Secondary battery electrode plate comprising electrode mixture regions having different binder contents and method for manufacturing secondary battery electrode using the same

By adopting an alternating high-binder and low-binder content zone structure in the secondary battery electrode, the problem of electrode breakage and high defect rate during the cutting process is solved, and the bonding strength and process efficiency of the electrode are improved.

CN113039667BActive Publication Date: 2024-10-29LG ENERGY SOLUTION LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202080005515.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-06
Publication Date
2024-10-29
Estimated Expiration
2040-10-06

AI Technical Summary

Technical Problem

When manufacturing secondary battery electrodes, the bonding force between the electrode current collector and the coating is reduced, resulting in high breakage and defect rates during the cutting process, especially at the boundaries between the electrode mixture area and the uncoated area.

Method used

The electrode mixture region structure containing different binder contents is adopted, and an alternating structure of high binder content regions and low binder content regions is formed on the surface of the electrode current collector layer to ensure improved bonding force and prevention during the slitting process. damaged.

Benefits of technology

It effectively reduces the breakage and defect rate of the electrode during the cutting process, improves the process efficiency, and enhances the internal bonding force of the electrode and the interface bonding force of the current collector layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113039667B_ABST
    Figure CN113039667B_ABST
Patent Text Reader

Abstract

The present invention relates to an electrode plate for a secondary battery and a method for manufacturing an electrode for a secondary battery including the electrode plate. The electrode plate includes: a current collector layer; a lower mixture layer formed on one side or both sides of the current collector layer; and an upper mixture layer formed on the lower mixture layer, wherein the upper mixture layer includes a high binder containing region with a high binder content and a low binder containing region with a low binder content, and the upper mixture layer has the following structure: based on a cross section in a width direction (TD), in a direction from one edge of the upper mixture layer to another edge of the upper mixture layer, a first high binder containing region, a first low binder containing region, a kth high binder containing region, a kth low binder containing region (k=2 to n-1) and an nth high binder containing region (n=3 to 10) are sequentially formed, wherein the high binder containing region is a region cut during electrode longitudinal cutting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrode plate for a secondary battery including electrode mixture regions having different binder contents, and a method for producing an electrode for a secondary battery using the same.

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0127744, filed on October 15, 2019, and the entire contents of this Korean Patent Application are incorporated herein by reference. Background Art

[0003] The latest trends in the electronics industry can be summarized as the trend of wireless mobility of devices and the transition from analog to digital. Representative examples include the rapid popularity of mobile devices and laptops, and the transition from analog cameras to digital cameras.

[0004] In addition to these trends, research and development of secondary batteries as working power sources for devices has also been actively carried out. Among them, lithium secondary batteries with high output and capacity per unit weight using lithium transition metal oxides or lithium composite oxides as positive electrode active materials have attracted much attention. In the structure of lithium secondary batteries, the electrode assembly of positive electrode / separator / negative electrode is embedded in a sealed container together with an electrolyte.

[0005] On the other hand, the electrode generates current through ion exchange, and the positive electrode and the negative electrode constituting the electrode have a structure in which an electrode active material is coated on an electrode current collector made of metal.

[0006] Generally, the negative electrode has a structure in which a carbon-based active material is coated on an electrode plate made of copper or aluminum, and the positive electrode has a structure in which an active material made of LiCoO2, LiMnO2 or LiNiO2, etc. is coated on an electrode plate made of aluminum, etc.

[0007] To manufacture a positive electrode or a negative electrode, an electrode mixture containing an electrode active material is coated at regular intervals on an electrode current collector made of a metal sheet that is long in one direction and then processed into a set electrode shape.

[0008] In the first step of the shape processing, the electrode current collector composed of a metal sheet long in one direction coated with the electrode mixture is cut by a cutting process of slitting or punching, thereby processing into two or more electrode strip shapes.

[0009] However, in the prior art, in the process of manufacturing such an electrode, in the process of transferring the electrode current collector made of a metal sheet longer in one direction coated with an electrode mixture to the longitudinal cutting device, due to the force of the transfer roller or the tension applied during the roll-to-roll process, the tensile force between the current collector and the coating is different, so the bonding force of the bonding surface between the current collector and the coating may be reduced. In addition, as the force of the cutter of the longitudinal cutting device shears the electrode current collector, the adhesion between the particles (active material, conductive material and adhesive) constituting the electrode coating is reduced, and the electrode layer with a single particle or multiple particles collected is crushed and generates coating debris. This debris itself becomes a foreign matter and may cause problems, and problems may also occur in the coating with partial defects due to the debris.

[0010] In particular, at the boundary between the region of the electrode current collector coated with the electrode mixture and the uncoated region, breakage is more frequent, which has become a major cause of an increase in product defect rate.

[0011] Therefore, a technology capable of reducing defects caused by damage or the like in a process of processing an electrode current collector of a secondary battery into a specific electrode shape is highly desired. Summary of the invention

[0012] [Technical issues]

[0013] The present invention is intended to solve the above-mentioned problems, and an object of the present invention is to provide an electrode plate including active material regions having different binder contents, and a method for manufacturing an electrode using the same.

[0014] [Technical solution]

[0015] The electrode plate for a secondary battery of the present invention includes: a current collector layer; and an electrode mixture layer formed on one side or both sides of the current collector layer. Specifically, the mixture layer includes a high binder containing region with a high binder content and a low binder containing region with a low binder content, and the mixture layer has the following structure: based on a cross section in the width direction (TD), a first high binder containing region, a first low binder containing region, a kth high binder containing region, a kth low binder containing region, and an nth high binder containing region are sequentially formed in a direction from one edge of the mixture layer to the other edge of the mixture layer, and k is an integer from 2 to n-1, and n is an integer from 3 to 10.

[0016] In one example, the deviation between the binder content of the high binder content region and the low binder content region is 20 wt % or more.

[0017] In one specific example, the ratio of the binder content of the high binder containing region to the low binder containing region is in the range of 1.2:1 to 30:1.

[0018] In yet another example, in the high binder content region, the binder content (B) at a height of 20% based on the thickness of the mixture layer is L ) and the binder content at 80% of the height (B H ) is less than 15 wt %.

[0019] In another example, the width of the high binder containing region (L BH ) and the width of the low binder content area (L BL ) ratio (L BH :L BL ) is in the range of 1:3 to 1:600.

[0020] In one example, for the electrode plate for a secondary battery of the present invention, both edges of the current collector include uncoated portions where the mixture layer is not formed, based on the cross section in the width direction (TD).

[0021] In one embodiment, the high binder content region is a region that is cut by slitting or punching during the electrode slitting process.

[0022] In addition, the present invention provides a method for manufacturing an electrode using the electrode plate for a secondary battery.

[0023] In one example, the manufacturing method of the electrode for a secondary battery of the present invention includes: a step of forming an electrode mixture layer on one surface or both surfaces of a current collector layer; and a step of longitudinally cutting the current collector layer formed with the mixture layer. Specifically, the step of forming the mixture layer includes: forming the mixture layer to include a high binder containing region formed by releasing an electrode mixture slurry with a high binder content and a low binder containing region formed by releasing an electrode mixture slurry with a low binder content, and based on a cross section in the width direction (TD), in a direction from one edge of the mixture layer to the other edge of the mixture layer, a first high binder containing region, a first low binder containing region, a kth high binder containing region, a kth low binder containing region, and an nth high binder containing region are sequentially formed, and k is an integer from 2 to n-1, and n is an integer from 3 to 10.

[0024] In one example, in the step of forming the mixture layer, a deviation between the binder contents of the high binder content region and the low binder content region is 20 wt % or more.

[0025] In yet another example, the step of forming the mixture layer is performed by strip coating using a double slit coating apparatus, the first slit releases the first slurry in a pattern on the current collector layer, and the second slit releases the second slurry in a form filling gaps between the first slurry patterns released on the current collector layer.

[0026] In one specific example, the first slurry released through the first slit is a slurry having a high binder content, and the second slurry released through the second slit is a slurry having a low binder content.

[0027] In another example, the method for manufacturing an electrode for a secondary battery of the present invention includes: before the step of forming the mixture layer, a step of forming a lower mixture layer by releasing a slurry with a high binder content on a current collector. Specifically, the step of forming the mixture layer is performed by forming an upper mixture layer on the formed lower mixture layer.

[0028] In one specific example, the deviation between the binder content of the lower mixture layer and the binder content of the high binder containing region of the upper mixture layer is 15 wt % or less. In addition, in the upper mixture layer, the deviation between the binder content of the high binder containing region and the low binder containing region is 20 wt % or more.

[0029] In one example, a thickness ratio of the lower mixture layer to the upper mixture layer is in a range of 1:1.5 to 1:20.

[0030] [Beneficial Effects]

[0031] According to the electrode plate for secondary batteries and the electrode manufacturing method using the same of the present invention, in the electrode, the problem of breakage occurring in the portion coated with the electrode mixture or at the boundary between the portion coated with the electrode mixture and the uncoated portion not coated with the electrode mixture during cutting can be solved, and the process efficiency can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 and Figure 2 Each of the schematic diagrams shows a cross-sectional structure of a battery electrode plate according to an embodiment of the present invention.

[0033] Figure 3 It is a plan view showing a battery electrode plate according to an embodiment of the present invention. DETAILED DESCRIPTION

[0034] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The terms and words used in this specification and claims should not be interpreted as limited to common or dictionary terms, and the inventors can appropriately define the concepts of the terms to best describe their inventions. The terms and words should be interpreted as meanings and concepts consistent with the technical ideas of the present invention.

[0035] In the present invention, the electrode plate for a secondary battery refers to a structure in which an electrode mixture including an active material is applied to an electrode current collector made of a metal sheet that is long in one direction.

[0036] In the present invention, the above-mentioned mixture refers to a mixture used as an electrode for a secondary battery, for example, a composition in which an active material, a binder, a conductive agent, and other components are mixed, and each of these elements will be described later.

[0037] The present invention provides an electrode plate for a battery, comprising: a current collector layer; and an electrode mixture layer formed on one side or both sides of the current collector layer. In one embodiment, the mixture layer includes a high binder containing region with a high binder content and a low binder containing region with a low binder content, and the mixture layer has the following structure: based on the cross section in the width direction (TD), a first high binder containing region, a first low binder containing region, a kth high binder containing region, a kth low binder containing region, and an nth high binder containing region are sequentially formed in the direction from one edge of the active material layer to the other edge of the mixture layer. Here, k is an integer from 2 to n-1, and n is an integer from 3 to 10. For example, n can be in the range of 3 to 8 or 3 to 5.

[0038] The electrode plate for secondary batteries is processed into the form of two or more electrode strips by longitudinal cutting (longitudinal cutting in the length direction) in the subsequent longitudinal cutting process. In the electrode plate for secondary batteries of the present invention, based on the cross section in the width direction (TD), high binder containing regions with high binder content and low binder containing regions with low binder content are alternately formed, and the two ends have a structure with high binder containing regions.

[0039] In addition, in the secondary battery electrode plate of the present invention, the high binder content region corresponds to the position where longitudinal cutting is performed. In the present invention, by forming the high binder content region in the region for longitudinal cutting of the electrode plate, it has the effect of preventing the damage or separation of the mixture layer or the opening between the mixture layer and the current collector layer that may occur during the longitudinal cutting process.

[0040] In one embodiment, the adhesive content deviation between the high adhesive containing region and the low adhesive containing region is 20% by weight or more. Specifically, the adhesive content deviation between the high adhesive containing region and the low adhesive containing region is in the range of 20 to 500% by weight, 20 to 400% by weight, 20 to 300% by weight, 100 to 500% by weight, 200 to 500% by weight, 300 to 500% by weight, 20 to 150% by weight, 30 to 100% by weight or 50 to 90% by weight. The adhesive content deviation is a value obtained by converting the difference between the adhesive content in the high adhesive region and the adhesive content in the low adhesive region into a percentage relative to the adhesive content in the low adhesive region.

[0041] In one embodiment, the ratio of the binder content of the high binder containing region and the low binder containing region is in the range of 1.2: 1 to 30: 1. Specifically, the ratio of the binder content of the high binder containing region and the low binder containing region is in the range of 1.2: 1 to 20: 1, 1.2: 1 to 10: 1, 1.2: 1 to 50: 1, 1.5: 1 to 10: 1 or 1.5: 1 to 3: 1. The high binder containing region is a region containing a binder having a high content compared to the active material content. When the content of the binder is increased, the internal bonding force of the mixture layer is improved, and the interfacial bonding force with the current collector layer is improved. However, if the content of the binder is too high, the capacity of the battery is reduced due to the reduction in the content of the active material, and there is a limitation of increased resistance.

[0042] In another embodiment, in the high binder content region, the binder content (B) at a height of 20% based on the thickness of the mixture layer is L ) and the binder content at 80% of the height (B H Specifically, in the high binder content region, the binder content at the height 20% point (B L ) and the binder content at 80% of the height (B H ) is within the range of 0.01 to 15 wt %, 0.01 to 10 wt %, 0.01 to 5 wt %, 0.01 to 3 wt %, 0.1 to 3 wt % or 0.01 to 1 wt %. In the high binder containing region of the present invention, the content of the binder is substantially equal. However, in the process of manufacturing the electrode (e.g., drying the electrode), the content of the binder may vary partially depending on the height.

[0043] In another example, the width of the high binder containing region (L BH ) and the width of the low binder content area (L BL ) ratio (L BH :L BL ) is in the range of 1:3 to 1:600. Specifically, the high binder containing region (L BH ) and low binder containing area (L BL ) width ratio (L BH :L BL ) is in the range of 1:3 to 1:500, 1:3 to 1:300, 1:50 to 1:600, 1:50 to 1:400 or 1:80 to 1:200. In terms of battery characteristics, it is advantageous to set the width L of the low binder containing region to BL However, by appropriately adjusting the width L of the high binder containing region BH, damage to the electrode during the process of forming the electrode plate can be prevented and separation of the mixture can be minimized.

[0044] For example, based on the cross section in the width direction (TD), at the two edges of the current collector, the electrode plate includes an uncoated portion where the mixture layer is not formed. The uncoated portion becomes a region for forming an electrode tab. For example, in addition to the two edges in the width direction of the electrode plate, one or more uncoated portions may be additionally formed in the portion between the regions where the mixture layer is formed.

[0045] In addition, the present invention provides a method for manufacturing an electrode using the electrode plate.

[0046] In one embodiment, the electrode manufacturing method of the present invention includes the following steps: forming an electrode mixture layer on one or both surfaces of a current collector layer; and longitudinally cutting the current collector layer formed with the mixture layer. At this time, the "longitudinal cutting" step includes not only linearly cutting the current collector layer with a cutter, but also punching with a die for punching, and refers to the step of cutting the electrode during electrode processing. Specifically, the step of forming a mixture layer includes: forming a mixture layer to include a high binder-containing region formed by releasing a slurry for an electrode mixture with a high binder content and a low binder-containing region formed by releasing a slurry for an electrode mixture with a low binder content, and based on a cross section in the width direction (TD), in the direction from one edge of the mixture layer to the other edge of the mixture layer, a first high binder-containing region, a first low binder-containing region, a kth high binder-containing region, a kth low binder-containing region, and an nth high binder-containing region are sequentially formed, and k is an integer from 2 to n-1, and n is an integer from 3 to 10.

[0047] The electrode manufacturing method of the present invention is carried out by the following process: by strip coating, a mixture with different binder contents is released onto the current collector layer with a slurry. In this case, in the step of forming the mixture layer, the deviation of the binder content between the high binder containing region and the low binder containing region is 20% by weight or more. Specifically, the deviation of the binder content between the high binder containing region and the low binder containing region is in the range of 20 to 500% by weight, 20 to 400% by weight, 20 to 300% by weight, 100 to 500% by weight, 200 to 500% by weight, 300 to 500% by weight, 20 to 150% by weight, 30 to 100% by weight or 50 to 90% by weight. The deviation of the binder content is a value obtained by converting the difference between the binder content in the high binder region and the binder content in the low binder region into a percentage relative to the binder content in the low binder region.

[0048] In another embodiment, the step of forming the mixture layer is performed by strip coating using a double slit coating device. For example, the double slit has a structure of sequentially forming a first and a second slit, the first slit releasing the first slurry in a pattern on the current collector layer, and the second slit releasing the second slurry in the form of filling the gap between the first slurry patterns released on the current collector layer.

[0049] In a specific example, the first slurry released through the first slit is a slurry with a high binder content, and the second slurry released through the second slit is a slurry with a low binder content. This is to release the slurry with a high binder content first to form a pattern, and release the slurry with a low binder content to fill the gap between the formed patterns. In the present invention, the release order of the first and second slurries is not particularly limited, but by first releasing the slurry with a high binder content, it has the effect of increasing the binding force with the current collector layer and fixing the release position in the process.

[0050] In one embodiment, the electrode manufacturing method of the present invention may include: before the step of forming the mixture layer, forming a lower mixture layer by releasing a slurry with a high binder content on a current collector. Specifically, the step of forming the mixture layer can be performed by forming an upper mixture layer on the formed lower mixture layer.

[0051] For example, the deviation between the binder content of the lower mixture layer and the binder content of the high binder content region of the upper mixture layer is 15% by weight or less. In addition, in the upper mixture layer, the deviation of the binder content between the high binder content region and the low binder content region is 20% by weight or more. The numerical value or deviation range according to each binder content is omitted here because the range overlaps with the above range.

[0052] In another embodiment, the thickness ratio of the lower mixture layer to the upper mixture layer is in the range of 1:1.5 to 1:20. Specifically, the thickness ratio of the lower mixture layer to the upper mixture layer is in the range of 1:2.5 to 1:15, 1:5 to 1:20, 1:5 to 1:10, 1:1.5 to 1:5, or 1:15 to 1:20. The thickness ratio is selected in consideration of the capacity of the electrode and the bonding force between the current collector layer and the mixture layer.

[0053] The electrode plate for a secondary battery of the present invention may be a positive electrode or a negative electrode. The electrode plate or electrode of the present invention may be applied to a secondary battery, specifically a lithium secondary battery. The structure of a secondary battery includes: an electrode assembly comprising a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; a non-aqueous electrolyte solution in which the electrode assembly is impregnated; and a battery housing containing the electrode assembly and the non-aqueous electrolyte solution. The non-aqueous electrolyte solution is, for example, an electrolyte solution containing a lithium salt. Hereinafter, the specific composition of each electrode will be described, but the scope of the present invention is not limited thereto.

[0054] The positive electrode has a structure in which a positive electrode mixture layer is stacked on one or both sides of a positive electrode current collector. In one example, the positive electrode mixture layer contains a positive electrode active material, a conductive material, a binder polymer, etc., and, if necessary, may further include positive electrode additives commonly used in the art.

[0055] The positive electrode active material may be a lithium-containing oxide, which may be the same or different. As the lithium-containing oxide, a lithium-containing transition metal oxide may be used.

[0056] For example, the lithium-containing transition metal oxide may be selected from the group consisting of Li x CoO2 (0.5 < x < 1.3), Li x NiO2 (0.5 < x < 1.3), Li x MnO2 (0.5 < x < 1.3), Li x Mn2O4 (0.5 < x < 1.3), Li x (Ni a Co b Mn c )O2 (0.5 < x < 1.3, 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), Li x Ni 1-y Co y O2 (0.5 < x < 1.3, 0 < y < 1), Li x Co 1-y Mn y O2 (0.5 < x < 1.3, 0 ≤ y < 1), Li x Ni 1-y Mn y O2 (0.5 < x < 1.3, 0 ≤ y < 1), Li x (Ni a Co b Mn c )O4 (0.5 < x < 1.3, 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), Li x Mn 2-z Ni z O4 (0.5 < x < 1.3, 0 < z < 2), Li x Mn 2-z Co z O4 (0.5 < x < 1.3, 0 < z < 2), Li x CoPO4 (0.5 < x < 1.3) and Li xAny one or more mixtures in the group consisting of FePO4 (0.5 < x < 1.3), and the lithium-containing transition metal oxide may be coated with a metal or metal oxide such as aluminum (Al). In addition, in addition to the lithium-containing transition metal oxide, one or more of sulfides, selenides, and halides may be used.

[0057] The positive electrode active material may be included in the positive electrode mixture layer in the range of 94.0 to 98.5% by weight. When the content of the positive electrode active material satisfies the above range, it is advantageous in terms of manufacturing a high-capacity battery and providing sufficient electrical conductivity of the positive electrode or adhesion between electrode materials.

[0058] The current collector for the positive electrode is a metal with high electrical conductivity, and any metal that can be easily attached to the positive electrode mixture slurry and is non-reactive within the voltage range of the electrochemical device can be used. Specifically, non-limiting examples of the current collector for the positive electrode include aluminum, nickel, or foils made of a combination thereof.

[0059] The positive electrode mixture layer further includes a conductive material. Based on the total weight of the mixture layer containing the positive electrode active material, the addition amount of the conductive material is generally 1 to 30% by weight. There is no particular limitation on such a conductive material as long as it has electrical conductivity and does not cause chemical changes in the secondary battery. For example, as the conductive material, the following can be used: graphite, such as natural graphite or artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal cracking carbon black; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as fluorocarbons, aluminum, or nickel powders; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; and polyphenylene derivatives.

[0060] As the binder component, binder polymers commonly used in the art can be used without limitation. For example, various binders such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) can be used.

[0061] The content of the binder polymer is proportional to the content of the conductive material included in the upper positive electrode active material layer and the lower positive electrode active material layer. This is to impart adhesion to the conductive material having a relatively small particle size compared to the active material, and because when the content of the conductive material increases, more binder polymer is required, and when the content of the conductive material decreases, less binder polymer can be used.

[0062] In addition, the negative electrode has a structure in which a negative electrode mixture layer is stacked on one or both sides of a negative electrode current collector. In one example, the negative electrode mixture layer includes a negative electrode active material, a conductive material and a binder polymer, and if necessary, may further include a negative electrode additive commonly used in the art.

[0063] The negative electrode active material may include a carbon material, lithium metal, silicon or tin. When a carbon material is used as the negative electrode active material, both low crystalline carbon and high crystalline carbon may be used. Representative examples of low crystalline carbon include soft carbon and hard carbon. Representative examples of high crystalline carbon include natural graphite, kish graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, mesocarbon microspheres, mesophase pitch and high temperature calcined carbon, such as coke derived from petroleum or coal tar pitch.

[0064] Non-limiting examples of the current collector for the negative electrode include foils made of copper, gold, nickel, copper alloys, or combinations thereof. In addition, the current collector may be used by stacking substrates made of the above materials.

[0065] In addition, the negative electrode may include a conductive material and a binder generally used in the art.

[0066] The separator may be made of any porous substrate used in a lithium secondary battery, for example, a polyolefin-based porous film or nonwoven fabric may be used, but the present invention is not particularly limited thereto.

[0067] Examples of the polyolefin-based porous film include polyethylene (eg, high-density polyethylene, linear low-density polyethylene, low-density polyethylene, ultra-high molecular weight polyethylene), and films formed of polyolefin-based polymers (eg, polypropylene, polybutene, or polypentene) each alone or in a mixture thereof.

[0068] As the nonwoven fabric, in addition to the polyolefin-based nonwoven fabric, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, polyethylene naphthalene, etc. can be used alone or as a mixture of polymers to form the nonwoven fabric. The structure of the nonwoven fabric may be a spunbond nonwoven fabric or a meltblown nonwoven fabric composed of long fibers.

[0069] The thickness of the porous substrate is not particularly limited but may be 5 to 50 μm, and the pore size and porosity present in the porous substrate are also not particularly limited but may be 0.01 to 50 μm and 10 to 95%, respectively.

[0070] Meanwhile, in order to improve the mechanical strength of the separator composed of the porous substrate and suppress a short circuit between the positive electrode and the negative electrode, a porous coating layer including inorganic particles and a binder polymer may be further included on at least one surface of the porous substrate.

[0071] The electrolyte may contain an organic solvent and an electrolyte salt, and the electrolyte salt is a lithium salt. As the lithium salt, those conventionally used in lithium secondary battery electrolytes may be used without limitation. For example, as anions of the lithium salt, anions selected from F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - One or more of the groups.

[0072] As the organic solvent included in the above-mentioned electrolyte, those conventionally used in lithium secondary battery electrolytes can be used without restriction, and for example, ethers, esters, amides, linear carbonates and cyclic carbonates can be used alone or in combination of two or more. Among them, representatively, cyclic carbonates, linear carbonates or carbonate compounds as mixtures thereof can be included.

[0073] Specific examples of cyclic carbonate compounds include any one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinyl ethylene carbonate and halides thereof, and mixtures thereof. These halides include, for example, fluoroethylene carbonate (FEC), but are not limited thereto.

[0074] In addition, specific examples of the linear carbonate compound include any one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methylpropyl carbonate and ethylpropyl carbonate, or a mixture of two or more thereof may be typically used, but is not limited thereto.

[0075] In particular, among carbonate organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents and have a high dielectric constant, so that the lithium salt in the electrolyte can be more easily dissociated, and if the cyclic carbonate is mixed with a low-viscosity, low-dielectric-constant linear carbonate (e.g., dimethyl carbonate and diethyl carbonate) in an appropriate proportion, an electrolyte solution with higher electronic conductivity can be prepared.

[0076] In addition, as the ether of the organic solvent, any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether and ethyl propyl ether, or a mixture of two or more thereof may be used, but is not limited thereto.

[0077] Furthermore, the ester in the organic solvent includes any one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone and ε-caprolactone, or a mixture of two or more thereof, but the present invention is not limited thereto.

[0078] In the manufacturing process of the electrochemical device, the injection of the nonaqueous electrolyte can be performed at an appropriate step according to the manufacturing process and the desired physical properties of the final product. That is, it can be applied before assembling the electrochemical device or in the final stage of assembling the electrochemical device.

[0079] Hereinafter, the present invention will be described in more detail through drawings and examples.

[0080] Preparation Example 1: Preparation of a mixture with a high binder content (first mixture)

[0081] 100 parts by weight of NCM (LiNi 0.8 Co 0.1 Mn 0.1 O2), 1.5 parts by weight of carbon black (FX35, Denka, average diameter (D50) 15 to 40 nm) as a conductive material and 3.5 parts by weight of polyvinylidene fluoride (KF9700, Kureha) as a binder polymer are added to NMP (N-methyl-2-pyrrolidone) as a solvent to prepare a first mixture slurry.

[0082] Preparation Example 2: Preparation of a mixture with a low binder content (second mixture)

[0083] 100 parts by weight of NCM (LiNi 0.8 Co 0.1 Mn 0.1 O2), 0.1 parts by weight of carbon black (FX35, Denka, average diameter (D50) 15 to 40 nm) as a conductive material and 2 parts by weight of KF9700 (Kureha) as a binder polymer are added to NMP (N-methyl-2-pyrrolidone) as a solvent to prepare a second mixture slurry.

[0084] Example 1: Preparation of electrode plates for secondary batteries

[0085] The first and second mixture slurries were strip-coated on a current collector layer formed of aluminum foil using a double-slit coating device. Specifically, in the double-slit coating device, the first slit was coated with 600 mg / 25 cm 2 The first mixture slurry is strip-coated at a loading amount of 1000 μm so that three lines are formed on the current collector layer, and then the second mixture slurry is released at the same loading amount through the second slit to fill the gaps between the released first mixture slurry lines. In the double slit coating device, the number and width of the released lines are controlled by the shape of the core set at the release port. The ratio of the width of the released first mixture slurry to the width of the second mixture slurry is 1:10. Thereafter, the thickness of the positive electrode mixture layer after vacuum drying is 100 μm on average.

[0086] The cross-sectional structure of the manufactured electrode plate is as follows: Figure 1 shown. Figure 1 Schematic diagram showing a cross section of the manufactured electrode plate 100 in the width direction (TD). Figure 1 The electrode plate 100 manufactured according to the above embodiment has the following structure: a mixture layer 120 is formed on a current collector layer 110 formed of aluminum foil, which is divided into regions 121a and 121b with high binder content and regions 122a and 122b with low binder content. The average thickness (D1) of the mixture layer 120 is measured to be 100 μm.

[0087] In the electrode plate 100, the binder-rich regions 121a and 121b are formed at both edges 121a and the center 121b of the mixture layer 120, and the binder-rich regions 122a and 122b have a structure filling a gap between the binder-rich regions 121a and 121b.

[0088] In addition, based on the mixture layer 120 of the electrode plate 100, in the regions 121a and 121b with high binder content, at the height 20% point (D L1 ) and the height 80% point (D H1) is less than 12 wt %, and the actual difference is at the level of 1 wt %. This means that the adhesive contents of the regions 121a and 121b with high adhesive contents are generally uniform.

[0089] Example 2: Preparation of electrode plates for secondary batteries

[0090] An electrode plate for a secondary battery was manufactured in the same manner as in Example 1, except that the ratio of the width of the discharged first mixture slurry to the width of the second mixture slurry was at a level of 1:500.

[0091] Example 3: Preparation of electrode plates for secondary batteries

[0092] An electrode plate for a secondary battery was manufactured in the same manner as in Example 1, except that the first mixture slurry was discharged so as to form five lines through the first slit in the double slit coating apparatus.

[0093] Example 4: Preparation of electrode plates for secondary batteries

[0094] The first mixture slurry was prepared at 60 mg / 25 cm 2 The loading amount of the mixture is coated on the aluminum foil to form a lower mixture layer. An upper mixture layer is formed on the formed lower mixture layer.

[0095] Regarding the upper mixture layer, in a double slot coating device, 540 mg / 25 cm 2 The first mixture slurry is strip-coated with a loading amount of 1000 Å to form three lines on the current collector layer, and then the second mixture slurry is released with the same loading amount through the second slit to fill the gaps between the released first mixture slurry lines. The ratio of the width of the released first mixture slurry to the width of the second mixture slurry is 1:10.

[0096] The thickness of the positive electrode mixture layer after vacuum drying was 100 μm on average.

[0097] The cross-sectional structure of the manufactured electrode plate is as follows: Figure 2 shown. Figure 2 is a schematic diagram showing a cross section in the width direction (TD) of the manufactured electrode plate 200. Figure 2 The electrode plate 200 manufactured according to the above embodiment has the following structure: a lower mixture layer 220 and an upper mixture layer 230 are sequentially formed on a current collector layer 210 formed of an aluminum foil. In addition, the upper mixture layer 230 has a structure divided into regions 231a and 231b with a high binder content and regions 232a and 232b with a low binder content. The average thickness (D2) of the mixture layer 220 was measured to be 100 μm.

[0098] In addition, based on the entire mixture layer of the electrode plate 200, in the regions 231a and 231b with a high binder content, at a height of 20% (D L2 ) and the height 80% point (D H2 ) is less than 12 wt %, and the actual difference is at the level of 1 wt %. This result means that the adhesive content of the regions 231a and 231b with high adhesive content is generally uniform.

[0099] Example 5

[0100] An electrode plate for a secondary battery was manufactured in the same manner as in Example 3, except that carbon nanotubes (LUCAN-BT1001M, LG Chem, aspect ratio 100-300) were used as the conductive material in preparing the mixture slurry forming the lower mixture layer.

[0101] Comparative Example: Preparation of electrode plates for secondary batteries

[0102] An electrode plate for a secondary battery was manufactured in the same manner as in Example 1, except that only the second mixture slurry was discharged to form a mixture layer.

[0103] Experimental example: longitudinal cutting of electrode plates

[0104] Each sample prepared in Examples 1 and 2 and the comparative example was longitudinally cut to determine whether there were defects. For the samples of Examples 1 and 2, longitudinal cutting was performed along the area coated with the first mixture slurry. For the samples of the comparative example, longitudinal cutting was performed at positions corresponding to the longitudinal cutting positions of Examples 1 and 2, respectively.

[0105] Figure 3 FIG. 2 is a front view of the electrode plate of the present embodiment, showing the electrode plate before the longitudinal cutting process. Figure 3 , the electrode plate 300 has the following form: on the current collector layer 310, a mixture layer having the following structure: regions 321a and 321b with high binder content and regions 322a and 322b with low binder content are repeated alternately in the width direction TD. The two edges of the current collector layer 310 in the width direction TD are uncoated portions where the mixture layer is not formed. In addition, based on the width direction (TD), the width (L) of the regions 321a and 321b with high binder content is BH ) and the width (L BL ) is 1:10 in Example 1 and 1:500 in Example 2. Slitting is performed in the longitudinal direction along the regions 321a and 321b with a high binder content in the electrode plate 300.

[0106] Each of the 10 samples was longitudinally cut and defects were determined by visual observation. As a result, it was confirmed that all samples were normal in the case of Examples 1 and 2. However, in the case of the comparative example, it was determined that there were defects in a total of 3 samples, specifically, it was confirmed that some damage to the mixture layer was observed in two samples, and the interface between the current collector layer and the mixture layer was widened in one sample.

[0107] The present invention has been described in more detail above through the drawings and embodiments. Therefore, the embodiments described in the specification and the configurations described in the drawings are only the most preferred embodiments of the present invention and do not represent all technical ideas of the present invention. It should be understood that various equivalents and variants may exist to replace them when submitting this application.

[0108] <Description of Reference Numerals>

[0109] 100, 200, 300: electrode plate

[0110] 110, 210, 310: Current collector layer

[0111] 120: Mixture layer

[0112] 121a, 121b, 231a, 231b, 321a, 321b: Areas with high adhesive content

[0113] 122a, 122b, 232a, 232b, 322a, 322b: Areas with low adhesive content

[0114] 220: Lower mixture layer

[0115] 230: Upper mixture layer.

Claims

1. An electrode plate for a secondary battery, the electrode plate comprising: a current collector layer; a lower mixture layer formed on one or both sides of the current collector layer; as well as forming an upper mixture layer on the lower mixture layer, wherein the upper mixture layer includes a high binder containing region having a high binder content and a low binder containing region having a low binder content, The upper mixture layer has the following structure: based on the cross section in the width direction (TD), in the direction from one edge of the upper mixture layer to the other edge of the upper mixture layer, a first high adhesive content region, a first low adhesive content region, a k-th high adhesive content region, a k-th low adhesive content region and an n-th high adhesive content region are sequentially formed, Wherein, k is an integer from 2 to n-1, and n is an integer from 3 to 10; The high binder content region is the region that is cut during the electrode longitudinal cutting process. wherein the deviation between the binder content of the high binder content region and the binder content of the low binder content region is 30 wt % to 500 wt %, The width L of the high adhesive containing region is BH The width L of the low binder containing area BL Ratio L BH :L BL In the range of 1:10 to 1:500; wherein a thickness ratio of the lower mixture layer to the upper mixture layer is in a range of 1:1.5 to 1:20; and The difference between the binder content of the lower mixture layer and the binder content of the high binder content region of the upper mixture layer is 15 wt % or less.

2. The electrode plate according to claim 1, wherein: A ratio of the binder content of the high binder content region to the low binder content region is in the range of 1.5:1 to 3:

1.

3. The electrode plate according to claim 1, wherein: In the high binder content region, the binder content B at the 20% height point based on the thickness of the upper mixture layer is L and the adhesive content B at 80% of the height H The deviation between them is 15 wt % or less.

4. The electrode plate according to claim 1, wherein The width L of the high binder containing area BH The width L of the low binder containing area BL Ratio L BH : L BL In the range of 1:50 to 1:

400.

5. The electrode plate according to claim 1, wherein: Both edges of the current collector based on a cross section in a width direction (TD) include uncoated portions where a mixture layer is not formed.

6. A method for manufacturing an electrode for a secondary battery, the method comprising: a step of forming a lower mixture layer on one surface or both surfaces of the current collector layer by releasing a slurry having a high binder content; forming an upper mixture layer on the formed lower mixture layer; as well as a step of longitudinally cutting the current collector layer having the mixture layer formed thereon, The step of forming the upper mixture layer includes: forming the upper mixture layer to include a high binder content region formed by releasing the electrode mixture slurry having a high binder content, and a low binder content region formed by releasing the electrode mixture slurry having a low binder content, wherein, based on a cross section in the width direction (TD), in a direction from one edge of the upper mixture layer to the other edge of the upper mixture layer, a first high adhesive content region, a first low adhesive content region, a k-th high adhesive content region, a k-th low adhesive content region, and an n-th high adhesive content region are sequentially formed, Wherein, k is an integer from 2 to n-1, n is an integer from 3 to 10, wherein, in the step of longitudinally cutting the current collector layer, cutting the high binder containing region, wherein the difference between the binder content of the lower mixture layer and the binder content of the high binder content region of the upper mixture layer is 15 wt % or less, and wherein, in the step of forming the upper mixture layer, a deviation between the binder contents of the high binder content region and the low binder content region is 30 wt % to 500 wt %; The width L of the high adhesive containing region is BH The width L of the low binder containing area BL Ratio L BH :L BL In the range of 1:10 to 1:500; Wherein, a thickness ratio of the lower mixture layer to the upper mixture layer is in a range of 1:1.5 to 1:

20.

7. The method of claim 6, wherein: The step of forming the mixture layer is performed by strip coating using a double slit coating apparatus, wherein the first slit releases the first slurry in a pattern on the current collector layer, and The second slit releases the second slurry in the form of filling gaps between the first slurry patterns released on the current collector layer.

8. The method of claim 7, wherein: The first slurry released through the first slit is a high binder containing slurry having a high binder content, and The second slurry released through the second slit is a low-binder slurry having a low binder content.

9. The method of claim 6, wherein: A thickness ratio of the lower mixture layer to the upper mixture layer is in a range of 1:2.5 to 1:15.

Citation Information

Patent Citations

  • Planetary transmission for a roll stabiliser having a spring mechanism

    KR1020190127744A

  • Bipolar laminated all-solid-state lithium-ion rechargeable battery and method for manufacturing same

    CN107180995A

  • Method for manufacturing electrode slurry for lithium secondary battery

    CN110199421A

  • electrodes with improved coating and methods of their manufacture

    DE102017207439A1

  • Power storage element

    JP2013206743A