt and the hydrogen evolution inhibiting carbon material;

[0022] The barium salt is a water-soluble barium salt;

[0023] The complexing agent is an aminopolycarboxylic acid chelating agent.

[0024] Specifically, the amount of the barium salt is independently selected from 1%, 30.9%, 47.2%, 57.3%, 64.2% and 65% of the total mass of the barium salt and the hydrogen evolution inhibiting carbon material.

[0025] The barium salt can be selected from barium salts other than barium sulfate and barium carbonate, such as barium nitrate, barium chloride, etc. In the present invention, barium nitrate is preferably used.

[0026] The complexing agent can be selected from any one of ethylenediaminetetraacetic acid (EDTA), tetrasodium iminodisuccinate (IDS), diethyltriaminepentaacetic acid (DTPA), and nitrilotriacetic acid (NTA).

[0027] Optionally, a method for preparing a modified carbon material at least comprises:

[0028] The carbon-based material is activated and pore-formed by using alkaline solution to obtain an activated carbon material;

[0029] The activated carbon material is impregnated and mixed in a solution of a hydrogen evolution inhibitor to obtain an impregnated product, and the impregnated product is dried and sintered to obtain a carbon material that inhibits hydrogen evolution;

[0030] The barium salt is subjected to a complexing reaction with a complexing agent to obtain a barium salt complex;

[0031] adding a carbon material that inhibits hydrogen evolution into a barium salt complex for impregnation to obtain a carbon material rich in the barium salt complex;

[0032] sintering the carbon material rich in the barium salt complex to obtain a carbon material rich in barium oxide;

[0033] The carbon material rich in barium oxide is reacted with a sulfuric acid solution to obtain a carbon material rich in nano-barium sulfate.

[0034] Optionally, the sintering parameters of the impregnated product are: keeping warm at 200-900° C. for 2-5 hours under atmosphere protection.

[0035] The lower limit of the sintering temperature is independently selected from 200°C, 300°C, 400°C, 500°C, and 800°C; the upper limit of the drying temperature is independently selected from 250°C, 450°C, 600°C, 700°C, and 900°C.

[0036] The sintering time is independently selected from 2h, 2.5h, 3h, 4h, and 5h.

[0037] Optionally, the process of obtaining the modified carbon material rich in barium salt complex and the process of obtaining the modified carbon material rich in nano-barium sulfate at least comprises:

[0038] Drying the modified carbon material rich in barium salt complex and the modified carbon material rich in nano-barium sulfate;

[0039] The drying temperature is 80-120°C.

[0040] The lower limit of the drying temperature is independently selected from 80°C, 90°C, 95°C, 100°C, and 110°C; the upper limit of the drying temperature is independently selected from 90°C, 100°C, 110°C, 115°C, and 120°C.

[0041] The drying time can be determined according to the dryness of the product, based on removing the free water therein.

[0042] Optionally, the sintering parameters of the modified carbon material rich in barium salt complex are: keeping warm at 600-900° C. for 1-5 hours under atmosphere protection.

[0043] The lower limit of the sintering temperature is independently selected from 600°C, 650°C, 700°C, 750°C, and 800°C; the upper limit of the drying temperature is independently selected from 650°C, 750°C, 800°C, 850°C, and 900°C.

[0044] The sintering time is independently selected from 1 h, 2 h, 3 h, 4 h, and 5 h.

[0045] Optionally, the density of the sulfuric acid solution is 1.05 to 1.5 g / cm 3 ;

[0046] The mass of sulfuric acid in the sulfuric acid solution is 11% to 37% of the total mass of the barium salt and the carbon material for inhibiting hydrogen evolution.

[0047] The amount of sulfuric acid solution used determines the loading amount of nano-barium sulfate in the modified carbon material, thus affecting the discharge capacity of the battery. If too little sulfuric acid solution is added, too little nano-barium sulfate will be generated, and sufficient lead sulfate crystallization sites cannot be generated at the negative electrode, and the effect of increasing the discharge capacity of the battery cannot be achieved; on the contrary, if too much sulfuric acid solution is added, the content of nano-barium sulfate will not continue to increase, resulting in a waste of resources.

[0048] Specifically, the amount of sulfuric acid is independently selected from 11%, 18.50%, 25.90%, 34.88%, and 37% of the total mass of the barium salt and the hydrogen evolution inhibiting carbon material; in a specific embodiment of the present invention, the density is 1.275 g / cm at 25 ° C. 3 The amount of sulfuric acid solution is greater than 30% of the total mass of the barium salt and the carbon-based material, and the amount of sulfuric acid solution is independently selected from 50%, 70%, 94.25%, and 100% of the total mass of the barium salt and the carbon-based material.

[0049] The third aspect of the present invention provides a negative electrode lead paste for a low-temperature lead-carbon battery, comprising at least one of any of the above-mentioned modified carbon materials and the modified carbon materials prepared according to any of the above-mentioned methods;

[0050] The components of the negative electrode lead paste include: 100 parts by weight of lead powder, 0.1 to 10 parts by weight of additives, 0.01 to 100 parts by weight of modified carbon material, 10 to 21 parts by weight of deionized water, and 4 to 100 parts by weight of sulfuric acid solution;

[0051] Sulfuric acid solution density 1.1~1.4g / cm 3 .

[0052] Specifically, in the negative electrode lead paste, the additive adopts at least one of the commonly used lead paste additives, such as lignin, humic acid, etc., and the lower limit of the additive content is independently selected from 0.1 weight parts, 2 weight parts, 5 weight parts, and 8 weight parts; the upper limit of the additive content is independently selected from 0.2 weight parts, 4 weight parts, 6 weight parts, and 9 weight parts.

[0053] In the negative electrode lead paste, the lower limit of the content of the modified carbon material is independently selected from 0.01 parts by weight, 12.6 parts by weight, 19.5 parts by weight, and 50 parts by weight; the upper limit of the content of the carbon material is independently selected from 16.2 parts by weight, 23.4 parts by weight, 70 parts by weight, and 100 parts by weight.

[0054] In the negative electrode lead paste, the lower limit of the deionized water content is independently selected from 10 parts by weight, 12.5 parts by weight, 15.5 parts by weight, and 17 parts by weight; the upper limit of the carbon material content is independently selected from 11 parts by weight, 14 parts by weight, 19 parts by weight, and 21 parts by weight.

[0055] In the negative electrode lead paste, the lower limit of the content of the sulfuric acid solution is independently selected from 4 parts by weight, 8.5 parts by weight, 20 parts by weight, and 50 parts by weight; the upper limit of the content of the carbon material is independently selected from 10 parts by weight, 25 parts by weight, 70 parts by weight, and 100 parts by weight.

[0056] A fourth aspect of the present invention provides a low-temperature lead-carbon battery, wherein the negative electrode of the battery is coated with the negative electrode lead paste.

[0057] The beneficial effects of the present invention are:

[0058] 1. The present invention can increase the lead sulfate crystallization sites of the negative electrode of the lead-carbon battery by loading nano-barium sulfate on the surface of the carbon-based material, thereby improving the discharge capacity and charge acceptance of the negative electrode of the lead-carbon battery at low temperatures.

[0059] 2. The present invention can significantly increase the hydrogen evolution overpotential of the negative electrode of the lead-carbon battery by loading a hydrogen evolution inhibitor on the surface of the carbon-based material, thereby reducing the amount of hydrogen evolution during the negative electrode charging process.

[0060] 3. The preparation method of the modified carbon material proposed in the present invention is applicable to a variety of carbon-based materials, including activated carbon, graphene, carbon nanotubes, ordered mesoporous carbon materials, etc.

[0061] 4. The present invention sintered the activated carbon material impregnated with the hydrogen evolution inhibitor to form a coordination bond between the hydrogen evolution inhibitor and the carbon material, thereby effectively improving the hydrogen evolution problem during the charging process of the carbon material and increasing the charging capacity of the battery.

[0062] 5. The lead-carbon battery prepared by adding the modified carbon material of the present invention to the negative electrode can still maintain excellent battery performance under low temperature conditions of -40°C to 0°C, thereby expanding the application field of lead-carbon batteries. DETAILED DESCRIPTION

[0063] The present invention is described in detail below with reference to embodiments.

[0064] Unless otherwise specified, the raw materials in the examples were purchased from commercial sources and used directly without further treatment; the instruments and equipment used were based on the parameters recommended by the manufacturer.

[0065] In the embodiment, the normal temperature and low temperature discharge capacity test of the lead-carbon battery is tested using a blue electric charge and discharge instrument.

[0066] In the embodiment, the specific surface area of ​​the activated carbon material is measured by using a fully automatic static volumetric specific surface area and porosity analyzer.

[0067] In the embodiment, the method for detecting the particle size distribution of nano-barium sulfate on the modified carbon material is: fully sintering the carbon additive loaded with barium sulfate at 600° C. in an air environment, removing carbon particles in the mixture, and using a laser particle size analyzer to test the particle size distribution of the sintered product.

[0068] Example 1

[0069] 1. Preparation of modified carbon materials:

[0070] (1) Activated carbon material: Take 20g of activated carbon and disperse it in 500ml of 3M potassium hydroxide solution. After fully stirring, dry the product. Transfer the dried product to an atmosphere sintering furnace and sinter it in a nitrogen environment at a sintering temperature of 800°C. Keep it warm for 5 hours and cool it naturally. This is recorded as sample C1.

[0071] The specific surface area and porosity analyzer was used to test the sample C1. The specific surface area of ​​the activated carbon material was between 300 and 2500 m 2 / g range.

[0072] (2) The carbon material activated in step (1) is dispersed into 500 ml of 0.5 M zinc nitrate solution, and the product is dried after being fully stirred and mixed. The dried carbon material is transferred to an atmosphere sintering furnace and kept at 200° C. for 5 hours under an inert atmosphere to obtain a carbon material that inhibits hydrogen evolution.

[0073] (3) Preparation of solution A: 9.072 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 17.384 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0074] (4) Preparation of Solution B: 8.06 g of barium nitrate was fully dissolved in 750 g of ultrapure water, and then 18 g of the hydrogen evolution inhibiting carbon material prepared in step (2) was added to the solution.

[0075] (5) Pour liquid A into liquid B and stir thoroughly to mix. Transfer the obtained mixture into an electric drying oven and dry it at 80° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ba complex.

[0076] (6) The product obtained in step (5) is transferred to a tubular furnace and sintered at 600° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in barium oxide.

[0077] (7) The barium-rich oxide carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 13.03 g of a carbon nanotube with a density of 1.275 g / cm was added thereto. 3 The mixture was stirred with high-speed magnetic stirring, and the obtained product was transferred to an electric drying oven and dried at 80°C for 24h to obtain a modified carbon material, which was recorded as sample C2.

[0078] Sample C2 was sintered and tested, and the results showed that the particle size distribution of nano-barium sulfate was in the range of 0.1 to 500 nm.

[0079] 2. Preparation of lead-carbon battery negative electrode:

[0080] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 12.6 parts of modified carbon material into a container of a paste mixer and dry mix for 3 minutes to fully mix the components to obtain a mixture;

[0081] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 2 minutes while slowly stirring the powder. Continue stirring for 3 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 5 minutes. After all the sulfuric acid solution is added, stirring is continued for 13 minutes to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0082] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0083] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0084] After the assembled lead-carbon battery was formed, the discharge capacity test was carried out at room temperature and low temperature. The discharge capacity of the lead-carbon battery reached 4.21Ah at -10℃.

[0085] Example 2

[0086] 1. Preparation of modified carbon materials:

[0087] (1) Activated carbon material: Take 20g of activated carbon and disperse it in 500ml of 6M potassium hydroxide solution. After fully stirring, dry the product. Transfer the dried product to an atmosphere sintering furnace and sinter it in a nitrogen environment at 900°C. Keep it warm for 5 hours and cool it naturally. This is recorded as sample C1.

[0088] The specific surface area and porosity analyzer was used to test the sample C1. The specific surface area of ​​the activated carbon material was between 300 and 2500 m 2 / g range.

[0089] (2) The activated carbon material in step (1) is dispersed into 500 ml of 1 M bismuth nitrate solution, and the product is dried after being fully stirred and mixed. The dried carbon material is transferred to an atmosphere sintering furnace and kept at 900° C. for 2 hours under an inert atmosphere to obtain a carbon material that inhibits hydrogen evolution.

[0090] (3) Preparation of solution A: 18.144 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 36.764 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0091] (4) Then prepare liquid B: take 16.12g of barium nitrate and fully dissolve it in 750g of ultrapure water, then add 18g of the hydrogen evolution inhibiting carbon material prepared in step (2) into the solution.

[0092] (5) Pour liquid A into liquid B and stir to mix. Transfer the obtained mixture into an electric drying oven and dry it at 120° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ba complex.

[0093] (6) The carbon material rich in EDTA-Ba complex obtained in step (5) is transferred to a tubular furnace and sintered at 700° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in barium oxide.

[0094] (7) The barium-rich oxide carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 23.88 g of a carbon nanotube with a density of 1.275 g / cm was added thereto. 3 The mixture was stirred with high-speed magnetic stirring, and the obtained product was transferred to an electric drying oven and dried at 120°C for 24 hours to obtain a modified carbon material, which was recorded as sample C2.

[0095] Sample C2 was sintered and tested, and the results showed that the particle size distribution of nano-barium sulfate was in the range of 0.1 to 500 nm.

[0096] 2. Preparation of lead-carbon battery negative electrode:

[0097] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 16.2 parts of modified carbon material into a container of a paste mixer and dry mix for 5 minutes to fully mix the components to obtain a mixture;

[0098] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 3 minutes while slowly stirring the powder. Continue stirring for 6 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 10 minutes. After all the sulfuric acid solution is added, continue stirring for 20 minutes to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0099] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0100] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0101] After the assembled lead-carbon battery was formed, the discharge capacity test was carried out at room temperature and low temperature. The discharge capacity of the lead-carbon battery reached 4.30Ah at -10℃.

[0102] Example 3

[0103] 1. Preparation of modified carbon materials:

[0104] (1) Activated carbon material: Take 20g of activated carbon and disperse it in 500ml of 3M potassium hydroxide solution. After fully stirring, dry the product. Transfer the dried product to an atmosphere sintering furnace and sinter it in a nitrogen environment at a sintering temperature of 1000°C. Keep it warm for 5 hours and cool it naturally. This is recorded as sample C1.

[0105] The specific surface area and porosity analyzer was used to test the sample C1. The specific surface area of ​​the activated carbon material was between 300 and 2500 m 2 / g range.

[0106] (2) The carbon material activated in step (1) is dispersed into 500 ml of 0.5 M cadmium nitrate solution, and the product is dried after being fully stirred and mixed. The dried carbon material is transferred to an atmosphere sintering furnace and kept at 500° C. for 4 hours under an inert atmosphere to obtain a carbon material that inhibits hydrogen evolution.

[0107] (3) Preparation of solution A: 27.216 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 52.148 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0108] (4) Then prepare liquid B: take 24.18g of barium nitrate and fully dissolve it in 750g of ultrapure water, then add 18g of the hydrogen evolution inhibiting carbon material prepared in step (2) into the solution.

[0109] (5) Pour liquid A into liquid B and stir to mix. Transfer the obtained mixture into an electric drying oven and dry it at 100° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ba complex.

[0110] (6) The carbon material rich in EDTA-Ba complex obtained in step (5) is transferred to a tubular furnace and sintered at 800° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in barium oxide.

[0111] (7) The barium-rich oxide carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 39.76 g of a carbon having a density of 1.275 g / cm 3 The mixture was stirred with high-speed magnetic stirring, and the obtained product was transferred to an electric drying oven and dried at 100°C for 24h to obtain a modified carbon material, which was recorded as sample C2.

[0112] Sample C2 was sintered and tested, and the results showed that the particle size distribution of nano-barium sulfate was in the range of 0.1 to 500 nm.

[0113] 2. Preparation of lead-carbon battery negative electrode:

[0114] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 19.8 parts of modified carbon material into a container of a paste mixer and dry mix for 4 minutes to fully mix the components to obtain a mixture;

[0115] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 2 minutes while slowly stirring the powder. Continue stirring for 4 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 7 minutes. After all the sulfuric acid solution is added, continue stirring for 15 minutes to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0116] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0117] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0118] After the assembled lead-carbon battery was formed, the discharge capacity test was carried out at room temperature and low temperature. The discharge capacity of the lead-carbon battery reached 4.29Ah at -10℃.

[0119] Example 4

[0120] 1. Preparation of modified carbon materials:

[0121] (1) Activated carbon material: Take 20g of activated carbon and disperse it in 500ml of 3M potassium hydroxide solution. After fully stirring, dry the product. Transfer the dried product to an atmosphere sintering furnace and sinter it in a nitrogen environment at a sintering temperature of 700°C. Keep it warm for 5 hours and cool it naturally. This is recorded as sample C1.

[0122] The specific surface area and porosity analyzer was used to test the sample C1. The specific surface area of ​​the activated carbon material was between 300 and 2500 m 2 / g range.

[0123] (2) The carbon material activated in step (1) is dispersed into 500 ml of 0.5 M lead nitrate solution, and the product is dried after being fully stirred and mixed. The dried carbon material is transferred to an atmosphere sintering furnace and kept at 700° C. for 3 hours under an inert atmosphere to obtain a carbon material that inhibits hydrogen evolution.

[0124] (3) Preparation of solution A: 36.287 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 69.212 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0125] (4) Preparation of Solution B: 32.24 g of barium nitrate was fully dissolved in 750 g of ultrapure water, and then 18 g of the hydrogen evolution inhibiting carbon material prepared in step (2) was added to the solution.

[0126] (5) Pour liquid A into liquid B and stir to mix. Transfer the obtained mixture into an electric drying oven and dry it at 110° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ba complex.

[0127] (6) The carbon material rich in EDTA-Ba complex obtained in step (5) is transferred to a tubular furnace and sintered at 900° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in barium oxide.

[0128] (7) The barium-rich oxide carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 50.24 g of a carbon nanotube with a density of 1.275 g / cm was added thereto. 3 The mixture was stirred with high-speed magnetic stirring, and the obtained product was transferred to an electric drying oven and dried at 110°C for 24h to obtain a modified carbon material, which was recorded as sample C2.

[0129] Sample C2 was sintered and tested, and the results showed that the particle size distribution of nano-barium sulfate was in the range of 0.1 to 500 nm.

[0130] 2. Preparation of lead-carbon battery negative electrode:

[0131] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 23.4 parts of modified carbon material into a container of a paste mixer and dry mix for 3 minutes to fully mix the components to obtain a mixture;

[0132] (2) Weigh 15.5 parts of deionized water and add it to the powder mixed in step (1) for 3 minutes while slowly stirring the powder. Continue stirring for 5 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 9 minutes. After all the sulfuric acid solution is added, stirring is continued for 17 minutes to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0133] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0134] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0135] After the assembled lead-carbon battery was formed, the discharge capacity test was carried out at room temperature and low temperature. The discharge capacity of the lead-carbon battery reached 4.19Ah at -10℃.

[0136] Comparative Example 1

[0137] 1. Preparation of lead-carbon battery negative electrode:

[0138] (1) Pour 100 parts of lead powder, additives (1.2 parts of barium sulfate, 0.2 parts of lignin), and 1.0 parts of unmodified carbon material into a paste machine container and dry mix for 3 minutes to fully mix the components to obtain a mixture;

[0139] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 2 minutes while slowly stirring the powder. Continue stirring for 3 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 5 minutes. After all the sulfuric acid solution is added, stirring is continued for 13 minutes to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0140] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is directly coated on the negative electrode grid, and after rolling and acid treatment, it is placed in a controllable humidity high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0141] 2. Use the lead-carbon battery negative electrode prepared in step 1 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0142] After the assembled lead-carbon battery is formed, the discharge capacity test at room temperature and low temperature is carried out. Compared with Example 1, the discharge capacity of the lead-carbon battery added with unmodified carbon material in this comparative example is only 3.96Ah at -10°C, while the discharge capacity of the lead-carbon battery added with nano-barium sulfate modified carbon material in Example 1 reaches 4.21Ah at -10°C.

[0143] Comparative Example 2

[0144] 1. Preparation of lead-acid battery negative electrode:

[0145] (1) Pour 100 parts of lead powder, additives (1.2 parts of barium sulfate, 0.2 parts of lignin), and 0.2 parts of acetylene black into a paste machine container and dry mix for 3 minutes to fully mix the components to obtain a mixture;

[0146] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 2 minutes while slowly stirring the powder. Continue stirring for 3 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 5 minutes. After all the sulfuric acid solution is added, stirring is continued for 13 minutes to obtain the negative electrode lead paste of the lead-acid battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0147] (3) The lead paste for the negative electrode of the lead-acid battery obtained in step (2) is directly coated on the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the negative electrode of the lead-acid battery.

[0148] 2. Use the lead-acid battery negative electrode and lead-acid battery positive electrode prepared in step 1 to assemble a 2V5.2Ah lead-acid battery.

[0149] After the assembled lead-acid battery is formed, the discharge capacity test at room temperature and low temperature is carried out. Compared with Example 1, the discharge capacity of the lead-acid battery in this comparative example is only 4.11Ah at -10°C, while the discharge capacity of the lead-carbon battery added with the nano-barium sulfate modified carbon material in Example 1 reaches 4.21Ah at -10°C.

[0150] Comparative Example 3

[0151] 1. Preparation of modified carbon materials:

[0152] (1) Activated carbon material: Take 20g of activated carbon and disperse it in 500ml of 3M potassium hydroxide solution. After fully stirring, dry the product. Transfer the dried product to an atmosphere sintering furnace and sinter it in a nitrogen environment at a sintering temperature of 800°C. Keep it warm for 5 hours and cool it naturally. This is recorded as sample C1.

[0153] The specific surface area and porosity analyzer was used to test the sample C1. The specific surface area of ​​the activated carbon material was between 300 and 2500 m 2 / g range.

[0154] (2) The activated carbon material prepared in step (1) is dispersed into 500 ml of 0.5 M zinc nitrate solution, and the product is dried after being fully stirred and mixed. The dried carbon material is transferred to an atmosphere sintering furnace and kept at 200° C. for 5 hours under an inert atmosphere to obtain a carbon material that inhibits hydrogen evolution.

[0155] (3) Preparation of solution A: 9.072 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 17.384 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0156] (4) Preparation of Solution B: 8.06 g of calcium nitrate was fully dissolved in 750 g of ultrapure water, and then 18 g of the hydrogen evolution inhibiting carbon material prepared in step (2) was added to the solution.

[0157] (5) Pour liquid A into liquid B and stir to mix. Transfer the obtained mixture into an electric drying oven and dry it at 80° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ca complex.

[0158] (6) The carbon material rich in EDTA-Ca complex obtained in step (5) is transferred to a tubular furnace and sintered at 600° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in calcium oxide.

[0159] (7) The calcium oxide-rich carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 13.03 g of a carbon nanotube with a density of 1.275 g / cm was added thereto. 3 The mixture was stirred magnetically at a high speed, and the obtained product was transferred to an electric drying oven and dried at 80° C. for 24 h to obtain a modified carbon material.

[0160] 2. Preparation of lead-carbon battery negative electrode:

[0161] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 12.6 parts of modified carbon material into a container of a paste mixer and dry mix for 3 minutes to fully mix the components to obtain a mixture;

[0162] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 2 to 3 minutes while slowly stirring the powder. Continue stirring for 3 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution, the entire acid adding time is controlled within 5 minutes, and stirring is continued for 13 minutes after all the sulfuric acid solution is added to obtain the negative electrode lead paste of the lead-carbon battery.

[0163] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0164] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0165] After the assembled lead-carbon battery is formed, the discharge capacity test at room temperature and low temperature is carried out. Compared with Example 1, the discharge capacity of the lead-carbon battery mixed with the modified carbon material loaded with nano calcium sulfate in this comparative example is only 3.83Ah at -10°C, while the discharge capacity of the lead-carbon battery mixed with the modified carbon material loaded with nano barium sulfate in Example 1 reaches 4.21Ah at -10°C.

[0166] Comparative Example 4

[0167] 1. Preparation of modified carbon materials:

[0168] (1) Activated carbon material: Take 20g of activated carbon and disperse it in 500ml of 6M potassium hydroxide solution. After fully stirring, dry the product. Transfer the dried product to an atmosphere sintering furnace and sinter it in a nitrogen environment at 900°C. Keep it warm for 5 hours and cool it naturally. This is recorded as sample C1.

[0169] The specific surface area and porosity analyzer was used to test the sample C1. The specific surface area of ​​the activated carbon material was between 300 and 2500 m 2 / g range.

[0170] (2) The activated carbon material prepared in step (1) is dispersed into 500 ml of 1M bismuth nitrate solution, and the product is dried after being fully stirred and mixed. The dried carbon material is transferred to an atmosphere sintering furnace and kept at 900° C. for 2 hours under an inert atmosphere to obtain a carbon material that inhibits hydrogen evolution.

[0171] (3) Preparation of solution A: 18.144 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 36.764 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0172] (4) Then prepare liquid B: take 16.12g of calcium nitrate and fully dissolve it in 750g of ultrapure water, then add 18g of the hydrogen evolution inhibiting carbon material prepared in step (2) into the solution.

[0173] (5) Pour liquid A into liquid B and stir to mix. Transfer the obtained mixture into an electric drying oven and dry it at 120° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ba complex.

[0174] (6) The carbon material rich in EDTA-Ba complex obtained in step (5) is transferred to a tubular furnace and sintered at 700° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in barium oxide.

[0175] (7) The barium-rich oxide carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 8.06 g of a carbon nanotube with a density of 1.275 g / cm was added thereto. 3 The mixture was stirred with high-speed magnetic stirring, and the obtained product was transferred to an electric drying oven and dried at 120°C for 24 hours to obtain a modified carbon material, which was recorded as sample C2.

[0176] Sample C2 was sintered and tested, and the results showed that the particle size distribution of nano-barium sulfate was in the range of 0.1 to 500 nm.

[0177] 2. Preparation of lead-carbon battery negative electrode:

[0178] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 16.2 parts of modified carbon material into a container of a paste mixer and dry mix for 3 to 5 minutes to fully mix the components to obtain a mixture;

[0179] (2) Weigh 15.5 parts of deionized water, add it to the mixture obtained in step (1) quickly for 3 minutes while slowly stirring the powder, continue stirring for 6 minutes, then slowly add 8.5 parts of sulfuric acid solution with a density of 1.4 g / cm3, the entire acid addition time is controlled within 10 minutes, and continue stirring for 20 minutes after all the sulfuric acid solution is added to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, the paste outlet temperature should not exceed 40°C, and the apparent density of the lead paste should be controlled to be 3.6-4.4 g / cm3.

[0180] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0181] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0182] After the assembled lead-carbon battery is formed, the discharge capacity at room temperature and low temperature is tested. Compared with Example 2, after reducing the amount of sulfuric acid added in this comparative example, the discharge capacity of the lead-carbon battery at -10°C is only 3.91Ah, while the discharge capacity of the lead-carbon battery in Example 2 at -10°C reaches 4.30Ah.

[0183] Comparative Example 5

[0184] 1. Preparation of modified carbon materials:

[0185] (1) Take 20g of activated carbon and sinter it in a nitrogen environment at a temperature of 1000°C. Keep it at this temperature for 5 hours and cool it naturally.

[0186] (2) The carbon material obtained in step (1) is dispersed in 500 ml of 0.5 M cadmium nitrate solution, and the product is dried after being fully stirred and mixed. The dried carbon material is transferred to an atmosphere sintering furnace and kept at 500° C. for 4 hours under an inert atmosphere.

[0187] (3) Preparation of solution A: 27.216 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 52.148 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0188] (4) Preparation of Solution B: 24.18 g of calcium nitrate was fully dissolved in 750 g of ultrapure water, and then 18 g of the carbon material prepared in step (2) was added to the solution.

[0189] (5) Pour liquid A into liquid B and stir to mix. Transfer the obtained mixture into an electric drying oven and dry it at 100° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ba complex.

[0190] (6) The carbon material rich in EDTA-Ba complex obtained in step (5) is transferred to a tubular furnace and sintered at 800° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in barium oxide.

[0191] (7) The barium-rich oxide carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 39.76 g of a carbon having a density of 1.275 g / cm 3 The mixture was stirred with high-speed magnetic stirring, and the obtained product was transferred to an electric drying oven and dried at 100°C for 24h to obtain a modified carbon material, which was recorded as sample C2.

[0192] Sample C2 was sintered and tested, and the results showed that the particle size distribution of nano-barium sulfate was in the range of 0.1 to 500 nm.

[0193] 2. Prepare the negative electrode of the lead-carbon battery by the following steps:

[0194] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 19.8 parts of modified carbon material into a container of a paste mixer and dry mix for 4 minutes to fully mix the components to obtain a mixture;

[0195] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 2 minutes while slowly stirring the powder. Continue stirring for 4 minutes, then slowly add a 1.4 g / cm 3 8.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 7 minutes. After all the sulfuric acid solution is added, continue stirring for 15 minutes to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0196] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0197] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0198] After the assembled lead-carbon battery is formed, the discharge capacity test at room temperature and low temperature is carried out. Compared with Example 3, after the activation step of the carbon material is eliminated in this comparative example, the lead-carbon battery mixed with the modified carbon material loaded with barium sulfate has a discharge capacity of 4.06Ah at -10°C, while the lead-carbon battery mixed with the modified carbon material loaded with nano-barium sulfate obtained after the carbon material is activated in Example 3 has a discharge capacity of 4.29Ah at -10°C.

[0199] Comparative Example 6

[0200] 1. Preparation of modified carbon materials:

[0201] (1) Activated carbon material: Take 20g of activated carbon and disperse it in 500ml of 3M potassium hydroxide solution. After fully stirring, dry the product. Transfer the dried product to an atmosphere sintering furnace and sinter it in a nitrogen environment at a sintering temperature of 700°C. Keep it warm for 5 hours and cool it naturally. This is recorded as sample C1.

[0202] The specific surface area and porosity analyzer was used to test the sample C1. The specific surface area of ​​the activated carbon material was between 300 and 2500 m 2 / g range.

[0203] (2) The activated carbon material prepared in step (1) is dispersed into 500 ml of 0.5 M lead nitrate solution, stirred and mixed thoroughly, and then the product is dried to obtain a carbon material that inhibits hydrogen evolution.

[0204] (3) Preparation of solution A: 36.287 g of ethylenediaminetetraacetic acid was added to 200 g of ultrapure water, followed by 69.212 g of 25-28% ammonia water, and the mixture was stirred until the solution became clear and transparent.

[0205] (4) Preparation of Solution B: 32.24 g of calcium nitrate was fully dissolved in 750 g of ultrapure water, and then 18 g of the hydrogen evolution inhibiting carbon material prepared in step (2) was added to the solution.

[0206] (5) Pour liquid A into liquid B and stir to mix. Transfer the obtained mixture into an electric drying oven and dry it at 110° C. for 24 h to remove free water therein, thereby obtaining a carbon material rich in EDTA-Ba complex.

[0207] (6) The carbon material rich in EDTA-Ba complex obtained in step (5) is transferred to a tubular furnace and sintered at 900° C. for 5 hours under a nitrogen atmosphere to obtain a carbon material rich in barium oxide.

[0208] (7) The barium-rich oxide carbon material obtained in step (6) was dispersed in 200 g of ultrapure water, and 50.24 g of a carbon nanotube with a density of 1.275 g / cm was added thereto. 3 The mixture was stirred with high-speed magnetic stirring, and the obtained product was transferred to an electric drying oven and dried at 110°C for 24h to obtain a modified carbon material, which was recorded as sample C2.

[0209] Sample C2 was sintered and tested, and the results showed that the particle size distribution of nano-barium sulfate was in the range of 0.1 to 500 nm.

[0210] 2. Preparation of lead-carbon battery negative electrode:

[0211] (1) Pour 100 parts of lead powder, 0.2 parts of lignin, and 23.4 parts of modified carbon material into a container of a paste mixer and dry mix for 3 minutes to fully mix the components to obtain a mixture;

[0212] (2) Weigh 15.5 parts of deionized water and add it to the mixture obtained in step (1) for 3 minutes while slowly stirring the powder. Continue stirring for 5 minutes, then slowly add a 1.4 g / cm 38.5 parts of sulfuric acid solution are added, and the entire acid addition time is controlled within 9 minutes. After all the sulfuric acid solution is added, stirring is continued for 17 minutes to obtain the negative electrode lead paste of the lead-carbon battery. During the mixing process of the lead paste, the temperature of the lead paste and the container should not exceed 65°C, and the paste temperature should not exceed 40°C. At the same time, the apparent density of the lead paste should be controlled to be 3.6-4.4g / cm 3 .

[0213] (3) The lead paste of the lead-carbon battery negative electrode obtained in step (2) is scraped onto the negative electrode grid, and after rolling and acid treatment, it is placed in a humidity-controlled high and low temperature box for curing and drying, and cured at 45° C. and 95% relative humidity for 36 hours, and then dried at 85° C. for 9 hours to obtain the lead-carbon battery negative electrode.

[0214] 3. Use the lead-carbon battery negative electrode prepared in step 2 and the lead-acid battery positive electrode to assemble a 2V5.2Ah lead-carbon battery.

[0215] After the assembled lead-carbon battery is formed, the discharge capacity test at room temperature and low temperature is carried out. Compared with Example 4, the sintering step of the carbon material impregnated with the hydrogen evolution inhibitor is cancelled in this comparative example, and no coordination bond is formed between the hydrogen evolution inhibitor and the carbon material, so that the hydrogen evolution is serious during the charging process of the carbon material, and the charging capacity is reduced, and finally the discharge capacity of the lead-carbon battery added with the modified carbon material loaded with barium sulfate at -10°C is only 3.92Ah, while the discharge capacity of the lead-carbon battery added with the modified carbon material loaded with nano-barium sulfate in Example 4 at -10°C reaches 4.19Ah.

[0216] The discharge capacities of the batteries in the embodiments of the present invention and the comparative examples at -10°C are compared as follows:

[0217]

[0218] As can be seen from the above table, the lead-carbon battery provided by the present invention has a significantly improved discharge capacity at -10°C compared to ordinary lead-carbon batteries, and is higher than the discharge capacity of ordinary lead-acid batteries. It can be seen that the present invention provides a large number of lead sulfate crystallization sites at the end of battery discharge and reduces the amount of hydrogen released at the end of battery charging by loading a large number of nano-barium sulfate crystal nuclei and hydrogen evolution inhibitors on the surface of the carbon material, thereby improving the low-temperature discharge capacity and low-temperature cycle life of the battery and expanding the application field of lead-carbon batteries.

[0219] The present invention verifies that the addition of nano-barium sulfate can increase the lead sulfate crystallization sites, thereby improving the battery discharge capacity by changing the raw materials and the amount of the nano-crystal cores added, while other raw materials cannot achieve the above technical effects; at the same time, the amount of nano-barium sulfate added determines the increase in the lead sulfate crystallization sites in the battery, which directly affects the battery discharge capacity.

[0220] The present invention compares the discharge performance of the lead-carbon battery obtained before and after the activation of the carbon material, and verifies that the use of the activated carbon material can improve the discharge capacity of the battery at low temperatures.

[0221] The present invention compares the discharge performance of the lead-carbon battery obtained by sintering the activated carbon material impregnated with the hydrogen evolution inhibitor before and after sintering, and verifies that sintering can form a coordination bond between the hydrogen evolution inhibitor and the carbon material, thereby improving the hydrogen evolution problem during the charging process of the carbon material and increasing the battery charging capacity.

[0222] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a modified carbon material, characterized in that: The modified carbon material comprises an activated pore-forming carbon-based material, and the surface of the carbon-based material is loaded with nano-barium sulfate and a hydrogen evolution inhibitor; The preparation method at least comprises: The carbon-based material is activated and pore-formed by using alkaline solution to obtain an activated carbon material; The activated carbon material is impregnated and mixed in a solution of a hydrogen evolution inhibitor to obtain an impregnated product, and the impregnated product is dried and sintered to obtain a carbon material that inhibits hydrogen evolution; The barium salt is subjected to a complexing reaction with a complexing agent to obtain a barium salt complex; adding the hydrogen evolution inhibiting carbon material into a barium salt complex for impregnation to obtain a carbon material rich in the barium salt complex; Sintering the carbon material rich in barium salt complex to obtain a carbon material rich in barium oxide; reacting the carbon material rich in barium oxide with a sulfuric acid solution to obtain a carbon material rich in nano-barium sulfate; The hydrogen evolution inhibitor is a single substance or compound of an element with high hydrogen evolution overpotential; The high hydrogen evolution overpotential element includes at least one of Zn, Bi, Cd, Pb, In, and Sn; The compound includes at least one of nitrate, acetate and alkoxide.

2. The preparation method according to claim 1, characterized in that: The content of the nano barium sulfate is 0.1% to 99% of the total mass of the modified carbon material; The amount of the hydrogen evolution inhibitor used is 0.1% to 91% of the total mass of the hydrogen evolution inhibitor and the carbon-based material.

3. The preparation method according to claim 1, characterized in that: The specific surface area of ​​the carbon-based material is 300-2500 m 2 / g.

4. The preparation method according to claim 1, characterized in that: The amount of the barium salt is 1% to 65% of the total mass of the barium salt and the hydrogen evolution inhibiting carbon material; The barium salt is a water-soluble barium salt; The complexing agent is an aminopolycarboxylic acid chelating agent.

5. The method for preparing a modified carbon material according to claim 1, characterized in that: The sintering parameters of the impregnated product are: keeping at 200-900° C. for 2-5 hours under atmosphere protection; The process of obtaining the carbon material rich in barium salt complex and the carbon material rich in nano-barium sulfate at least comprises: Drying the carbon material rich in barium salt complex and the carbon material rich in nano-barium sulfate; The drying temperature is 80-120°C; The sintering parameters of the modified carbon material rich in barium salt complex are: keeping the temperature at 600-900° C. for 1-5 hours under atmosphere protection; The density of the sulfuric acid solution is 1.05-1.5 g / cm 3 ; The mass of sulfuric acid in the sulfuric acid solution is 11% to 37% of the total mass of the barium salt and the hydrogen evolution inhibiting carbon material.

6. A negative electrode lead paste for a low-temperature lead-carbon battery, characterized in that: Including at least one of the modified carbon materials prepared by the preparation method according to any one of claims 1 to 5; The components of the negative electrode lead paste include: 100 parts by weight of lead powder, 0.1 to 10 parts by weight of additives, 0.01 to 100 parts by weight of the modified carbon material, 10 to 21 parts by weight of deionized water, and 4 to 100 parts by weight of sulfuric acid solution.

7. A low-temperature lead-carbon battery, characterized in that: The negative electrode of the low-temperature lead-carbon battery is coated with the negative electrode lead paste of the low-temperature lead-carbon battery according to claim 6.

Citation Information

Patent Citations

  • Nano barium sulfate carbon composite material and preparation method and application therefor

    CN105576240A

  • Modified carbon material and preparation method thereof, cathode lead paste, polar plate and lead carbon battery

    CN105958076A