A method for preparing single crystal BaTiO3

The method of preparing single-crystal BaTiO3 using polycrystalline ceramic rods in the optical floating zone solves the problems of long preparation cycle and seed crystal dependence in the existing technology, and achieves efficient single crystal growth and shortened sample cycle.

CN113186593BActive Publication Date: 2024-11-19XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110288424.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-11-19
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Existing technologies for preparing single-crystal BaTiO3 ferroelectric materials suffer from long preparation cycles and the need for additional seed crystals, which limit the efficiency and flexibility of single-crystal growth.

Method used

The single-crystal growth of polycrystalline ceramic rods was carried out using the optical floating zone single-crystal method. The process involved grinding, pre-firing, granulation, pressing, sintering, single-crystal growth, and secondary sintering to prepare a high-efficiency single-crystal BaTiO3 sample.

Benefits of technology

It breaks through the limitations of crucible preparation, has a fast growth rate, significantly shortens the sample cycle, and does not require additional seed crystals, thus achieving efficient preparation of single-crystal BaTiO3.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113186593B_ABST
    Figure CN113186593B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing single crystal BaTiO3, which relates to the technical field of ferroelectric ceramic preparation, and comprises the following steps: S100, grinding BaTiO3 and TiO2 powders once and then pre-sintering, grinding them twice and granulating them to obtain granules; S200, pressing the granules into tablets and sintering them into material rods; S300, performing single crystal growth on the material rods to obtain samples; S400, sintering the samples twice. The invention provides a reference for the method for preparing single crystal BaTiO3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic preparation, and in particular to a method for preparing single crystal BaTiO3. Background Art

[0002] At present, based on the excellent electrical properties and scalability of ferroelectric materials, their application prospects are becoming increasingly broad, and they are also one of the frontiers and hotspots of current high-tech research. The reasons can be summarized as dielectric properties, ferroelectric switching effect, piezoelectric effect, pyroelectric effect, electro-optic effect, acousto-optic effect, photorefractive effect and nonlinear optical effect. This material can use the above effects alone to make components with different functions, or use several different effects to prepare multifunctional devices and highly integrate them, which has inspired countless scientific researchers to conduct research one after another.

[0003] High-performance ferroelectric materials are a type of functional materials with broad application prospects, but current research is still in the early development stage of ferroelectric high-performance material research. Researchers are conducting research and exploration from two aspects. One is to select different material systems for research, and the other is to explore different preparation processes. So far, high-performance ferroelectric material systems have achieved initial results. Based on these material systems, thin film and single crystal have become an important research direction for improving the performance of ferroelectric materials.

[0004] Compared with other methods of pulling single crystals, the optical floating zone single crystal method for preparing barium titanate single crystals has broken through the preparation limitations of the crucible. The two ceramic crystal rods used in the preparation process are polycrystalline samples, and no additional seed crystals are required for single crystal growth. In addition, the growth rate of single crystals prepared by this method is relatively fast. The sample preparation cycle depends on the sample size. The basic growth rate is 2-10mm / h, which greatly shortens the sample preparation cycle compared to other methods. Summary of the invention

[0005] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a method for preparing single-crystalline BaTiO3, which proposes an important direction for the research on single crystalization of BaTiO3.

[0006] To achieve the above object, the present invention provides a method for preparing single crystal BaTiO3, characterized in that the method comprises the following steps:

[0007] S100, grinding BaTiO3 and TiO2 powders once, pre-calcining, grinding them again, and granulating them to obtain pellets;

[0008] S200, pressing the pellets into tablets and sintering them into rods;

[0009] S300, growing the material rod by using an optical floating zone single crystal method to obtain a sample;

[0010] S400, sintering the sample for a second time.

[0011] The present invention also provides an application of the single crystal BaTiO3 prepared by the preparation method in a piezoelectric device, wherein the piezoelectric device includes any one of the following: a piezoelectric ultrasonic motor, a piezoelectric transformer, and a piezoelectric transducer.

[0012] The present invention provides a reference direction for the preparation of single crystal BaTiO3.

[0013] Compared with the prior art, the present invention has the following advantages:

[0014] (1) Compared with other methods for preparing single crystals by pulling, the optical floating zone single crystal method used in the present invention to prepare barium titanate single crystals breaks through the preparation limitation of crucibles, and the two ceramic crystal rods used in the preparation process are polycrystalline samples, and no additional seed crystals are required for single crystal growth;

[0015] (2) The growth rate of single crystals prepared by the method of the present invention is relatively fast. The sample preparation cycle depends on the sample size. The basic growth rate is 2-10 mm / h, which is significantly shortened compared with other methods.

[0016] The concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, characteristics and effects of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of preparing single crystal BaTiO3 using an optical floating zone single crystal furnace;

[0018] Figure 2 This is the X-ray diffraction pattern of the BaTiO3 tetragonal ferroelectric polycrystal before growth;

[0019] Figure 3 It is the X-ray diffraction pattern measured by cutting the BaTiO3 single crystal sample horizontally;

[0020] Figure 4 It is the X-ray diffraction pattern measured by cutting a BaTiO3 single crystal sample longitudinally. DETAILED DESCRIPTION

[0021] The following reference manual is attached Figures 1 to 4 The present invention is described in detail in order to make its technical contents clearer and easier to understand. The present invention can be embodied in many different forms of embodiments, and the protection scope of the present invention is not limited to the embodiments mentioned in the text.

[0022] In the drawings, components with the same structure are indicated by the same numerical reference numerals, and components with similar structures or functions are indicated by similar numerical reference numerals. The size and thickness of each component shown in the drawings are arbitrarily shown, and the present invention does not limit the size and thickness of each component. In order to make the illustration clearer, the thickness of the components is appropriately exaggerated in some places in the drawings.

[0023] The present invention provides a method for preparing single crystal BaTiO3, comprising the following steps:

[0024] S100, grinding BaTiO3 and TiO2 powders once and then pre-burning, grinding them twice and granulating them to obtain pellets; wherein the first grinding time is 5-8h, the pre-burning temperature is 1200-1400°C, the pre-burning time is 6-8h, and the second grinding time is 8-10h;

[0025] S200, pressing the granules into tablets and sintering them into rods; wherein the pressing includes placing the granules into a material column bag and pressing them tightly, then placing the material column bag into a water medium hydraulic pipe and pressing it at a pressure of 15-20 MPa for 2-5 minutes to obtain a rod, and placing the rod in a muffle furnace and setting the temperature to 1450-1500° C. and sintering for 6-10 hours;

[0026] S300, growing a single crystal from the material rod to obtain a sample; wherein the schematic diagram of growing a single crystal from the material rod in a single crystal furnace in an optical floating zone is as shown in Figure 1 As shown in the figure, 2 and 8 are two material rods to be prepared placed one above the other. At this time, material rod 2 and material rod 8 are polycrystalline samples, quartz tube 4 provides space for preparing single crystal samples, 3 is the gas atmosphere provided in quartz tube 4 for preparing single crystal samples, halogen lamp 6 provides the required energy for the entire sample preparation process, and the gold-plated concave mirror 5 concentrates the light energy emitted by the halogen lamp 6 into the melting zone 7. The upper rotating rod 1 carries material rod 2, and the lower rotating rod 9 carries material rod 8. Material rod 2 and material rod 8 are rotated in the same direction or in the opposite direction and directed to grow single crystal samples upward or downward. Among them, the conditions for single crystal growth of material rod 2 and material rod 8 in the optical floating zone single crystal furnace are 55-57W, relative rotation speed 20-30r / min, and growth rate 2-5mm / h to obtain single crystal samples.

[0027] S400, sintering the single crystal sample again, wherein the secondary sintering temperature is 1600-1650° C., and the sintering time is 8-10 hours.

[0028] The specific implementation of the preparation method of the present invention is described below in conjunction with specific examples.

[0029] Example 1

[0030] A method for preparing single crystal BaTiO3 comprises the following steps:

[0031] S100, grinding BaTiO3 and TiO2 powders once, pre-calcining, grinding them again, and granulating them to obtain pellets;

[0032] Among them, the first grinding time is 5h, the pre-burning temperature is 1200℃, the pre-burning time is 8h, and the second grinding time is 8h;

[0033] S200, pressing the pellets into tablets and sintering them into rods;

[0034] The tableting process includes placing the pellets into a material column bag and pressing them tightly, then placing the material column bag into a water medium hydraulic pipe and pressing it for 5 minutes at a pressure of 15 MPa to obtain a material rod, and placing the material rod in a muffle furnace and setting the temperature to 1450° C. for sintering for 10 hours;

[0035] S300, growing a single crystal from the material rod to obtain a sample;

[0036] Among them, the conditions for the single crystal growth of the material rod in the optical floating zone single crystal furnace are 55W, the relative speed is 20r / min, and the growth rate is 2mm / h to obtain a single crystal sample;

[0037] S400, sintering the sample again, wherein the secondary sintering temperature is 1600° C. and the sintering time is 10 h.

[0038] Example 2

[0039] A method for preparing single crystal BaTiO3 comprises the following steps:

[0040] S100, grinding BaTiO3 and TiO2 powders once, pre-calcining, grinding them again, and granulating them to obtain pellets;

[0041] Among them, the first grinding time is 6.5h, the pre-burning temperature is 1300℃, the pre-burning time is 7h, and the second grinding time is 9h;

[0042] S200, pressing the pellets into tablets and sintering them into rods;

[0043] The tableting process includes placing the pellets into a material column bag and pressing them tightly, then placing the material column bag into a water medium hydraulic pipe and pressing it for 3 minutes at a pressure of 18 MPa to obtain a material rod, and placing the material rod in a muffle furnace and setting the temperature to 1470° C. for sintering for 8 hours;

[0044] S300, growing a single crystal from the material rod to obtain a sample;

[0045] Among them, the conditions for the single crystal growth of the material rod in the optical floating zone single crystal furnace are 56W, the relative speed is 25r / r / min, and the growth rate is 3.5mm / h to obtain a single crystal sample;

[0046] S400, sintering the sample again, wherein the secondary sintering temperature is 1625° C. and the sintering time is 9 hours.

[0047] Example 3

[0048] A method for preparing single crystal BaTiO3 comprises the following steps:

[0049] S100, grinding BaTiO3 and TiO2 powders once, pre-calcining, grinding them again, and granulating them to obtain pellets;

[0050] Among them, the first grinding time is 8h, the pre-burning temperature is 1400℃, the pre-burning time is 6h, and the second grinding time is 10h;

[0051] S200, pressing the pellets into tablets and sintering them into rods;

[0052] The tableting process includes placing the pellets into a material column bag and pressing them tightly, then placing the material column bag into a water medium hydraulic pipe and pressing it for 5 minutes at a pressure of 20 MPa to obtain a material rod, and placing the material rod in a muffle furnace and setting the temperature to 1500° C. for sintering for 6 hours;

[0053] S300, growing a single crystal from the material rod to obtain a sample;

[0054] Among them, the conditions for the single crystal growth of the material rod in the optical floating zone single crystal furnace are 57W, the relative speed is 30r / r / min, and the growth rate is 5mm / h to obtain a single crystal sample;

[0055] S400, sintering the sample again, wherein the secondary sintering temperature is 1650° C. and the sintering time is 8 hours.

[0056] The prepared samples were characterized and tested, and the results are as follows:

[0057] like Figure 2 As shown in the X-ray diffraction pattern of the BaTiO3 tetragonal ferroelectric polycrystal before growth, diffraction peaks were generated at 2θ of approximately 22°, 31°, 39.8°, 45°, 51°, 56°, 66°, 70°, 75°, 80°, and 84.6°.

[0058] like Figure 3The X-ray diffraction spectrum of the BaTiO3 single crystal sample measured by cutting it in the transverse direction shows that when 2θ is about 22°, the diffraction peaks of the (001) crystal plane and the (100) crystal plane are produced, when 2θ is about 31°, the diffraction peaks of the (101) crystal plane and the (110) crystal plane are produced, when 2θ is about 39.8°, the diffraction peak of the (111) crystal plane is produced, when 2θ is about 45°, the diffraction peaks of the (002) crystal plane and the (200) crystal plane are produced, when 2θ is about 51°, the diffraction peaks of the (102) crystal plane, the (201) crystal plane and the (210) crystal plane are produced, and when 2θ is about 56°, the diffraction peaks of the (111) crystal plane are produced. When 2θ is about 66°, the diffraction peaks of (211) crystal plane and (202) crystal plane are generated; when 2θ is about 70°, the diffraction peaks of (220) crystal plane and (212) crystal plane are generated; when 2θ is about 75°, the diffraction peaks of (300) crystal plane and (103) crystal plane are generated; when 2θ is about 80°, the diffraction peaks of (113) crystal plane and (311) crystal plane are generated; when 2θ is about 80°, the diffraction peaks of (113) crystal plane and (311) crystal plane are generated; when 2θ is about 84.6°, the diffraction peaks of (222) crystal plane and (203) crystal plane are generated;

[0059] like Figure 4 The X-ray diffraction pattern of the BaTiO3 single crystal sample cut in the longitudinal direction shows that, similarly, diffraction peaks of the (001) crystal plane and the (100) crystal plane are produced at 2θ of about 22°, diffraction peaks of the (101) crystal plane and the (110) crystal plane are produced at 2θ of about 31°, diffraction peaks of the (111) crystal plane are produced at 2θ of about 39.8°, diffraction peaks of the (002) crystal plane and the (200) crystal plane are produced at 2θ of about 45°, diffraction peaks of the (102) crystal plane, the (201) crystal plane and the (210) crystal plane are produced at 2θ of about 51°, and diffraction peaks of the (102) crystal plane, the (201) crystal plane and the (210) crystal plane are produced at 2θ of about 56°. At about 2θ, the diffraction peaks of (113) and (311) planes are generated, at about 2θ of 80°, the diffraction peaks of (113) and (311) planes are generated, at about 2θ of 80°, the diffraction peaks of (222) and (203) planes are generated, but from Figure 3 and Figure 4 From the above, it can be seen that after cutting the sample horizontally and vertically, the X-ray diffraction patterns measured have corresponding enhancement and weakening of the diffraction peak intensity on the same crystal plane, thus judging that the sample is a BaTiO3 tetragonal ferroelectric single crystal sample.

[0060] The single crystal BaTiO3 prepared by the single crystal BaTiO3 preparation method of the present invention can be used in the following devices: pressure sensor, piezoelectric ultrasonic motor, optical information storage, micro displacement driver, piezoelectric transformer, piezoelectric transducer.

[0061] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in the field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in the technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing single crystal BaTiO3 for piezoelectric devices, characterized in that: The method comprises the following steps: S100, grinding BaTiO3 and TiO2 powders once, pre-calcining, grinding them again, and granulating them to obtain pellets; S200, pressing the pellets into tablets and sintering them into rods; S300, growing the material rod by using an optical floating zone single crystal method to obtain a sample; S400, sintering the sample for a second time; in, The two ceramic crystal rods used in the preparation process are polycrystalline samples, and no additional seed crystals are required for single crystal growth; The growth rate is 2-5 mm / h to obtain single crystal samples, which greatly shortens the sample preparation cycle compared to other methods; in, In step S100, the grinding time is 5-8 hours, the pre-sintering temperature is 1200-1400° C., and the pre-sintering time is 6-8 hours; The secondary grinding time in step S100 is 8-10 hours; The tableting in step S200 includes placing the pellets into a material column bag and pressing them tightly, and then placing the material column bag into a water medium hydraulic pipe and pressing it at a pressure of 15-20 MPa for 2-5 minutes to obtain a material rod; The material rod is placed in a muffle furnace and set to a temperature of 1450-1500° C. for sintering for 6-10 hours; In step S300, the material rod is grown into a single crystal in a single crystal furnace in an optical floating zone, and the growth conditions are that the power is set to 55-57W and the relative speed is 20-30r / min; The temperature of the secondary sintering in step S400 is 1600-1650°C, and the sintering time is 8-10h; in, The X-ray diffraction spectrum of the BaTiO3 tetragonal ferroelectric polycrystal before growth in step S300 produces diffraction peaks at 2θ of 22°, 31°, 39.8°, 45°, 51°, 56°, 66°, 70°, 75°, 80°, and 84.6°; The X-ray diffraction spectrum of the BaTiO3 single crystal sample measured along the transverse section shows that when 2θ is 22°, the diffraction peaks of the (001) crystal plane and the (100) crystal plane are produced; when 2θ is 31°, the diffraction peaks of the (101) crystal plane and the (110) crystal plane are produced; when 2θ is 39.8°, the diffraction peak of the (111) crystal plane is produced; when 2θ is 45°, the diffraction peaks of the (002) crystal plane and the (200) crystal plane are produced; when 2θ is 51°, the diffraction peaks of the (102) crystal plane, the (201) crystal plane and the (210) crystal plane are produced; when 2θ is 56°, the diffraction peaks of the (111) crystal plane are produced. 12) diffraction peaks of crystal planes. When 2θ is 66°, the diffraction peaks of (211) crystal plane and (202) crystal plane are generated. When 2θ is 70°, the diffraction peaks of (220) crystal plane and (212) crystal plane are generated. When 2θ is 75°, the diffraction peaks of (300) crystal plane and (103) crystal plane are generated. When 2θ is 80°, the diffraction peaks of (113) crystal plane and (311) crystal plane are generated. When 2θ is 80°, the diffraction peaks of (113) crystal plane and (311) crystal plane are generated. When 2θ is 84.6°, the diffraction peaks of (222) crystal plane and (203) crystal plane are generated. The X-ray diffraction spectrum of the BaTiO3 single crystal sample measured along the longitudinal section shows that when 2θ is 22°, the diffraction peaks of the (001) crystal plane and the (100) crystal plane are produced; when 2θ is 31°, the diffraction peaks of the (101) crystal plane and the (110) crystal plane are produced; when 2θ is 39.8°, the diffraction peak of the (111) crystal plane is produced; when 2θ is 45°, the diffraction peaks of the (002) crystal plane and the (200) crystal plane are produced; when 2θ is 51°, the diffraction peaks of the (102) crystal plane, the (201) crystal plane and the (210) crystal plane are produced; when 2θ is 56°, the diffraction peaks of the (111) crystal plane are produced. 12) diffraction peaks of crystal planes. When 2θ is 66°, the diffraction peaks of (211) crystal plane and (202) crystal plane are generated. When 2θ is 70°, the diffraction peaks of (220) crystal plane and (212) crystal plane are generated. When 2θ is 75°, the diffraction peaks of (300) crystal plane and (103) crystal plane are generated. When 2θ is 80°, the diffraction peaks of (113) crystal plane and (311) crystal plane are generated. When 2θ is 80°, the diffraction peaks of (113) crystal plane and (311) crystal plane are generated. When 2θ is 84.6°, the diffraction peaks of (222) crystal plane and (203) crystal plane are generated. Moreover, the X-ray diffraction patterns measured after cutting the sample horizontally and vertically show corresponding enhancement and weakening of the diffraction peak intensity produced on the same crystal plane.

2. An application of single crystal BaTiO3 prepared by the method according to claim 1 in a piezoelectric device, wherein the piezoelectric device comprises any one of the following: a piezoelectric ultrasonic motor, a piezoelectric transformer, and a piezoelectric transducer.