Method for removing thermal barrier coating in air film hole
The use of chemical etchant to remove the thermal barrier coating in the air membrane hole of the turbine blades by spraying or brushing methods, solving the problems of degraded cooling performance of the turbine blades and substrate damage, achieving efficient and accurate coating removal and protection.
Patent Information
- Application Number
- CN202411120770.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to effectively remove the thermal barrier coating in the air membrane pore of the turbine blade, resulting in a degradation of cooling performance and the high-temperature alloy matrix and metal bonded bottom layer are easily damaged.
Use chemical etchants to remove thermal barrier coatings, including hydrofluoric acid, nitric acid, dilute sulfuric acid, surfactant, corrosion inhibitor and stabilizer. After neutralization, clean with ultrapure water to ensure fine etching and protect substrate.
The rapid and efficient removal of thermal barrier coatings is achieved, ensuring the cooling performance and structural integrity of the turbine blades, and avoiding over-etching and substrate damage by traditional mechanical methods.
Smart Images

Figure CN118996420A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of thermal barrier coating removal of turbine blades, and specifically discloses a method for removing thermal barrier coating in air film holes. Background Art
[0002] The turbine blades of an engine are key parts that enable the engine to achieve a thermal cycle. During the operation of the engine, as the temperature before the turbine continues to rise, and due to the uneven temperature field in the engine combustion chamber and the limitations of the high temperature resistance of the turbine blade material itself, the cooling of the blade itself is the key to solving the high temperature resistance problem. The current method to improve the cooling performance of the blade itself is to process a number of cooling air film holes on one side of the blade body to achieve air film cooling and reduce the blade temperature.
[0003] The thermal barrier coating of turbine blades has a harsh service environment. It is easy to peel off under the influence of high temperature and high speed gas, high stress, high corrosion, alternating load, hot and cold cycle shock, etc., resulting in coating failure. As a key component of aircraft engines, turbine blades have a complex structure and use precision casting technology. The manufacturing cycle is long, the process is complex and difficult, and the part qualification rate is low. Repairing the engine by replacing new parts is bound to result in excessive costs and increase the production pressure of on-site batch production of parts. If the coating of the blades with failed coating is removed and re-coated so that it can be used again, the production cycle can be shortened and the manufacturing cost can be reduced.
[0004] During the process of re-coating the thermal barrier coating on the turbine blades, the coating is inevitably deposited on the inner surface of the air film hole, resulting in a decrease in the diameter of the air film hole. Since the diameter of the air film hole (cross-sectional area) directly determines the flow rate of the cooling medium, it affects the air film cooling drop of the turbine blade. Therefore, it is necessary to clean the thermal barrier coating in the air film hole. At present, the main methods for removing the ceramic surface layer of the thermal barrier coating are dry sand blowing method and high-pressure water method. The above method is difficult to control the thickness of the coating removed, resulting in insufficient wall thickness of the turbine blade and easy damage to the high-temperature alloy substrate and the metal bonding bottom layer. Summary of the invention
[0005] In view of the above problems, the present invention discloses a method for removing thermal barrier coating in air film holes.
[0006] The purpose of the present invention is achieved through the following technical solutions.
[0007] A method for removing a thermal barrier coating in an air film hole, wherein the thermal barrier coating in the air film hole is attached to a titanium alloy material, and is removed by spraying a chemical etchant by spraying or brushing, and then a neutralizer is sprayed by spraying or brushing, and then rinsed with ultrapure water after the neutralization reaction is complete;
[0008] The chemical etchant comprises the following raw materials by weight:
[0009]
[0010] The thermal barrier coating consists of an upper ceramic heat-insulating layer and a lower metal bonding layer. The ceramic heat-insulating layer material contains Y2O3-stabilized ZrO2; and the metal bonding layer contains MCrAlY alloy.
[0011] Furthermore, in the above method for removing thermal barrier coating in air film pores, the hydrofluoric acid concentration in the hydrofluoric acid aqueous solution is 30-35wt%, the concentration of concentrated nitric acid is 8-10M, and the concentration of dilute sulfuric acid is 0.5-1.5M.
[0012] Furthermore, in the above method for removing thermal barrier coating in air film pores, the surfactant is selected from Triton-X-100.
[0013] Furthermore, in the above method for removing thermal barrier coating in air film pores, the corrosion inhibitor is selected from complex salts.
[0014] Furthermore, in the above method for removing thermal barrier coating in air film pores, the stabilizer is selected from sodium sulfonate.
[0015] Furthermore, in the above method for removing thermal barrier coating in air film pores, the neutralizing agent is an aqueous solution of sodium hydroxide and sodium carbonate, the concentration of the sodium hydroxide is 2-3M, and the concentration of the sodium carbonate is 0.5-1M.
[0016] Furthermore, the above method for removing thermal barrier coating in air film holes,
[0017] The chemical etchant is prepared by the following method:
[0018] First, slowly add hydrofluoric acid aqueous solution into a corrosion-resistant reaction vessel. Since hydrofluoric acid is highly volatile and toxic, equipment with good sealing and exhaust systems should be used;
[0019] Under stirring, gradually add nitric acid and sulfuric acid. Both acids are strong acids and may generate heat when mixed. Therefore, it is necessary to control the addition speed and stirring intensity to avoid local overheating.
[0020] Then, add hydrogen peroxide, surfactant and corrosion inhibitor in sequence. Each additive should be fully stirred before adding the next one to ensure that each component is evenly distributed.
[0021] Finally, stabilizers are added to complete the solution.
[0022] Furthermore, the above method for removing the thermal barrier coating in the air film hole comprises the following steps:
[0023] (1) Pre-treatment:
[0024] Check the size, shape and position of the air film holes before processing to ensure that the state of the air film holes before processing meets the processing requirements. Clean the air film holes and surrounding areas to remove oil, dust and other impurities on the surface to improve the etching effect.
[0025] (2) Chemical etching:
[0026] Chemical etching is applied by spray or brush, including:
[0027] Spray method: Use a spray device to evenly spray the chemical etchant on the air film hole area to ensure that the etchant can fully cover and penetrate into the hole;
[0028] Or brushing method: Use a brush to apply the etchant to the inner wall of the air film hole to ensure that the coating is in full contact with the etchant;
[0029] Closely monitor the etching process and control parameters such as etching time and temperature to avoid over-etching or under-etching; check the status of the air film holes every 10-20 minutes and observe the coating removal using a microscope;
[0030] (3) Spraying neutralizer;
[0031] Neutralizers can be applied by spray or brush, including:
[0032] Spray method: Use a spray device to evenly spray the neutralizer on the air film hole area;
[0033] Or brushing method: Use a brush to brush the neutralizer on the inner wall of the air film hole to ensure that the coating is in full contact with the neutralizer;
[0034] Neutralization reaction 1-2h,
[0035] (4) Cleaning and post-processing
[0036] After neutralization, rinse the parts thoroughly with ultrapure water to remove residual etchant and etching products, and dry the parts.
[0037] Furthermore, the present invention also discloses the use of the above method for removing thermal barrier coating in air film holes in the maintenance of engine turbine blades.
[0038] Preferably, the above-mentioned engine is an aircraft engine.
[0039] Compared with the existing technology, the present invention has the following advantages and beneficial effects:
[0040] The present invention discloses a method for removing thermal barrier coating in air film holes, which is a specially designed formula and method for double-layer thermal barrier coating attached to titanium alloy material. Hydrofluoric acid in the formula is one of the strong acids and has strong corrosiveness to silicate materials such as glass and ceramics. During the etching process, it can penetrate and dissolve the surface layer of these materials to achieve a fine etching effect. In particular, in glass wet chemical etching, hydrofluoric acid reacts with silicon dioxide in the glass through its corrosiveness and permeability to achieve the purpose of etching. The addition of hydrofluoric acid can also work synergistically with other acidic components to improve the etching efficiency and stability of the entire system. Nitric acid has strong oxidizing properties and can convert the surface layer of the target material into soluble salts or other oxides, thereby accelerating the etching process. The etching speed and depth can be controlled by adjusting the concentration and temperature of nitric acid to meet different etching requirements. Sulfuric acid, as a strong acid, can adjust the pH value of the etching solution to keep it within a range suitable for the etching reaction. Although dilute sulfuric acid itself does not directly react with hydrofluoric acid, it can play an auxiliary role in the mixed system to improve the etching efficiency and improve the etching surface quality. The hydrogen peroxide oxidizing agent in the formula has good cleaning performance, which can remove impurities and residues generated during the etching process and maintain the cleanliness of the etching surface. The surfactant in the formula can improve the homogenization performance of the etching solution and ensure the stability and consistency of the etching quality. The corrosion inhibitor in the formula can form a complex with the metal ions in the reagent or adsorb on the metal surface to form a protective film, thereby slowing down the etching rate and preventing quality problems caused by excessive etching. The addition of the stabilizer in this formula can keep the etching solution stable in performance and composition during storage and use, and prevent the etching effect from decreasing due to decomposition or precipitation of the components.
[0041] In summary, the present invention uses chemical etchants by spraying or brushing to quickly and effectively remove thermal barrier coatings attached to titanium alloy materials. This method is more efficient than traditional mechanical methods, especially when dealing with air film holes of complex shapes. Compared with mechanical methods, by closely monitoring the etching process and controlling parameters such as etching time and temperature, it can ensure that only the target coating is removed without damaging the substrate, achieving precise control. This helps maintain the integrity and performance of the turbine blades. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a comparison chart of etching time (min) in the test examples. DETAILED DESCRIPTION
[0043] A method for removing a thermal barrier coating in an air film hole, wherein the thermal barrier coating in the air film hole is attached to a titanium alloy material, and is removed by spraying a chemical etchant by spraying or brushing, and then a neutralizer is sprayed by spraying or brushing, and then rinsed with ultrapure water after the neutralization reaction is complete;
[0044] The chemical etchant comprises the following raw materials by weight:
[0045]
[0046]
[0047] The thermal barrier coating is composed of an upper ceramic insulation layer and a lower metal bonding layer, wherein the ceramic insulation layer material contains Y2O3-stabilized ZrO2; and the metal bonding layer contains MCrAlY alloy;
[0048] The hydrofluoric acid aqueous solution has a hydrofluoric acid concentration of 30-35 wt %, a concentrated nitric acid concentration of 8-10 M, and a dilute sulfuric acid concentration of 0.5-1.5 M;
[0049] The surfactant is selected from Triton-X-100;
[0050] The corrosion inhibitor is selected from magnesium chromate;
[0051] The stabilizer is selected from sodium sulfonate;
[0052] The neutralizing agent is sodium hydroxide and sodium carbonate aqueous solution, the concentration of the sodium hydroxide is 2-3M, and the concentration of the sodium carbonate is 0.5-1M.
[0053] The chemical etchant is prepared by the following method:
[0054] First, slowly add hydrofluoric acid aqueous solution into a corrosion-resistant reaction vessel. Since hydrofluoric acid is highly volatile and toxic, equipment with good sealing and exhaust systems should be used;
[0055] Under stirring, gradually add nitric acid and sulfuric acid. Both acids are strong acids and may generate heat when mixed. Therefore, it is necessary to control the addition speed and stirring intensity to avoid local overheating.
[0056] Then, add hydrogen peroxide, surfactant and corrosion inhibitor in sequence. Each additive should be fully stirred before adding the next one to ensure that each component is evenly distributed.
[0057] Finally, stabilizers are added to complete the solution.
[0058] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0059] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0060] Example 1
[0061] A method for removing a thermal barrier coating in an air film hole, wherein the thermal barrier coating in the air film hole is attached to a titanium alloy material, and is removed by spraying a chemical etchant by spraying or brushing, and then a neutralizer is sprayed by spraying or brushing, and then rinsed with ultrapure water after the neutralization reaction is complete;
[0062] The chemical etchant comprises the following raw materials by weight:
[0063]
[0064] The thermal barrier coating is composed of an upper ceramic insulation layer and a lower metal bonding layer, wherein the ceramic insulation layer material contains Y2O3-stabilized ZrO2; and the metal bonding layer contains MCrAlY alloy;
[0065] The hydrofluoric acid aqueous solution has a hydrofluoric acid concentration of 30 wt %, a concentrated nitric acid concentration of 8 M, and a dilute sulfuric acid concentration of 0.5 M;
[0066] The surfactant is selected from Triton-X-100;
[0067] The corrosion inhibitor is selected from magnesium chromate;
[0068] The stabilizer is selected from sodium sulfonate;
[0069] The neutralizing agent is sodium hydroxide and sodium carbonate aqueous solution, the concentration of the sodium hydroxide is 2M, and the concentration of the sodium carbonate is 0.5M.
[0070] The chemical etchant is prepared by the following method:
[0071] First, slowly add hydrofluoric acid aqueous solution into a corrosion-resistant reaction vessel. Since hydrofluoric acid is highly volatile and toxic, equipment with good sealing and exhaust systems should be used;
[0072] Under stirring, gradually add nitric acid and sulfuric acid. Both acids are strong acids and may generate heat when mixed. Therefore, it is necessary to control the addition speed and stirring intensity to avoid local overheating.
[0073] Then, add hydrogen peroxide, surfactant and corrosion inhibitor in sequence. Each additive should be fully stirred before adding the next one to ensure that each component is evenly distributed.
[0074] Finally, stabilizers are added to complete the solution.
[0075] Example 2
[0076] A method for removing a thermal barrier coating in an air film hole, wherein the thermal barrier coating in the air film hole is attached to a titanium alloy material, and is removed by spraying a chemical etchant by spraying or brushing, and then a neutralizer is sprayed by spraying or brushing, and then rinsed with ultrapure water after the neutralization reaction is complete;
[0077] The chemical etchant comprises the following raw materials by weight:
[0078]
[0079] The thermal barrier coating is composed of an upper ceramic insulation layer and a lower metal bonding layer, wherein the ceramic insulation layer material contains Y2O3-stabilized ZrO2; and the metal bonding layer contains MCrAlY alloy;
[0080] The hydrofluoric acid aqueous solution has a hydrofluoric acid concentration of 33 wt %, a concentrated nitric acid concentration of 9 M, and a dilute sulfuric acid concentration of 1 M;
[0081] The surfactant is selected from Triton-X-100;
[0082] The corrosion inhibitor is selected from magnesium chromate;
[0083] The stabilizer is selected from sodium sulfonate;
[0084] The neutralizing agent is sodium hydroxide and sodium carbonate aqueous solution, the concentration of the sodium hydroxide is 2.5M, and the concentration of the sodium carbonate is 0.75M.
[0085] The chemical etchant is prepared by the following method:
[0086] First, slowly add hydrofluoric acid aqueous solution into a corrosion-resistant reaction vessel. Since hydrofluoric acid is highly volatile and toxic, equipment with good sealing and exhaust systems should be used;
[0087] Under stirring, gradually add nitric acid and sulfuric acid. Both acids are strong acids and may generate heat when mixed. Therefore, it is necessary to control the addition speed and stirring intensity to avoid local overheating.
[0088] Then, add hydrogen peroxide, surfactant and corrosion inhibitor in sequence. Each additive should be fully stirred before adding the next one to ensure that each component is evenly distributed.
[0089] Finally, stabilizers are added to complete the solution.
[0090] Example 3
[0091] A method for removing a thermal barrier coating in an air film hole, wherein the thermal barrier coating in the air film hole is attached to a titanium alloy material, and is removed by spraying a chemical etchant by spraying or brushing, and then a neutralizer is sprayed by spraying or brushing, and then rinsed with ultrapure water after the neutralization reaction is complete;
[0092] The chemical etchant comprises the following raw materials by weight:
[0093]
[0094] The thermal barrier coating is composed of an upper ceramic insulation layer and a lower metal bonding layer, wherein the ceramic insulation layer material contains Y2O3-stabilized ZrO2; and the metal bonding layer contains MCrAlY alloy;
[0095] The hydrofluoric acid aqueous solution has a hydrofluoric acid concentration of 35 wt %, a concentrated nitric acid concentration of 10 M, and a dilute sulfuric acid concentration of 1.5 M;
[0096] The surfactant is selected from Triton-X-100;
[0097] The corrosion inhibitor is selected from magnesium chromate;
[0098] The stabilizer is selected from sodium sulfonate;
[0099] The neutralizing agent is sodium hydroxide and sodium carbonate aqueous solution, the concentration of the sodium hydroxide is 3M, and the concentration of the sodium carbonate is 1M.
[0100] The chemical etchant is prepared by the following method:
[0101] First, slowly add hydrofluoric acid aqueous solution into a corrosion-resistant reaction vessel. Since hydrofluoric acid is highly volatile and toxic, equipment with good sealing and exhaust systems should be used;
[0102] Under stirring, gradually add nitric acid and sulfuric acid. Both acids are strong acids and may generate heat when mixed. Therefore, it is necessary to control the addition speed and stirring intensity to avoid local overheating.
[0103] Then, add hydrogen peroxide, surfactant and corrosion inhibitor in sequence. Each additive should be fully stirred before adding the next one to ensure that each component is evenly distributed.
[0104] Finally, stabilizers are added to complete the solution.
[0105] Comparative Example 1
[0106] Concentrated nitric acid and dilute sulfuric acid are not contained, and the rest is the same as in Example 2.
[0107] Comparative Example 2
[0108] Concentrated nitric acid is not contained, and the rest is the same as in Example 2.
[0109] Comparative Example 3
[0110] The dilute sulfuric acid is not contained, and the rest is the same as in Example 2.
[0111] Test Case
[0112] After a thermal barrier coating was sprayed on the surface of a turbine blade of an aircraft engine by electron beam physical vapor deposition (EB-PVD), the coating was deposited in the film pores, the aperture of the blade film pores was reduced from 0.55 mm to 0.38 mm, and the aperture shape of the film pores changed; the thermal barrier coating consisted of an upper ceramic insulation layer and a lower metal bonding layer, the ceramic insulation layer material contained Y2O3-stabilized ZrO2; the metal bonding layer contained MCrAlY alloy; the blade was made of titanium alloy.
[0113] Using Examples 1-3 and Comparative Examples 1-3 discloses a chemical etchant for cleaning, comprising the following steps:
[0114] (1) Pre-treatment:
[0115] Check the size, shape and position of the air film holes before processing to ensure that the state of the air film holes before processing meets the processing requirements. Clean the air film holes and surrounding areas to remove oil, dust and other impurities on the surface to improve the etching effect.
[0116] (2) Chemical etching:
[0117] Chemical etching using aerosol spraying, including:
[0118] Spray method: Use a spray device to evenly spray the chemical etchant on the air film hole area to ensure that the etchant can fully cover and penetrate into the hole;
[0119] Closely monitor the etching process and control parameters such as etching time and temperature to avoid over-etching or under-etching; check the status of the air film holes every 10-20 minutes and observe the coating removal using a microscope;
[0120] (3) Spraying neutralizer;
[0121] Neutralizers can be applied by spray or brush, including:
[0122] Spray method: Use a spray device to evenly spray the neutralizer on the air film hole area;
[0123] Or brushing method: Use a brush to brush the neutralizer on the inner wall of the air film hole to ensure that the coating is in full contact with the neutralizer;
[0124] Neutralization reaction 1.5h,
[0125] (4) Cleaning and post-processing
[0126] After neutralization, rinse the parts thoroughly with ultrapure water to remove residual etchant and etching products, and dry the parts.
[0127] The test results of step (2) chemical etching completion time and the internal conditions of the air film hole are shown in Tables 1 and Figure 1 As shown:
[0128] Table 1 Thermal barrier coating removal status.
[0129] Etching time (min) Internal situation of air film hole Example 1 30 smooth Example 2 20 smooth Example 3 20 smooth Comparative Example 1 90 Rough Comparative Example 2 80 Rough Comparative Example 3 70 Rough
[0130] It can be seen from Table 1 above that when the thermal barrier coating is composed of an upper ceramic insulation layer and a lower metal bonding layer, the ceramic insulation layer material contains Y2O3-stabilized ZrO2; the metal bonding layer contains MCrAlY alloy; and the blade is made of titanium alloy, the etching can be completed within 70 minutes using Examples 1-3 of the chemical etchant disclosed in the present invention, and 0.17 mm of the thermal barrier coating can be removed, which greatly saves time compared to Comparative Examples 1-3. At the same time, when a combination of hydrofluoric acid, nitric acid and sulfuric acid is used, a smooth effect is also achieved inside the air film pores, reflecting that the combination of the above acids can remove the thermal barrier coating more thoroughly without damaging the bottom titanium metal layer.
[0131] As can be seen from the above examples, thermal barrier coatings attached to titanium alloy materials can be removed quickly and effectively. This method is more efficient than traditional mechanical methods, especially when dealing with complex-shaped air film holes. Compared with mechanical methods, by closely monitoring the etching process and controlling parameters such as etching time and temperature, it can be ensured that only the target coating is removed without damaging the substrate, achieving precise control. This helps maintain the integrity and performance of the turbine blades.
[0132] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Therefore, based on the innovative concept of the present invention, changes and modifications to the embodiments described herein, or equivalent structural or equivalent process transformations made using the contents of the specification and drawings of the present invention, directly or indirectly applying the above technical solutions to other related technical fields are all included in the protection scope of the patent of the present invention.
Claims
1. A method for removing thermal barrier coating in air film pores, characterized in that: The thermal barrier coating in the air film hole is attached to the titanium alloy material, and is removed by spraying a chemical etchant by spraying or brushing. After removal, a neutralizer is sprayed by spraying or brushing, and then rinsed with ultrapure water after the neutralization reaction is complete; The chemical etchant comprises the following raw materials by weight: The thermal barrier coating consists of an upper ceramic heat-insulating layer and a lower metal bonding layer. The ceramic heat-insulating layer material contains Y2O3-stabilized ZrO2; and the metal bonding layer contains MCrAlY alloy.
2. The method for removing thermal barrier coating in air film pores according to claim 1, characterized in that: The hydrofluoric acid aqueous solution has a hydrofluoric acid concentration of 30-35 wt %, a concentrated nitric acid concentration of 8-10 M, and a dilute sulfuric acid concentration of 0.5-1.5 M.
3. The method for removing thermal barrier coating in air film pores according to claim 1, characterized in that: The surfactant is selected from Triton-X-100.
4. The method for removing thermal barrier coating in air film pores according to claim 1, characterized in that: The corrosion inhibitor is selected from complex salts.
5. The method for removing thermal barrier coating in air film pores according to claim 1, characterized in that: The stabilizer is selected from sodium sulfonate.
6. The method for removing thermal barrier coating in air film pores according to claim 1, characterized in that: The neutralizing agent is sodium hydroxide and sodium carbonate aqueous solution, the concentration of the sodium hydroxide is 2-3M, and the concentration of the sodium carbonate is 0.5-1M.
7. The method for removing thermal barrier coating in air film pores according to claim 1, characterized in that: The chemical etchant is prepared by the following method: First, slowly add hydrofluoric acid aqueous solution into a corrosion-resistant reaction vessel. Since hydrofluoric acid is highly volatile and toxic, equipment with good sealing and exhaust systems should be used; Under stirring, gradually add nitric acid and sulfuric acid. Both acids are strong acids and may generate heat when mixed. Therefore, it is necessary to control the addition speed and stirring intensity to avoid local overheating. Then, add hydrogen peroxide, surfactant and corrosion inhibitor in sequence. Each additive should be fully stirred before adding the next one to ensure that each component is evenly distributed. Finally, stabilizers are added to complete the solution.
8. The method for removing thermal barrier coating in air film pores according to claim 1, characterized in that: The following steps are involved: (1) Pre-treatment: Check the size, shape and position of the air film holes before processing to ensure that the state of the air film holes before processing meets the processing requirements. Clean the air film holes and surrounding areas to remove oil, dust and other impurities on the surface to improve the etching effect. (2) Chemical etching: Chemical etching is applied by spray or brush, including: Spray method: Use a spray device to evenly spray the chemical etchant on the air film hole area to ensure that the etchant can fully cover and penetrate into the hole; Or brushing method: Use a brush to apply the etchant to the inner wall of the air film hole to ensure that the coating is in full contact with the etchant; Closely monitor the etching process and control parameters such as etching time and temperature to avoid over-etching or under-etching; check the status of the air film holes every 10-20 minutes and observe the coating removal using a microscope; (3) Spraying neutralizer; Neutralizers can be applied by spray or brush, including: Spray method: Use a spray device to evenly spray the neutralizer on the air film hole area; Or brushing method: Use a brush to brush the neutralizer on the inner wall of the air film hole to ensure that the coating is in full contact with the neutralizer; Neutralization reaction 1-2h, (4) Cleaning and post-processing After neutralization, rinse the parts thoroughly with ultrapure water to remove residual etchant and etching products, and dry the parts.
9. Use of the method for removing thermal barrier coating in air film holes as claimed in claims 1 to 8 in the maintenance of engine turbine blades.
10. The use according to claim 9, wherein the engine is an aircraft engine.