Resin composition and optical filter element
By using a resin composition with components such as titanium black and carbon black in a liquid crystal display device, the problems of screen flicker and poor resolution of filter elements under low-frequency operation of the liquid crystal display device are solved, and the high resolution and optical resolution of the filter element are achieved. The penetration rate improves the operating efficiency of CMOS image sensing components.
Patent Information
- Application Number
- CN202010063949.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-04-12
AI Technical Summary
Existing liquid crystal display equipment will produce screen flickering under low-frequency operation, causing the traditional electronic shutter mode to produce false images, affecting the normal operation of CMOS image sensing elements. At the same time, the resolution and transmittance of the filter elements are poor. Titanium The problem of different precipitation speeds of black and carbon black.
A resin composition is used, including titanium black and carbon black as black colorants, ethylenically unsaturated monomers, solvents, resins and photoinitiators. By adjusting the proportion and particle size of each component, a product with good resolution and development can be formed. filter element for properties, adhesion, coating uniformity and light transmittance.
It has improved the high resolution, developability, adhesion and light transmittance of the filter element, improved the screen flicker problem of liquid crystal display equipment, and improved the operating efficiency of CMOS image sensing elements.
Smart Images

Figure BDA0002375385470000021 
Figure BDA0002375385470000022 
Figure BDA0002375385470000023
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, and in particular to a resin composition suitable for a filter element and the filter element. Background Art
[0002] With the rapid development of liquid crystal display device technology, in order to improve the energy saving effect of liquid crystal display devices, the driving frequency of liquid crystal display devices is usually reduced. However, the low-frequency operation of the currently used liquid crystal display devices will produce a flickering phenomenon, which may cause the traditional electronic shutter mode to produce a pseudo image, thereby causing the complementary metal oxide semiconductor (CMOS) image sensor element to not operate normally.
[0003] Filter elements are usually used in liquid crystal display devices to improve the problem of screen flicker. However, the currently used filter elements have problems such as poor resolution or poor transmittance. For example, the composition of the current filter element will cause the precipitation speed of titanium black and other black colorants to be different, thereby affecting the performance of the device using the filter element. Summary of the invention
[0004] In view of this, the present invention provides a resin composition and a filter element that can form a film having good resolution, developability, adhesion, coating uniformity and light transmittance.
[0005] A resin composition of the present invention comprises a black colorant (A), an ethylenically unsaturated monomer (B), a solvent (C), a resin (D) and a photoinitiator (E). The black colorant (A) comprises titanium black (A-1) and carbon black (A-2). Based on the total usage of titanium black (A-1) and carbon black (A-2) being 100 parts by weight, the usage of titanium black (A-1) is 50 parts by weight to 75 parts by weight.
[0006] In one embodiment of the present invention, the cured film obtained from the above resin composition has a thickness of 0.3 micrometers to 3.0 micrometers and a resolution of less than 2 micrometers.
[0007] In one embodiment of the present invention, the thickness of the hardened film obtained from the resin composition is between 0.3 micrometers and 3.0 micrometers, and the visible light transmittance is between 5% and 50%.
[0008] In one embodiment of the present invention, the particle sizes of the titanium black (A-1) and the carbon black (A-2) are less than 100 nanometers.
[0009] In one embodiment of the present invention, based on the usage of resin (D) being 100 parts by weight, the usage of black colorant (A) is 25 parts by weight to 430 parts by weight, the usage of ethylenically unsaturated monomer (B) is 78 parts by weight to 115 parts by weight, the usage of solvent (C) is 965 parts by weight to 2550 parts by weight, and the usage of photoinitiator (E) is 4 parts by weight to 12 parts by weight.
[0010] In one embodiment of the present invention, the ethylenically unsaturated monomer (B) includes at least one selected from the group consisting of acryloxy-containing compounds and methacryloyloxy-containing compounds.
[0011] In one embodiment of the present invention, the ethylenically unsaturated monomer (B) includes dipentaerythritol hexaacrylate and multifunctional polyurethane acrylate.
[0012] In one embodiment of the present invention, the ethylenically unsaturated monomer (B) has 4-14 functional groups, and the functional groups include at least one of an ester group, an acyl group, an acyloxy group, and an amide group.
[0013] In one embodiment of the present invention, the solvent (C) comprises at least one of a compound represented by the following formula (C-1) and a compound represented by the following formula (C-2),
[0014]
[0015] In formula (C-1), R 1 and R 2 are alkyl groups, m is 1 or 2,
[0016]
[0017] In formula (C-2), R 3 and R 4 are alkyl groups, and n is an integer greater than or equal to 1.
[0018] In one embodiment of the present invention, the resin (D) has a bisphenol fluorene structure, and the molecular weight of the resin (D) is 2000-20000.
[0019] In one embodiment of the present invention, the resin (D) is composed of a monomer represented by the following formula (D-1):
[0020]
[0021] In formula (D-1), R 5 and R 6 are carbonyl-containing groups respectively.
[0022] In one embodiment of the present invention, the photoinitiator (E) includes an oxime ester photoinitiator (E-1) and an acetophenone photoinitiator (E-2). Based on the total usage of the oxime ester photoinitiator (E-1) and the acetophenone photoinitiator (E-2) being 100 parts by weight, the usage of the oxime ester photoinitiator (E-1) is 50 parts by weight to 70 parts by weight.
[0023] A filter element of the present invention is formed from the above resin composition.
[0024] Based on the above, the resin composition of the present invention uses a black colorant (A) including titanium black (A-1) and carbon black (A-2), and the amount of titanium black (A-1) used is 50 to 75 parts by weight based on the total amount of titanium black (A-1) and carbon black (A-2) used being 100 parts by weight. Thus, when the resin composition is used to form a filter element, the filter element can have good resolution, developability, adhesion, coating uniformity and light transmittance.
[0025] In order to make the above features and advantages of the present invention more obvious and easy to understand, embodiments are specifically described in detail below. DETAILED DESCRIPTION
[0026] <Resin composition>
[0027] The present invention provides a resin composition, comprising a black colorant (A), an ethylenically unsaturated monomer (B), a solvent (C), a resin (D) and a photoinitiator (E). In addition, the resin composition of the present invention may further comprise an additive (F) such as a surfactant as needed. The above-mentioned various components will be described in detail below.
[0028] It should be noted that, hereinafter, (meth)acrylic acid refers to acrylic acid and / or methacrylic acid, and (meth)acrylate refers to acrylate and / or methacrylate.
[0029] Black colorant (A)
[0030] The black colorant (A) includes titanium black (A-1) and carbon black (A-2). However, the present invention is not limited thereto, and the black colorant (A) may also include organic black pigments (e.g., lactam organic black, RGB black, RVB black, etc.), inorganic black pigments (e.g., aniline black, perylene black, cyanine black, lignin black, etc.), combinations of the aforementioned black pigments, or other suitable black colorants.
[0031] The particle size of titanium black (A-1) and carbon black (A-2) is not particularly limited, and an appropriate particle size can be selected according to the needs, preferably less than 100 nanometers (nm).
[0032] The black colorant (A) is used in an amount of 25 to 430 parts by weight based on 100 parts by weight of the resin (D).
[0033] Based on 100 parts by weight of the total amount of titanium black (A-1) and carbon black (A-2), the amount of titanium black (A-1) is 50 to 75 parts by weight, preferably 50 to 70 parts by weight, and more preferably 50 to 66 parts by weight.
[0034] When the resin composition contains a black colorant (A) including titanium black (A-1) and carbon black (A-2), and the amount of titanium black (A-1) used falls within the above range, the hardened film formed by the resin composition can have good resolution, developability, adhesion, coating uniformity and light transmittance, and can be used for filter elements. At the same time, when the particle size of titanium black (A-1) and carbon black (A-2) is less than 100 nanometers, the hardened film and filter element formed by the resin composition can have better resolution.
[0035] Ethylenically unsaturated monomer (B)
[0036] In this embodiment, the ethylenically unsaturated monomer (B) may include at least one selected from the group consisting of compounds containing acryloyloxy groups and compounds containing methacryloyloxy groups. In other embodiments, the ethylenically unsaturated monomer (B) may have 4-14 functional groups, preferably 6, 10 or more functional groups, wherein the functional group includes at least one of an ester group, an acyl group, an acyloxy group and an amide group, preferably at least one of an acyloxy group and an amide group.
[0037] For example, the ethylenically unsaturated monomer (B) may include a compound represented by the following formula (B-1), dipentaerythritol hexaacrylate (DPHA), multifunctional polyurethane acrylate (trade name: DPHA-40H, Nippon Kayaku Co., Ltd. Co., LTD), ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 2,2-bis(4-(meth)acryloyloxydiethoxyphenyl)propane, 2,2-bis(4-(meth)acryloyloxypolyethoxyphenyl)propane alkane, 2-hydroxy-3-(meth)acryloxypropyl(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, phthalic acid diglycidyl ester di(meth)acrylate, glycerol triacrylate, glycerol polyglycidyl ether poly(meth)acrylate, urethane (meth)acrylate, trimethylhexamethylene diisocyanate and a reaction product of hexamethylene diisocyanate and 2-hydroxyethyl (meth)acrylate, N,N'-methylenebis(meth)acrylamide, (meth)acrylamide methylene ether, a condensate of a polyol and N-methylol(meth)acrylamide, triacrylate formal or other suitable monomers, preferably including dipentaerythritol hexaacrylate and multifunctional urethane acrylate (trade name: DPHA-40H, manufactured by Nippon Kayaku Co., LTD). The ethylenically unsaturated monomer (B) may be used alone or in combination of two or more.
[0038]
[0039] In formula (B-1), Z 1 and Z 2 are respectively a divalent group having an acyloxy group, Y 1 and Y 2 are alkyl or similar functional groups substituted with hydroxyl groups,
[0040] u and w are integers of 1-3 respectively, v and x are integers of 0-2 respectively, the sum of u and v is 3, and the sum of w and x is 3.
[0041] Preferred specific examples of the compound represented by formula (B-1) include dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate.
[0042] Based on 100 parts by weight of the resin (D), the amount of the ethylenically unsaturated monomer (B) is 78 parts by weight to 115 parts by weight, preferably 85 parts by weight to 104 parts by weight, and more preferably 86 parts by weight to 100 parts by weight.
[0043] When the ethylenically unsaturated monomer (B) in the resin composition has 4 to 14 functional groups, wherein the functional groups include at least one of ester groups, acyl groups, acyloxy groups and amide groups, the hardened film and the optical filter element formed by the resin composition can have better adhesion and resolution. In addition, when the amount of the ethylenically unsaturated monomer (B) used falls within the above range, the hardened film and the optical filter element formed by the resin composition can have better adhesion, resolution and developability.
[0044] Solvent (C)
[0045] There is no particular limitation on the solvent (C), and an appropriate solvent can be selected according to the requirements. The solvent (C) may include at least one of the compound represented by the following formula (C-1) and the compound represented by the following formula (C-2). The solvent (C) may be used alone or in combination.
[0046]
[0047] In formula (C-1), R 1 and R 2 are alkyl groups, and m is 1 or 2.
[0048] In formula (C-1), R1 and R2 are preferably alkyl groups having 1 to 5 carbon atoms, and more preferably methyl groups. Preferred specific examples of the compound represented by formula (C-1) include propylene glycol methyl etheracetate (PMA or PGMEA) or dipropylene glycol methyl etheracetate (DPMA or DPGMEA). The compound represented by formula (C-1) may be used alone or in combination of multiple compounds.
[0049]
[0050] In formula (C-2), R 3 and R 4are alkyl groups, and n is an integer greater than or equal to 1.
[0051] In formula (C-2), R 3 and R 4 Preferably, they are alkyl groups having 1 to 6 carbon atoms, more preferably, they are methyl groups, and n is preferably an integer of 1 to 2. Preferred specific examples of the compound represented by formula (C-2) include PGMEA, etc. The compound represented by formula (C-2) can be used alone or in combination with multiple compounds.
[0052] Based on 100 parts by weight of the resin (D), the amount of the solvent (C) is 965 parts by weight to 2550 parts by weight, and more preferably 1000 parts by weight to 2500 parts by weight.
[0053] When the solvent (C) in the resin composition includes the compound represented by formula (C-2), the precipitation rate of the particles in the resin composition can be improved, so that the hardened film and filter element formed therefrom have good stability, and the performance of the device using the filter element can be improved by, for example, reducing the problem of mura.
[0054] Resin (D)
[0055] In this embodiment, the resin (D) may have a bisphenol fluorene structure, and the molecular weight of the resin (D) is 2000-20000, preferably 3000-7000, and more preferably 4500-5000. In other embodiments, the resin (D) may be composed of a monomer represented by the following formula (D-1) or other suitable monomers. The resin (D) may be composed of a single monomer or a plurality of monomers.
[0056]
[0057] In formula (D-1), R 5 and R 6 are carbonyl-containing groups respectively.
[0058] In formula (D-1), R 5 and R 6 Preferred are groups containing a carbonyl group and a hydroxyl group or groups containing an acrylate group and a hydroxyl group. Preferred specific examples of the monomer represented by formula (D-1) include monomers represented by the following formula (d-1).
[0059]
[0060] When the resin composition includes a resin (D) having a bisphenol fluorene structure, and the molecular weight of the resin (D) is 2000-20000, the hardened film and the filter element prepared therefrom can have better adhesion. When the resin composition includes a resin (D) composed of a monomer represented by formula (D-1), and R in formula (D-1) 5 and R 6 When they are respectively carbonyl-containing groups, the cured film and filter element prepared from the resin composition can have better adhesion, resolution and developability.
[0061] Photoinitiator (E)
[0062] The photoinitiator (E) includes an oxime ester photoinitiator (E-1) and an acetophenone photoinitiator (E-2). However, the present invention is not limited thereto, and the photoinitiator (E) may also include other suitable photoinitiators.
[0063] There is no particular limitation on the oxime ester photoinitiator (E-1), and an appropriate oxime ester photoinitiator can be selected according to the requirements. For example, the oxime ester photoinitiator (E-1) can include Irgacure OXE-01, OXE-02, OXE-03, OXE-04 (trade names; manufactured by BASF) or other suitable oxime ester photoinitiators. The oxime ester photoinitiators can be used alone or in combination.
[0064] There is no particular limitation on the acetophenone-based photoinitiator (E-2), and an appropriate acetophenone-based photoinitiator can be selected according to the requirements. For example, the acetophenone-based photoinitiator (E-2) can include Benzalkonium 369E, Chemcure-96 (trade name; manufactured by Hengqiao Industrial Co., Ltd.) or other suitable acetophenone-based photoinitiators. Acetophenone-based photoinitiators can be used alone or in combination.
[0065] Based on the total usage of oxime ester photoinitiator (E-1) and acetophenone photoinitiator (E-2) being 100 parts by weight, the usage of oxime ester photoinitiator (E-1) may be 50 parts by weight to 70 parts by weight.
[0066] Based on 100 parts by weight of the resin (D), the amount of the photoinitiator (E) is 4 to 12 parts by weight, preferably 6 to 12 parts by weight, and more preferably 6 to 10 parts by weight.
[0067] When the photoinitiator (E) in the resin composition includes an oxime ester photoinitiator (E-1) and an acetophenone photoinitiator (E-2), and the amount of the oxime ester photoinitiator (E-1) is within the above range, the hardened film and the filter element prepared therefrom can have better resolution.
[0068] Additives (F)
[0069] The resin composition may further include an additive (F). In the present embodiment, the additive (F) may include a surfactant. There is no particular limitation on the surfactant, and an appropriate surfactant may be selected according to the needs. For example, the surfactant may include a fluorine-based surfactant or other suitable surfactants. The fluorine-based surfactant may include Megaface F575, F563, and F444 (trade name; perfluoroalkyl ethylene oxide adduct, manufactured by DIC Corporation). The surfactant may be used alone or in combination. The additive (F) may be used alone or in combination.
[0070] Based on 100 parts by weight of the resin (D), the additive (F) is used in an amount of 1 to 20 parts by weight, preferably 1 to 10 parts by weight, and more preferably 1 to 3 parts by weight.
[0071] When the resin composition further includes a fluorine-based surfactant as an additive (F), the formed cured film and filter element can have good coating uniformity.
[0072] <Method for preparing resin composition>
[0073] The method for preparing the resin composition is not particularly limited. For example, a black colorant (A), an ethylenically unsaturated monomer (B), a solvent (C), a resin (D) and a photoinitiator (E) are placed in a stirrer and stirred to uniformly mix them into a solution state. An additive (F) may also be added if necessary. After uniform mixing, a liquid resin composition can be obtained.
[0074] <Method for producing cured film>
[0075] The hardened film is obtained from the above-mentioned resin composition. In the present embodiment, the hardened film has a thickness of 0.3 microns to 3.0 microns, a resolution of less than 2 microns, preferably a resolution of 0.9 microns to 1.4 microns, and more preferably a resolution of 0.9 microns to 1.1 microns. In other embodiments, the hardened film has a thickness of 0.3 microns to 3.0 microns, and a visible light transmittance of 5% to 50%. For example, the visible light transmittance of the hardened film may be 5%, 10% or 50%, and may be applied to a filter element so that the filter element has a specific light transmittance.
[0076] The hardened film can be formed by coating the above-mentioned resin composition on a substrate to form a coating film, and pre-baking, exposing, developing and post-baking the coating film. For example, after the resin composition is coated on the substrate to form a coating film, it is pre-baked at 90°C for 2 minutes. Then, the pre-baked coating film is exposed to 1400 J / m with an I-line exposure machine (wavelength of 365 nm). 2 Then, the substrate was developed with a developer at 23° C. for 84 seconds. Then, the substrate was post-baked at 220° C. for 5 minutes to form a cured film on the substrate.
[0077] The substrate may be a glass substrate, a silicon wafer substrate, or a plastic substrate material such as a polyethersulfone (PES) board or a polycarbonate (PC) board, and the type thereof is not particularly limited.
[0078] The coating method is not particularly limited, but spray coating, roll coating, spin coating or the like may be used, and generally, spin coating is widely used. In addition, a coating film is formed, and then in some cases, the residual solvent may be partially removed under reduced pressure.
[0079] The developer is not particularly limited, and an appropriate developer can be selected according to the requirements. For example, the developer can be tetramethyl ammonium hydroxide (TMAH), and its concentration can be 0.3 wt %.
[0080] <Method for Manufacturing Filter Element>
[0081] An exemplary embodiment of the present invention provides a filter element, which is the above-mentioned hardened film.
[0082] The method for manufacturing the filter element may be the same as the method for manufacturing the cured film, and will not be further described herein.
[0083] Hereinafter, the present invention will be described in detail with reference to examples. The following examples are provided for describing the present invention, and the scope of the present invention includes the scope described in the claims and its substitutes and modifications, and is not limited to the scope of the examples.
[0084] Examples of resin composition and cured film
[0085] Examples 1 to 5 and Comparative Examples 1 to 5 of the resin composition and the cured film are described below:
[0086] Example 1
[0087] a. Resin composition
[0088] 145 parts by weight of titanium black with a particle size of less than 100 nanometers, 78 parts by weight of carbon black with a particle size of less than 100 nanometers, 47 parts by weight of dipentaerythritol hexaacrylate, 47 parts by weight of DPHA-40H, 100 parts by weight of cardol resin (molecular weight 5300; manufactured by KISCO), 4 parts by weight of Inlac OXE-04, 4 parts by weight of Inlac 369E and 2 parts by weight of Megafax F444 were added to a mixed solvent of 1199 parts by weight of propylene glycol methyl ether acetate and 514 parts by weight of ethylene glycol ethers, and stirred evenly with a stirrer to obtain the resin composition of Example 1.
[0089] b. Hardening film
[0090] The resin compositions prepared in the examples were coated on the substrate by spin coating (spin coating machine model TEL-MK8, manufactured by Tokyo Electron Co., Ltd., with a rotation speed of about 1800 rpm). Then, the substrate was pre-baked at 90° C. for 2 minutes. Then, the substrate was exposed to 1400 J / m by an I-line exposure machine (wavelength of 365 nm) (exposure machine model FPA-5500iZa, manufactured by Canon) for 1400 J / m 2 , to form a semi-finished product. Then, at a temperature of 23°C, TMAH with a concentration of 0.3 wt% was used as a developer for 84 seconds. Then, post-baking was performed at 220°C for 5 minutes to obtain a hardened film. The hardened film obtained was evaluated in the following evaluation methods, and the results are shown in Table 1.
[0091] Examples 2 to 5 and Comparative Examples 1 to 5
[0092] The resin compositions of Examples 2 to 5 and Comparative Examples 1 to 5 were prepared in the same steps as Example 1, except that the types of components and the amounts used in the resin compositions were changed (as shown in Table 1). The prepared resin compositions were made into hardened films and evaluated in the following evaluation methods, and the results are shown in Table 1.
[0093] [Table 1]
[0094]
[0095]
[0096] [Table 1] (Continued)
[0097]
[0098]
[0099] In Table 1, the ethylenically unsaturated monomer (B) having a structure with three functional groups may be a compound represented by the following formula (b-1), wherein m+n+p=3 (trade name: NK ESTER A-TMPT-3EO, manufactured by ShinNakamura Chemical Co., Ltd.). The ethylenically unsaturated monomer (B) having a structure with 15 functional groups may be a compound represented by the following formula (b-2), wherein q+r+s=15 (trade name: TP-153, manufactured by Hannong Chemical Co., Ltd.).
[0100]
[0101] In Table 1, the structure of cardol resin CAP01 (molecular weight 4393; manufactured by MIWON Specialty Chemical Co., Ltd.) having a molecular weight of less than 5000 may be a structure represented by the following formula (d-2), wherein r is approximately 4.
[0102]
[0103] In Table 1, the molecular weight of KBR series (trade name; manufactured by KISCO) with a molecular weight between 5000 and 10000 may be 5300, and the molecular weight of KBR series (trade name; manufactured by KISCO) with a molecular weight greater than 10000 may be 16797.
[0104] <Evaluation method>
[0105] a. Resolution
[0106] The prepared hardened film (thickness 0.4 μm) was observed by a critical dimension scanning electron microscope (CD-SEM) (model: S-8840, manufactured by Hitachi) at a magnification of 45K to observe the integrity of the dot pattern in the critical dimension 1 μm area to evaluate the resolution. When the pattern profile is more complete, it shows that the hardened film has good resolution.
[0107] The evaluation criteria for resolution are as follows:
[0108] ○: The pattern outline is complete;
[0109] △: The pattern outline is slightly protruding or missing, but it does not affect the practical application;
[0110] ╳: The pattern outline is incomplete.
[0111] b. Development
[0112] The prepared hardened film (thickness 0.4 μm) was observed by a critical dimension scanning electron microscope (CD-SEM) (model: S-8840, manufactured by Hitachi) at a magnification of 35K to observe whether there was residue in the unexposed area with a critical dimension of 1 μm to evaluate the developability. When the residue is less, it shows that the hardened film has good developability.
[0113] The evaluation criteria for developability are as follows:
[0114] ○: no residue;
[0115] △: There is a little residue, but it does not affect the practical application;
[0116] ╳: There is obvious residue.
[0117] c. Adhesion
[0118] The prepared hardened film (thickness 0.4 μm) was observed under an optical microscope (OM) (model: BH3-SIC6, manufactured by Olympus) at a magnification of 50 times to evaluate the adhesion of the pattern. The smaller the width when the pattern does not peel off, the better the adhesion of the hardened film.
[0119] The evaluation criteria for adhesion are as follows:
[0120] ○: 1μm≦pattern width<2μm;
[0121] △: 2μm≦pattern width<3μm;
[0122] ╳: 3μm≦pattern width.
[0123] d. Coating uniformity
[0124] The prepared hardened film (thickness 0.4 μm) was measured for transmittance at wavelengths of 400-700 nm at 13 points on the film using a colorimeter (model: MCPD-3000, manufactured by Otsuka Electronics Co., Ltd.) to calculate the deviation value (3-sigma). The initial measurement value and the measurement value after three weeks of placement were recorded and the deviation values were calculated respectively. The difference in the deviation values before and after placement was compared to evaluate the coating uniformity.
[0125] The evaluation criteria for coating uniformity are as follows:
[0126] ○: The deviation of the membrane penetration rate is less than 0.5%;
[0127] △: 0.5% ≦ membrane penetration deviation value ≦ 1%;
[0128] ╳: 1%<membrane penetration deviation value.
[0129] e. Light transmittance
[0130] The transmittance of the prepared cured film (thickness 0.4 μm) at a wavelength of 400-700 nm was measured at 13 points selected on the film using a colorimeter (model: MCPD-3000, manufactured by Otsuka Electronics Co., Ltd.), and the average value of the obtained transmittance was taken as the light transmittance shown in Table 1.
[0131] <Evaluation Results>
[0132] As shown in Table 1, the resin composition contains a black colorant (A) including titanium black (A-1) and carbon black (A-2), and the amount of titanium black (A-1) used is 50 to 75 parts by weight based on 100 parts by weight of the total amount of titanium black (A-1) and carbon black (A-2). The cured films formed in Examples 1-5 have good resolution, developability, adhesion, coating uniformity and light transmittance, and are suitable for use in filter elements. In contrast, the cured films formed in Comparative Examples 1-3, in which the amount of titanium black (A-1) used in the resin composition is not within the above range, have poor adhesion and coating uniformity.
[0133] In addition, compared with the hardened film (Example 5) prepared by using titanium black (A-1) and carbon black (A-2) in the resin composition with a particle size greater than or equal to 100 nanometers, the hardened film (Examples 1-4) prepared by using titanium black (A-1) and carbon black (A-2) in the resin composition with a particle size less than 100 nanometers has a more complete pattern outline. It can be seen that when using titanium black (A-1) and carbon black (A-2) with a particle size less than 100 nanometers, the hardened film formed by the resin composition can have a better resolution.
[0134] In addition, compared with the hardened film prepared by the ethylenically unsaturated monomer (B) in the resin composition not including 4-14 functional groups, wherein the functional groups include at least one of ester group, acyl group, acyloxy group and amide group (Comparative Example 4), the hardened film prepared by the ethylenically unsaturated monomer (B) in the resin composition including 4-14 functional groups (Examples 1-5) has a smaller pattern width and a lower film transmittance deviation value. It can be seen that when the ethylenically unsaturated monomer (B) having 4-14 functional groups is used, wherein the functional groups include at least one of ester group, acyl group, acyloxy group and amide group, the hardened film formed by the resin composition can have better adhesion and resolution.
[0135] In addition, based on the usage of resin (D) being 100 parts by weight, compared with the hardened film (Comparative Example 5) prepared by using 76 parts by weight of the ethylenically unsaturated monomer (B) in the resin composition, the hardened film (Examples 1-5) prepared by using 78 to 115 parts by weight of the ethylenically unsaturated monomer (B) in the resin composition has a more complete pattern profile, less residue and a lower film transmittance deviation value. It can be seen that when the usage of the ethylenically unsaturated monomer (B) is 78 to 115 parts by weight, the hardened film formed by the resin composition can have better adhesion, resolution and developability.
[0136] In addition, compared to the hardened film prepared by the resin (D) in the resin composition not having the bisphenol fluorene structure (Comparative Examples 1 and 3), the hardened film prepared by the resin (D) in the resin composition having the bisphenol fluorene structure and the molecular weight of the resin (D) being 2000-20000 (Examples 1-5) has a smaller pattern width and a lower intra-film permeability deviation value. It can be seen that when a resin (D) having a bisphenol fluorene structure is used and the molecular weight of the resin (D) is 2000-20000, the hardened film formed by the resin composition can have better adhesion. And when the resin composition includes a resin (D) composed of a monomer shown in the above formula (D-1), and R5 and R6 in the formula (D-1) are respectively carbonyl-containing groups, the hardened film formed by the resin composition can also have better adhesion, resolution and developability.
[0137] In addition, when the resin (D) in the resin composition has a bisphenol fluorene structure, the hardened film (Example 1-3) prepared with a molecular weight of the resin (D) less than 5000 has a more complete pattern profile or less residue, compared to the hardened film (Example 4) prepared with a molecular weight of the resin (D) between 5000 and 10000 and the hardened film (Example 5) prepared with a molecular weight of the resin (D) greater than 10000. It can be seen that when a resin (D) having a bisphenol fluorene structure is used and the molecular weight of the resin (D) ranges from greater than or equal to 5000 to less than or equal to 10000, the hardened film formed by the resin composition has better developability or resolution.
[0138] In addition, compared to the hardened film (Comparative Examples 4 and 5) prepared by the photoinitiator (E) in the resin composition not including the acetophenone-based photoinitiator (E-2), the photoinitiator (E) in the resin composition includes an oxime ester photoinitiator (E-1) and an acetophenone-based photoinitiator (E-2), and the hardened film (Examples 1-5) prepared by the use of 4 to 12 parts by weight of the photoinitiator (E) based on the use amount of 100 parts by weight of the resin (D) has a lower film transmittance deviation value. It can be seen that when a photoinitiator (E) including an oxime ester photoinitiator (E-1) and an acetophenone-based photoinitiator (E-2) is used, and the use amount of the oxime ester photoinitiator (E-1) falls within the above range, the hardened film formed by the resin composition can have a better resolution.
[0139] In summary, the resin composition of the present invention contains a black colorant (A) including titanium black (A-1) and carbon black (A-2), and when the amount of the titanium black (A-1) used is 50 to 75 parts by weight based on 100 parts by weight of the total amount of the titanium black (A-1) and the carbon black (A-2), the cured film formed by the resin composition has good resolution, developability, adhesion, coating uniformity and light transmittance, and can be applied to filter elements, thereby improving the performance of devices using filter elements.
[0140] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Any person having ordinary knowledge in the technical field may make some changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the appended claims.
Claims
1. A resin composition comprising: Black colorant; An ethylenically unsaturated monomer, wherein the ethylenically unsaturated monomer has 4 to 14 functional groups, and the functional groups include at least one of an ester group, an acyl group, an acyloxy group, and an amide group; Solvents; Resin, wherein the resin has a bisphenol fluorene structure and the molecular weight of the resin is 2000-20000; and Photoinitiator, The black colorant includes titanium black and carbon black, and based on 100 parts by weight of the total amount of the titanium black and the carbon black, the amount of the titanium black is 50 parts by weight to 75 parts by weight. Wherein based on the usage of the resin being 100 parts by weight, the usage of the black colorant is 25 parts by weight to 430 parts by weight, the usage of the ethylenically unsaturated monomer is 78 parts by weight to 115 parts by weight, the usage of the solvent is 965 parts by weight to 2550 parts by weight, and the usage of the photoinitiator is 4 parts by weight to 12 parts by weight. 2 . The resin composition according to claim 1 , wherein the thickness of a hardened film obtained from the resin composition is 0.3 μm to 3.0 μm and the resolution is less than 2 μm. 3 . The resin composition according to claim 1 , wherein the thickness of a hardened film obtained from the resin composition is between 0.3 μm and 3.0 μm, and the visible light transmittance is between 5% and 50%. The resin composition according to claim 1 , wherein the particle size of the titanium black and the carbon black is less than 100 nanometers. 5 . The resin composition according to claim 1 , wherein the ethylenically unsaturated monomer comprises at least one selected from the group consisting of acryloxy-containing compounds and methacryloyloxy-containing compounds. 6 . The resin composition according to claim 1 , wherein the ethylenically unsaturated monomer comprises dipentaerythritol hexaacrylate and multifunctional urethane acrylate.
7. The resin composition according to claim 1, wherein the solvent comprises at least one of a compound represented by the following formula (C-1) and a compound represented by the following formula (C-2), In formula (C-1), R 1 and R 2 are alkyl groups, m is 1 or 2, In formula (C-2), R 3 and R 4 are alkyl groups, and n is an integer greater than or equal to 1.
8. The resin composition according to claim 1, wherein the resin is composed of a monomer represented by the following formula (D-1): In formula (D-1), R 5 and R 6 are carbonyl-containing groups respectively.
9. The resin composition according to claim 1, wherein the photoinitiator comprises an oxime ester photoinitiator and an acetophenone photoinitiator, and based on the total usage of the oxime ester photoinitiator and the acetophenone photoinitiator as 100 parts by weight, the usage of the oxime ester photoinitiator is 50 parts by weight to 70 parts by weight. 10 . A filter element, formed from the resin composition according to claim 1 .