Semiconductor structure and method for forming the same

By forming small-size openings and doped regions on the surface of the semiconductor to be etched, and forming a large-size mask, the problem of poor graphics accuracy in the lithography process is solved, and the performance and graphics accuracy of semiconductor products are improved.

CN113078049BActive Publication Date: 2024-11-22SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010011099.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-06
Publication Date
2024-11-22
Estimated Expiration
2040-01-06

AI Technical Summary

Technical Problem

During semiconductor manufacturing, the pattern accuracy transferred to the layer to be etched during the photolithography process is poor, resulting in poor performance of semiconductor products.

Method used

By forming the first and second openings on the surface of the layer to be etched, and forming connected doped regions in these openings, these doped regions are used as masks for etching to improve pattern accuracy and morphology. The specific steps include forming small-sized openings and doped regions on the sacrificial layer and forming large-sized masks through these openings to improve pattern transfer accuracy.

Benefits of technology

The graphical transfer of high precision and high morphology is achieved, the performance of the semiconductor structure is improved, the graphics accuracy and morphology are ensured, and the maximum size of the mask is controlled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113078049B_ABST
    Figure CN113078049B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the same, the method comprising: providing a layer to be etched, the layer to be etched comprising a first region; forming a first pattern material layer on the surface of the layer to be etched; forming a sacrificial layer on the surface of the first pattern material layer; forming a first opening in the sacrificial layer in the first region, the first opening exposing a portion of the surface of the first pattern material layer in the first region; after forming the first opening, using the sacrificial layer as a mask, forming a first doped region in the first pattern material layer; after forming the first doped region, forming a second opening in the sacrificial layer in the first region, the second opening exposing a portion of the surface of the first pattern material layer in the first region; after forming the second opening, using the sacrificial layer as a mask, forming a second doped region in the first pattern material layer, the second doped region being connected to the first doped region. The semiconductor structure and the method for forming the same can improve the performance of semiconductor products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a forming method thereof. Background Art

[0002] In the process of forming and manufacturing semiconductor products, the pattern is usually transferred from the mask to the surface of the silicon wafer through the photolithography process to form a semiconductor product that meets the design requirements. In the photolithography process, first, through the exposure step, the light passes through the light-transmitting or light-reflecting area in the mask to irradiate the layer to be etched coated with photoresist, and a photochemical reaction occurs with the photoresist; then, through the development step, the degree of solubility of the photosensitive and non-photosensitive photoresists in the developer is used to form a photolithography pattern to achieve the transfer of the mask pattern; then, through the etching step, the layer to be etched is etched based on the photolithography pattern formed by the photoresist layer, and the mask pattern is further transferred to the layer to be etched.

[0003] However, the accuracy of the pattern transferred to the layer to be etched is still poor, resulting in poor performance of the semiconductor product. Summary of the invention

[0004] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the accuracy of the pattern transferred to the layer to be etched, thereby improving the performance of the semiconductor structure.

[0005] To solve the above technical problems, the technical solution of the present invention provides a method for forming a semiconductor structure, comprising: providing a layer to be etched, the layer to be etched comprising a first region; forming a first graphic material layer on the surface of the layer to be etched; forming a sacrificial layer on the surface of the first graphic material layer; forming a first opening in the sacrificial layer in the first region, the first opening exposing a portion of the surface of the first graphic material layer in the first region; after forming the first opening, using the sacrificial layer as a mask to form a first doped region in the first graphic material layer; after forming the first doped region, forming a second opening in the sacrificial layer in the first region, the second opening exposing a portion of the surface of the first graphic material layer in the first region; after forming the second opening, using the sacrificial layer as a mask to form a second doped region in the first graphic material layer, the second doped region being connected to the first doped region.

[0006] Optionally, it also includes: after forming the second doping region, removing the sacrificial layer; after removing the sacrificial layer, forming a first graphic layer, the first graphic layer including the first doping region and the second doping region, and the first graphic layer is located on the surface of the layer to be etched in the first region; using the first graphic layer as a mask, etching the layer to be etched in the first region.

[0007] Optionally, the method for forming the first opening includes: forming a second graphic layer on the surface of the sacrificial layer, the second graphic layer exposing a portion of the surface of the sacrificial layer in the first area; and etching the sacrificial layer using the second graphic layer as a mask until the surface of the first graphic material layer is exposed.

[0008] Optionally, the method for forming the second opening includes: after forming the first doped region, forming a first barrier layer in the first opening; after forming the first barrier layer, forming a third graphic layer on the surface of the first barrier layer and the sacrificial layer, the third graphic layer exposing a portion of the sacrificial layer surface of the first region; using the third graphic layer as a mask, etching the sacrificial layer until the surface of the first graphic material layer is exposed.

[0009] Optionally, the method for forming the second opening includes: after forming the first doped region, forming a first barrier layer in the first opening; after forming the first barrier layer, forming a third graphic layer on the surface of the first barrier layer and the sacrificial layer, the third graphic layer exposing a portion of the sacrificial layer surface of the first region and a portion of the first barrier layer surface, and the exposed sacrificial layer surface is connected to the surface of the first barrier layer; using the third graphic layer as a mask, etching the sacrificial layer until the surface of the first graphic material layer is exposed.

[0010] Optionally, after removing the sacrificial layer and before forming the first graphic layer, the surface of the first graphic material layer is cleaned.

[0011] Optionally, the method for forming the first graphic layer includes: after removing the sacrificial layer, etching the first graphic material layer.

[0012] Optionally, the process of etching the first pattern material layer includes a wet etching process, and the etching rate of the first pattern material layer by the wet etching process is greater than the etching rate of the first doping region and the second doping region.

[0013] Optionally, the process of forming the first doping region includes a first ion implantation process.

[0014] Optionally, the process of forming the second doping region includes a second ion implantation process.

[0015] Optionally, the type of ions doped in the first doping region is the same as the type of ions doped in the second doping region.

[0016] Optionally, the first opening has a first projection on the surface of the layer to be etched, and the second opening has a second projection on the surface of the layer to be etched, the first projection and the second projection are arranged at intervals along a first direction, and the distance between the first projection and the second projection is less than 20 nanometers.

[0017] Optionally, the first opening has a first projection on the surface of the layer to be etched, and the second opening has a second projection on the surface of the layer to be etched, the first projection and the second projection are arranged along a first direction, the first projection and the second projection partially overlap, and, in the first direction, the spacing between the edges of the overlapping parts of the first projection and the second projection is less than 20 nanometers.

[0018] Optionally, along the first direction, the width of the first projection ranges from 30 nanometers to 50 nanometers, and the width of the second projection ranges from 30 nanometers to 50 nanometers.

[0019] Optionally, the layer to be etched also includes a second area; the method for forming the semiconductor structure also includes: forming a fourth graphic layer on the surface of the layer to be etched in the second area, wherein in a second direction perpendicular to the first direction, a projection of the fourth graphic layer on the surface of the layer to be etched has a first length, and the first length is greater than 50 nanometers; using the fourth graphic layer as a mask, etching the layer to be etched in the second area.

[0020] Optionally, the sacrificial layer includes a sacrificial barrier layer located on the surface of the first graphic material layer, and an anti-reflection layer located on the surface of the sacrificial barrier layer.

[0021] Optionally, the material of the first patterned material layer includes amorphous silicon.

[0022] Optionally, the ions doped in the first doping region include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions; and the ions doped in the second doping region include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions.

[0023] Optionally, the first graphic layer further includes a third doping region.

[0024] Correspondingly, the technical solution of the present invention also provides a semiconductor structure, including: a layer to be etched, the layer to be etched including a first area; a first graphic material layer located on the surface of the layer to be etched; a sacrificial layer located on the surface of the first graphic material layer; a first opening located in the sacrificial layer in the first area, the first opening exposing a portion of the surface of the first graphic material layer in the first area; a first doped area located in the first graphic material layer; a second opening located in the sacrificial layer in the first area, the second opening exposing a portion of the surface of the first graphic material layer in the first area; a second doped area located in the first graphic material layer, the second doped area being connected to the first doped area.

[0025] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0026] In the method for forming a semiconductor structure of the technical solution of the present invention, since the first opening and the second opening are formed, and the first doped region and the second doped region connected to each other are formed through the first opening and the second opening, therefore, in the extension direction where the first doped region connects the second doped region, through the first opening and the second opening of small size, a mask with a large size in the extension direction can be formed subsequently, that is, a mask including the first doped region and the second doped region, thereby realizing the transfer of the pattern with a large size in the extension direction to the layer to be etched; not only that, since the first opening and the second opening are small in size in the extension direction, when the photoresist layer is exposed through the exposure step to form the pattern layer of the first opening and the second opening, a pattern layer pattern with high precision can be obtained, therefore, the formed first opening and the second opening pattern has high precision and good morphology, thereby, the pattern of the first doped region and the second doped region formed through the first opening and the second opening has high precision and good morphology, that is, the pattern of the mask including the first doped region and the second doped region has high precision and good morphology, thereby improving the precision of the pattern transferred to the layer to be etched, and improving the performance of the semiconductor structure.

[0027] Furthermore, since the first projection and the second projection are arranged at intervals along the first direction, and the distance between the first projection and the second projection is less than 20 nanometers, the distance between the first opening and the second opening is small, so that when the first doping region and the second doping region are formed, the diffusion of doping ions can connect the first doping region and the second doping region.

[0028] Furthermore, since the first projection and the second projection are arranged along the first direction, the first projection and the second projection partially overlap, and, in the first direction, the spacing between the edges of the overlapping parts of the first projection and the second projection is less than 20 nanometers, therefore, on the one hand, a mask layer having a graphic size larger than the first opening or the second opening can be formed, and on the other hand, the maximum size of the mask layer is controlled, so that a mask layer having an appropriate graphic size can be formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the top view structure of a mask;

[0030] Figures 2 to 12 It is a schematic cross-sectional structure diagram of a semiconductor structure forming process according to an embodiment of the present invention. DETAILED DESCRIPTION

[0031] As described in the background art, the pattern accuracy transferred to the layer to be etched is still poor, resulting in poor performance of semiconductor products.

[0032] Figure 1It is a schematic diagram of the top view structure of a mask.

[0033] Please refer to Figure 1 , the mask includes area A and area B.

[0034] In the A region, the mask has a plurality of first openings 10 ; in the B region, the mask has a second opening 11 .

[0035] The first opening 10 and the second opening 11 both serve as light-transmitting or light-reflecting areas of the mask, so that, through an exposure step, light can be irradiated onto a silicon wafer coated with a photoresist through the first opening 10 and the second opening 11 in the mask, and undergo a photochemical reaction with the photoresist. Then, through a development step, a photolithography pattern is formed by utilizing the degree of solubility of the photosensitive and non-photosensitive photoresists in the developer, thereby realizing the transfer of the mask pattern.

[0036] In the above embodiment, the length H of the first opening 10 in the Y direction is relatively large and the length P in the X direction is relatively small. At the same time, in the entire mask, the number of the first openings 10 is greater than that of the second openings 11. Therefore, by adjusting the parameters of the light source during the exposure process, the exposure range of the exposure process in the Y direction is larger and the accuracy is higher. Therefore, the morphology of the lithography pattern corresponding to the larger number of the first openings 10 is better.

[0037] However, the exposure process cannot take into account the exposure range and accuracy in the Y direction and in the X direction at the same time. Since the parameters of the light source are adjusted to make the exposure range of the exposure process larger and more accurate in the Y direction, the exposure range and accuracy of the exposure process in the X direction become worse. Therefore, when the length Q of the second opening 11 in the B area in the X direction is much greater than the length P, the exposure accuracy of the profile of the second opening 11 with a larger width Q in the X direction is poor, and the morphology of the photolithography pattern corresponding to the second opening 11 is poor. Therefore, the accuracy of the pattern transferred to the layer to be etched is still poor, resulting in poor performance of the semiconductor product.

[0038] In order to solve the above problems, the present invention provides a semiconductor structure and a method for forming the same, by forming a first opening and a second opening of small size and good morphology on a sacrificial layer, and forming a first graphic layer as a mask layer for the layer to be etched through the first opening and the second opening, thereby improving the accuracy of the graphics transferred to the layer to be etched, thereby improving the performance of the semiconductor structure.

[0039] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0040] Figures 2 to 12It is a schematic cross-sectional structure diagram of a semiconductor structure forming process according to an embodiment of the present invention.

[0041] Please refer to Figure 2 , providing a layer to be etched 100 , wherein the layer to be etched 100 includes a first region I; and forming a first pattern material layer 110 on a surface of the layer to be etched 100 .

[0042] The first pattern material layer 100 is used to form a first pattern layer in the first region I.

[0043] The material of the layer 100 to be etched includes oxide or nitride.

[0044] In this embodiment, the material of the layer to be etched 100 is silicon oxide.

[0045] In this embodiment, the layer to be etched 100 further includes a second region II. In other embodiments, the layer to be etched does not include a second region.

[0046] The process of forming the first pattern material layer 110 includes: a deposition process or a spin coating process.

[0047] In this embodiment, the method of forming the first pattern material layer 110 includes a chemical vapor deposition process.

[0048] In this embodiment, the material of the first pattern material layer 110 includes amorphous silicon.

[0049] In this embodiment, a substrate 101 is further provided, and the layer to be etched 100 is located on the surface of the substrate.

[0050] The material of the substrate 101 includes a semiconductor material. In this embodiment, the material of the substrate 101 includes silicon. In other embodiments, the material of the first substrate includes silicon carbide, silicon germanium, a multi-element semiconductor material composed of III-V group elements, silicon on insulator (SOI) or germanium on insulator. Among them, the multi-element semiconductor material composed of III-V group elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP.

[0051] In this embodiment, the substrate 101 has a device layer (not shown). The device layer may include a device structure, such as a PMOS transistor or an NMOS transistor. The device layer may also include an interconnection structure electrically connected to the device structure, and an insulating layer surrounding the device structure and the interconnection structure.

[0052] Please refer to Figure 3 , a sacrificial layer 120 is formed on the surface of the first graphic material layer 110 .

[0053] In this embodiment, the sacrificial layer 120 includes a sacrificial barrier layer (not shown) formed on the surface of the first pattern material layer 110, and an anti-reflection layer (not shown) formed on the surface of the sacrificial barrier layer.

[0054] The method of forming the sacrificial barrier layer includes a deposition process or a spin coating process.

[0055] In this embodiment, the method of forming the sacrificial barrier layer includes a spin coating process.

[0056] In this embodiment, the material of the sacrificial barrier layer is spin-on carbon.

[0057] The process of forming the anti-reflection layer includes a deposition process or a spin coating process.

[0058] In this embodiment, the material of the anti-reflection layer is a dielectric material, and the material of the anti-reflection layer includes one or more combinations of silicon oxide, silicon nitride, hafnium oxide, tantalum oxide and aluminum oxide.

[0059] Please refer to Figure 4 , a first opening 131 is formed in the sacrificial layer 120 in the first region I, and the first opening 131 exposes a portion of the surface of the first pattern material layer 110 .

[0060] In this embodiment, the first opening 131 has a first projection on the surface of the to-be-etched layer 100 , and along the first direction X, a width A of the first projection ranges from 30 nanometers to 50 nanometers.

[0061] If the width A is too small, it will not be possible to form a first graphic layer with a large size after cooperating with the second opening; if the width A is too large, the accuracy of the photoresist layer pattern obtained after exposing the photoresist material layer used to form the first opening 131 will be poor, thereby failing to form the first opening 131 with good accuracy and good morphology; therefore, the width A is within a suitable range and can be used to form a first graphic layer with a large size after cooperating with the second opening, and at the same time, form a first opening 131 with good accuracy and good morphology.

[0062] The method for forming the first opening 131 includes: forming a second graphic layer (not shown) on the surface of the sacrificial layer 120, that is, the surface of the anti-reflection layer, wherein the second graphic layer exposes a portion of the surface of the sacrificial layer 120 in the first area I; and etching the sacrificial layer 120 using the second graphic layer as a mask until the surface of the first graphic material layer 110 is exposed.

[0063] In this embodiment, the material of the second pattern layer is photoresist.

[0064] The method for forming the second graphic layer includes: forming a first photoresist material layer (not shown) on the surface of the sacrificial layer 120, exposing and developing the first photoresist material layer, thereby removing part of the first photoresist material layer on the surface of the sacrificial layer 120 in the first area I to form the second graphic layer.

[0065] The process of etching the sacrificial layer 120 includes a dry etching process or a wet etching process.

[0066] In this embodiment, the process of etching the sacrificial layer 120 includes a dry etching process.

[0067] In this embodiment, after the first opening 131 is formed, the second pattern layer is removed.

[0068] The process of removing the second pattern layer includes an ashing process.

[0069] Please refer to Figure 5 After forming the first opening 131 , a first doping region M is formed in the first pattern material layer 110 using the sacrificial layer 120 as a mask.

[0070] The process of forming the first doping region M includes a first ion implantation process.

[0071] The parameters of the first ion implantation process include: the doped ions include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions. Thus, the ions doped in the first doping region M include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions.

[0072] In this embodiment, the ions doped into the first doping region M are boron ions.

[0073] In this embodiment, the size of the first doping region M required by the design is formed by adjusting the process parameters of the first ion implantation process and the size of the first opening 131 .

[0074] Please refer to Figure 6 After forming the first doping region M, a first barrier layer 140 is formed in the first opening 131 .

[0075] The first barrier layer 140 is used to protect the morphology of the first doping region M, thereby reducing the influence of the first doping region M on the subsequent process of forming the second opening and the second doping region.

[0076] The process of forming the first barrier layer 140 includes a deposition process and a spin coating process.

[0077] In this embodiment, the process of forming the first barrier layer 140 includes a spin coating process.

[0078] The material of the first barrier layer 140 includes spin-on carbon.

[0079] Please refer to Figure 7 After forming the first doping region M, a second opening 132 is formed in the sacrificial layer 120 of the first region I, and the second opening 132 exposes a portion of the surface of the first pattern material layer 110 .

[0080] In this embodiment, the second opening 132 has a second projection on the surface of the to-be-etched layer 100 , and along the first direction X, a width B of the second projection ranges from 30 nanometers to 50 nanometers.

[0081] If the width B is too small, it cannot form a large-sized first graphic layer after cooperating with the first opening 131; if the width B is too large, after exposing the photoresist material layer used to form the second opening 132, the accuracy of the photoresist layer pattern obtained is poor, thereby failing to form the second opening 132 with good accuracy and good morphology; therefore, the width B is within a suitable range, and can form a large-sized first graphic layer after cooperating with the first opening 131, and at the same time, form a second opening 132 with good accuracy and good morphology.

[0082] In this embodiment, the first projection and the second projection are arranged at intervals along the first direction X, and the interval between the first projection and the second projection is less than 20 nanometers.

[0083] Since the first projection and the second projection are arranged at intervals along the first direction X, and the distance between the first projection and the second projection is less than 20 nanometers, the distance between the first opening 131 and the second opening 132 is small, so that when the first doping region M and the second doping region N are formed, the diffusion of doping ions can connect the first doping region M and the second doping region N.

[0084] In this embodiment, the method for forming the second opening 132 includes: after forming the first barrier layer 140, forming a third graphic layer (not shown) on the surface of the first barrier layer 140 and the sacrificial layer 120, the third graphic layer exposing a portion of the surface of the sacrificial layer 120 in the first region I; using the third graphic layer as a mask, etching the sacrificial layer 120 until the surface of the first graphic material layer 110 is exposed.

[0085] In this embodiment, the material of the third pattern layer is photoresist.

[0086] The method for forming the third graphic layer includes: forming a second photoresist material layer (not shown) on the surface of the sacrificial layer 120, exposing and developing the second photoresist material layer, thereby removing part of the second photoresist material layer on the surface of the sacrificial layer 120 in the first area I, and forming the third graphic layer.

[0087] The process of etching the sacrificial layer 120 includes a dry etching process or a wet etching process.

[0088] In this embodiment, the process of etching the sacrificial layer 120 includes a dry etching process.

[0089] In this embodiment, after the second opening 132 is formed, the third pattern layer is removed.

[0090] The process of removing the second pattern layer includes an ashing process.

[0091] In another embodiment, the first projection and the second projection are arranged along a first direction, the first projection and the second projection partially overlap, and, in the first direction, a spacing between edges of the overlapping portions of the first projection and the second projection is less than 20 nanometers.

[0092] Since the first projection and the second projection are arranged along the first direction X, the first projection and the second projection partially overlap, and, in the first direction X, the spacing between the edges of the overlapping portions of the first projection and the second projection is less than 20 nanometers, therefore, on the one hand, a first graphic layer having a graphic size larger than the first opening or the second opening can be formed subsequently, and on the other hand, the maximum size of the first graphic layer is controlled, so that a first graphic layer with a suitable graphic size can be formed.

[0093] In another embodiment, the method for forming the second opening includes: after forming the first barrier layer, forming a third graphic layer on the surface of the first barrier layer and the sacrificial layer, the third graphic layer exposing a portion of the sacrificial layer surface of the first area and a portion of the first barrier layer surface, and the exposed sacrificial layer surface is connected to the surface of the first barrier layer; using the third graphic layer as a mask, etching the sacrificial layer until the surface of the first graphic material layer is exposed.

[0094] Please refer to Figure 8 After forming the second opening 132 , a second doping region N is formed in the first pattern material layer 110 by using the sacrificial layer 120 as a mask, and the second doping region N is connected to the first doping region M.

[0095] Since the first opening 131 and the second opening 132 are formed, and the first doping region M and the second doping region N connected to each other are formed through the first opening 131 and the second opening 132, therefore, in the first direction X where the first doping region M is connected to the second doping region N, through the small-sized first opening 131 and the second opening 132, a mask with a large size in the first direction X can be subsequently formed, that is, a first graphic layer including the first doping region M and the second doping region N, thereby realizing the transfer of the graphic with a large size in the first direction X to the layer 100 to be etched.

[0096] Moreover, since the first opening 131 and the second opening 132 are relatively small in size in the first direction X, when the photoresist layer is exposed through the exposure step to form the pattern layer of the first opening 131 and the second opening 132, a pattern layer pattern with high precision can be obtained. Therefore, the pattern of the first opening 131 and the second opening 132 formed is of high precision and good morphology, so that the pattern of the first doping region M and the second doping region N formed by the first opening 131 and the second opening 132 is of high precision and good morphology, that is, the pattern of the first pattern layer including the first doping region M and the second doping region N formed subsequently is of high precision and good morphology, thereby improving the pattern precision transferred to the layer to be etched 100 and improving the performance of the semiconductor structure.

[0097] It should be noted that the first doping region M and the second doping region N are connected, which means that the boundary between the first doping region M and the second doping region N is just in contact, or the first doping region M and the second doping region N partially overlap.

[0098] The process of forming the second doping region N includes a second ion implantation process.

[0099] The parameters of the second ion implantation process include: the doped ions include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions. Thus, the ions doped in the second doping region N include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions.

[0100] The type of ions doped in the second doping region N is the same as the type of ions doped in the first doping region M.

[0101] In this embodiment, the size of the second doping region N required by the design is formed by adjusting the process parameters of the second ion implantation process and the size of the second opening 132 .

[0102] Please refer to Fig. 9After forming the second doping region N, the sacrificial layer 120 is removed; after removing the sacrificial layer 120, a first graphic layer 111 is formed, the first graphic layer 111 includes the first doping region M and the second doping region N, and the first graphic layer 111 is located on the surface of the layer to be etched 100 in the first region I.

[0103] In another embodiment, the first graphic layer further includes a third doping region, and the method for forming the third doping region is the same as the method for forming the second doping region, which is not repeated here. Due to the formation of the third doping region, a first graphic layer with a larger size in the first direction X is formed.

[0104] In other embodiments, the first graphic layer further includes a plurality of fourth doping regions, the number of which is adjusted according to the size of the first graphic layer to be formed, that is, the size of the graphic to be subsequently transferred to the layer to be etched, and the method for forming the fourth doping region is the same as the method for forming the second doping region, which will not be described in detail herein. Since a plurality of fourth doping regions are formed, a first graphic layer having a larger size in the first direction X can be formed.

[0105] The process of removing the sacrificial layer 120 includes an etching process or a planarization process.

[0106] In this embodiment, after removing the sacrificial layer 120, the surface of the first pattern material layer 110 is cleaned before forming the first pattern layer 111. Therefore, the residue on the surface of the first pattern material layer 110 can be removed, so as to avoid the residue from contaminating the surface of the layer to be etched after the subsequent etching of the layer to be etched 100, thereby reducing the residue contamination problem of the semiconductor device and improving the performance of the semiconductor device.

[0107] In this embodiment, the solution used to clean the surface of the first pattern material layer 110 includes sulfuric acid.

[0108] The method for forming the first pattern layer 111 includes: after removing the sacrificial layer 120 , etching the first pattern material layer 110 .

[0109] The process of etching the first pattern material layer 110 includes a wet etching process. Since the first doping region M and the second doping region N are doped with ions, the etching rate of the first pattern material layer 110 by the wet etching process is greater than the etching rate of the first doping region M and the second doping region N. Thus, while retaining the first doping region M and the second doping region N, the remaining part of the first pattern material layer 111 can be removed to form the first pattern layer 111.

[0110] In this embodiment, the etching solution of the wet etching process includes ammonia water.

[0111] Please refer to Fig.10 , using the first pattern layer 111 as a mask, etching the to-be-etched layer 100 in the first region I. Thus, an etching pattern layer 102 is formed in the first region I.

[0112] In this embodiment, the etched pattern layer 102 has a width K in the first direction X, and the width K is greater than 50 nanometers.

[0113] The process of etching the to-be-etched layer 100 in the first region I includes a dry etching process or a wet etching process.

[0114] In this embodiment, before etching the layer 100 to be etched in the first region I, a first barrier layer 150 is formed on the surface of the layer 100 to be etched in the second region II. Thus, the etching process of etching the layer 100 to be etched in the first region I is prevented from affecting the layer 100 to be etched in the second region II.

[0115] In this embodiment, after the etching pattern layer 102 is formed, the first pattern layer 111 is removed.

[0116] Please refer to Fig.11 and Fig.12 , Fig.12 yes Fig.11 , after forming the etching pattern layer 102, a fourth pattern layer (not shown) is formed on the surface of the layer to be etched 100 in the second region II, and the layer to be etched 100 in the second region II is etched using the fourth pattern layer as a mask. Thus, an etching pattern layer 103 is formed in the second region II.

[0117] The process of etching the to-be-etched layer 100 in the second region II includes a wet etching process or a dry etching process.

[0118] In this embodiment, the material of the fourth pattern layer is photoresist.

[0119] In this embodiment, after the etching pattern layer 103 is formed, the fourth pattern layer is removed.

[0120] The process of removing the fourth pattern layer includes an ashing process.

[0121] In this embodiment, the fourth pattern layer is formed after the first pattern layer 111 is removed, and after the first pattern layer 111 is removed and before the fourth pattern layer is formed, a second barrier layer (not shown) is formed on the exposed surface of the substrate 101 in the first region I and the surface of the etching pattern layer 102. Thus, the subsequent process of forming the etching layer pattern 103 is prevented from affecting the exposed surface of the substrate 101 in the first region I and the etching layer pattern 102.

[0122] In this embodiment, the method for forming the fourth graphic layer includes: after forming the second barrier layer, removing the first barrier layer 150 on the surface of the layer to be etched 100 in the second region II; after removing the first barrier layer 150, forming a fourth graphic material layer on the surface of the layer to be etched 100 in the second region II; exposing and developing the fourth graphic material layer to form the fourth graphic layer.

[0123] In this embodiment, after the etching pattern layer 103 is formed, the second barrier layer is removed.

[0124] In this embodiment, in the second direction Y perpendicular to the first direction X, the projection of the fourth pattern layer on the surface of the to-be-etched layer 100 has a first length T, and the first length T is greater than 50 nanometers. Thus, the etched pattern layer 103 also has the first length T greater than 50 nanometers in the second direction Y.

[0125] In this embodiment, the etched pattern layer 103 has a width S in the first direction X, and the first length T and the width K are both much larger than the width S.

[0126] In this embodiment, the etched pattern layer 102 has a second length W in the second direction Y, and the width K is much greater than the second length W.

[0127] Therefore, the etched pattern layer 102 and the etched pattern layer 103 are of different types. The etched pattern layer 102 has a large size in the first direction X and a small size in the second direction Y, while the etched pattern layer 103 has a small size in the first direction X and a large size in the second direction Y.

[0128] Therefore, through the above-mentioned formation method, an etching graphic layer 102 and an etching graphic layer 103 with high graphic accuracy and good morphology can be formed simultaneously, that is, while adjusting the exposure process for the etching graphic 103 (the accuracy is better and the exposure range is larger in the second direction Y, but the accuracy is poorer and the range is smaller in the first direction X), the etching graphic layer 102 with a larger size in the first direction X can be taken into account.

[0129] Correspondingly, an embodiment of the present invention further provides a semiconductor structure, comprising: a layer to be etched 100, the layer to be etched 100 comprising a first region I; a first graphic material layer 110 located on the surface of the layer to be etched 100; a sacrificial layer 120 located on the surface of the first graphic material layer 110; a first opening 131 located in the sacrificial layer 120 in the first region I, the first opening 131 exposing a portion of the surface of the first graphic material layer 110 in the first region I; a first doped region M located in the first graphic material layer 110; a second opening 132 located in the sacrificial layer in the first region I, the second opening 132 exposing a portion of the surface of the first graphic material layer 110 in the first region I; a second doped region N located in the first graphic material layer 110, the second doped region N being connected to the first doped region M.

[0130] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that: include: Providing a layer to be etched, wherein the layer to be etched includes a first region; Forming a first pattern material layer on the surface of the layer to be etched; forming a sacrificial layer on the surface of the first graphic material layer; forming a first opening in the sacrificial layer in the first region, wherein the first opening exposes a portion of the surface of the first pattern material layer in the first region; After forming the first opening, using the sacrificial layer as a mask, forming a first doped region in the first pattern material layer; After forming the first doped region, forming a second opening in the sacrificial layer of the first region, wherein the second opening exposes a portion of the surface of the first pattern material layer of the first region; After forming the second opening, using the sacrificial layer as a mask, forming a second doped region in the first pattern material layer, wherein the second doped region is connected to the first doped region; forming a first graphic layer, wherein the first graphic layer includes the first doped region and the second doped region, and the first graphic layer is located on a surface of the layer to be etched in the first region; The first graphic layer is used as a mask to etch the layer to be etched in the first area.

2. The method for forming a semiconductor structure according to claim 1, wherein: Also includes: After forming the second doped region, removing the sacrificial layer; After removing the sacrificial layer, a first pattern layer is formed.

3. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the first opening includes: forming a second graphic layer on the surface of the sacrificial layer, the second graphic layer exposing a portion of the surface of the sacrificial layer in the first area; etching the sacrificial layer using the second graphic layer as a mask until the surface of the first graphic material layer is exposed.

4. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the second opening includes: after forming the first doped region, forming a first barrier layer in the first opening; after forming the first barrier layer, forming a third graphic layer on the surface of the first barrier layer and the sacrificial layer, the third graphic layer exposing a portion of the sacrificial layer surface of the first region; using the third graphic layer as a mask, etching the sacrificial layer until the surface of the first graphic material layer is exposed.

5. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the second opening includes: after forming the first doped region, forming a first barrier layer in the first opening; after forming the first barrier layer, forming a third graphic layer on the surface of the first barrier layer and the sacrificial layer, wherein the third graphic layer exposes a portion of the sacrificial layer surface of the first region and a portion of the first barrier layer surface, and the exposed sacrificial layer surface is connected to the surface of the first barrier layer; using the third graphic layer as a mask, etching the sacrificial layer until the surface of the first graphic material layer is exposed.

6. The method for forming a semiconductor structure according to claim 2, wherein: After removing the sacrificial layer and before forming the first graphic layer, the surface of the first graphic material layer is cleaned.

7. The method for forming a semiconductor structure according to claim 2, wherein: The method for forming the first pattern layer includes: after removing the sacrificial layer, etching the first pattern material layer.

8. The method for forming a semiconductor structure according to claim 7, wherein: The process of etching the first pattern material layer includes a wet etching process, and the etching rate of the first pattern material layer by the wet etching process is greater than the etching rate of the first doping region and the second doping region.

9. The method for forming a semiconductor structure according to claim 1, wherein: The process of forming the first doping region includes a first ion implantation process.

10. The method for forming a semiconductor structure according to claim 1, wherein: The process of forming the second doping region includes a second ion implantation process.

11. The method for forming a semiconductor structure according to claim 1, wherein: The type of ions doped in the first doping region is the same as the type of ions doped in the second doping region.

12. The method for forming a semiconductor structure according to claim 1, wherein: The first opening has a first projection on the surface of the layer to be etched, and the second opening has a second projection on the surface of the layer to be etched. The first projection and the second projection are arranged at intervals along a first direction, and the distance between the first projection and the second projection is less than 20 nanometers.

13. The method for forming a semiconductor structure according to claim 1, wherein: The first opening has a first projection on the surface of the layer to be etched, and the second opening has a second projection on the surface of the layer to be etched, the first projection and the second projection are arranged along a first direction, the first projection and the second projection partially overlap, and, in the first direction, a spacing between edges of the overlapping portions of the first projection and the second projection is less than 20 nanometers.

14. The method for forming a semiconductor structure according to claim 12, wherein: Along the first direction, a width of the first projection ranges from 30 nanometers to 50 nanometers, and a width of the second projection ranges from 30 nanometers to 50 nanometers.

15. The method for forming a semiconductor structure according to claim 12, wherein: The layer to be etched also includes a second area; the method for forming the semiconductor structure also includes: forming a fourth graphic layer on the surface of the layer to be etched in the second area, wherein a projection of the fourth graphic layer on the surface of the layer to be etched in a second direction perpendicular to the first direction has a first length, and the first length is greater than 50 nanometers; using the fourth graphic layer as a mask, etching the layer to be etched in the second area.

16. The method for forming a semiconductor structure according to claim 1, wherein: The sacrificial layer includes a sacrificial barrier layer located on the surface of the first pattern material layer, and an anti-reflection layer located on the surface of the sacrificial barrier layer.

17. The method for forming a semiconductor structure according to claim 1, wherein: The material of the first patterned material layer includes amorphous silicon.

18. The method for forming a semiconductor structure according to claim 1, wherein: The ions doped in the first doping region include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions; the ions doped in the second doping region include boron ions, boron fluoride ions, indium ions, phosphorus ions, arsenic ions or antimony ions.

19. The method for forming a semiconductor structure according to claim 1, wherein: The first patterned layer also includes a third doping region.

20. A semiconductor structure, characterized in that: include: A layer to be etched, the layer to be etched comprising a first area; a first graphic material layer located on the surface of the layer to be etched, the first graphic material layer comprising: a first graphic layer, the first graphic layer being suitable for being used as a mask in the process of etching the layer to be etched in the first area, the first graphic layer comprising: a first doping area, the first doping area being located on the surface of the layer to be etched in the first area; a second doping area, the second doping area being located on the surface of the layer to be etched in the first area, and the second doping area being connected to the first doping area; a sacrificial layer located on the surface of the first graphic material layer, the sacrificial layer comprising: a first opening, the position of the first opening corresponding to the position of the first doping area and exposing a portion of the first doping area; a second opening, the position of the second opening corresponding to the position of the second doping area and exposing a portion of the second doping area.