Method for forming a semiconductor device and semiconductor device
By forming barrier dielectric layers with different thicknesses on the first and second regions of the semiconductor device, the etching rate of the plug groove is controlled, and the damage caused by the difference in the etching rate of the dielectric layer during the plug groove formation process is solved, and the damage problem is achieved. More even and precise plug groove formation.
Patent Information
- Application Number
- CN202010046318.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-01-16
AI Technical Summary
During the plug groove formation process of semiconductor devices, the etching rates of dielectric layers in different regions with different spacing between gate structures are different, resulting in over-etching or etching of dielectric layers in areas with smaller spacing between gate structures. Inadequate, damages the source-drain doped region.
A barrier dielectric layer is formed on the first dielectric layer of the first region and the second region, and the barrier dielectric layer thickness of the first region is greater than the barrier dielectric layer of the second region, forming a first insertion through the first dielectric layer and the barrier dielectric layer. The plug groove and the second plug groove are controlled by the etching process, and the etching rate of the first plug groove is slowed down by the low etching rate of the barrier dielectric layer.
Overetching of the source-drain doped region of the first region is effectively avoided, damage is prevented, the uniformity and accuracy of the plug groove are ensured, and the preparation quality of the semiconductor device is improved.
Smart Images

Figure CN113140631B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for forming a semiconductor device and a semiconductor device. Background Art
[0002] In order to comply with the development of Morgan's Law and meet people's requirements for various electronic products to have smaller size, occupy less space, and be easier to carry and operate, semiconductor manufacturing technology is developing rapidly with high integration, low power consumption and high performance as the goal. At present, as the semiconductor industry advances to the process node of 10nm or even below, the preparation of semiconductor devices is restricted by various physical limits.
[0003] In order to continuously improve the current driving ability of transistor circuits and further suppress the short channel effect, semiconductor devices have developed from planar semiconductor devices to three-dimensional semiconductor devices, such as fin field effect transistors (FinFET). Compared with planar semiconductor devices, FinFET is an advanced semiconductor device used for process nodes of 20nm and below. Because the three-dimensional structure of FinFET can effectively increase the actual distance between the source and the gate, and the gate and the drain, FinFET can effectively reduce the short channel effect and effectively increase the density of semiconductor devices formed on the substrate. At the same time, the gate in FinFET is set around the fin, so it can control the current from three sides. Therefore, the ability of FinFET devices to control current is also better than that of planar semiconductor devices.
[0004] Although FinFET has lower voltage and smaller device volume, if the size of the device continues to shrink, the challenges faced by FinFET are also increasing. For example, when etching the dielectric layer between the gate structures to form a plug trench, the etching rate of the dielectric layer in the regions with different spacings between the gate structures is different, and the etching rate of the dielectric layer in the first region with a smaller spacing between the gate structures is usually greater than the etching rate of the dielectric layer in the second region with a larger spacing between the gate structures. Therefore, the source and drain doping regions in the first region will be damaged during the formation of the plug trench. Summary of the invention
[0005] The purpose of the present invention is to solve the problem in the prior art that the source-drain doping region of the first region is damaged during the formation of the plug groove. The present invention provides a method for forming a semiconductor device, which can prevent the source-drain doping region of the first region from being damaged during the formation of the plug groove.
[0006] To solve the above technical problems, an embodiment of the present invention discloses a method for forming a semiconductor device, comprising: providing a substrate, the substrate comprising a first region and a second region, the substrate having a gate structure, the spacing between the gate structures in the first region being smaller than the spacing between the gate structures in the second region, and the substrate having source and drain doping regions on both sides of the gate structure;
[0007] forming a first dielectric layer covering a portion of the sidewall of the gate structure on the substrate, wherein a top surface of the first dielectric layer is lower than a top surface of the gate structure;
[0008] forming a blocking dielectric layer on the first dielectric layer in the first and second regions, wherein the thickness of the blocking dielectric layer in the first region is greater than the thickness of the blocking dielectric layer in the second region;
[0009] A first plug trench penetrating the first dielectric layer and the blocking dielectric layer is formed on the source-drain doped region of the first region. During the process of forming the first plug trench, a second plug trench penetrating the first dielectric layer and the blocking dielectric layer is formed on the source-drain doped region of the second region.
[0010] Preferably, the method for forming the first dielectric layer comprises: forming a first initial dielectric layer on the substrate to cover the entire sidewall of the gate structure; and etching back the first initial dielectric layer to form the first dielectric layer.
[0011] Preferably, the blocking dielectric layer in the second region has a dielectric recess, and in a direction perpendicular to the top surface of the gate structure, the thickness of the blocking dielectric at the bottom of the dielectric recess is less than the thickness of the blocking dielectric layer in the first region;
[0012] The method for forming a semiconductor device further includes: before forming the first plug trench and the second plug trench, filling the dielectric recess with a second dielectric layer; after forming the second plug trench, the second plug trench also penetrates the second dielectric layer.
[0013] Preferably, the method for forming the blocking dielectric layer and the second dielectric layer includes: forming a blocking material layer on the sidewall and top of the gate structure in the first region, the surface of the first dielectric layer in the first region, the sidewall and top of the gate structure in the second region, and the surface of the first dielectric layer in the second region, wherein the blocking material layer in the first region has a first recess located on the first dielectric layer, and the blocking material layer in the second region has a second recess located on the first dielectric layer, and the thickness of the blocking material layer at the bottom of the first recess is greater than the thickness of the blocking material layer in the second recess; forming a second dielectric material layer in the first recess and the second recess, and on the blocking material layer; planarizing the second dielectric material layer and the blocking material layer until the top surface of the gate structure is exposed, so that the blocking material layer forms the blocking dielectric layer, the second dielectric material layer forms the second dielectric layer, and the second recess forms a dielectric recess located in the blocking dielectric layer.
[0014] Preferably, the process for forming the barrier material layer includes an atomic layer deposition process; and the process for forming the second dielectric material layer includes a fluid chemical vapor deposition process or a plasma chemical vapor deposition process.
[0015] Preferably, in a direction perpendicular to the top surface of the gate structure, a ratio of a thickness of the blocking dielectric at the bottom of the dielectric recess to a thickness of the blocking dielectric layer in the first region is 1.4 to 2.2.
[0016] Preferably, the material of the second dielectric layer includes silicon oxide.
[0017] Preferably, the process of forming the first plug trench and the second plug trench is an etching process; in the process of forming the first plug trench and the second plug trench, the etching rate of the second dielectric layer is greater than the etching rate of the blocking dielectric layer.
[0018] Preferably, in the process of forming the first plug trench and the second plug trench, the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer; the ratio of the etching rate of the blocking dielectric layer to the etching rate of the first dielectric layer is 10 to 100.
[0019] Preferably, the material of the first dielectric layer includes silicon oxide; and the material of the blocking dielectric layer includes silicon nitride.
[0020] Preferably, a dimension of the first plug trench along the channel length direction of the first region is smaller than a dimension of the second plug trench along the channel length direction of the second region.
[0021] Preferably, the channel length at the bottom of the gate structure in the first region is smaller than the channel length at the bottom of the gate structure in the second region.
[0022] Preferably, it also includes: after forming the blocking dielectric layer and before forming the first plug trench and the second plug trench, removing the gate structure to form a gate opening in the first dielectric layer and the blocking dielectric layer; forming a metal gate structure in the gate opening, and the spacing between the metal gate structures in the first region is smaller than the spacing between the metal gate structures in the second region.
[0023] An embodiment of the present invention further discloses a semiconductor device, comprising:
[0024] a substrate comprising a first region and a second region;
[0025] a target gate structure located on the substrate, wherein a spacing between the target gate structures in the first region is smaller than a spacing between the target gate structures in the second region;
[0026] Source and drain doped regions in the substrate respectively located on both sides of the target gate structure;
[0027] a first dielectric layer located on the substrate and covering a portion of the sidewall of the target gate structure, wherein a top surface of the first dielectric layer is lower than a top surface of the target gate structure;
[0028] a blocking dielectric layer located on the first dielectric layer in the first and second regions, wherein the thickness of the blocking dielectric layer in the first region is greater than the thickness of the blocking dielectric layer in the second region;
[0029] A first plug trench located on the source-drain doped region of the first region and penetrating the first dielectric layer and the blocking dielectric layer;
[0030] A second plug trench is located on the source-drain doped region of the second region and penetrates the first dielectric layer and the blocking dielectric layer.
[0031] Preferably, the blocking dielectric layer in the second region has a dielectric recess, and in a direction perpendicular to the top surface of the target gate structure, the thickness of the blocking dielectric at the bottom of the dielectric recess is less than the thickness of the blocking dielectric layer in the first region; the semiconductor device also includes: a second dielectric layer located in the dielectric recess; and the second plug groove also penetrates the second dielectric layer.
[0032] Preferably, the material of the second dielectric layer includes silicon oxide; the material of the first dielectric layer includes silicon oxide; and the material of the blocking dielectric layer includes silicon nitride.
[0033] Preferably, a dimension of the first plug trench along the channel length direction of the first region is smaller than a dimension of the second plug trench along the channel length direction of the second region.
[0034] Preferably, a channel length at the bottom of the target gate structure in the first region is smaller than a channel length at the bottom of the target gate structure in the second region.
[0035] Preferably, it further comprises: a first plug located in the first plug slot; and a second plug located in the second plug slot.
[0036] Preferably, the base comprises a semiconductor substrate and a fin located on the semiconductor substrate; and the target gate structure spans across the fin.
[0037] The beneficial effects of the present invention are:
[0038] The method for forming a semiconductor device provided by the present invention first forms a blocking dielectric layer on the first dielectric layer of the first region and the second region, and the thickness of the blocking dielectric layer of the first region is greater than the thickness of the blocking dielectric layer of the second region, and then forms a first plug groove penetrating the first dielectric layer and the blocking dielectric layer on the source-drain doped region of the first region, and forms a second plug groove penetrating the first dielectric layer and the blocking dielectric layer on the source-drain doped region of the second region. In the process of etching to form the first plug groove and the second plug groove, since the blocking dielectric layer has a blocking effect and the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer, the etching rate of the first plug groove relative to the second plug groove can be slowed down, thereby avoiding the problem of over-fast etching when forming the first plug groove in the first region, and finally preventing the source-drain doped region of the first region from being over-etched, thereby avoiding damage to the source-drain doped region. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 is a flow chart of a method for forming a semiconductor device provided by an embodiment of the present invention;
[0040] Figures 2 to 10 It is a structural schematic diagram corresponding to the method for forming a semiconductor device provided in an embodiment of the present invention.
[0041] Reference numerals:
[0042] 1. substrate; 11. first region; 12. second region; 2. gate structure; 21. metal gate structure; 22. etch barrier layer; 23. mask; 3. source-drain doped region; 4. first dielectric layer; 41. first initial dielectric layer; 5. blocking dielectric layer; 51. dielectric recess; 52. blocking material layer; 6. second dielectric layer; 61. second dielectric material layer; 7. first plug trench; 8. second plug trench; 9. side wall. DETAILED DESCRIPTION
[0043] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0044] It should be noted that in this specification, similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings.
[0045] In the description of this embodiment, it should be noted that the terms "upper", "lower", "inner", "bottom", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the inventive product is usually placed when used. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0046] The terms “first”, “second”, etc. are only used for distinguishing descriptions and should not be understood as indicating or implying relative importance.
[0047] In the description of this embodiment, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this embodiment can be understood according to specific circumstances.
[0048] In order to solve the problem that the dielectric layer in the region with a smaller spacing between the gate structures is over-etched or the dielectric layer in the region with a larger spacing between the gate structures is under-etched due to the different etching rates of the dielectric layer in the region with different spacing between the gate structures in the prior art, the present invention provides a method for forming a semiconductor device, specifically, as follows Figure 1The flowchart of the method for forming a semiconductor device provided by the embodiment of the present invention is shown. The method for forming a semiconductor device provided by the embodiment of the present invention specifically includes the following steps:
[0049] Step S1: providing a substrate, the substrate comprising a first region and a second region, the substrate having a gate structure, the spacing between the gate structures in the first region being smaller than the spacing between the gate structures in the second region, and the substrate having source and drain doping regions on both sides of the gate structure respectively.
[0050] Step S2: forming a first dielectric layer on the substrate that covers a portion of the sidewalls of the gate structure, wherein a top surface of the first dielectric layer is lower than a top surface of the gate structure.
[0051] Step S3: forming a blocking dielectric layer on the first dielectric layer in the first region and the second region, wherein the thickness of the blocking dielectric layer in the first region is greater than the thickness of the blocking dielectric layer in the second region.
[0052] Step S4: forming a first plug trench penetrating the first dielectric layer and the blocking dielectric layer on the source / drain doped region of the first region, and in the process of forming the first plug trench, forming a second plug trench penetrating the first dielectric layer and the blocking dielectric layer on the source / drain doped region of the second region.
[0053] The above method can prevent the problem of over-etching of the dielectric layer in the region with a smaller spacing between the gate structures, or the problem of under-etching of the dielectric layer in the region with a larger spacing between the gate structures, which is caused by the different etching rates of the dielectric layer in the regions with different spacing between the gate structures. Specifically, in the method for forming a semiconductor device provided by this embodiment, a blocking dielectric layer is first formed on the first dielectric layer in the first region and the second region, and the thickness of the blocking dielectric layer in the first region is greater than the thickness of the blocking dielectric layer in the second region, and then a first plug groove penetrating the first dielectric layer and the blocking dielectric layer is formed on the source-drain doped region of the first region, and a second plug groove penetrating the first dielectric layer and the blocking dielectric layer is formed on the source-drain doped region of the second region. In the process of etching to form the first plug groove and the second plug groove, since the blocking dielectric layer has a blocking effect and the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer, the etching rate of the first plug groove relative to the second plug groove can be slowed down, thereby avoiding the problem of over-fast etching when forming the first plug groove in the first region, and finally preventing the source-drain doped region of the first region from being over-etched, thereby avoiding damage to the source-drain doped region.
[0054] Combine the following Figures 1 to 10 The method for forming the semiconductor device is described in detail. Figures 2 to 10 It is a structural schematic diagram corresponding to the method for forming a semiconductor device provided in an embodiment of the present invention.
[0055] First, if Figure 1 and Figure 4 As shown, a substrate 1 is provided, the substrate 1 includes a first area 11 and a second area 12, a gate structure 2 is provided on the substrate 1, the spacing between the gate structures 2 in the first area 11 is smaller than the spacing between the gate structures 2 in the second area 12, and source and drain doping regions 3 are respectively provided in the substrate 1 on both sides of the gate structure 2.
[0056] Continue to refer Figure 4 A first dielectric layer 4 is formed on the substrate 1 to cover a portion of the sidewall of the gate structure 2 , and a top surface of the first dielectric layer 4 is lower than a top surface of the gate structure 2 .
[0057] It should be noted that, in this embodiment, a sidewall is formed on the sidewall of the gate structure, and an etching stop layer is formed on the surface of the sidewall; and before forming the first dielectric layer, a mask is also formed on the top of the gate structure.
[0058] The following description will be made by taking an example where a sidewall spacer and an etching stopper layer are formed on the sidewall of the gate structure, and a mask is formed on the top of the gate structure.
[0059] Specifically, this embodiment forms Figure 4 The specific process of the structure shown is as follows Figure 2-4 shown.
[0060] More specifically, in this embodiment, forming the first dielectric layer 4 includes:
[0061] First, if Figure 2 As shown, a mask 23 is formed on the top of the gate structure 2, a sidewall 9 is formed covering the sidewall of the gate structure 2 and part of the sidewall of the mask 23, and an etching stopper 22 is formed covering the sidewall 9 and the sidewall and top of the mask 23. It should be noted that in this embodiment, an etching stopper 22 is also formed on the surface of the source and drain doping region 3.
[0062] A first initial dielectric layer 41 covering the entire sidewall of the gate structure 2 is formed on the substrate 1 , specifically, the first initial dielectric layer 41 is formed with a top not lower than the top position of the etching stop layer 22 , and then the first initial dielectric layer 41 is subjected to a chemical mechanical polishing process.
[0063] Then as Figure 3 As shown, the first initial dielectric layer 41 , the etch stop layer 22 and the mask 23 are chemically mechanically polished until the tops of the first initial dielectric layer 41 , the etch stop layer 22 and the mask 23 are flush with the tops of the sidewalls 9 .
[0064] Next, if Figure 4As shown, the first initial dielectric layer 41 is etched back to form the first dielectric layer 4. Specifically, during the back etching process, the mask 23 is removed, and the etch stop layer 22 and the sidewall 9 are etched to be flush, and the top surfaces of the finally formed etch stop layer 22 and the sidewall 9 are lower than the top surface of the gate structure 2 and higher than the top surface of the first dielectric layer 4.
[0065] Specifically, the material of the substrate 1 in this embodiment includes but is not limited to single crystal silicon, polycrystalline silicon, amorphous silicon, germanium silicon material, carbon silicon material, etc., and this embodiment does not make any specific limitation on this.
[0066] In this embodiment, the base 1 includes a semiconductor substrate and a fin located on the semiconductor substrate. Other semiconductor structures such as an isolation structure may also be formed on the base 1, which is not specifically limited in this embodiment.
[0067] The first area 11 in this embodiment is Figure 4 The left half of the region, in which the spacing between the gate structures 2 is small; the second region 12 in this embodiment is Figure 4 The right half of the middle region has a larger spacing between the gate structures 2 .
[0068] In this embodiment, the channel length at the bottom of the gate structure 2 in the first region 11 is less than the channel length at the bottom of the gate structure 2 in the second region 12. In other embodiments of this embodiment, the channel length at the bottom of the gate structure 2 in the first region 11 and the channel length at the bottom of the gate structure 2 in the second region 12 may also be the same.
[0069] Next, Figure 7 As shown, a blocking dielectric layer 5 is formed on the first dielectric layer 4 in the first region 11 and the second region 12, and the thickness of the blocking dielectric layer 5 in the first region 11 is greater than the thickness of the blocking dielectric layer 5 in the second region 12.
[0070] This embodiment forms Figure 7 The specific process of the structure shown is as follows Figure 5-7 shown.
[0071] It should be noted that, in this embodiment, a dielectric recess 51 is formed in the blocking dielectric layer 5 in the second region 12 , and a second dielectric layer 6 is also formed in the dielectric recess 51 .
[0072] The method for forming the blocking dielectric layer 5 and the second dielectric layer 6 comprises: firstly Figure 5As shown in FIG. 1 , a barrier material layer 52 is formed on the sidewall and top of the gate structure 2 in the first region 11, the surface of the first dielectric layer 4 in the first region 11, the sidewall and top of the gate structure 2 in the second region 12, and the surface of the first dielectric layer 4 in the second region 12. The barrier material layer 52 in the first region 11 has a first recess located on the first dielectric layer 4, and the barrier material layer 52 in the second region 12 has a second recess located on the first dielectric layer 4. The thickness of the barrier material layer 52 at the bottom of the first recess is greater than the thickness of the barrier material layer 52 in the second recess. A second dielectric material layer 61 is formed in the first recess, the second recess, and on the barrier material layer 52. Then, as shown in FIG. Figure 6 As shown, the second dielectric material layer 61 is subjected to a chemical mechanical polishing process. Figure 7 As shown, the second dielectric material layer 61 and the blocking material layer 52 are planarized until the top surface of the gate structure 2 is exposed, so that the blocking material layer 52 forms a blocking dielectric layer, the second dielectric material layer 61 forms a second dielectric layer 6, and the second recess forms a dielectric recess 51 located in the blocking dielectric layer 5.
[0073] It should be noted that Figure 7 The medium recess 51 shown in the dotted box does not represent the actual medium recess 51 . It only represents the medium recess 51 that provides space for the second medium layer 6 . The size and shape of the medium recess 51 can be determined according to actual needs.
[0074] Preferably, in this embodiment, the material of the first dielectric layer 4 includes silicon oxide, and the material of the blocking dielectric layer 5 includes silicon nitride. In addition, in this embodiment, the material of the first dielectric layer 4 may also include silicon oxycarbide, silicon oxynitride, etc., which can be specifically selected as needed.
[0075] It should be noted that, in this embodiment, Figure 7 As shown, the blocking dielectric layer 5 of the second region 12 has a dielectric recess 51 , and in a direction perpendicular to the top surface of the gate structure 2 , the thickness of the blocking dielectric layer 5 at the bottom of the dielectric recess 51 is less than the thickness of the blocking dielectric layer 5 of the first region 11 .
[0076] It should also be noted that in this embodiment, only the dielectric recess 51 is formed in the second region 12, and no dielectric recess is formed in the blocking dielectric layer 5 in the first region 11. However, this is only a schematic representation of this embodiment, and those skilled in the art may choose to form a dielectric recess in the blocking dielectric layer in the first region, and also form a dielectric recess in the blocking dielectric layer in the second region, and the thickness of the blocking dielectric layer at the bottom of the dielectric recess in the first region is less than the thickness of the blocking dielectric layer at the bottom of the dielectric recess in the second region.
[0077] Preferably, in a direction perpendicular to the top surface of the gate structure 2, the ratio of the thickness of the blocking dielectric at the bottom of the dielectric recess 51 to the thickness of the blocking dielectric layer 5 in the first region 11 is 1.4 to 2.2. Specifically, the thickness of the blocking dielectric at the bottom of the dielectric recess 51 is about 700 angstroms, and the thickness of the blocking dielectric layer 5 in the first region 11 is 1000 angstroms to 1500 angstroms.
[0078] Furthermore, the material of the second dielectric layer 6 includes at least one of silicon oxide, silicon oxynitride, and silicon oxycarbide, which can be specifically selected according to needs.
[0079] Preferably, in this embodiment, the barrier material layer 52 is formed by an atomic layer deposition process; and the second dielectric layer 6 is formed by a fluid chemical vapor deposition process or a plasma chemical vapor deposition process.
[0080] Finally Fig.10 As shown, a first plug trench 7 penetrating the first dielectric layer 4 and the blocking dielectric layer is formed on the source / drain doped region 3 of the first region 11. In the process of forming the first plug trench 7, a second plug trench 8 penetrating the first dielectric layer 4 and the blocking dielectric layer is formed on the source / drain doped region 3 of the second region 12.
[0081] After forming the blocking dielectric layer 5 and before forming the first plug trench 7 and the second plug trench 8, the method further includes: Figure 8 As shown, the gate structure 2 is removed, and a gate opening is formed in the first dielectric layer 4 and the blocking dielectric layer; then Fig. 9 A metal gate structure 21 is formed in the gate opening, and the spacing between the metal gate structures 21 in the first region 11 is smaller than the spacing between the metal gate structures 21 in the second region 12. Fig.10 , etching to form a first plug groove 7 and a second plug groove 8.
[0082] Furthermore, a dimension of the first plug trench 7 along the channel length direction of the first region 11 is smaller than a dimension of the second plug trench 8 along the channel length direction of the second region 12 .
[0083] Preferably, the process of forming the first plug trench 7 and the second plug trench 8 is an etching process; in the process of forming the first plug trench 7 and the second plug trench 8, the etching rate of the second dielectric layer 6 is greater than the etching rate of the blocking dielectric layer.
[0084] In the process of forming the first plug groove 7 and the second plug groove 8, the etching rate of the blocking dielectric layer is less than the etching rate of the first dielectric layer 4; the ratio of the etching rate of the blocking dielectric layer to the etching rate of the first dielectric layer 4 is 10 to 100, which can be 10-50, such as 10, 20, 30, 40, 50, etc., or 50-100, such as 60, 70, 80, 90, 100, or other values, which is not specifically limited in this embodiment.
[0085] It should be noted that if Figure 7 As shown, in this embodiment, before forming the first plug groove 7 and the second plug groove 8 , the second dielectric layer 6 is filled in the dielectric recess 51 ; after forming the second plug groove 8 , the second plug groove 8 also penetrates the second dielectric layer 6 .
[0086] By adopting the above scheme, a blocking dielectric layer is first formed on the first dielectric layer of the first region and the second region, and the thickness of the blocking dielectric layer of the first region is greater than that of the blocking dielectric layer of the second region, and then a first plug groove penetrating the first dielectric layer and the blocking dielectric layer is formed on the source-drain doped region of the first region, and a second plug groove penetrating the first dielectric layer and the blocking dielectric layer is formed on the source-drain doped region of the second region. In the process of etching to form the first plug groove and the second plug groove, since the blocking dielectric layer has a blocking effect and the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer, the etching rate of the first plug groove relative to the second plug groove can be slowed down, thereby avoiding the problem of over-fast etching when forming the first plug groove in the first region, and finally preventing the source-drain doped region of the first region from being over-etched, thereby avoiding damage to the source-drain doped region.
[0087] Based on the above-mentioned method for forming a semiconductor device, this embodiment further provides a semiconductor device, specifically, Fig.10 As shown, the semiconductor device provided in this embodiment specifically includes:
[0088] A substrate 1, wherein the substrate 1 includes a first region 11 and a second region 12;
[0089] The target gate structures are located on the substrate 1, and the spacing between the target gate structures in the first area 11 is smaller than the spacing between the target gate structures in the second area 12;
[0090] Source and drain doped regions 3 in the substrate 1 respectively located on both sides of the target gate structure;
[0091] A first dielectric layer 4 is located on the substrate 1 and covers a portion of the sidewall of the target gate structure, wherein the top surface of the first dielectric layer 4 is lower than the top surface of the target gate structure;
[0092] A blocking dielectric layer located on the first dielectric layer 4 in the first region 11 and the second region 12, wherein the thickness of the blocking dielectric layer in the first region 11 is greater than the thickness of the blocking dielectric layer in the second region 12;
[0093] A first plug trench 7 located on the source-drain doped region 3 of the first region 11 and penetrating the first dielectric layer 4 and the blocking dielectric layer;
[0094] A second plug trench 8 is located on the source-drain doped region 3 of the second region 12 and penetrates the first dielectric layer 4 and the blocking dielectric layer.
[0095] The first zone 11 is Fig.10 The left half of the region shown in FIG. 1 is a region where the spacing between the target gate structures is smaller; the second region 12 is Fig.10 The right half of the region is shown, in which the spacing between the target gate structures is larger.
[0096] In this embodiment, the target gate structure may be a dummy gate or a metal gate structure, which is not specifically limited in this embodiment.
[0097] It should be noted that, in the present embodiment, the blocking dielectric layer of the second region 12 has a dielectric recess 51, and in a direction perpendicular to the top surface of the target gate structure, the thickness of the blocking dielectric at the bottom of the dielectric recess 51 is less than the thickness of the blocking dielectric layer of the first region 11; the semiconductor device further includes: a second dielectric layer 6 located in the dielectric recess 51; and the second plug groove 8 also penetrates the second dielectric layer 6.
[0098] Preferably, the material of the second dielectric layer 6 includes: an oxide layer; the material of the first dielectric layer 4 includes: silicon oxide; and the material of the blocking dielectric layer includes silicon nitride.
[0099] It should also be noted that the dimension of the first plug trench 7 along the channel length direction of the first region 11 is smaller than the dimension of the second plug trench 8 along the channel length direction of the second region 12; the channel length at the bottom of the gate structure of the first region 11 is smaller than the channel length at the bottom of the gate structure of the second region 12.
[0100] In this embodiment, the semiconductor device further includes: a first plug located in the first plug groove 7 ; and a second plug located in the second plug groove 8 .
[0101] Preferably, in this embodiment, the base 1 includes a semiconductor substrate and a fin located on the semiconductor substrate; and the target gate structure spans across the fin.
[0102] Specifically, the material of the semiconductor substrate includes but is not limited to single crystal silicon, polycrystalline silicon, amorphous silicon, germanium silicon material, carbon silicon material, etc., which is not specifically limited in this embodiment.
[0103] The semiconductor device formed by the above scheme first forms a blocking dielectric layer on the first dielectric layer in the first region and the second region, and the thickness of the blocking dielectric layer in the first region is greater than that of the blocking dielectric layer in the second region, and then forms a first plug groove penetrating the first dielectric layer and the blocking dielectric layer on the source-drain doped region of the first region, and forms a second plug groove penetrating the first dielectric layer and the blocking dielectric layer on the source-drain doped region of the second region. In the process of etching to form the first plug groove and the second plug groove, since the blocking dielectric layer has a blocking effect and the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer, the etching rate of the first plug groove relative to the second plug groove can be slowed down, thereby avoiding the problem of over-fast etching when forming the first plug groove in the first region, and finally preventing the source-drain doped region of the first region from being over-etched, thereby avoiding damage to the source-drain doped region.
[0104] Although the present invention has been illustrated and described with reference to certain preferred embodiments of the present invention, it should be understood by those skilled in the art that the above is a further detailed description of the present invention in conjunction with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. Those skilled in the art may make various changes in form and details, including making several simple deductions or substitutions, without departing from the spirit and scope of the present invention.
Claims
1. A method for forming a semiconductor device, characterized in that: include: Providing a substrate, the substrate comprising a first region and a second region, the substrate having a gate structure, the spacing between the gate structures in the first region being smaller than the spacing between the gate structures in the second region, and the substrate having source and drain doping regions on both sides of the gate structure respectively; forming a first dielectric layer covering a portion of the sidewall of the gate structure on the substrate, wherein a top surface of the first dielectric layer is lower than a top surface of the gate structure; forming a blocking dielectric layer on the first dielectric layer in the first and second regions, wherein the thickness of the blocking dielectric layer in the first region is greater than the thickness of the blocking dielectric layer in the second region; A first plug trench penetrating the first dielectric layer and the blocking dielectric layer is formed on the source / drain doped region of the first region. During the process of forming the first plug trench, a second plug trench penetrating the first dielectric layer and the blocking dielectric layer is formed on the source / drain doped region of the second region, wherein the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer.
2. The method for forming a semiconductor device according to claim 1, wherein: The method for forming the first dielectric layer includes: forming a first initial dielectric layer covering the entire side wall of the gate structure on the substrate; etching back the first initial dielectric layer to form a first dielectric layer.
3. The method for forming a semiconductor device according to claim 1, wherein: The blocking dielectric layer in the second region has a dielectric recess, and in a direction perpendicular to the top surface of the gate structure, the thickness of the blocking dielectric layer at the bottom of the dielectric recess is less than the thickness of the blocking dielectric layer in the first region; The method for forming a semiconductor device further includes: before forming the first plug trench and the second plug trench, filling a second dielectric layer in the dielectric recess; After the second plug trench is formed, the second plug trench also penetrates the second dielectric layer.
4. The method for forming a semiconductor device according to claim 3, wherein: The method for forming the blocking dielectric layer and the second dielectric layer comprises: forming a blocking material layer on the sidewall and top of the gate structure in the first region, the surface of the first dielectric layer in the first region, the sidewall and top of the gate structure in the second region, and the surface of the first dielectric layer in the second region, wherein the blocking material layer in the first region has a first recess located on the first dielectric layer, and the blocking material layer in the second region has a second recess located on the first dielectric layer, and the thickness of the blocking material layer at the bottom of the first recess is greater than the thickness of the blocking material layer in the second recess; forming a second dielectric material layer in the first recess, the second recess, and on the blocking material layer; flattening the second dielectric material layer and the blocking material layer until the top surface of the gate structure is exposed, so that the blocking material layer forms the blocking dielectric layer, the second dielectric material layer forms the second dielectric layer, and the second recess forms a dielectric recess located in the blocking dielectric layer.
5. The method for forming a semiconductor device according to claim 4, wherein: The barrier material layer is formed by an atomic layer deposition process; the second dielectric material layer is formed by a fluid chemical vapor deposition process or a plasma chemical vapor deposition process.
6. The method for forming a semiconductor device according to claim 3, wherein: In a direction perpendicular to the top surface of the gate structure, a ratio of a thickness of the blocking dielectric layer in the first region to a thickness of the blocking dielectric layer at the bottom of the dielectric recess is 1.4 to 2.
2.
7. The method for forming a semiconductor device according to claim 3, wherein: The material of the second dielectric layer includes silicon oxide.
8. The method for forming a semiconductor device according to claim 3, wherein: The process of forming the first plug trench and the second plug trench is an etching process; in the process of forming the first plug trench and the second plug trench, the etching rate of the second dielectric layer is greater than the etching rate of the blocking dielectric layer.
9. The method for forming a semiconductor device according to claim 1, wherein: During the formation of the first plug trench and the second plug trench, the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer; the ratio of the etching rate of the first dielectric layer to the etching rate of the blocking dielectric layer is 10 to 100.
10. The method for forming a semiconductor device according to claim 1, wherein: The material of the first dielectric layer includes silicon oxide; the material of the blocking dielectric layer includes silicon nitride.
11. The method for forming a semiconductor device according to claim 1, wherein: A dimension of the first plug trench along a channel length direction of the first region is smaller than a dimension of the second plug trench along a channel length direction of the second region.
12. The method for forming a semiconductor device according to claim 1, wherein: The channel length of the bottom of the gate structure in the first region is smaller than the channel length of the bottom of the gate structure in the second region.
13. The method for forming a semiconductor device according to claim 1, wherein: Also includes: After forming the blocking dielectric layer and before forming the first plug trench and the second plug trench, the gate structure is removed to form a gate opening in the first dielectric layer and the blocking dielectric layer; a metal gate structure is formed in the gate opening, and the spacing between the metal gate structures in the first region is smaller than the spacing between the metal gate structures in the second region.
14. A semiconductor device, characterized in that: include: a substrate comprising a first region and a second region; a target gate structure located on the substrate, wherein a spacing between the target gate structures in the first region is smaller than a spacing between the target gate structures in the second region; Source and drain doped regions in the substrate respectively located on both sides of the target gate structure; a first dielectric layer located on the substrate and covering a portion of the sidewall of the target gate structure, wherein a top surface of the first dielectric layer is lower than a top surface of the target gate structure; a blocking dielectric layer located on the first dielectric layer in the first and second regions, wherein the thickness of the blocking dielectric layer in the first region is greater than the thickness of the blocking dielectric layer in the second region; A first plug trench located on the source-drain doped region of the first region and penetrating the first dielectric layer and the blocking dielectric layer; A second plug trench is located on the source-drain doped region of the second region and penetrates the first dielectric layer and the blocking dielectric layer, wherein the etching rate of the blocking dielectric layer is lower than the etching rate of the first dielectric layer.
15. The semiconductor device according to claim 14, wherein: The blocking dielectric layer in the second region has a dielectric recess, and in a direction perpendicular to the top surface of the target gate structure, the thickness of the blocking dielectric at the bottom of the dielectric recess is less than the thickness of the blocking dielectric layer in the first region; the semiconductor device also includes: a second dielectric layer located in the dielectric recess; and the second plug groove also penetrates the second dielectric layer.
16. The semiconductor device according to claim 15, wherein: The material of the second dielectric layer includes silicon oxide; the material of the first dielectric layer includes silicon oxide; and the material of the blocking dielectric layer includes silicon nitride.
17. The semiconductor device according to claim 14, wherein: A dimension of the first plug trench along a channel length direction of the first region is smaller than a dimension of the second plug trench along a channel length direction of the second region.
18. The semiconductor device according to claim 14, wherein: A channel length at a bottom of the target gate structure in the first region is smaller than a channel length at a bottom of the target gate structure in the second region.
19. The semiconductor device according to claim 14, wherein: Also includes: a first plug located in the first plug slot; A second plug is positioned in the second plug slot.
20. The semiconductor device according to claim 14, wherein The base includes a semiconductor substrate and a fin located on the semiconductor substrate; the target gate structure spans across the fin.