Chemical pre-alkalization of electrodes

By contacting the electrode material with a mixture of aromatic compounds, alkali metals and organic solvents for prelithiation in ambient air, the problem that the pre-alkalinization method in the prior art is complicated and limited to inert gas conditions is solved, and an efficient electrode is achieved Pre-lithiation and battery energy density improvement.

CN113039675BActive Publication Date: 2024-10-22UWM RESEARCH FOUNDATION INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980075168.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-24
Filing Date
2019-09-24
Publication Date
2024-10-22
Estimated Expiration
2039-09-24

AI Technical Summary

Technical Problem

Existing lithium-ion battery packs suffer from initial capacity loss and when paired with high-capacity positive electrodes, the pre-alkalinization method is complex and limited to inert gas conditions, making it difficult to effectively increase the energy density of the battery.

Method used

The electrode material is prelithiated in ambient air by contacting it with a mixture containing aromatic compounds, alkali metals, and organic solvents to form a stable alkali metal electrode, reduce the consequences of solid electrolyte interface formation, and improve the electrode's performance Alkali metal content.

Benefits of technology

It achieves efficient electrode prelithiation in ambient air, improves the Coulombic efficiency of the electrode and the energy density of the battery, simplifies the operation process, and reduces the cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113039675B_ABST
    Figure CN113039675B_ABST
Patent Text Reader

Abstract

Disclosed herein is a method for making an electrode. The method includes contacting an electrode material with a mixture comprising an alkali metal, an organic solvent, and an aromatic compound. Also disclosed herein is a method for making a battery comprising an electrode provided by the disclosed method.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Application No. 62 / 735,831, filed on September 24, 2018, which is incorporated herein by reference in its entirety. Background Art

[0003] Pre-alkalization of the negative electrode (NE) is an attractive strategy to increase the available energy density of alkali metal ion batteries (e.g., lithium ion batteries - LIBs) because it can compensate for initial capacity loss and pair with high-capacity positive electrodes (PEs). However, existing pre-alkalization methods involve complex operations or are limited to inert gas conditions. Therefore, alkali metal ion batteries require more efficient pre-alkalization methods to realize their full potential. Summary of the invention

[0004] In one aspect, a method of making an electrode is disclosed, the method comprising contacting an electrode material with a mixture comprising an aromatic compound, an alkali metal, and an organic solvent to provide the electrode.

[0005] In another aspect, a method of making a battery is disclosed, the method comprising making an electrode as disclosed herein; arranging a separator so that it is located between the electrode and a second electrode to provide a battery; and adding a non-aqueous electrolyte to the battery to provide the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] This patent or application file contains at least one drawing drawn in color. Copies of this patent or patent application publication with color drawing(s) will be provided by the Office upon request and payment of the necessary fee.

[0007] Figure 1 Figure 2 shows the capacity and potential of various active materials for LIBs (top). Cyclic voltammograms in ether-based (a') and carbonate-based (b') electrolytes at a scan rate of 20 mV / s (bottom). (a) 0.1 M biphenyl (Bp) and 1 M LiPF in dimethoxyethane (DME) 6 , (b) 0.1 M Bp and 1 M LiPF in ethylene carbonate (EC) / diethyl carbonate (DEC) (1:1 v / v) 6 (a') and (b') are the resulting solutions after reaction with Li metal. The active materials in the shaded area can be pre-lithiated using the disclosed method.

[0008] Figure 2 shows the characterization of red P and Sn powder samples before and after pre-lithiation. Figure 2A )Digital image. Figure 2B )Chemical composition. Figure 2C )X-ray diffraction (XRD) pattern. Figure 2D )Scanning electron microscope (SEM) image.

[0009] FIG3 is a series of graphs showing electrochemical characterization of pristine and pre-lithiated P / C electrodes. Figure 3A ) and the voltage curve of the pre-lithiation P / C electrode ( Figure 3B The red curve represents the initial segment. The first ( Figure 3C ) and the second ( Figure 3D ) Cyclic voltage curves. Capacity of original P / C and pre-lithiated P / C electrodes ( Figure 3E ), initial coulombic efficiency (CE) and degree of prelithiation (DOPL) ( Figure 3F ).

[0010] FIG. 4 depicts an embodiment of the disclosed method in ambient air. Figure 4A ) Digital images of 1M Li-Bp tetrahydrofuran (THF) exposed to ambient air for different durations. ( Figure 4B )Snapshot of 1M Li-Bp THF under stirring in ambient air or after addition of water. ( Figure 4C ) Schematic diagram of the prelithiation process in ambient air. ( Figure 4D ) in ( Figure 4A ) shows the capacity of the pre-lithiated P / C electrode prepared by using 1M Li-Bp THF at different exposure times. ( Figure 4E ) corresponding to the DOPL and initial CE.

[0011] FIG5 is a series of graphs showing the electrochemical performance of NMC(111) / graphite, NMC(111) / original P / C, and NMC(111) / partially pre-lithiated P / C full LIBs. Figure 5A ) rate capacity. Figure 5B ) Cycling performance at 1C.

[0012] FIG. 6 is a series of graphs showing the electrochemical performance of pre-lithiated P / C, S / C half-cells, and S / P LIBs. Fig. 6A ) Rate performance of pristine and pre-lithiated P / C. Both start with Li extraction. Figure 6B ) at 1A g -1 Cycling performance of pristine (initial CE = 7.5%) and pre-lithiated P / C (initial CE = 87.8%) under S / C ( Figure 6C ) and S / P LIB( Fig. 6E ) rate performance. At 1A g -1 Next, S / C( Fig.6D ) and S / P LIB( Fig. 6F ) cycle performance.

[0013] Figure 7 is a schematic diagram of a battery pack containing electrodes prepared by the disclosed methods relative to a battery pack containing electrodes not prepared by the disclosed methods.

[0014] FIG. 8 is a graph showing Li( Fig. 8A )、P( Figure 8B ) and Sn( Figure 8C The solutions were prepared by a stepwise dissolution technique, which is equivalent to dissolving 15 mg of powder sample (Li-P or Li-Sn) in 3 L of water solvent.

[0015] FIG. 9 is a diagram showing a P / C composite ( Fig. 9A )、Original P / C electrode( Fig. 9B ), pre-lithiation P / C electrode treated for 10 min ( Fig. 9C )、Cu foil substrate( Fig.9D )、Pristine Sn thin film electrode( Fig.9E ) and pre-lithiated Sn thin film electrode treated for 20 min ( Fig.9F ) of a series of SEM images.

[0016] FIG. 10 is a series of graphs showing voltage curves of a mesoporous C electrode (C:super C65:CMC=75:10:15, by weight) at 0.1 A / g. Fig. 10A ) Original C electrode. ( Fig. 10B ) C electrode treated with 1M Li-Bp THF for 10 min. The electrochemical performance was measured using a half-cell with Li metal as the counter electrode. The electrolyte was 1M LiPF in EC / DEC (1:1 v / v, BASF) with 10 wt% fluoroethylene carbonate (FEC) and 2 wt% vinylene carbonate (VC). 6 .

[0017] Fig.11 A set of voltage curves for pristine (upper) and pre-lithiated (lower) Sn thin film electrodes. The inset is a digital image of the corresponding electrode. The red curve indicates the initial segment.

[0018] Fig.12 is a microscope image of a protective film formed on the surface of a 1 M Li-Bp THF solution in ambient air.

[0019] FIG. 13 is a graph showing the voltage curves of pre-lithiated P / C electrodes prepared using a pre-lithiated reagent exposed to ambient conditions for 1 to 9 days ( Fig.13A -1st cycle; Fig. 13B -2nd cycle). Current density: 0.1 A / g.

[0020] Fig.14 is a schematic diagram of a scalable roll-to-roll embodiment of the disclosed method in ambient air.

[0021] Fig.15 is a graph of the voltage curves of NMC(111) / graphite, NMC(111) / original P / C and NMC(111) / partially pre-lithiated P / C full LIBs at 1C.

[0022] Figure 16 shows the characterization of an electrode embodiment. SEM images of S / C composites, energy dispersive X-ray spectroscopy (EDX) elemental mapping ( Fig.16A ) and thermogravimetric analysis (TGA) curves ( Fig. 16B ).

[0023] Fig.17 It is the cyclic voltammogram of P / C and S / C complexes at a scan rate of 0.1 mV / s.

[0024] FIG. 18 is a set of diagrams showing ( Fig.18A ) Voltage curves of S / C and pre-lithiated P / C half-cells at different current densities. Fig.18B ) Voltage curves of S / P LIB at different current densities. The inset is the theoretical and actual energy density of S / P LIB.

[0025] Fig.19 It shows that the P / C electrode is at 2A g -1 Plot of the long-term stability and Coulombic efficiency for 2000 cycles.

[0026] Fig. 20 is a schematic diagram showing compensation for initial capacity loss of electrodes within a battery pack.

[0027] Fig.21 is a graph showing the open circuit voltage (OCV) of control and pre-lithiated SiO / G composite (using 1 M Li-naphthalene (Nap) THF reagent) half-cells at different immersion times.

[0028] Fig. 22 is a graph showing the 1st discharge (lithium insertion) and charge (lithium extraction) in the 0.05C voltage curves of control and pre-lithiated SiO / G composite (using 1 M Li-Nap THF reagent) half-cells at different immersion times.

[0029] Fig.23 is a graph showing the OCV of control and pre-lithiated SiO / G composite half-cells (using 1 M Li-BpTHF reagent) at different immersion times.

[0030] Fig.24is a graph showing the 1st discharge (lithium insertion) and charge (lithium extraction) in the 0.05C voltage curves of control and pre-lithiated SiO / G composite half-cells (using 1 M Li-BpTHF reagent) at different immersion times.

[0031] Fig.25 Figure 2 shows the full cell (LiNi 0.6 Co 0.2 Mn 0.2 Graph of the first charge and discharge in the 0.05C voltage curve of a cathode (as a full cell configuration).

[0032] Fig.26 is a graph showing the full cell cycling performance at 0.5C of control and pre-lithiated SiO / G composites (using 1 M Li-Bp THF for 30 min).

[0033] Fig. 27 is a graph showing the voltage curves of a pre-lithiated SiO / G composite (using 1 M Li-99FL THF reagent for 10 min) half-cell at 0.05C, 0.1C and 0.2C for 3 cycles.

[0034] Fig.28 is a graph showing the half-cell cycling performance of control and pre-lithiated SiO / G composites (using 1 M Li-99FL THF for 10 min) at 0.5C.

[0035] Fig.29 is a graph showing the OCV of pristine and pre-sodiated hard carbon half-cells (using 1 M Na-Bp THF as the pre-sodiation chemical reagent) at different treatment times.

[0036] Fig.30 is a graph showing the initial Na extraction capacity of different pre-sodiated hard carbon half-cells (using 1 M Na-Bp THF as the pre-sodiation chemical reagent) at 0.05C.

[0037] Fig.31 is a graph showing the voltage profiles of pristine and pre-sodiated hard carbon half-cells (using 1 M Na-Bp THF as the pre-sodiation chemical) at different treatment times during the 1st discharge (sodium insertion) and charge (sodium extraction) cycles at 0.05C.

[0038] Fig.32is a graph showing the initial Na extraction capacity and voltage curves of pristine and pre-sodiated hard carbon half-cells (using 1 M Na-Nap THF as the pre-sodiation chemical reagent) during the 1st discharge (sodium insertion) and charge (sodium extraction) cycles at 0.05C with 2 min treatment time. DETAILED DESCRIPTION

[0039] Lithium-ion batteries (LIBs) with high energy density and good cycling performance are highly desired for the widespread use of portable electronic devices and the emerging electric vehicle market. Conventional LIBs are mainly based on graphite negative electrodes (NE) and lithium metal oxide (LMO) positive electrodes (PE), and their energy densities are typically 150-200 Wh kg -1 , which is difficult to meet the growing demand.

[0040] Considerable efforts have been invested in developing high-capacity NE and PE materials for next-generation LIBs with improved energy density. Various lithium-free NEs (e.g., P, Sn, Si, metal oxides) have been considered as promising alternatives. However, due to solid electrolyte interphase (SEI) formation and irreversible parasitic reactions (e.g., Li+ / -2O+ / -2O+ / -3O+ / -1O+ / -2 ... 2 O formation), most of which have low initial Coulombic efficiency (CE, 50%~85%). This is especially true when nanostructure design is utilized to improve power capacity and cycling performance. A large amount of active Li from PE is consumed during the first charge and permanently trapped in NE, resulting in a significant decrease in the capacity of the full cell. In addition, the optional Li-rich PE is usually limited to LMO with low specific capacity (<200mAh g-1), which hinders further improvement of the energy density of the full cell.

[0041] Prelithiation of NE can be an attractive approach to overcome these drawbacks ( Figure 7 and Fig. 20 ). Prelithiation of NE can compensate for the initial active Li loss and enable the use of high-capacity Li-free PEs (e.g., sulfur, oxygen, V 2 O 5 ) pairing. However, electrode materials are generally difficult to pre-lithiate due to their low potential. In addition, it is also difficult to control the amount of pre-lithiation. Various strategies have been developed to prepare pre-lithiated electrodes. However, since these strategies must be performed in strict environments (e.g., inert environments), these strategies can be complex, time-consuming, technically challenging, and burdensome. Similar problems occur with other alkali metal-based electrodes (e.g., sodium ion batteries). Disclosed herein are methods for overcoming the aforementioned obstacles to effectively and efficiently pre-alkalize electrode materials.

[0042] 1. Definition

[0043] Unless otherwise defined, all technical and scientific terms used in this article have the same meaning as those generally understood by those of ordinary skill in the art. In the event of a conflict, this document (including definitions) shall prevail. Preferred methods and materials are described below, but methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention. All disclosures, patent applications, patents and other references mentioned herein are incorporated herein by reference in their entirety. The materials, methods and examples disclosed herein are illustrative only and are not intended to be limiting.

[0044] As used herein, the terms "including," "comprising," "having," "has," "may," "containing," and variations thereof are intended to be open transitional phrases, terms, or words that do not exclude the possibility of additional actions or structures. Unless the context clearly dictates otherwise, the singular forms "a," "and," and "the" include plural referents. Whether explicitly stated or not, the present disclosure also encompasses other embodiments that "comprise," "consist of," and "consist essentially of" the embodiments or elements presented herein.

[0045] The modifier "about" used in conjunction with an amount includes the stated value and has the meaning dictated by the context (e.g., it includes at least the degree of error associated with the measurement of a particular amount). The modifier "about" should also be considered to disclose a range defined by the absolute values ​​of the two endpoints. For example, the expression "from about 2 to about 4" also discloses a range "from 2 to 4". The term "about" can refer to plus or minus 10% of the indicated number. For example, "about 10%" can indicate a range of 9% to 11%, and "about 1" can mean 0.9-1.1. Other meanings of "about" may be apparent from the context, such as rounding, so, for example, "about 1" can also mean 0.5 to 1.4.

[0046] For reciting numerical ranges herein, each intervening number with the same degree of precision is expressly contemplated. For example, for a range of 6-9, in addition to 6 and 9, the numbers 7 and 8 are also contemplated, and for a range of 6.0-7.0, the numbers 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, and 7.0 are expressly contemplated.

[0047] Definitions of specific functional groups and chemical terms are described in more detail below. For the purposes of this disclosure, chemical elements are identified according to the Periodic Table of the Elements, CAS version, Handbook of Chemistry and Physics, 75th ed., inside cover, and specific functional groups are generally defined as described therein. In addition, general principles of organic chemistry as well as specific functional moieties and reactivities are described in Organic Chemistry, Thomas Sorrell, University Science Books, Sausalito, 1999; Smith and March, March's Advanced Organic Chemistry, 5th ed., John Wiley & Sons, Inc., New York, 2001; Larock, Comprehensive Organic Transformations, VCH Publishers, Inc., New York, 1989; Carruthers, Some Modern Methods of Organic Synthesis, 3rd ed., Cambridge University Press, Cambridge, 1987; the entire contents of each of which are incorporated herein by reference.

[0048] As used herein, the term "alkyl" refers to a straight or branched saturated hydrocarbon chain containing 1 to 30 carbon atoms. y -C z "Alkyl" refers to a straight or branched hydrocarbon having from y to z carbon atoms. Representative examples of alkyl include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, 3-methylhexyl, 2,2-dimethylpentyl, 2,3-dimethylpentyl, n-heptyl, n-octyl, n-nonyl, n-decyl, and n-dodecyl.

[0049] As used herein, the term "alkenyl" means a straight or branched unsaturated hydrocarbon chain containing at least one carbon-carbon double bond and 2 to 30 carbon atoms. As used herein, alkenyl can have 1, 2, 3, 4 or 5 carbon-carbon double bonds. The carbon-carbon double bond can be a cis or trans isomer.

[0050] As used herein, the term "alkylene" refers to a divalent group derived from a straight or branched hydrocarbon having 1 to 50 carbon atoms, such as 2 to 5 carbon atoms. Representative examples of alkylene include, but are not limited to, -CH 2 CH 2 -、-CH 2 CH 2 CH 2 -、-CH 2 CH 2 CH 2 CH 2 -and-CH 2 CH 2 CH 2 CH 2 CH 2 -. The term "C y -C z "Alkylene" means a straight or branched chain hydrocarbon having from y to z carbon atoms.

[0051] As used herein, the term "alkynyl" refers to a straight or branched hydrocarbon group containing 2 to 10 carbon atoms and containing at least one carbon-carbon triple bond. Representative examples of alkynyl include, but are not limited to, ethynyl, 1-propynyl, 2-propynyl, 3-butynyl, 2-pentynyl, and 1-butynyl.

[0052] As used herein, the term "aromatic compound" refers to a compound having at least one aromatic ring in its structure.

[0053] As used herein, the term "aryl" refers to a phenyl group.

[0054] As used herein, the term "cycloalkyl" refers to a saturated ring system containing all carbon atoms as ring members without double bonds. Representative examples of cycloalkyl include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, and cyclodecyl.

[0055] As used herein, the term "cycloalkenyl" refers to a non-aromatic ring system in which all carbon atoms are ring members and contain at least one carbon-carbon double bond and preferably each ring has 5-10 carbon atoms. Representative cycloalkenyls include, but are not limited to, cyclopentenyl, cyclohexenyl and cycloheptenyl.

[0056] The term "carbocycle" includes both "cycloalkyl" and "cycloalkenyl".

[0057] 2. Method of manufacturing electrodes

[0058] Disclosed herein are methods for making electrodes. The electrode can be a negative electrode (e.g., an anode) or a positive electrode (e.g., a cathode). The method includes contacting an electrode material with a mixture comprising an aromatic compound, an alkali metal, and an organic solvent to provide an electrode. These methods are directed to pre-alkalization of the electrode material, and thus provide an electrode. Pre-alkalization refers to the incorporation of an alkali metal into the electrode material to provide an electrode. Therefore, the disclosed method can increase the amount of alkali metal present in the electrode compared to the amount of alkali metal present in the electrode material. By introducing alkali metals into the electrode material and its electrode, these methods can reduce the consequences of solid electrolyte interface formation. Examples of pre-alkalization include, but are not limited to, pre-lithiation, pre-sodiumization, and pre-potassiumization.

[0059] In addition, due to the use of a mixture, the method can be advantageously performed in ambient air. Therefore, in some embodiments, these methods are not performed in an inert gas environment. As used herein, an inert gas environment refers to a gas environment comprising a non-reactive gas known in the art. Examples of non-reactive gases that can be used to provide an inert gas environment include, but are not limited to, nitrogen, argon and other rare gases (and combinations thereof). Therefore, in some embodiments, the method is performed in an environment that does not include nitrogen, argon or a combination thereof. An inert gas environment may have trace amounts of reactive gases (e.g., less than or equal to 5ppm of water and / or less than or equal to 10ppm of oxygen). However, the disclosed method provides a robust process for providing an electrode, which can also allow the method to be performed in an inert environment. Therefore, in some embodiments, these methods are performed in an inert environment. In some embodiments, these methods are performed in an ambient air environment or an inert environment.

[0060] Electrode material can be contacted with mixture for different time amounts.Changing time can realize that there are different amounts of alkali metal in electrode.Therefore, changing time can realize desired characteristic, including but not limited to irreversible capacity and efficiency.Electrode material can be contacted with mixture for about 1 minute to about 2 days, such as about 5 minutes to about 2 days, about 30 minutes to about 2 days, about 1 hour to about 2 days, about 5 hours to about 2 days, about 30 minutes to about 1.5 days, about 1 hour to about 1.5 days, about 5 hours to about 1.5 days, about 10 hours to about 2 days or about 12 hours to about 2 days.In certain embodiments, electrode material is contacted with mixture for greater than 1 minute, greater than 10 minutes, greater than 1 hour, greater than 5 hours, greater than 10 hours, greater than 16 hours or greater than 1 day.In certain embodiments, electrode material is contacted with mixture for less than 2 days, less than 1.5 days, less than 1 day, less than 16 hours or less than 10 hours.

[0061] The provided electrode can be washed with, for example, a non-aqueous solvent. In some embodiments, the electrode is washed with a non-aqueous solvent in 1 to 5 separate washing steps. In some embodiments, the provided electrode may contain residual components of the mixture (e.g., alkali metals, aromatic compounds, solvents, or combinations thereof).

[0062] A. Electrode Materials

[0063] As mentioned above, the provided electrode can be a positive electrode or a negative electrode. Thus, the electrode material can be a positive electrode material or a negative electrode material, wherein the positive electrode material is used to provide the positive electrode, and the negative electrode material is used to provide the negative electrode. In some embodiments, the electrode material itself can be used as an electrode, however, its capacity is reduced compared to the provided electrode of the disclosed method. In a preferred embodiment, the electrode material is a negative electrode material.

[0064] The electrode material may include C, Si, Sn, Sb, P, S, or a combination thereof. The elements described herein may be referred to by their full names (e.g., carbon) or by their abbreviations (e.g., C). In some embodiments, the electrode material includes C, SiO, SnO, or a combination thereof. In some embodiments, the electrode material includes C, SiO, SnO, Li 3 P.Li 22 Sn 5 , SiO / C composite or a combination thereof. In some embodiments, the electrode material is selected from C, SiO, SnO, Li 3 P.Li 22 Sn 5 and SiO / C composites. These elements and their combinations are also referred to as active materials of electrode materials (and electrodes thereof). For example, the electrode material may include an active material, wherein the active material may include C, Si, Sn, Sb, P, S or a combination thereof.

[0065] Examples of carbon include, but are not limited to, graphite, disordered carbon (also referred to as amorphous carbon), carbon black, expanded graphite, graphene, carbon nanotubes, mesoporous carbon, and combinations thereof. Examples of disordered carbon include, but are not limited to, hard carbon and soft carbon. In some embodiments, carbon is selected from the group consisting of graphite, disordered carbon, carbon black, expanded graphite, graphene, carbon nanotubes, and mesoporous carbon. In some embodiments, carbon is selected from the group consisting of graphite, mesoporous carbon, and disordered carbon. Discussions on different types of carbon can be found in Fitzer et al., Pure & Applied Chem. [Pure & Applied Chemistry], Vol. 67, No. 3, pp. 473-506, 1995, which is incorporated herein by reference in its entirety.

[0066] In addition to active materials, electrode materials may also include conductive materials and adhesives. The example of conductive materials includes but is not limited to carbon black (e.g., Ketjenblack, Acetylene black, Vulcan, Furnace black, Ensaco and / or Super), activated carbon, carbon nanotubes, carbon nanofibers and graphene. The example of adhesive includes but is not limited to polyvinylidene fluoride, carboxymethyl cellulose, styrene butadiene rubber, poly (carboxylic acid) and alginate. In certain embodiments, the electrode material includes about 50% to about 100% active material, such as about 60% to about 99% active material, about 70% to about 99% active material, about 60% to about 100% active material or about 75% to about 100% active material.

[0067] The electrode material can be made in a variety of different ways known in the art. For example, the electrode material can be made by coating a slurry of active material and optionally a binder and / or conductive material on a metal (e.g., copper foil). The electrode material can then be dried. In some embodiments, the electrode material is dried at about 20° C. to about 100° C. before being used in the disclosed method. In addition, the electrode material can be dried at about 1 t / cm 2 To about 8t / cm 2 The electrode material is dried under pressure.

[0068] B.Mixture

[0069] The mixture comprises an aromatic compound, an alkali metal and an organic solvent. The components of the mixture can provide advantageous properties, such as allowing the method to be performed under ambient air conditions. Assuming that you are not bound by a particular theory, a film can be formed on the surface of the mixture by the alkali metal and the aromatic compound. The film can limit and / or prevent the reaction of the mixture components and the electrode material with a reactive gas (e.g., ambient air / oxygen), and can limit and / or prevent the evaporation of the organic solvent. Therefore, the method can include a mixture having a film on the surface of the mixture.

[0070] The alkali metal and the aromatic compound can be added to the organic solvent together or one by one. In some embodiments, the aromatic compound is added (e.g., dissolved) to the organic solvent before the alkali metal. The alkali metal can then be added to the organic solvent to provide a mixture. The mixture can then be equilibrated for a period of about 2 minutes to about 24 hours before being used in the disclosed method.

[0071] The mixture may also have a favorable redox potential, allowing it to be used with a variety of electrode materials. For example, the mixture may have a redox potential of less than 1.2V, less than 500mV, less than 200mV, less than 20mV, or less than 10mV. In some embodiments, the mixture has a redox potential greater than 0.1mV, greater than 1mV, greater than 5mV, or greater than 10mV. The redox potential of the mixture may be measured for an electrode material or electrode.

[0072] The mixture may contain various combinations of alkali metals, organic solvents, and aromatic compounds. In some embodiments, the mixture contains an alkali metal selected from the group consisting of Li, Na, K, and combinations thereof; an organic solvent; and an aromatic compound. In some embodiments, the mixture contains an alkali metal; an ether; and an aromatic compound. In some embodiments, the mixture contains an alkali metal; an ether; and an aromatic compound having 1 to 5 rings. In some embodiments, the mixture contains an alkali metal selected from the group consisting of Li, Na, and K; an ether; and an aromatic compound having 1 to 5 rings. In some embodiments, the mixture contains Li and an ether; and an aromatic compound having 1 to 3 rings.

[0073] 1. Aromatic compounds

[0074] The aromatic compound may be a monocyclic aromatic compound or a polycyclic aromatic compound. The aromatic compound may contain 1 to 5 rings. In some embodiments, the aromatic compound contains 1 to 3 rings. The number of rings included in the aromatic compound refers to the rings in a single ring and a fused ring system. For example, biphenyl is an aromatic compound with 2 rings. In addition, isoindene is an aromatic compound with two rings.

[0075] In some embodiments, the aromatic compound has formula (I)

[0076]

[0077] or a salt thereof, wherein: X is C 1 -C 10 Alkyl, C 1 -C 10 Alkylene-G 1 , G 2 or H; G 1 is aryl or C 3 -C 12 Carbon ring; G 2 is aryl or C 3 -C 12 carbocyclic ring; and G is an optionally monocyclic, bicyclic, tricyclic or tetracyclic ring system.

[0078] In some embodiments, X is C 1 -C 5 Alkyl, C 1-C 5 Alkylene-G 1 , G 2 or H; G 1 is an aryl group; G 2 is aryl or C 3 -C 12 carbocyclic ring; and G is an optionally monocyclic, bicyclic or tricyclic ring system.

[0079] In some embodiments, X is C 1 -C 3 Alkylene-G 1 , G 2 or H; G 1 is an aryl group; G 2 is aryl or C 3 -C 12 carbocycle; and G is an optionally monocyclic or bicyclic ring system.

[0080] In some embodiments, the aromatic compound has formula (Ia)

[0081]

[0082] or a salt thereof, wherein: X is C 1 -C 10 Alkyl, C 1 -C 10 Alkylene-G 1 or G 2 ; G 1 is aryl or C 3 -C 12 Carbon ring; G 2 is aryl or C 3 -C 12 Carbon ring.

[0083] In some embodiments, G is present and X is H. In some embodiments, G is present and G is a 5 or 6 membered ring and X is H.

[0084] The alkyl, alkylene, aryl and carbocyclic rings may each independently be optionally substituted. For example, the alkyl, alkylene, aryl and carbocyclic rings may each independently be optionally substituted by an alkyl, an alkenyl, an alkynyl, an aryl or a combination thereof. In some embodiments, the alkyl and / or alkylene groups may each independently be optionally substituted by a C 1 -C 5 In some embodiments, aryl is optionally substituted with aryl. In addition, G can be optionally substituted. For example, in some embodiments, G is optionally substituted with alkyl or aryl. In some embodiments, G is optionally substituted with C 1 -C 5 Alkyl substitution.

[0085] Representative examples of aromatic compounds comprising a ring system fused to the parent phenyl moiety include, but are not limited to, naphthalene (e.g., a monocyclic ring system fused to the parent moiety), azulene (e.g., a monocyclic ring system fused to the parent moiety), anthracene (e.g., a bicyclic ring system fused to the parent moiety), triphenylene (e.g., a tricyclic ring system fused to the parent moiety), and perylene (e.g., a tetracyclic ring system fused to the parent moiety). The fused ring system may be attached to the parent phenyl moiety via any carbon atom contained within the ring.

[0086] In some embodiments, the aromatic compound is selected from the group consisting of tert-amylbenzene, biphenyl, phenylcyclohexane, 1-phenyl-1-cyclohexene, 4-phenylcyclohexene, naphthalene, 1-methylnaphthalene, 2-methylnaphthalene, azulene, indane, indene, isoindene, diphenylmethane, 2,2-diphenylpropane, anthracene, fluorene, 9,9-dimethylfluorene, acenaphthene, acenaphthene, phenanthrene, phenanthren, p-terphenyl, m-terphenyl, o-terphenyl, tetracene, The group consisting of triphenylene, pyrene, fluoranthene, benzo[a]fluorene, benzo[c]fluorene, benzo[a]anthracene, benzo[c]phenanthrene, pentacene, perylene, perylene, olympene, tetraphenylene, benzo[a]pyrene, benzo[e]pyrene, benzo[e]acetophenanthene, benzo[a]fluoranthene, benzo[j]fluoranthene, benzo[k]fluoranthene, dibenzo[a,h]anthracene and dibenzo[a,j]anthracene.

[0087] In some embodiments, the aromatic compound is selected from the group consisting of tert-amylbenzene, biphenyl, phenylcyclohexane, 1-phenyl-1-cyclohexene, 4-phenylcyclohexene, naphthalene, 1-methylnaphthalene, 2-methylnaphthalene, azulene, indane, indene, isoindene, diphenylmethane, 2,2-diphenylpropane, anthracene, fluorene, 9,9-dimethylfluorene, acenaphthene, acenaphthene, phenanthrene, phenanthren, p-terphenyl, m-terphenyl, o-terphenyl, tetracene, The group consisting of triphenylene, pyrene and fluoranthene.

[0088] In some embodiments, the aromatic compound is selected from the group consisting of tert-amylbenzene, biphenyl, phenylcyclohexane, 1-phenyl-1-cyclohexene, 4-phenylcyclohexene, naphthalene, 1-methylnaphthalene, 2-methylnaphthalene, azulene, indane, indene, isoindene, diphenylmethane, 2,2-diphenylpropane, anthracene, fluorene, 9,9-dimethylfluorene, acenaphthene, acenaphthene, phenanthrene, phenanthene, p-terphenyl, m-terphenyl, and o-terphenyl.

[0089] In some embodiments, the aromatic compound is selected from the group consisting of biphenyl, phenylcyclohexane, 1-phenyl-1-cyclohexene, 4-phenylcyclohexene, naphthalene, 1-methylnaphthalene, 2-methylnaphthalene, azulene, indane, indene, isoindene, diphenylmethane, 2,2-diphenylpropane, and 9,9-dimethylfluorene.

[0090] 2. Alkali metals

[0091] During the method, the alkali metal in the mixture can be incorporated into the electrode material. The alkali metal can be added to the mixture in metallic form. The incorporation of the alkali metal may depend on the time of performing the method and / or the concentration of the alkali metal in the mixture. In addition, the alkali metal may contribute to the formation of a film on the surface of the mixture, which has advantageous properties as discussed herein. The alkali metal can be any element (excluding hydrogen) of Group I of the periodic table that can be used in the disclosed electrodes and manufacturing methods. For example, the alkali metal includes Li, Na, K, Rb, Cs and Fr. In some embodiments, the alkali metal includes Li, Na, K or a combination thereof. In some embodiments, the alkali metal is selected from the group consisting of Li, Na, K and a combination thereof. In some embodiments, the alkali metal is selected from the group consisting of Li, Na, K and a combination thereof.

[0092] The alkali metal can be included in the mixture in different amounts. For example, the alkali metal can be included in the mixture at a concentration of about 0.1M to about 10M, such as about 0.5M to about 10M, about 0.75M to about 5M, about 0.1M to about 5M, about 0.1M to about 2M, or about 0.5M to about 2M. In some embodiments, the alkali metal is included in the mixture at a concentration greater than 0.1M, greater than 0.25M, greater than 0.5M, or greater than 0.75M. In some embodiments, the alkali metal is included in the mixture at a concentration less than 10M, less than 7M, less than 5M, or less than 2M. In some embodiments, the alkali metal is included in the mixture at an excess alkali metal solubility in the mixture.

[0093] 3. Organic solvents

[0094] The organic solvent can be any organic solvent that can be used to form a mixture with the alkali metal and the aromatic compound. In a preferred embodiment, the organic solvent includes an ether. Examples of ether-based organic solvents include, but are not limited to, diethyl ether, tetrahydrofuran, 1,4-dioxane, dimethoxyethane, methoxymethane, and diethoxyethane. In certain embodiments, the organic solvent is an ether.

[0095] In some embodiments, the organic solvent comprises tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, ether, dimethoxyethane, diethoxyethane, dimethylformamide, 1-methoxy-2-ethoxyethane, hexamethylphosphoramide, 1,3-dimethoxypropane, 1,2-dimethoxypropane, or a combination thereof. In some embodiments, the organic solvent is selected from the group consisting of tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, ether, dimethoxyethane, diethoxyethane, dimethylformamide, 1-methoxy-2-ethoxyethane, hexamethylphosphoramide, 1,3-dimethoxypropane, 1,2-dimethoxypropane, and a combination thereof.

[0096] C. Electrode

[0097] Electrodes may share some properties of electrode materials. Therefore, the description of electrode materials for active materials, binders, and conductive materials may be applied to electrodes. However, unlike electrode materials, due to the disclosed method, the provided electrode has an increased amount of alkali metal. The increased amount of alkali metal may provide favorable properties for the electrode. For example, the electrode may have a coulombic efficiency greater than or equal to 90%, greater than or equal to 91%, greater than or equal to 92%, greater than or equal to 93%, greater than or equal to 94%, or greater than or equal to 95%. In some embodiments, the electrode has a coulombic efficiency less than or equal to 100%. As used herein, coulombic efficiency refers to the ratio of the first dealkalization capacity (e.g., delithiation or desodiumization) to the first alkalization capacity (e.g., lithiation or sodiumization).

[0098] 2. Method of manufacturing battery pack

[0099] Due to the favorable properties of the provided electrodes, these electrodes can be used in a wide range of energy storage applications. Examples include, but are not limited to, batteries, rechargeable batteries, fuel cells, and redox flow batteries. On the other hand, a method for making a battery comprising the disclosed electrodes is disclosed. The method includes making an electrode as disclosed herein. The provided electrode may contain a residue of a mixture (e.g., an alkali metal, an aromatic compound, a solvent, or a combination thereof). The electrode may also be further processed. For example, the electrode may be processed by techniques including, but not limited to, slurry coating, dry pressing, and other techniques known in the art.

[0100] The method also includes arranging a separator so that the separator is located between the electrode and the second electrode to provide a battery. In the case where the provided electrode is a negative electrode, the second electrode is a positive electrode. And, in the case where the provided electrode is a positive electrode, the second electrode is a negative electrode. In a preferred embodiment, the electrode is a negative electrode and the second electrode is a positive electrode. The positive electrode may include LiCoO 2 、LiNiO 2 、LiMn 2 O 4 , Li 1+n Ni x Mn y Co z O 2 、LiFePO 4 、LiNi x Co y Al z O 2 、V 2 O 5 , sulfur, O 2 , or a combination thereof. In some embodiments, the positive electrode is selected from LiCoO 2 、LiNiO 2 、LiMn2 O 4 , Li 1+n Ni x Mn y Co z O 2 、LiFePO 4 、LiNi x Co y Al z O 2 、V 2 O 5 , sulfur and O 2 Composed of groups.

[0101] The method also includes adding a non-aqueous electrolyte to the battery to provide a battery pack. The non-aqueous electrolyte may include an alkali metal salt, a solvent, and an optional additive. Examples of solvents include, but are not limited to, ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and diethyl carbonate (DEC). Examples of additives include, but are not limited to, vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VEC), ethylene sulfite (ES), 1,3-propane sultone (PS), 1,3-propylene sultone (PRS), catechol carbonate (CC), cyclohexylbenzene (CHB), biphenyl, and pyrocarbonate. In some embodiments, the alkali metal of the alkali metal salt may be the same alkali metal contained in the mixture for providing an electrode. Examples of lithium salts include, but are not limited to, lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, and lithium hexafluoroarsenate. Examples of sodium salts include, but are not limited to, sodium perchlorate and sodium hexafluorophosphate.

[0102] In a preferred embodiment, the battery is a rechargeable lithium ion battery (LIB). In a LIB embodiment, the provided electrode is a negative electrode in contact with a mixture comprising lithium. And, the second electrode is a positive electrode. The positive electrode of the LIB embodiment may comprise LiCoO 2 、LiNiO 2 、LiMn 2 O 4 , Li 1+n Ni x Mn y Co z O 2 、LiFePO 4 、LiNi x Co y Al z O 2 、V 2 O 5 , sulfur, O 2or a combination thereof. In some embodiments, the positive electrode is selected from LiCoO 2 、LiNiO 2 、LiMn 2 O 4 , Li 1+n Ni x Mn y Co z O 2 、LiFePO 4 、LiNi x Co y Al z O 2 、V 2 O 5 , sulfur and O 2 Examples of lithium salts that may be included in LIB embodiments include the same salts listed above with respect to battery packs. In some LIB embodiments, the positive electrode is lithium-free.

[0103] 3. Examples

[0104] Example 1

[0105] Chemical treatment of lithium battery anodes

[0106] experiment

[0107] Preparation of prelithiation reagents : The pre-lithiation reagent was prepared by dissolving excess lithium metal into a biphenyl (Bp) and tetrahydrofuran (THF) solution in an argon-filled glove box. In a typical procedure, 1.54 g of Bp was dissolved in 10 ml of THF to make a 1 M Bp THF solution, and then a piece of Li metal (>0.069 g) was dissolved in this solution to form 1 M Li-BpTHF.

[0108] Pre-lithiation of red P and Sn powder samples :A certain amount of red P (100 mg) and Sn (200 mg) powders were added to 1M Li-Bp THF solution for overnight reaction. The precipitate was separated by centrifugation and washed several times with THF, and then dried under vacuum. In order to eliminate the possible influence of by-products on the following compositional and structural characterizations, all synthesis and washing processes were carried out in an argon-filled glove box. The initially synthesized powder samples were denoted as Li-P and Li-Sn, respectively. ICP analysis was used to determine the composition of Li-P and Li-Sn. First, 15 mg Li-P and 15 mg Li-Sn were added to about 0.5 ml ethanol, respectively, and then dried naturally under ambient conditions. For Li-P, the residue was dissolved and 5% nitric acid (HNO 3) stepwise dilution. For Li-Sn, the residue was dissolved in a few drops of concentrated hydrochloric acid (HCl) and then gradually diluted with deionized water (DI). The dilute solution was analyzed by using the ICP calibration curve method. The powder samples were sealed in an airtight polyethylene sample holder under argon atmosphere for XRD measurements.

[0109] Synthesis of P / C and S / C Composites : Pure P has poor reversibility and problematic cycling stability due to its low electronic conductivity and large volume change. Therefore, a P / C composite was prepared by an evaporation / adsorption strategy. Mesoporous carbon was synthesized by polymerizing resorcinol / formaldehyde onto multi-walled carbon nanotubes, which were subsequently carbonized at 800°C under an argon atmosphere. A certain amount of the as-synthesized mesoporous carbon (150 mg) and red phosphorus (P, 150 mg) were placed in sealed glass tubes under vacuum, respectively. The sealed glass tube was heated to 600°C at a heating rate of 5°C / min and kept at this temperature for 3h. After cooling to 260°C at a cooling rate of 1°C / min, the sealed glass tube was further kept at this temperature for 24h to convert white P into red P. After allowing the container to cool naturally to room temperature, the red P was converted to white P by treating it with CS 2 Wash and dry under vacuum to obtain P / C composite. S / C composite was also prepared by a similar method except using a different thermal treatment procedure. A sealed glass tube containing mesoporous carbon (150 mg) and sulfur (350 mg) was heated to 550°C at a heating rate of 5°C / min and kept at this temperature for 12 h. After allowing the container to cool naturally to room temperature, the S / C composite was obtained without further treatment. The actual contents of P (40 wt.%) and S (64.3 wt.%) were determined by TGA analysis.

[0110] Electrode preparation The P / C electrode was prepared by coating a slurry containing 75 wt.% P / C composite, 10 wt.% super C65 and 15 wt.% carboxymethyl cellulose (CMC) binder on a carbon-coated copper foil substrate. The electrode film was then dried in an oven at 60°C overnight. The mass loading of the P / C composite was 0.8 to 1.1 mg / cm 2 Sn thin film electrodes were prepared by electroless plating of Sn onto Cu foil at room temperature for 5 min. The plating bath contained 0.1 M SnSO 4, 1M thiourea, 0.5M sodium hypophosphite and 0.85M sulfuric acid. Pre-lithiated electrodes were prepared by immersing P / C or Sn thin film electrodes in a pre-lithiation reagent (1M Li-Bp THF) for treatment. The degree of pre-lithiation (DOPL) was controlled by the treatment time. To prevent further reaction, the pre-lithiated electrodes were immediately washed several times with THF to remove residual Li-Bp and then dried under vacuum. Unless otherwise stated, all operations were performed in an argon-filled glove box. To verify the feasibility of pre-lithiation in ambient air, a series of P / C electrodes were also immersed in a pre-lithiation reagent (1M Li-Bp THF) with different exposure times before battery pack assembly, followed by direct drying under vacuum. The immersion time was 10min. The S / C electrode was prepared by coating a slurry containing 70wt% S / C composite, 15wt% super C65 and 15wt% polyvinylidene fluoride (PVDF) binder on a carbon-coated aluminum foil substrate. The electrode film was then dried in an oven at 60°C overnight. The mass loading of the S / C composite was about 1.0 mg / cm 2 .

[0111] Electrochemical testing The electrochemical behavior of Bp / Li-Bp redox couple in ether-based and carbonate-based electrolytes was studied using a three-electrode electrochemical cell and a CHI660 potentiostat. Two blank electrolytes were prepared in advance, namely 1 M LiPF in dimethoxyethane (DME) and 6 and 1M LiPF6 in ethylene carbonate (EC) / diethyl carbonate (DEC) (1:1 v / v, BASF). 0.0925 g Bp and excess Li metal were added to 6 ml of blank electrolyte. The ether-based electrolyte quickly changed from colorless to dark green, indicating the formation of Li-Bp (0.1 M). In contrast, the carbonate-based electrolyte remained colorless. Cyclic voltammetry (CV) tests were performed in the two resulting electrolytes. The working electrode was a glassy carbon disk electrode (φ=3 mm). The counter electrode was a Pt wire electrode. The reference electrode was a Li / Li+ electrode, which was made by encapsulating a Li strip in a glass tube with a Celgard M824 membrane and filling it with the corresponding blank electrolyte. To verify the feasibility of the proposed pre-lithiation method, the electrochemical behavior of the original electrode and the pre-lithiation electrode was measured using a 2032-type button cell with Li metal as the counter electrode. The electrolyte was 1 M LiPF in EC / DEC (1:1 v / v, BASF) with 10 wt% fluoroethylene carbonate (FEC) and 2 wt% vinylene carbonate (VC). 6 Celgard 2325 polymer was used as separator.

[0112] Using 2032-type button cells, NMC(111) / graphite full LIBs were assembled using NMC(111) laminate PE (5 / 16 inch) and graphite laminate NE (7 / 16 inch). The loading of NMC(111) was 6.8 mg / cm -2 The corresponding capacity of PE is 0.93 mAh cm 2 The graphite loading was 3.25 g cm -2 The electrolyte was 1 M LiPF in EC / DEC (1:1 v / v, BASF) with 10 wt% fluoroethylene carbonate (FEC) and 2 wt% vinylene carbonate (VC). 6 . Celgard 2325 polymer was used as a separator. NMC(111) / pristine P / C and NMC(111) / partially prelithiated P / C full LIBs were assembled under similar conditions, except that the graphite NE was replaced by pristine P / C or partially prelithiated P / C NE. Since NMC(111) is in a Li-rich state, it should pair with Li-deficient NE. Partially prelithiated P / C NE was prepared by immersing the pristine P / C electrode in 1M Li-Bp THF for 10s treatment. The electrode was then immediately washed several times with THF to remove residual Li-Bp and dried under vacuum. Before S / P LIB assembly, NE(P / C) and PE(S / C) were also studied using 2032-type button cells with lithium metal as the counter electrode. The electrolyte was 1 M bis(trifluoromethanesulfonyl)imide (LiTFSI) in dimethoxyethane (DME) / 1,3-dioxolane (DOL) (1:1 v / v, BASF) with 0.4 M lithium nitrate (LiNO 3 ) as an additive. The S / P LIB was assembled in a 2032-type button cell with S / C PE (7 / 16 inch) and pre-lithiated P / C NE (1 / 2 inch) using the same ether-based electrolyte. The mass ratio of P / C to S / C was about 1.3:1.

[0113] All cells were assembled in an argon-filled glove box. Constant current charge / discharge tests were performed on an Arbin battery pack test system (BT2000) at room temperature.

[0114] Characterization Scanning electron microscopy (SEM) was performed on a Hitachi S-4800 at an accelerating voltage of 5 kV. Thermogravimetric analysis (TGA) was performed on a SDTQ600 thermal analyzer at a heating rate of 10 °C / min in an argon flow of 50 ml / min. The Cu Kα beam (40 kV, 40 mA, ) were used for X-ray diffraction (XRD). ICP atomic emission spectrophotometry was performed on a Perkin-Elmer Optima 2100DV ICP-OES instrument.

[0115] The theoretical energy density of the sulfur-phosphorus battery is estimated according to the following formula:

[0116]

[0117] The capacity of the S / P LIB is 686 mAh / g (S / C) at a current density of 0.1 A / g. The mass ratio of P / C to S / C is about 1.3:1. The capacity ratio of the first discharge plateau and the second discharge plateau is about 1:2. Therefore, the actual energy density of the sulfur-phosphorus battery is estimated according to the following formula:

[0118]

[0119] result

[0120] Prelithiation of phosphorus and tin :In order to verify the feasibility of the pre-lithiation method, red P and Sn powder samples were used as starting materials and added to 1M Li-Bp THF, respectively. After overnight reaction, the initial dark red P powder turned into an orange product (denoted as Li-P), while the initial light gray Sn powder turned into a dark gray product (denoted as Li-Sn, Figure 2A ). Figure 2B The chemical compositions of Li-P and Li-Sn determined by ICP analysis are given in Figure 8. The atomic ratios of Li / P and Li / Sn are 3.5 / 1 and 3.9 / 1, respectively, which are close to their fully lithiated products (Li 3 P and Li 22 Sn 5 ) stoichiometric ratio. The X-ray diffraction (XRD) patterns of Li-P and Li-Sn are similar to those of Li 3 P and Li 22 Sn 5 The standard data is very consistent, further confirming the complete pre-lithiation after treatment ( Figure 2C The morphology was characterized using scanning electron microscopy ( Figure 2D ). Red P and Li-P show aggregated states, but have different appearances. Sn particles have a smooth surface and become significantly rougher after pre-lithiation. Some Li-Sn particles even crack and break due to large volume expansion.

[0121] To further confirm the pre-lithiation effect, the electrochemical behaviors of the pristine electrode and the pre-lithiated electrode were compared in a half-cell configuration. Red P was pre-loaded into the mesoporous carbon material (P / C) by an evaporation / adsorption strategy, which was then coated on a carbon-coated copper foil to form the pristine P / C electrode. The pristine P / C electrode exhibited an initial open circuit voltage (OCV) of about 2.9 V, a charge / discharge rate of 1773 mAh g -1 The initial lithiation capacity (P / C) and subsequent lithiation capacity of about 1200 mAh g -1 (P / C) reversible capacity ( Figure 3A ). The irreversible capacity loss during the first lithiation is caused by the formation of the SEI layer. The pre-lithiated P / C electrodes were obtained by immersing the original P / C electrodes in 1M Li-Bp THF for different treatment times (Figure 9). Figure 3B The typical voltage curve of the pre-lithiated P / C electrode is shown. The voltage curve shows an initial OCV of about 0.8 V. Since the pre-lithiated P / C electrode is in a Li-rich state, the voltage curve is 0.8 V. -1 The delithiation capacity of (P / C) and similarly subsequently about 1200 mAh g -1 The reversible capacity of (P / C) begins to undergo lithium extraction. The increase in reversible capacity after the first delithiation can be attributed to the contribution of the carbon materials (mesoporous carbon and Super C65) in the electrode (Figure 10). Since the redox potential of Bp / Li-Bp is higher than the electrochemical lithiation potential of the carbon materials ( Figure 1 ), so the carbon material cannot be pre-lithiated by Li-Bp, but can be repeatedly lithiated / delithiated under cyclic conditions. Figure 3C and Figure 3D The first and second cycle voltage curves of the pre-lithiated P / C electrode at different treatment times are shown respectively. Compared with the capacity of the original P / C electrode, the corresponding capacities are summarized in Figure 3E Compared with the initial CE (75%) of the original P / C electrode, the pre-lithiated P / C electrode exhibited a higher initial CE (about 95%) ( Figure 3F ), indicating that a stable SEI layer was formed during prelithiation. The DOPL of prelithiated NE can be expressed as the ratio of the first delithiation capacity / the second delithiation capacity. The DOPL increases with the treatment time and reaches the maximum DOPL (about 80% reversible capacity of P / C) after about 5 minutes ( Figure 3F ), indicating the fine control of DOPL and the high efficiency of this pre-lithiation method. As discussed above, the remaining approximately 20% of the reversible capacity without pre-lithiation comes from the contribution of the carbon material. Similarly, the electrochemical behavior of the original and pre-lithiated Sn electrodes was also compared. The Sn thin film electrode was prepared by electroless plating (Figure 9). After pre-lithiation, the color of the Sn electrode changed from light gray to dark gray ( Fig.11Inset). The OCVs of the pristine and pre-lithiated Sn electrodes are about 2.7 V and about 0.28 V, respectively. The pristine Sn electrode shows an initial lithiation capacity of 0.67 mAh, while the pre-lithiated Sn electrode shows an initial delithiation capacity of 0.73 mAh ( Fig.11 ). These results confirm the effective prelithiation of NE based on P and Sn.

[0122] Prelithiation in ambient air : Prelithiation in ambient air is ideal but very challenging due to the high reactivity of the prelithiation reagents and the prelithiation NE product. Dilute Li-Bp THF (10 mM) will quickly change from dark green to colorless upon exposure to ambient air. However, it was unexpectedly found that concentrated Li-Bp THF (1 M) can be stored in ambient air for more than two weeks and can even withstand repeated stirring ( Figure 4A and Figure 4B ). However, the same volume of pure THF solvent will completely evaporate after only a few hours. This phenomenon can be attributed to the formation of a visible protective film on the surface of the liquid ( Fig.12 ), the protective film not only prevents further reaction of Li-Bp with oxygen or moisture, but also hinders THF evaporation. In addition, the reaction of Li-Bp THF (1M) with water is milder than that of Li metal ( Figure 4B ), thus reducing the handling risk. These features make concentrated Li-BpTHF (1 M) an acceptable pre-lithiation reagent in ambient air. However, subsequent washing to remove residual Li-Bp may expose the highly reactive pre-lithiated NE to ambient air and result in the loss of pre-loaded active Li. Bp can be easily dissolved in 1 M LiPF in dimethoxyethane (DME). 6 and 1 M LiPF in ethylene carbonate (EC) / diethyl carbonate (DEC) (1:1 by volume) 6 electrolyte, but after adding Li metal, only the former turns dark green ( Figure 1 Inset). Cyclic voltammetry (CV) was performed in both resulting solutions. A pair of quasi-reversible redox peaks were observed in the ether-based electrolyte, whereas no such peaks were found in the carbonate-based electrolyte, indicating that Bp is redox active only in ether-based electrolytes. Typically, soluble redox-active species in the electrolyte can react with the electrode materials and thus negatively affect battery performance. Therefore, the washing step is useful for LIBs using ether-based electrolytes, but is unnecessary for LIBs using carbonate-based electrolytes. Figure 4CA prelithiation procedure in ambient air was proposed in . The residual Li-Bp THF can act as a strong protective layer and prevent the prelithiated NE from being depleted in ambient air. During battery assembly, the residual Li-Bp may be consumed by the carbonate-based electrolyte and converted into soluble Bp, which has no effect on battery performance. To verify this procedure, a series of P / C electrodes were treated with 1M Li-Bp THF stored in ambient air for different days ( Figure 4A ) and dried in vacuo without washing. The electrochemical performance was evaluated using a half-cell configuration and carbonate-based electrolytes compared to a control pre-lithiated P / C electrode obtained by a similar method but in an argon-filled glove box and repeated washing. There were no significant differences in their capacity, initial CE, and DOPL ( Figure 4D , Figure 4E , Fig.13A and Fig. 13B ), confirming that the method can be performed in ambient air without adverse effects. We expect to implement it into a commercial manufacturing process using a scalable roll-to-roll design ( Fig.14 ).

[0123] Application of pre-lithiation As mentioned above, prelithiation can improve the available capacity of full LIB by compensating for the initial active Li loss. NMC (111) was used as PE and paired with graphite, pristine P / C, and partially prelithiated P / C NE, respectively. The voltage curves are shown in Fig.15 The full LIB using partially pre-lithiated P / C NE provides much higher capacity than the other two full cells ( Figure 5A and Figure 5B Sulfur has a higher theoretical capacity (1675 mAh g -1 ) and become a promising lithium-free PE, which is usually paired with Li metal NE. Although the resulting Li-S battery has a high theoretical energy density, Li metal NE remains a big obstacle due to its low CE and serious safety hazards. Most studies still rely on the use of a large amount of excess Li metal NE, limiting its actual energy density. Pre-lithiation can replace Li metal with other high-capacity NE. Sulfur / mesoporous carbon composites (S / C) were prepared as PE materials (Figure 16). Before full cell assembly, the electrochemical properties of NE and PE materials were studied using a half-cell configuration. Both NE and PE exhibited good rate capacity ( Fig. 6A and Figure 6C ) and cyclic stability ( Figure 6B and Fig.6D ; Fig.17 ). It is worth noting that, except for the initial few cycles, the rate capacity and cycling performance of the original and pre-lithiated P / C are almost identical to each other ( Fig. 6A , Figure 6B and Fig.19 ), indicating that the prelithiation treatment will not destroy the stability of the electrode. Subsequently, new S / P LIBs were assembled by coupling S / C PEs with prelithiated P / C NEs. In the case of using limited Li sources in prelithiated P / C NEs, S / PLIBs exhibited excellent electrochemical performance at 0.1, 0.2, 0.5, 1, 1.5, and 2 A g -1 The following shows 686, 589, 485, 421, 363 and 327 mAh g -1 When the current density returns to 0.1A g -1 It can provide 681mAh g -1 The reversible capacity of (S / C) Fig. 6E ). -1 Under the S / P LIB, 460mAh g -1 The initial capacity of (S / C) was 312 mAh g after 300 cycles. -1 (S / C) reversible capacity, where the capacity decreases by 0.10% per cycle and the average CE exceeds 99% ( Fig. 6F ).like Fig.18A and Fig.18B As shown in the figure, the S / P LIB exhibits a voltage curve similar to that of the S / C half-cell at different voltages, thus -1 The following figure shows two discharge plateaus at 1.4V and 1.1V. Despite the slightly lower output voltage, the newly configured S / P LIB can deliver 1222Wh kg -1 The theoretical maximum energy density is 2.3A g / cm2, because both S and P have high specific capacities. -1 The discharge capacity under the condition of 358Wh kg -1 The energy density ( Fig.18B Inset), which is much higher than that of conventional LIBs. In addition, both S and P are cheap and environmentally abundant. These properties make the newly configured S / P LIBs a potential candidate for next-generation battery packs.

[0124] Example 2

[0125] Chemical treatment of silicon-based anodes

[0126] Sample 1:Preparing pre-lithiation reagent by dissolving excess metallic lithium in naphthalene (Nap) and tetrahydrofuran (THF) solution. In a typical procedure, 1.28g Nap is dissolved in 10ml THF to make 1M Nap THF solution, and then excess lithium metal is dissolved in this solution to form 1M Li-Nap THF solution. Pre-lithiation is carried out by immersing SiO / graphite (SiO / G) composite electrode in the reagent. The degree of pre-lithiation can be controlled by immersion time.

[0127] Using pre-lithiated SiO / G as cathode, metallic lithium as anode, 1M LiPF dissolved in EC / EMC (volume ratio of 3:7) with 10wt.% FEC and 2wt.% VC additives 6 As electrolyte and glass fiber (GD / D type) as separator, a half-cell was assembled. -1 ) was used for the first formation charge / discharge cycle between 0.02 and 1.5 V. For the full cell structure, LiNi 0.6 Co 0.2 Mn 0.2 (NCM622) was used as cathode, pre-lithiated SiO / G was used as anode, and Celgard 2325 was used as separator. The reversible surface capacity of NCM622 and SiO / G was 3 mAh cm -2 . The sizes of SiO / G and NCM622 electrodes are 5 / 8 and 9 / 16 inches of OD, respectively. The reversible capacity (N / P ratio) of the negative electrode to the positive electrode is about 1.2. The formation process of the full battery test includes 3 cycles: constant current (CC) charging at 0.05C, 0.1C, and 0.2C, with constant voltage (CV) charging to 0.05C, followed by CC discharge at 0.05C, 0.1C, and 0.2C. The voltage range is 2.7 to 4.3V. The cycle test of the full battery test is CC charging at 0.5C, with CV charging to 0.05C, followed by CC discharge at 0.5C. The voltage range is 3 to 4.3V.

[0128] like Fig.21 As shown, the OCV of the pre-lithiation sample decreases with increasing immersion time, indicating that lithium ions have been pre-loaded into the silicon-based material. The first 10 min of pre-lithiation time resulted in a significant decrease in the OCV to about 1.1 V. Fig. 22 Typical voltage curves of control and pre-lithiated silicon-based electrodes with different pre-lithiation depths are shown. The initial discharge (lithium insertion) and charge (lithium extraction) capacities of the control sample are 1500 and 1070 mA h g, respectively. -1, indicating an initial CE of about 71%. Since the pre-lithiated Si-based electrode is in a Li-rich state, it starts with lithium extraction in the half-cell test. As the immersion time increases, the Li extraction capacity increases from 2 mAh g for 10 min pre-lithiated Si to 2 mAh g for 10 min pre-lithiated Si. -1 Increased to about 140 mAh g after 5 h pre-lithiation -1 . Meanwhile, the first discharge capacity decreases, while the charge capacity remains almost unchanged, so the initial CE increases. The 5 h pre-lithiation sample is an exception, where both the discharge / charge capacities decrease, which may be attributed to the structural deformation caused by the long pre-lithiation. A minimum pre-lithiation time of 1 h is useful to obtain a satisfactory initial CE of about 83%, with lithiation and delithiation capacities of 1070 and 1300 mA h g, respectively. -1 The decrease in irreversible capacity and increase in CE after prelithiation can be attributed to the formation of SEI and the prior prelithiation during the prelithiation process, which transfers lithium ions from the prelithiation reagent to the SiO / G composite.

[0129] Sample 2 : Biphenyl (Bp) was used to prepare the pre-lithiation reagent. The same process was used to prepare 1M Li-Bp THF solution. Fig.23 As shown in Figure 3, the OCV of the 10 min prelithiation sample is 0.8 V, indicating that the prelithiation effect is better than that of the Li-Nap THF reagent. Therefore, the shorter 30 min prelithiation time yields a high initial CE of about 85%, with lithiation and delithiation capacities of 1150 and 980 mA h g, respectively. -1 ( Fig.24 ). Fig.25 The full-cell tests in the study showed that the initial CE was greatly improved by pre-lithiation, i.e., 82.9% after 30 min of pre-lithiation compared to 48.8% for the control sample. In addition, the pre-lithiation process did not seem to have a negative impact on the full-cell cycling performance ( Fig.26 ).

[0130] Sample 3 : 9,9-dimethylfluorene (99FL) was used to prepare 1MLi-99FL THF solution for pre-lithiation. Fig. 27 As shown in Figure 2, the first lithiation and delithiation capacities of the 10 min pre-lithiation sample are 1200 and 1045 mA h g -1 , thus showing a high initial CE of 87%. Among all three reagents, the shortest pre-lithiation time of 10 min had the best pre-lithiation effect of 99 FL. Similarly, the half-cell cycling performance of the pre-lithiation sample did not change compared with the control sample ( Fig.28 ).

[0131] Example 3

[0132] Chemical treatment of sodium battery anodes

[0133] The pre-sodiumation reagent is prepared by dissolving excess metallic sodium in a solution of biphenyl (Bp) and tetrahydrofuran (THF). In a typical procedure, 1.54 g of Bp is dissolved in 10 ml of THF to make a 1 M Bp THF solution, and then a piece of sodium metal is dissolved in this solution to form 1 M Na-Bp THF. The resulting pre-sodiumation reagent is used to pre-sodiumize a hard carbon electrode. The degree of pre-sodiumization can be controlled by the treatment time. Using pre-sodiumized hard carbon as the cathode, metallic sodium as the anode, 1 M NaClO dissolved in EC / DMC (1:1 by volume) with 5 wt.% FEC additive 4 As electrolyte and glass fiber as separator, a half-cell was assembled. The first charge / discharge cycle was carried out at 0.05C (1C = 160 mA g -1 )

[0134] like Fig.29 As shown in , the OCV of the pre-sodiumized sample decreases with increasing treatment time. The original hard carbon electrode without pre-sodiumization exhibits an OCV of about 2.5 V, while the sample with a 5 min pre-sodiumization time exhibits an OCV of about 0.24 V, indicating that sodium ions have been inserted into the hard carbon material. Since the pre-sodiumized hard carbon electrode is in a Na-rich state, it starts with Na extraction. Fig.30 As shown in Figure 3, the Na extraction capacity increased with increasing pre-sodiumization time. Fig.31 Typical voltage curves of pristine and pre-sodiumized hard carbon electrodes with different pre-sodiumization depths are shown. The initial discharge (sodium insertion) and charge (sodium extraction) capacities of the pristine hard carbon electrode are 286.3 and 155 mA h g, respectively. -1 , indicating an initial Coulombic efficiency of about 54%.

[0135] At the same time, the first discharge capacity decreased, while the charge capacity remained almost unchanged, and thus the initial Coulombic efficiency increased. A short pre-sodiumization time of 2 min resulted in a high initial Coulombic efficiency of 92.8%, with the sodiumation and de-sodiumation capacities of 170.8 and 158.5 mA h g, respectively. -1 The decrease in irreversible capacity and increase in Coulombic efficiency after pre-sodiumization can be attributed to the pre-formation of SEI during the pre-sodiumization process.

[0136] Naphthalene was also used to prepare the pre-sodium chemical reagent, that is, excess sodium metal was dissolved in naphthalene (Nap) and THF solution to make 1M Na-Nap THF solution. The hard carbon electrode was immersed in the solution for 2 min at room temperature. The half-cell was assembled using the same electrolyte and separator as above. Fig.32As shown in Figure 2, the OCV of the pre-sodiumized sample is 0.37 V, indicating that sodium has been successfully inserted into the hard carbon material. The initial Na extraction capacity is about 69 mA h g -1 The first sodiumation and desodiumation capacities of the pre-sodiumized sample were 168.9 and 155.3 mA h g -1 , thus indicating a high initial Coulombic efficiency of 92%.

[0137] Example 4

[0138] Comparative pre-lithiation analysis

[0139] The pre-lithiation capabilities of different reagents and anode materials were analyzed. The results are listed in Table 1 below.

[0140] Table 1. Prelithiation capabilities of various anode materials by different reagents.

[0141]

[0142]

[0143] For reasons of completeness, various aspects of the invention are set out in the following numbered clauses:

[0144] Item 1. A method of manufacturing an electrode, the method comprising: contacting an electrode material with a mixture comprising an aromatic compound, an alkali metal, and an organic solvent to provide the electrode.

[0145] Clause 2. The method of Clause 1, wherein the method is performed under ambient air.

[0146] Clause 3. The method of Clause 1 or Clause 2, wherein the aromatic compound contains 1 to 5 rings.

[0147] Clause 4. The method of any one of clauses 1 to 3, wherein the aromatic compound has formula (I)

[0148]

[0149] or a salt thereof, wherein: X is C 1 -C 10 Alkyl, C 1 -C 10 Alkylene-G 1 , G 2 or H; G 1 is aryl or C 3 -C 12 Carbon ring; G 2 is aryl or C 3 -C 12 carbocyclic ring; and G is an optionally monocyclic, bicyclic, tricyclic or tetracyclic ring system.

[0150] Clause 5. The method according to clause 4, wherein X is C 1 -C 5 Alkyl, C 1 -C 5 Alkylene-G 1 , G 2 or H; G 1 is an aryl group; G 2 is aryl or C 3 -C 12 carbocyclic ring; and G is an optionally monocyclic, bicyclic or tricyclic ring system.

[0151] Clause 6. The method according to Clause 4, wherein X is C 1 -C 3 Alkylene-G 1 , G 2 or H; G 1 is an aryl group; G 2 is aryl or C 3 -C 12 carbocycle; and G is an optionally monocyclic or bicyclic ring system.

[0152] Clause 7. The method of any one of clauses 1 to 6, wherein the aromatic compound is selected from the group consisting of tert-amylbenzene, biphenyl, phenylcyclohexane, 1-phenyl-1-cyclohexene, 4-phenylcyclohexene, naphthalene, 1-methylnaphthalene, 2-methylnaphthalene, azulene, indane, indene, isoindene, diphenylmethane, 2,2-diphenylpropane, anthracene, fluorene, 9,9-dimethylfluorene, acenaphthene, acenaphthene, phenanthrene, phenanthren, p-terphenyl, m-terphenyl, o-terphenyl, tetracene, Triphenylene, pyrene, fluoranthene, benzo[a]fluorene, benzo[c]fluorene, benzo[a]anthracene, benzo[c]phenanthrene, pentacene, perylene, perylene, olympene, tetraphenylene, benzo[a]pyrene, benzo[e]pyrene, benzo[e]acetophenanthene, benzo[a]fluoranthene, benzo[j]fluoranthene, benzo[k]fluoranthene, dibenzo[a,h]anthracene, dibenzo[a,j]anthracene, and combinations thereof.

[0153] Clause 8. The method of any one of Clauses 1 to 7, wherein the organic solvent comprises an ether.

[0154] Clause 9. The method of any one of clauses 1 to 7, wherein the organic solvent comprises tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, diethyl ether, dimethoxyethane, diethoxyethane, dimethylformamide, 1-methoxy-2-ethoxyethane, hexamethylphosphoramide, 1,3-dimethoxypropane, 1,2-dimethoxypropane or a combination thereof.

[0155] Clause 10. The method of any one of Clauses 1 to 9, wherein the alkali metal comprises Li, Na, K, or a combination thereof.

[0156] Clause 11. The method of any one of Clauses 1 to 10, wherein the alkali metal is present in the mixture at a concentration of about 0.1 M to about 10 M.

[0157] Clause 12. The method of any one of Clauses 1 to 11, wherein the mixture has a redox potential of less than 1.2 V to the electrode.

[0158] Clause 13. The method of any one of Clauses 1 to 12, wherein the electrode material comprises C, Si, Sn, Sb, P, S, or a combination thereof.

[0159] Item 14. The method of Item 13, wherein the electrode comprises C, SiO, SnO, or a combination thereof.

[0160] Clause 15. The method of Clause 13 or Clause 14, wherein C comprises graphite, disordered carbon, carbon black, expanded graphite, graphene, carbon nanotubes, or a combination thereof.

[0161] Clause 16. The method of any one of Clauses 1 to 15, wherein the electrode material further comprises a binder, a conductive material, or a combination thereof.

[0162] Clause 17. The method of any one of Clauses 1 to 16, wherein the electrode material and the mixture are contacted for about 1 minute to about 2 days.

[0163] Clause 18. The method of any one of Clauses 1 to 17, wherein the Coulombic efficiency of the electrode is greater than or equal to 90%.

[0164] Item 19. A method of manufacturing a battery, the method comprising: manufacturing an electrode as described in Items 1 to 18; arranging a separator so that it is located between the electrode and a second electrode to provide a battery; and adding a non-aqueous electrolyte to the battery to provide the battery.

[0165] Clause 20. The method of Clause 19, wherein the second electrode comprises LiCoO 2 、LiNiO 2 、LiMn 2 O 4 , Li 1+n Ni x Mn y Co z O 2 、LiFePO 4 、LiNi x Co y Al z O 2 、V 2 O 5 , sulfur, O2 or a combination thereof.

[0166] Item 21. The method of Item 19 or Item 20, wherein the nonaqueous electrolyte comprises an alkali metal salt, a solvent, and optionally an additive.

Claims

1. A method for manufacturing an electrode, the method comprising: - contacting an electrode material with a mixture comprising an aromatic compound, an alkali metal, and an organic solvent to provide the electrode, the electrode material comprising an active material comprising C, Si, Sn, P, S, or Sb, or a combination thereof, and - washing the electrode with a non-aqueous solvent, The method is carried out under ambient air.

2. The method of claim 1, wherein the aromatic compound comprises 1 to 5 rings.

3. The method of claim 1, wherein the aromatic compound has formula (I) or a salt thereof, wherein: X is C1-C 10 Alkyl, C1-C 10 Alkylene-G 1 , G 2 or H; G 1 is aryl or C3-C 12 Carbon ring; G 2 is aryl or C3-C 12 Carbon rings; and G is an optional monocyclic, bicyclic, tricyclic or tetracyclic ring system.

4. The method of claim 3, wherein X is C1-C5 alkyl, C1-C5 alkylene-G 1 , G 2 or H; G 1 is an aromatic group; G 2 is aryl or C3-C 12 Carbon rings; and G is an optional monocyclic, bicyclic or tricyclic ring system.

5. The method of claim 3, wherein X is C1-C3 alkylene-G 1 , G 2 or H; G 1 is an aromatic group; G 2 is aryl or C3-C 12 Carbon rings; and G is an optional monocyclic or bicyclic ring system.

6. The method of claim 1, wherein the aromatic compound is selected from the group consisting of: tert-Amylbenzene; Biphenyl; Phenylcyclohexane; 1-phenyl-1-cyclohexene; 4-phenylcyclohexene; Naphthalene; 1-Methylnaphthalene; 2-Methylnaphthalene; Azulene; indica; indene; Isoindene; Diphenylmethane; 2,2-Diphenylpropane; Anthracene; Fluorene; 9,9-Dimethylfluorene; Acenaphthene; Acenaphthylene; Phenanthrene; Phenalene; p-Terphenyl; m-Terphenyl; o-Terphenyl; Tetracene; Triphenylene; Pyrene; Fluoranthene; Benzo[a]fluorene; Benzo[c]fluorene; Benzo[a]anthracene; Benzo[c]phenanthrene; Pentacene; Perylene; Picene; Olympicene; Tetracenequinone; Benzo[a]pyrene; Benzo[e]pyrene; Benzo[e]acephenanthrylene; Benzo[a]fluoranthene; Benzo[j]fluoranthene; Benzo[k]fluoranthene; Dibenzo[a,h]anthracene; Dibenzo[a,j]anthracene; and combinations thereof.

7. The method according to claim 1, wherein the organic solvent comprises an ether.

8. The method according to claim 1, wherein the organic solvent comprises tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, diethyl ether, dimethoxyethane, diethoxyethane, dimethylformamide, 1-methoxy-2-ethoxyethane, hexamethylphosphoramide, 1,3-dimethoxypropane, 1,2-dimethoxypropane, or combinations thereof.

9. The method according to claim 1, wherein the alkali metal comprises Li, Na, K, or combinations thereof.

10. The method according to claim 1, wherein the alkali metal is present in the mixture at a concentration of about 0.1 M to about 10 M, where about means plus or minus 10% of the indicated number.

11. The method according to claim 1, wherein the redox potential of the mixture with respect to the electrode is less than 1.2 V.

12. The method of claim 1, wherein the electrode comprises C, SiO, SnO or a combination thereof.

13. The method of claim 1 or claim 12, wherein C comprises graphite, disordered carbon, carbon black, expanded graphite, graphene, carbon nanotubes, or a combination thereof.

14. The method of claim 1, wherein the electrode material further comprises a binder, a conductive material or a combination thereof.

15. The method of claim 1, wherein the electrode material and the mixture are contacted for about 1 minute to about 2 days, wherein about refers to plus or minus 10% of the indicated number.

16. The method of claim 1, wherein the Coulombic efficiency of the electrode is greater than or equal to 90%.

17. A method for manufacturing a battery pack, the method comprising: - manufacturing an electrode as claimed in claim 1; - arranging the separator so that it is located between the electrode and a second electrode to provide a battery; as well as - Adding a non-aqueous electrolyte to the cell to provide the battery.

18. The method of claim 17, wherein the second electrode comprises LiCoO2, LiNiO2, LiMn2O4, Li 1+n Ni x Mn y Co z O2, LiFePO4, LiNi x Co y Al z O2, V2O5, sulfur, O2 or a combination thereof.

19. The method of claim 17 or claim 18, wherein the non-aqueous electrolyte comprises an alkali metal salt, a solvent and optionally an additive.