A production method for sharp hole drill

By surface treatment and magnetic adsorption of diamond, combined with the brazing process, the diamond edges and corners are arranged outward, which solves the problem of low usage rate of diamond abrasives in the existing technology and improves the strength and service life of the hole drill.

CN113137183BActive Publication Date: 2024-10-18JIANGSU FUNLIN SUPER HARD TOOLS
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202110503370.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-05-10
Publication Date
2024-10-18
Estimated Expiration
2041-05-10

AI Technical Summary

Technical Problem

In the existing technology, the diamond abrasives of single-layer brazing hole drills are uneven and cannot be arranged in an orderly manner with edges and corners facing outward, resulting in insufficient abrasive usage and affecting the service life of the hole drill.

Method used

By cleaning, sensitizing, activating and electroless plating the diamond surface, a diamond magnet is formed, and magnetically adsorbed and brazed on the drill base to ensure that the diamond edges and corners are arranged outward, thereby improving the strength and strength of the drill. service life.

Benefits of technology

Through the magnetic adsorption and brazing process of diamond magnets, the orderly arrangement of diamond edges and corners is achieved, which improves the strength and service life of sharp hole drills and solves the problem of low abrasive usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113137183B_ABST
    Figure CN113137183B_ABST
Patent Text Reader

Abstract

The invention discloses a production method of a sharp hole drill, comprising the following steps: a first step: diamond surface treatment; a second step: diamond magnet loading; firstly, glue is coated on the outer wall of the bottom of the hole drill base, a powdered diamond magnet is loaded into an open can and is located below the hole drill base, a magnet is placed on the top of the hole drill base, so that the hole drill base generates magnetism; then, the bottom of the hole drill base is placed above the diamond magnet, so that the diamond magnet is adsorbed on the outer wall of the hole drill base, and the magnet on the hole drill base is removed; a third step: brazing: thus a sharp hole drill is obtained; the invention greatly improves the strength and service life of the sharp hole drill when drilling a hole; solves the problem in the prior art that the diamond abrasive of a single-layer brazed hole drill is uneven, the edges and corners cannot be arranged outward in an orderly manner, resulting in an insufficient abrasive utilization rate, which affects the service life of the hole drill.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hole drilling, and in particular relates to a production method of a sharp hole drill. Background Art

[0002] The main function of the drill bit is to break rocks, form wellbores and drill holes in hard objects.

[0003] In the prior art, the diamond abrasives of the single-layer brazed hole drill are uneven, and the edges and corners cannot be arranged in an orderly manner outward, resulting in an insufficient abrasive utilization rate, which affects the service life of the hole drill. Summary of the invention

[0004] The purpose of the present invention is to solve the problem in the prior art that the diamond abrasives of a single-layer brazed hole drill are uneven and the edges cannot be arranged in an orderly manner facing outward, resulting in insufficient abrasive utilization rate and affecting the service life of the hole drill, and to propose a production method for a sharp hole drill.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for producing a sharp hole drill comprises the following steps:

[0007] Step 1: Diamond surface treatment; Diamond cleaning; Sensitization treatment; Activation treatment; Chemical plating: Add the activated diamond particles into the chemical plating solution, stir at a temperature of 50-70°C for 2 hours, take out and dry at 100°C for 2 hours; obtain a diamond magnet;

[0008] Step 2: Loading the diamond magnet; firstly, apply glue on the outer wall of the bottom of the drill base, put the powdered diamond magnet into the open tank and place it under the drill base, and place the magnet on the top of the drill base to make the drill base magnetic; then, place the bottom of the drill base on the diamond magnet so that the diamond magnet is adsorbed on the outer wall of the drill base, and remove the magnet on the drill base;

[0009] Step 3: Brazing: Add solder to the drill base and distribute it in the gaps between the diamond magnets. Then move it to a vacuum brazing furnace for brazing to obtain a sharp drill.

[0010] Preferably, the diamond is cleaned by adding the diamond particles into a nitric acid solution with a mass fraction of 1% and boiling for 10 minutes.

[0011] Preferably, the sensitization treatment is to add the cleaned diamond particles into a mixed solution of 10-20 g / L stannous chloride by mass and 10-40 mL / L hydrochloric acid by volume, and stir at room temperature for 1-5 min.

[0012] Preferably, the activation treatment is to add the sensitized diamond particles into a mixed solution of palladium chloride with a mass fraction of 0.25 g / L and hydrochloric acid with a volume fraction of 2-5 mL / L, and stir at room temperature for 1-3 min.

[0013] Preferably, 1L of chemical plating solution is composed of the following raw materials: nickel sulfate hexahydrate with a mass fraction of 25-35g / L, sodium hypophosphite with a mass fraction of 30-40g / L, cobalt sulfate with a mass fraction of 15-20g / L, acetic acid with a mass fraction of 5-10g, lactic acid with a mass fraction of 0.01-0.05g / L saccharin, and 0.01-0.05g sodium dodecyl sulfate.

[0014] Preferably, the glue is acrylic glue.

[0015] Preferably, the particle size of the powdered diamond magnetic inductor is 40 mesh, and the particle size of the solder is 50 mesh.

[0016] Preferably, the solder is composed of the following: nickel powder with a mass fraction of 5-10%, nickel powder with a mass fraction of 3.5-10%, and the balance is chromium powder.

[0017] Preferably, the brazing temperature is 1050-1080° C. and the brazing time is 30 min.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: the sharp-type hole drill prepared by the present invention through the process of diamond surface treatment, diamond magnet loading and brazing makes the edges and corners of the diamond face outward, that is, the side wall with a large area of ​​the diamond magnet is adsorbed on the hole drill base, and the tip part will point to the direction away from the side wall of the hole drill base, thereby greatly improving the strength and service life of the sharp-type hole drill during drilling; and solves the problem in the prior art that the diamond abrasive of the single-layer brazed hole drill is uneven and the edges and corners cannot be arranged in an orderly manner outward, resulting in insufficient abrasive utilization rate and affecting the service life of the hole drill. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings.

[0020] Figure 1 It is a schematic diagram of the structure of the sharp hole drill in the present invention.

[0021] Figure 2 It is a structural schematic diagram of the feeding mechanism in the present invention.

[0022] Figure 3 It is a three-dimensional structural schematic diagram of the connection relationship between the base plate and the slide plate in the present invention.

[0023] In the figure: 1. diamond drill body; 2. drilling base; 3. abrasive block; 4. mounting hole; 5. bolt hole; 6. chip removal hole; 12. base plate; 13. motor; 14. driving pulley; 15. driven pulley; 16. top plate; 17. screw rod; 18. first sleeve; 19. second sleeve; 20. mounting plate; 21. limit rod; 22. connecting rod; 23. magnet plate; 24. slide groove; 25. slide shaft; 26. clamping plate; 27. slide plate. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] A method for producing a sharp hole drill comprises the following steps:

[0027] Step 1: Diamond surface treatment: Clean the diamond, add the diamond particles to a nitric acid solution with a mass fraction of 10 minutes and cook for 10 minutes; Sensitization treatment: Add the cleaned diamond particles to a mixed solution of 10-g / L stannous chloride and 10-mL / L hydrochloric acid by volume, and stir for 1-5 minutes at room temperature for sensitization treatment; Activation treatment: Add the sensitized diamond particles to a mixed solution of 0.25g / L palladium chloride and 2mL / L hydrochloric acid by volume, and stir for 1 minute at room temperature for activation treatment; Chemical plating: Add the activated diamond particles to the chemical plating solution, stir for 2 hours at a temperature of 50°C, take out and dry for 2 hours at 100°C; Get a diamond magnetite;

[0028] 1L of chemical plating solution is composed of the following raw materials: 25g / L nickel sulfate hexahydrate, 30g / L sodium hypophosphite, 15g / L cobalt sulfate, 5g acetic acid, 50g lactic acid, 0.01g / L saccharin, and 0.01g sodium dodecyl sulfate. Adding saccharin can make the coating surface smooth, and adding sodium dodecyl sulfate has the advantages of good dispersibility and uniform coating.

[0029] Step 2: Loading the diamond magnet; firstly, apply glue on the outer wall of the bottom of the drill base, put the powdered diamond magnet into the open tank and place it under the drill base, and place the magnet on the top of the drill base to make the drill base magnetic; then, place the bottom of the drill base on the diamond magnet so that the diamond magnet is adsorbed on the outer wall of the drill base, and remove the magnet on the drill base;

[0030] During the adsorption process, the diamond magnet is adsorbed on the outer wall of the bottom surface of the drill base. Under the influence of magnetic attraction and the shape of the diamond magnet itself, the side wall with a large area of ​​the diamond magnet is adsorbed on the drill base, and the tip part will point in the direction away from the side wall of the drill base. After the adsorption is completed, the drill base is demagnetized, so that the diamond magnet that is not in the glue layer will automatically fall off.

[0031] Step 3: Brazing: Add solder to the drill base and distribute it in the gaps of the diamond magnet, then move it to a vacuum brazing furnace for brazing to obtain a sharp drill; the particle size of the powdered diamond magnet is 40 mesh, the particle size of the solder is 50 mesh, and the solder is composed of the following nickel powder with a mass fraction of 5%, nickel powder with a mass fraction of 3.5%, and the balance is chromium powder; the brazing temperature is 1050℃, and the brazing time is 30 minutes.

[0032] Example 2

[0033] A method for producing a sharp hole drill comprises the following steps:

[0034] Step 1: Diamond surface treatment: Diamond cleaning, adding diamond particles to a nitric acid solution with a mass fraction of 1% and boiling for 10 minutes; Sensitization treatment: adding the cleaned diamond particles to a mixed solution of 15g / L stannous chloride and 25mL / L hydrochloric acid by volume, and stirring for 3min at room temperature for sensitization treatment; Activation treatment: adding the sensitized diamond particles to a mixed solution of 0.25g / L palladium chloride and 3mL / L hydrochloric acid by volume, and stirring for 2min at room temperature for activation treatment; Chemical plating: adding the activated diamond particles to the chemical plating solution, stirring for 2h at a temperature of 60°C, taking out and drying for 2h at 100°C; obtaining a diamond magnetite;

[0035] 1L of chemical plating solution is composed of the following raw materials: 30g / L nickel sulfate hexahydrate, 35g / L sodium hypophosphite, 18g / L cobalt sulfate, 8g acetic acid, 80g lactic acid, 0.03g / L saccharin, and 0.03g sodium dodecyl sulfate;

[0036] Step 2: Loading the diamond magnet; firstly, apply glue on the outer wall of the bottom of the drill base, put the powdered diamond magnet into the open tank and place it under the drill base, and place the magnet on the top of the drill base to make the drill base magnetic; then, place the bottom of the drill base on the diamond magnet so that the diamond magnet is adsorbed on the outer wall of the drill base, and remove the magnet on the drill base;

[0037] During the adsorption process, the diamond magnet is adsorbed on the outer wall of the bottom surface of the drill base. Under the influence of magnetic attraction and the shape of the diamond magnet itself, the side wall with a large area of ​​the diamond magnet is adsorbed on the drill base, and the tip part will point in the direction away from the side wall of the drill base. After the adsorption is completed, the drill base is demagnetized, so that the diamond magnet that is not in the glue layer will automatically fall off.

[0038] Step 3: Brazing: Add solder to the drill base and distribute it in the gaps of the diamond magnet, then move it to a vacuum brazing furnace for brazing to obtain a sharp drill; the particle size of the powdered diamond magnet is 40 mesh, the particle size of the solder is 50 mesh, and the solder is composed of the following nickel powder with a mass fraction of 7%, nickel powder with a mass fraction of 6%, and the balance is chromium powder; the brazing temperature is 1065℃, and the brazing time is 30 minutes.

[0039] Example 3

[0040] A method for producing a sharp hole drill comprises the following steps:

[0041] Step 1: Diamond surface treatment: Diamond cleaning, adding diamond particles to a nitric acid solution with a mass fraction of 1% and boiling for 10 minutes; Sensitization treatment: adding the cleaned diamond particles to a mixed solution of 20g / L stannous chloride and 40mL / L hydrochloric acid by volume, and stirring for 5min at room temperature for sensitization treatment; Activation treatment: adding the sensitized diamond particles to a mixed solution of 0.25g / L palladium chloride and 5mL / L hydrochloric acid by volume, and stirring for 3min at room temperature for activation treatment; Chemical plating: adding the activated diamond particles to the chemical plating solution, stirring for 2h at a temperature of 70°C, taking out and drying for 2h at 100°C; obtaining a diamond magnetite;

[0042] 1L of chemical plating solution is composed of the following raw materials: 35g / L nickel sulfate hexahydrate, 40g / L sodium hypophosphite, 20g / L cobalt sulfate, 10g acetic acid, 10g lactic acid, 0.05g / L saccharin, and 0.05g sodium dodecyl sulfate.

[0043] Step 2: Loading the diamond magnet; firstly, apply glue on the outer wall of the bottom of the drill base, put the powdered diamond magnet into the open tank and place it under the drill base, and place the magnet on the top of the drill base to make the drill base magnetic; then, place the bottom of the drill base on the diamond magnet so that the diamond magnet is adsorbed on the outer wall of the drill base, and remove the magnet on the drill base;

[0044] During the adsorption process, the diamond magnet is adsorbed on the outer wall of the bottom surface of the drill base. Under the influence of magnetic attraction and the shape of the diamond magnet itself, the side wall with a large area of ​​the diamond magnet is adsorbed on the drill base, and the tip part will point in the direction away from the side wall of the drill base. After the adsorption is completed, the drill base is demagnetized, so that the diamond magnet that is not in the glue layer will automatically fall off.

[0045] Step 3: Brazing: Add solder to the drill base and distribute it in the gaps of the diamond magnet, then move it to a vacuum brazing furnace for brazing to obtain a sharp drill; the particle size of the powdered diamond magnet is 40 mesh, the particle size of the solder is 50 mesh, and the solder is composed of the following nickel powder with a mass fraction of 10%, nickel powder with a mass fraction of 10%, and the balance is chromium powder; the brazing temperature is 1080℃, and the brazing time is 30 minutes.

[0046] Example 4

[0047] See also Figure 2-3 As shown, the second step is performed by a feeding mechanism, which includes a base plate 12, a motor 13, a driving pulley 14, a driven pulley 15, a top plate 16, a screw 17, a first sleeve 18, a second sleeve 19, a mounting plate 20, a limit rod 21, an elastic rod 22, a magnet plate 23, a slide groove 24, a slide shaft 25, a clamping plate 26, and a slide plate 27; a motor 13 is installed on one side of the base plate 12, and the output end of the motor 13 is connected to the driving pulley 14, and the driving pulley 14 is connected to the driven pulley 15 through a belt. The driven pulley 15 is sleeved on the screw 17, and the screw 17 is rotatably installed between the base plate 12 and the top plate 16, and the top plate 16 is installed above the base plate 12. The upper and lower sides of the screw rod 17 are provided with opposite threads, and are respectively sleeved with a first sleeve 18 and a second sleeve 19, the second sleeve is connected to a slide plate 27, the slide plate 27 is slidably mounted on the front of the base plate 12, and moves up and down along the base plate 12, a plurality of groups of slide grooves 24 are symmetrically arranged on the slide plate 27, the slide grooves 24 are inclinedly arranged, the slide shaft 25 is located in the slide grooves 24, and moves along the slide grooves 24, the slide shaft 25 is installed on the clamping plate 26, the clamping plate 26 is a U-shaped structure, the vertical portion on one side of the clamping plate 26 is installed on the front of the base plate 12, and moves horizontally along the base plate 12, the vertical portion on the other side of the clamping plate 26 is located directly in front of the slide plate 27; the vertical portion on the other side of the clamping plate 26 is used to clamp and fix the hole drill;

[0048] The first sleeve 18 is connected to a mounting plate 20, and limit rods 21 are slidably arranged on both sides of the mounting plate 20. The limit rods 21 are installed between the base plate 12 and the top plate 16. The limit rods 21 play a role in limiting the upward and downward movement of the mounting plate 20. The bottom surface of the mounting plate 20 is connected to a magnet plate 23 through an elastic rod 22; the magnet plate 23 is used to magnetize the hole.

[0049] When the abrasive block is loaded in the second step, multiple groups of hole drills are first placed in the gaps between multiple groups of clamping plates 26, and then the motor 13 is started to work, and the screw rod 17 is driven to rotate through the active pulley 14 and the driven pulley 15. Since the threads on the upper and lower sides of the screw rod 17 are opposite, the slide plate 27 moves upward, so that the clamping plates 26 are driven to move closer to each other along the slide groove 24 through the sliding shaft 25, thereby clamping and fixing the hole drill. At the same time, the screw rod 17 will cause the mounting plate 20 to move downward, and the mounting plate 20 drives the magnet plate 23 to move downward through the elastic rod 22 and is located on the top of the hole drill, thereby magnetizing the hole drill; so the loading mechanism of the present invention can load multiple groups of hole drills at the same time, and at the same time, it also realizes the convenience of clamping multiple groups of hole drills. During the clamping and fixing, the hole drill will also be magnetized through the magnet plate 23, thereby greatly improving the working efficiency of the hole drill when loading the diamond hole drill.

[0050] Example 5

[0051] See also Figure 1 As shown, the diamond hole drill body 1 includes a drilling base 2, a diamond magnetic inductor 3, and a connector; a connector is provided at the top center of the drilling base 2;

[0052] A diamond magnet 3 is arranged on the outer wall of the bottom surface of the drilling base 2; the diamond magnet 3 is fixed on the outer wall of the drilling base 2 in a single layer, and the diamond magnet 3 can be evenly arranged on the outer wall of the sharp hole drill 1, so that the sharp hole drill 1 has good wear resistance.

[0053] A mounting hole 4 is provided on the top surface of the connector, and a bolt hole 5 is provided through the middle of the connector. The mounting hole 4 is located directly above the bolt hole 5. Through the mounting hole 4 and the bolt hole 5, the diamond drill body 1 can be conveniently installed at the output end of the drilling rig.

[0054] The side wall of the drilling base 2 is provided with a chip removal hole 6 , and by providing the chip removal hole 6 , waste chips generated by the diamond drill body 1 during drilling can be automatically discharged from the chip removal hole 6 .

[0055] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for producing a sharp hole drill, characterized in that: The following steps are involved: Step 1: Diamond surface treatment; Diamond cleaning; Sensitization treatment; Activation treatment; Chemical plating: Add the activated diamond particles into the chemical plating solution, stir at 50-70°C for 2h, take out and dry at 100°C for 2h to obtain a diamond magnetite; Step 2: Loading the diamond magnet; firstly, apply glue on the outer wall of the bottom of the drill base, put the powdered diamond magnet into the open tank and place it under the drill base, and place the magnet on the top of the drill base to make the drill base magnetic; then, place the bottom of the drill base on the diamond magnet so that the diamond magnet is adsorbed on the outer wall of the drill base, and remove the magnet on the drill base; Step 3: Brazing: Add solder to the drill base and distribute it in the gaps between the diamond magnets, then move it to a vacuum brazing furnace for brazing to obtain a sharp drill. The second step is to work through the feeding mechanism, which includes a base plate, a motor, a driving pulley, a driven pulley, a top plate, a screw, a first sleeve, a second sleeve, a mounting plate, a limit rod, an elastic rod, a magnet plate, a slide groove, a slide shaft, a clamping plate, and a slide plate; a motor is installed on one side of the base plate, the output end of the motor is connected to the driving pulley, the driving pulley is connected to the driven pulley through a belt, the driven pulley is sleeved on the screw, the screw is rotatably installed between the base plate and the top plate, the top plate is installed above the base plate, and the upper and lower sides of the screw are provided with The slide plate is provided with opposite threads, and is respectively provided with a first sleeve and a second sleeve, the second sleeve is connected to the slide plate, the slide plate is slidably mounted on the front side of the base plate, and moves up and down along the base plate, a plurality of sets of slide grooves are symmetrically arranged on the slide plate, the slide grooves are inclinedly arranged, the slide shaft is located in the slide grooves, and moves along the slide grooves, the slide shaft is installed on the clamping plate, the clamping plate is a U-shaped structure, the vertical part on one side of the clamping plate is installed on the front side of the base plate, and moves horizontally along the base plate, and the vertical part on the other side of the clamping plate is located directly in front of the slide plate; the vertical part on the other side of the clamping plate is used to clamp and fix the hole drill; The first sleeve is connected to a mounting plate, and limit rods are slidably arranged on both sides of the mounting plate. The limit rods are installed between the base plate and the top plate. The limit rods play a role in limiting the sliding of the mounting plate up and down. The bottom surface of the mounting plate is connected to a magnet plate through an elastic rod; the magnet plate is used to magnetize the holes.

Citation Information

Patent Citations

  • Preparation method for chemical plating of Ni-P plating on surface of diamond

    CN108823553A

  • Vacuum oil immersion device for capacitor production and working method thereof

    CN111029174A

  • Device and method for testing bonding strength of facing brick

    CN111912783A

  • Method for chemically plating nickel on surface of diamond

    CN112210771A

  • Asphalt concrete pavement construction process based on target mix proportion