Adhesives based on benzyl ether phenolic resins containing free phenol and free hydroxybenzyl alcohol
By optimizing the ratio of phenol to hydroxybenzyl alcohol in the benzyl ether type phenolic resin and delaying the addition of monomers, the problem of insufficient sand core strength and thermal strength in the existing technology is solved, and higher strength and thermal stability are achieved.
Patent Information
- Application Number
- CN202110489988.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-12-23
- Filing Date
- 2017-12-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2037-12-22
AI Technical Summary
Existing benzyl ether type phenolic resin binders have insufficient strength and thermal strength when producing sand cores, especially since free hydroxybenzyl alcohol is considered a chain terminator, lower strength and reduced thermal strength are expected.
By delaying the addition of monomers in the first addition step of aromatic phenol rings and formaldehyde, the ratio of phenol to hydroxybenzyl alcohol is optimized so that the ratio of free hydroxybenzyl alcohol to free phenol is greater than 1, thereby improving the strength and thermal strength of the sand core.
The strength and thermal strength of the sand core are significantly improved, exceeding the expected effect. The high concentration of hydroxybenzyl alcohol is greater than 1.1, especially at the ratio of 1.8 to 13, achieving better strength and thermal stability.
Smart Images

Figure BDA0003051972750000041 
Figure BDA0003051972750000051 
Figure BDA0003051972750000071
Abstract
Description
[0001] This application is a divisional application of Chinese Patent Application No. 201780079950.X, filed on December 22, 2017, entitled “Adhesive based on benzyl ether type phenolic resin containing free phenol and free hydroxybenzyl alcohol”. Technical Field
[0002] The invention relates to a binder based on a benzyl ether phenolic resin and an isocyanate compound having at least two isocyanate groups, containing free phenol and free hydroxybenzyl alcohol in a specific ratio to one another in the polyol component, for use in a cold box method (PUCB method) of phenolic resins and polyurethanes and / or in a no bake method (PUNB method) of phenolic resins and polyurethanes. The invention also relates to a mold material mixture containing the binder and to cores, molds or risers produced with the mold material mixture and to their use in metal casting. Background Art
[0003] The use of PUCB and / or PUNB methods to make cores and molds has achieved great significance in the foundry industry. Here, a two-component polyurethane system is used to bond refractory mold base materials. The polyol component is composed of a polyol having at least two OH groups per molecule, and the isocyanate component is an isocyanate having at least two NCO groups per molecule. Phenolic resin is one of the polyol components used. The mixture of the mold base material and the adhesive, also referred to as the mold material mixture, is cured in the PUCB method with the aid of a low-boiling tertiary amine, which is passed through the mold material mixture after molding in gaseous form or as an aerosol (see US3409579). Typically, this is done with the aid of a carrier gas, such as air, nitrogen or CO2, in which at least one tertiary amine is metered. In the PUNB method, a liquid tertiary amine and / or a metal compound are added as a catalyst to the mold material mixture.
[0004] Previous benzyl ether type phenolic resins (referring to pure phenolic resins, without solvents and additives), made from phenol as the only phenolic base material and formaldehyde, generally had a residual phenol concentration of 4.0 to 18.0 wt% (free phenol) and a free hydroxybenzyl alcohol concentration of 4.2-17.9 wt%, the concentration of free hydroxybenzyl alcohol being always lower than the concentration of free phenol. Hydroxybenzyl alcohol includes o-hydroxybenzyl alcohol (saligenin), m-hydroxybenzyl alcohol and / or p-hydroxybenzyl alcohol (homosaligenin). If the concentration of hydroxybenzyl alcohol is subsequently mentioned (whether in the singular or in the plural sense), this refers to the sum of o-, m- and p-hydroxybenzyl alcohol.
[0005] Previous benzyl ether type phenolic resins (referring to pure phenolic resins, without solvents and additives), made from phenol and o-cresol as phenolic base materials and formaldehyde, generally had a residual phenol concentration of 3.0 to 12.0 wt %, a residual cresol concentration of 2.0-6.0 wt %, and a hydroxybenzyl alcohol concentration of 3.2-11.9 wt %, wherein the hydroxybenzyl alcohol concentration was always lower than the phenol concentration.
[0006] DE 102015107016.2 teaches in the examples of Table 1 that the salicyl alcohol concentration of exemplary phenolic resins of the benzyl ether type made from phenol and formaldehyde has a higher free phenol concentration than the free salicyl alcohol. The weight ratio of phenol to salicyl alcohol or hydroxybenzyl alcohol is always 1 to less than 1, respectively. US 4205188 describes the selective production of salicyl alcohol from phenol and formaldehyde in an alkaline environment. A solution extraction process is carried out using excess phenol to remove unconverted phenol again.
[0007] Mission of the present invention
[0008] The object of the present invention is to provide a binder based on a benzyl ether phenolic resin which improves the strength and thermal strength of the sand cores produced with the binder. Summary of the invention
[0009] This object is achieved by the subject matter of the independent claim. Advantageous developments are the subject matter of the dependent claims or are described below.
[0010] The present invention therefore provides an adhesive containing a benzyl ether-type phenolic resin and an isocyanate with a defined phenol or hydroxybenzyl alcohol ratio. Surprisingly, it was found that delayed addition of the monomers in the first addition step of the aromatic phenol rings with formaldehyde improves the strength and the tendency to deformation. This is surprising because, for example, hydroxybenzyl alcohol (with catalytic activation) reacts preferably with isocyanates via the -CH2OH group, which in fact leads to chain termination. This observation is surprising because hydroxybenzyl alcohol is considered to be a chain terminator for polyaddition reactions with diisocyanates and, in connection with this, lower strength and reduced hot strength would be expected.
[0011] The invention further relates to a mould material mixture containing a binder based on a benzyl ether phenolic resin, a refractory mould base material and an isocyanate, and optionally a catalyst, and cores, moulds and feeders produced from the mould material mixture after hardening. The invention also relates to the use of cores, moulds and feeders for metal casting, in particular iron and aluminium casting. DETAILED DESCRIPTION
[0012] All conventionally used phenolic compounds are suitable for preparing benzyl ether phenolic resins. Together with unsubstituted phenols, substituted phenols or mixtures of these can be used. The phenolic compound is preferably unsubstituted at both ortho positions or at one ortho and para positions. The remaining carbon atoms in the ring may be substituted. The choice of substituent is not particularly limited, as long as the substituent does not adversely affect the reaction of the phenol with the aldehyde.
[0013] Examples of substituted phenols are alkyl-substituted, alkoxy-substituted, aryl-substituted and aryloxy-substituted phenols.
[0014] The basic structure of a phenolic resin of the benzyl ether type has a -CH2-O-CH2-linked phenol unit together with a -CH2-linked phenol unit and can be represented as an example (with reference to the product implemented only with formaldehyde) as follows:
[0015]
[0016] The various units are usually distributed statistically (ie also linked in a sequence other than that shown above). The phenol units may also have para bonds to a certain extent. Here, R 1 is independently in each case a hydrogen (especially m and n) in the ortho, meta or para position relative to the phenolic hydroxyl group or a phenolic C1-C 26 Alkyl substituent (saturated or unsaturated, linear or branched); the sum of m and n is at least 2, and the ratio of m:n is at least 1; R is independently hydrogen, -CH2OH or -CH2O-R 2 , where R 2 = C1-C9 hydrocarbon. 2 The radicals may be straight-chain or branched, saturated or unsaturated.
[0017] The above substituents have, for example, 1 to 26, preferably 1 to 15 carbon atoms. Examples of suitable phenols are o-cresol, m-cresol, p-cresol, 3,5-xylenol, 3,4-xylenol, 3,4,5-trimethylphenol, 3-ethylphenol, 3,5-diethylphenol, p-butylphenol, 3,5-dibutylphenol, p-pentylphenol, cyclohexylphenol, p-octylphenol, p-nonylphenol, cardanol, 3,5-dicyclohexylphenol, p-crotylphenol, p-phenylphenol, 3,5-dimethoxyphenol and p-phenoxyphenol.
[0018] Phenol itself is particularly preferred. Even more highly condensed phenols such as bisphenol A are also suitable. Furthermore, polyfunctional phenols are also suitable, ie those having more than one phenolic hydroxyl group.
[0019] Preferred polyfunctional phenols have 2 to 4 phenolic hydroxyl groups. Specific examples of suitable polyfunctional phenols are catechol, resorcinol, hydroquinone, pyrogallol, phloroglucinol, 2,5-dimethylresorcinol, 4,5-dimethylresorcinol, 5-methylresorcinol, cardanol or 5-ethylresorcinol. Mixtures of various mono- and polyfunctional and / or substituted and / or condensed phenolic components can also be used to prepare the polyol component.
[0020] In one embodiment, the phenol of formula I
[0021]
[0022] For preparing the phenolic resin component, A, B and C are independently selected from: a hydrogen atom, a branched or unbranched alkyl or alkenyl moiety, which may have, for example, 1 to 26, preferably 1 to 15 carbon atoms, a branched or unbranched alkoxy moiety, which may have, for example, 1 to 26, preferably 1 to 15 carbon atoms, a branched or unbranched alkenyloxy moiety, which may have, for example, 1 to 26, preferably 1 to 15 carbon atoms, and an aryl or alkaryl moiety such as a bisphenyl group.
[0023] Along with formaldehyde, aldehydes of the following formula are also suitable as further aldehydes for preparing phenol-formaldehyde resins of the benzyl ether type:
[0024] R-CHO
[0025] wherein R is a carbon atom moiety having 1 to 3 carbon atoms, preferably one carbon atom. Specific examples are acetaldehyde and propionaldehyde. Particular preference is given to using formaldehyde in liquid form, as paraformaldehyde or in the form of trioxane.
[0026] In order to obtain a benzyl ether type phenolic resin, it is preferred to use at least an equimolar amount of the aldehyde compound relative to the molar number of the phenolic compound. The molar ratio of the aldehyde compound to the phenol compound is preferably comprised between 1.05:1.0 and 2.5:1, particularly preferably between 1.1:1 and 2.2:1, and most preferably between 1.2:1 and 2.0:1.
[0027] According to EP 0177871 A2, aliphatic monohydric alcohols having 1 to 8 carbon atoms can be added as further reaction components. The alkoxylation is intended to give the phenolic resins a higher thermal stability and a longer sand service life.
[0028] The production of benzyl ether phenolic resins is carried out according to methods known to the person skilled in the art. Here, phenol and aldehyde are converted in the presence of divalent metal ions at a temperature preferably below 130° C. The water formed is distilled off. For this purpose, suitable entrainers, such as toluene or xylene, can be added to the reaction mixture, or the distillation can be carried out under reduced pressure.
[0029] Suitable catalysts for preparing benzyl ether phenolic resins are salts of divalent ions of metals, such as Mn, Zn, Cd, Mg, Co, Ni, Fe, Pb, Ca and Ba, especially Zn salts. Zinc acetate is preferably used. The amount used is not critical. Typical amounts of metal catalysts include 0.02 to 0.3 wt%, preferably 0.02 to 0.18 wt%, relative to the total amount of phenolic compound and aldehyde compound.
[0030] These resins are described, for example, in US Pat. No. 3,485,797 and EP 1,137,500 B1; explicit reference is made here to these disclosures, both of which relate to phenol-formaldehyde resins of the benzyl ether type per se and to their preparation. Analysis of these resins shows that the weight ratio of free phenol (hydroxybenzene) to free hydroxybenzyl alcohol is always 1: less than 1.
[0031] The first reaction step of the formaldehyde addition reaction consisting of 1 mol of phenol and 1 mol of formaldehyde forms hydroxybenzyl alcohols, in particular salicyl alcohol (saligenin). Due to the ortho-ortho-localization effect of the metal catalyst, mainly
[0032]
[0033] Salicyl alcohol (2-hydroxybenzyl alcohol or o-hydroxybenzyl alcohol) Mw: 124.14 g / mol. However, the formation
[0034]
[0035] Homosaligenin (4-hydroxybenzyl alcohol or p-hydroxybenzyl alcohol)
[0036] Also possible. Mixtures of positional isomers are also possible, so that the -CH2-OH groups can be attached in the ortho and ortho positions, ortho and para positions, and ortho, ortho and para positions. In another embodiment, one, two or three -CH2-OH groups can be etherified with a C1-C9 monoalcohol. The monoalcohol can be linear or branched, saturated or unsaturated.
[0037] The statements regarding the example of phenol also apply to the phenolic base materials o-cresol and m-cresol. Possible mixtures of positional isomers of the -CH2-OH group are located in the ortho or para position as well as in the ortho and para position. In another embodiment, one or both -CH2-OH groups can be etherified with a C1-C9 monoalcohol. The monoalcohol can be linear or branched, saturated or unsaturated.
[0038] If cardanol and / or cardol are used as phenolic base materials, the -CH2-OH groups can be attached in ortho and ortho, ortho and para, ortho, ortho and para. In another embodiment, one, two or three -CH2-OH groups can be etherified with C1-C9 monoalcohols.
[0039] The monohydric alcohol may be linear or branched, saturated or unsaturated.
[0040] Surprisingly, it has now been found that a ratio of free hydroxybenzyl alcohol to free phenol in a benzyl ether phenolic resin of greater than 1, in particular greater than 1.1, improves the strength and hot strength of sand cores produced therefrom.
[0041] Monomeric addition products are defined as the first reaction step of a phenolic base material with formaldehyde, in which up to three hydrogens on the ring of the phenolic base material may be replaced by –CH2-OH groups. The molar masses of the phenol-based monomeric addition products are 124 g / mol (hydroxybenzyl alcohol) up to 184 g / mol (phenol plus up to 3 –CH2OH). Any C1-C26-alkyl groups which are bonded to the phenolic base material and / or as alkenyl groups to etherified –CH2-OH groups are not included in the given molar weights.
[0042] Preferably, phenol and hydroxybenzyl alcohol are used in a weight ratio of 1: greater than 1.2 to 1:30, 1:1.3 to 1:20 is more preferred, 1:1.6 to 1:15 is particularly preferred, and 1:1.8 to 1:13 is most preferred.
[0043] Preferably, phenol and salicyl alcohol (o-hydroxybenzyl alcohol) are used in a weight ratio of 1: greater than 1.1 to 1:25, 1:1.2 to 1:15 is more preferred, 1:1.5 to 1:10 is particularly preferred, and 1:1.8 to 1:8 is most preferred.
[0044] In particular, the weight of the benzyl ether type phenolic resin refers to the sum of the weights of the phenolic resin and the associated (free) monomers, wherein the phenolic resin is a conversion product of at least one formaldehyde compound and a phenolic compound, including polymer-like conversion products, such as alkoxylation of the terminal groups.
[0045] The free phenol concentration preferably comprises less than 3 wt%, in particular less than 2.5 wt% or even less than 2 wt%, relative to the weight of the benzyl ether type phenolic resin.
[0046] Thus, the salicyl alcohol (o-hydroxybenzyl alcohol) concentration is in total 2 to 16 wt %, or for example 1 to 8 wt %, and the hydroxybenzyl alcohol concentration is 2 to 26 wt %, or for example 1 to 13 wt %, in each case relative to the weight of the phenolic resin of benzyl ether type.
[0047] The benzyl ether phenolic resin can contain a desired concentration of free hydroxybenzyl alcohol, especially free salicyl alcohol, by controlling during or after the benzyl ether phenolic resin forming reaction, or by adding hydroxybenzyl alcohol, especially salicyl alcohol, before, after or during the phenolic resin forming reaction, especially after the phenolic resin forming reaction.
[0048] The ratio of free phenol to hydroxybenzyl alcohol, in particular salicyl alcohol, in the benzyl ether phenol-formaldehyde resin can also be controlled by subsequently removing free phenol, preferably free phenol, from the benzyl ether phenol-formaldehyde resin, for example by steam distillation, azeotropic distillation or leaching with water according to DIN 53704, and for example by filtering. If desired, the addition of hydroxybenzyl alcohol, in particular salicyl alcohol, can also be carried out after this step.
[0049] Molar mass of benzyl ether phenolic resin without phenol and monomer condensation products (HPLC Agilent 11100, RI detector, PSS SDV 5 μm precolumn, PSS SDV 5 μm column PSS SDV 5μm Column THF mobile medium, column temperature 35°C, calibration relative to PSS Polystyrene ReadyCal Kit [Low] (Mp 266-67500D), the internal standard PSS Polystyrene ReadyCal Kit [Low] (Mp 266-67500D) is preferably 500 to 1100 g / mol, particularly preferably 550 to 1000 g / mol, and most preferably 560 to 980 g / mol.
[0050] The hydroxyl number (determined according to DIN 53240), which is used to further characterize the benzyl ether phenolic resin, is 500 to 900 mg KOH / g, particularly preferably 550 to 850 mg KOH / g, most preferably 560 to 750 mg KOH / g.
[0051] The isocyanate component of the binder system comprises an aliphatic, cycloaliphatic or aromatic monomeric or polymeric isocyanate, preferably having an average of 2 to 5 isocyanate groups per molecule.
[0052] Depending on the properties desired, mixtures of isocyanates may also be used.
[0053] Suitable isocyanates include aliphatic isocyanates such as hexamethylene diisocyanate, cycloaliphatic isocyanates such as 4,4'-dicyclohexylmethane diisocyanate and its dimethyl derivatives. Examples of suitable aromatic isocyanates are toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, 1,5-naphthalene diisocyanate, triphenylmethane triisocyanate, xylene diisocyanate and its methyl derivatives, and polymethylene polyphenyl isocyanates. Preferred isocyanates are aromatic isocyanates, particularly preferred are polymethylene polyphenyl polyisocyanates, such as technically 4,4'-diphenylmethane diisocyanate, i.e. 4,4'-diphenylmethane diisocyanate with a portion of isomers and higher homologs.
[0054] Isocyanates can also be derivatized by converting isocyanates that can form bonds with each other in such a way that a portion of their isocyanate groups are derivatized to form biuret, allophanat, uretdion or carbodiimide groups. For example, uretdion groups with dimerization products such as MDI or TDI are interesting. However, such derivatized isocyanates are preferably used as a component only together with the above-mentioned non-derivatized isocyanates.
[0055] Preferably, the isocyanate is used in an amount in which the number of isocyanate groups relative to the number of free hydroxyl groups of the resin amounts to 80 to 120%.
[0056] The isocyanate component of the binder system is preferably used as a solution in an organic solvent or a combination of organic solvents. A solvent may therefore be required, for example, in order to keep the components of the binder under sufficiently low viscosity conditions. This is necessary, among other things, in order to obtain uniform crosslinking of the refractory mould material and to maintain its free-flowing properties.
[0057] The corresponding polyol component or isocyanate component of the binder system is preferably used as a solution in an organic solvent or a combination of organic solvents. A solvent may therefore be required, for example, in order to keep the components of the binder under sufficiently low viscosity conditions. This is necessary, among other things, in order to obtain a uniform crosslinking of the refractory mould material and to maintain its free-flowing properties.
[0058] Known aromatic solvents, such as those designated as naphtha, can be used as solvents for the polyol component. Starting from benzene, alkyl and / or alkenyl groups are substituted independently of one another on the aromatic rings, these having a chain length of C1 to C30, preferably C1 to C20, particularly preferably C1 to C16. Independently of one another, one to six hydrogen atoms on the benzene ring may be replaced by alkyl and / or alkenyl groups; preferably, 1 to 4, particularly preferably 1 to 3 hydrogen atoms on the ring are replaced. Independently of this, the alkyl or alkenyl chain may be straight-chain or branched.
[0059] In addition, oxygen-rich organic solvents can be used. Dicarboxylates, glycol ether esters, glycol diesters, glycol diethers, cyclic ketones, cyclic esters (lactones), cyclic carbonates or silicates or mixtures thereof are particularly suitable. Dicarboxylates, cyclic ketones, silicates and cyclic carbonates are preferably used.
[0060] Typical dicarboxylic acid esters have the formula R1OOC-R2-COOR1, wherein the R1 groups are in each case independent of one another (especially from the second R1) and are alkyl groups having 1 to 12 carbon atoms, preferably 1 to 6 carbon atoms, and R2 is a straight-chain or branched hydrocarbon group having 1 to 7 carbon atoms. Examples are dimethyl esters of carboxylic acids having 4 to 6 carbon atoms, which are available, for example, from DuPont under the name "dibasic esters".
[0061] Typical glycol ether esters are compounds having the formula R3-O-R4-OOCR5, wherein R3 is an alkyl group having 1-4 carbon atoms, R4 is a hydrocarbon group having 2-4 carbon atoms, and R5 is an alkyl group having 1 to 3 carbon atoms, such as butyl glycol acetate; glycol ether acetates are preferred.
[0062] Typical glycol diesters have the general formula R3COO-R4-OOCR5, wherein R3 to R5 are as defined above and the groups are selected independently of one another in each case (e.g. propylene glycol diacetate). Glycol diacetates are preferred. Glycol diethers can be characterized by the formula R3-O-R4-O-R5, wherein R3 to R5 are as defined above and the groups are selected independently of one another in each case (e.g. dipropylene glycol dimethyl ether).
[0063] Typical cyclic ketones, cyclic esters and cyclic carbonates having 4 to 5 carbon atoms are also suitable (eg propylene carbonate). The carbons may be attached in a branched or unbranched manner and may be saturated or unsaturated.
[0064] Also suitable are fatty acid esters -R6-OOCR7-, wherein R7 is a C8 to C32 hydrocarbon and R6 is a C1 to C9 hydrocarbon, particularly 1 to 4, such as rapeseed fatty acid methyl ester, butyl oleate and isopropyl esters of various fatty acids.
[0065] Silicate esters are also suitable in their monomeric or oligomeric form, as is known from WO 2009 / 130335 A2. Suitable alkyl / alkoxysilanes or alkyl / alkoxysiloxanes are, for example, esters of orthosilicic acid in which 1, 2 or 3 alcohol groups are substituted by substituted or unsubstituted hydrocarbon moieties, of the formula R 1 n Si(OR) 4-nA compound wherein n=1, 2 or 3, for each R group, refers to an organic group independent of any other R group, preferably a branched or unbranched C1 to C30 alkyl or aryl group, as defined in conjunction with the first aspect. Here R 1 is a substituted or unsubstituted, branched or unbranched hydrocarbon group, and in the case where n=2 or 3, R 1 The groups are the same or different. Preferably, R 1 The group is a substituted or unsubstituted, branched or unbranched C1-C30 alkyl group, or a substituted or unsubstituted aryl group, and is particularly preferably a substituted or unsubstituted, branched or unbranched C1-C6 alkyl group, or a substituted or unsubstituted C6-C10 aryl group. Most preferably, it is an unsubstituted, branched or unbranched C1-C6 alkyl group or an unsubstituted phenyl group. Furthermore, particularly preferred here are methyl, ethyl and propyl groups.
[0066] The modified ester is preferably selected from the group consisting of tetraalkoxysilane, monoalkyltrialkoxysilane, dialkyldialkoxysilane, trialkylmonoalkoxysilane, monoaryltrialkoxysilane, diaryldialkoxysilane and triarylmonoalkoxysilane, wherein the alkyl or alkoxy group is preferably a C1-C6 alkyl group.
[0067] Preferably, these are modified esters selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltributoxysilane, ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-glycidylpropyltrimethoxysilane, 3-glycidylpropyltriethoxysilane, 3,4-epoxycyclohexyltrimethoxysilane, dimethoxydimethylsilane, diethoxydimethylsilane, diethyldimethoxysilane and diethyldiethoxysilane.
[0068] Tetraethyl orthosilicate, tetrapropyl orthosilicate, mixtures thereof and oligomers or mixtures of oligomers thereof are particularly preferred. Tetraethyl orthosilicate and tetrapropyl orthosilicate or mixtures thereof are particularly preferred.
[0069] Aromatic solvents, the abovementioned polar solvents or mixtures thereof are used as solvents for the isocyanates. Fatty acid esters and silicates are also suitable.
[0070] The proportion of the solvent in the adhesive may include 2 to 57 wt %, in particular 3 to 53 wt %.
[0071] Together with the components already mentioned, the adhesive system may contain further additives, for example silanes (for example according to EP 1 137 500 B1), internal mold release agents, for example fatty alcohols (for example according to US 4,602,069), drying oils (for example according to US 4,268,425), complexing agents (for example according to US 5,447,968) and additives for extending the processing time (for example according to US 4,540,724), flow improvers of the silicone surfactant type or mixtures thereof.
[0072] Conventional and known materials for producing cast molds and mixtures thereof can be used as refractory mold base materials (hereinafter referred to as "mold base materials"). Examples of suitable materials are quartz sand, zircon sand, chrome ore sand, olivine, vermiculite, bauxite, refractory clay and so-called artificial mold base materials, i.e. mold base materials that are made into a spherical or approximately spherical shape (e.g., an ellipsoid) by industrial molding methods.
[0073] Examples of this are glass beads, glass granules or artificial spherical ceramic sand - so-called besides or "Carboaccucast" - and hollow microspheres, since they can be separated in the form of fly ash components, for example hollow aluminum silicate spheres (microspheres). Mixtures of the refractory materials mentioned are also possible.
[0074] Particularly preferred are refractory materials which contain more than 50 wt% of quartz sand relative to the mold base material. A refractory mold base material is understood to be a base material having a high melting point (melting temperature). Preferably, the melting point of the refractory mold base material is greater than 600° C., more preferably greater than 900° C., particularly preferably greater than 1200° C., and most preferably greater than 1500° C.
[0075] The refractory mould base material preferably contains more than 80 wt %, in particular more than 90 wt % and particularly preferably more than 95 wt % of the mould material mixture.
[0076] The average diameter of the refractory mold base material is generally 100 μm to 600 μm, preferably 120 μm to 550 μm and particularly preferably 150 μm to 500 μm. The particle size can be determined, for example, by passing through a sieve in accordance with DIN ISO 3310. Particularly preferred particle shapes have a ratio of maximum length extension to minimum length extension (at right angles to each other and in all cases for all spatial directions) of 1:1 to 1:5 or 1:1 to 1:3, i.e., those which are not fibrous, for example.
[0077] The refractory mold base material is preferably in a free-flowing state, in particular in order to be able to process the mold material mixture according to the invention in conventional core-shooting machines.
[0078] Tertiary amines are suitable catalysts. Volatile tertiary amines are used in the PUCB process, such as trimethylamine ("TMA", CAS RN 75-50-3), dimethylethylamine ("DMEA", CAS 75-64-9), dimethyl-n-propylamine ("DMPA", CAS RN 926-63-6), dimethylisopropylamine ("DMIPA", CAS 996-35-0), diethylmethylamine (DEMA), triethylamine ("TEA", CAS RN 121-44-8), tri-n-propylamine, triisopropylamine, tri-n-butylamine and triisobutylamine.
[0079] Liquid tertiary amines are used in the PUNB process. At room temperature (25° C.), this includes liquid tertiary amines and those that become liquid, for example, upon heating to 40° C., or those dissolved in a suitable solvent. Examples are 4-(C1-C4 alkyl)pyridines, such as tris-(3-dimethylamino)propylamine and isoquinoline. Arylpyridines, such as phenylpyridine, pyridine, acridine, 2-methoxypyridine, pyridazine, 3-chloropyridine, quinoline, N-methylimidazole, N-ethylimidazole, 4,4'-bipyridine, 4-phenylpropylpyridine, 1-methylbenzimidazole and 1,4-thiazine.
[0080] Furthermore, the invention relates to a method for producing a mould material mixture, comprising
[0081] (a) mixing a refractory mold base material with the binder of the present invention in an amount of 0.2 to 12 wt %, preferably 0.3 to 13 wt %, particularly preferably 0.4 to 12 wt %, relative to the amount of the refractory mold base material and the catalyst, and adding separately at the same time (in the PUNB process) or later (in the PUCB process) to obtain a mold material mixture;
[0082] (b) placing the mold material mixture obtained in step (a) into a mold;
[0083] (c) adding a catalyst (PUCB) which can be added separately later and hardening the mold material mixture in a mold using the catalyst of the invention to obtain a core or cast mold; and
[0084] (d) The core or mold is then separated from the tool and possibly further hardened.
[0085] To produce the mould material mixture, first the components of the binder system can be combined and then added to the refractory mould base material.However, it is also possible to add the binder components to the refractory mould base material simultaneously or one after the other in any sequence.
[0086] Conventional methods may be used to obtain a homogeneous mixture of the components for the mould material mixture.The mould material mixture may also contain other conventional ingredients, such as iron oxide, ground flax fibres, sawdust particles, asphalt, flow improvers of the silicon surfactant type and refractory metals.
[0087] According to the invention, curing can be carried out by the PUCB or PUNB method. In the case of the PUCB method, for hardening, a low-boiling tertiary amine is passed through the shaped mold material mixture using an inert carrier gas in gaseous form or as an aerosol. No separate catalyst is added. All known cold box amine catalysts can be used.
[0088] In the case of the PUCB method, the amine or metal catalyst may be already dissolved in the binder or mixed with the refractory material as a separate component, with the addition amount comprising about 0.1 wt % to about 5 wt % relative to the mold material mixture.
[0089] The mold body produced according to the method can have any conventional shape used in foundries. In a preferred embodiment, the mold body is in the shape of a casting mold, a core or a riser. They are distinguished by high mechanical stability.
[0090] The invention also relates to the use of the mould body for metal casting, in particular iron and aluminium casting.
[0091] The present invention is described in more detail below based on preferred embodiments or experimental examples, respectively, but is not limited thereto.
[0092] Experimental Examples
[0093] Components used
[0094] All percentage information is by weight.
[0095] Benzyl ether type phenolic resin (o-cresol / phenol / cardanol copolymer), characterized by the following analytical figures:
[0096] The molecular weight (Mw) is about 900 g / mol, the hydroxyl value is about 560 mg KOH / g, the free phenol concentration is 1.8%, and the salicyl alcohol (saligenin) concentration is 3.8%.
[0097] ECOCURE 370 / 5 Part 1 - Benzyl ether type phenolic resin, partially etherified with n-butanol, supplied by ASK-Chemicals GmbH, free phenol concentration 4.5%, salicyl alcohol concentration 3.8%.
[0098] Isocyanate component: a homogeneous mixture of 80% Lupranat M 20S and 20% RME
[0099] KATALYSATOR 706 - Dimethylpropylamine, supplied by ASK-Chemicals GmbH
[0100] Quartz sand H 32 - supplied by Quarzwerke GmbH
[0101] MIRATEC DC 3 - water-based laminar flow, flow time 12 sec / 4 mm cup, supplied by ASK-Chemicals GmbH
[0102] LUPRANAT M 20S: polymeric MDI, functionality 2.6, supplied by BASF SE
[0103] DBE - mixture of dimethyl esters of C4-C6 dicarboxylic acids, supplied by DuPont
[0104] RME - distilled rapeseed oil fatty acid methyl ester, provided by Cargill
[0105] Silan 2201EQ - 50% ureidosilane in methanol supplied by Evonik Industries
[0106] Phenol - provided by Sigma Aldrich
[0107] o-Hydroxybenzyl alcohol - provided by Sigma Aldrich
[0108] p-Hydroxybenzyl alcohol - provided by Sigma Aldrich
[0109] Measurement of phenol and salicyl alcohol concentration
[0110] Phenol and salicyl alcohol concentrations were determined by gas chromatography as follows
[0111] Method Description:
[0112] Calibration: Internal standard method, seven-point calibration for each substance to be determined
[0113] Internal standard: 2,4,6-trimethylphenol pa
[0114] Standard substances: phenol PA and salicyl alcohol (o-hydroxybenzyl alcohol) PA.
[0115] Gas Chromatograph: Agilent 7890Plus with FID, capillary column, autosampler and Agilent ChemStation
[0116] Instrument parameters:
[0117] Input system: Split / splitless injector, 2 minutes run time 20ml / min then split 50:1 (79,9.l / min)
[0118] Temperature: 280℃
[0119] Carrier gas: Hydrogen 5.0, flow rate 1ml / min, constant flow method
[0120] Capillary column: HP-5MS, HP 19091S-105, length 50m,
[0121] Diameter 0.2mm, membrane 0.33μm
[0122] Temperature program: 60°C, 1.5 min; 4.0°C / min to 140°C, hold for 0 min,
[0123] Then, the temperature was raised at 20°C / min to a maximum of 325°C and maintained at 325°C for 6 minutes.
[0124] Detector: FID, temperature 320℃
[0125] Combustible gas: 20ml / min hydrogen 5.0, 350ml / min synthetic
[0126] Air 5.0, 25ml / min Supplementary gas: Nitrogen 5.0
[0127] Autosampler: 10μl GC syringe, 1μl injection, fast injection mode
[0128] Quantitation: Agilent ChemStation Standard Settings
[0129] Internal standard method, the result information is in weight percentage
[0130]
[0131] Table 1 shows the composition of polyols produced based on benzyl ether type phenolic resins; the numerical information represents weight percentage.
[0132]
[0133] Table 2 shows the composition of polyols produced based on ECOCURE 370 / 5 part 1; the numerical information represents weight percent.
[0134] In N / cm2 Determination of the strength of the meter
[0135] In a Hobart mixer, a sand mixture consisting of quartz sand H 32 plus 0.60% of the abovementioned binder composition (in each case individually used in Examples A1 to B11) and 0.60% of the isocyanate component was mixed for 2 minutes until homogeneous.
[0136] The sand mixture was transferred to a Roeper H 1 core shooter and two cores with dimensions (1×w×h) of 220 mm×22.4 mm×22.4 mm were placed in the mold using compressed air in each case, with a closing pressure of 4 bar. The sand was hardened using catalyst 706 (0.5 ml, gassing time 10 seconds at 2 bar purge pressure). After hardening, the cores were removed and the strength was determined after 15 seconds or 30 seconds, respectively, using a Multiserw bending device.
[0137] To determine the hot strength, the 10-minute cores were immersed in a MIRATEC DC 3 stream for 4 seconds and dried for 30 minutes in a circulating air dryer at 150° C. After 30 minutes at 150° C., the cores were removed and immediately tested for flexural strength while hot in a Multiserw apparatus.
[0138] In N / cm 2 Bending strength of the meter
[0139]
[0140] Table 3 shows the 2 The bending strength is measured in units of
[0141]
[0142]
[0143] Table 4 shows the results in N / cm using ECOCURE 370 / 5 part 1 as an example. 2 The flexural strength is measured in units of .
[0144] Both tables have results indicating that the addition of o-hydroxybenzyl alcohol or p-hydroxybenzyl alcohol increases the immediate and hot strength. Approximately the same ratio of free phenol to free salicyl alcohol (A1 and A2, respectively) indicates lower immediate and hot strength.
Claims
1. A benzyl ether phenolic resin, wherein the benzyl ether phenolic resin comprises free phenol and free salicyl alcohol, and the weight ratio of the free phenol to the free salicyl alcohol is 1: greater than 1.1 in total, and the benzyl ether phenolic resin comprises less than 2.5 wt % of free phenol and 1 to 16 wt % of free salicyl alcohol, each relative to the weight of the benzyl ether phenolic resin.
2. The benzyl ether phenolic resin according to claim 1, wherein the weight ratio of the free phenol to the free salicyl alcohol is in the range of 1: greater than 1.1 up to 1:
25.
3. The benzyl ether phenolic resin according to claim 1, wherein the weight ratio of the free phenol to the free salicyl alcohol is in the range of 1:1.2 up to 1:15 in total.
4. The benzyl ether phenolic resin according to claim 1, wherein the weight ratio of the free phenol to the free salicyl alcohol is in the range of 1:1.5 up to 1:10 in total.
5. The benzyl ether phenolic resin according to claim 1, wherein the weight ratio of the free phenol to the free salicyl alcohol is in the range of 1:1.8 up to 1:8 in total.
6. The benzyl ether phenolic resin according to claim 1, wherein The benzyl ether phenolic resin comprises 2 to 16 wt % of free salicyl alcohol relative to the weight of the benzyl ether phenolic resin.
7. The benzyl ether phenolic resin according to claim 1, wherein The benzyl ether phenolic resin contains less than 2 wt % of free phenol relative to the weight of the benzyl ether phenolic resin.
8. The benzyl ether phenolic resin according to claim 1, wherein the benzyl ether phenolic resin further contains one or more of free cresol, free cardanol and free cardanol. 9 . The benzyl ether phenolic resin according to claim 1 , wherein the benzyl ether phenolic resin has a hydroxyl value of 500 to 900 mg KOH / g according to DIN 53240. 10 . The benzyl ether phenolic resin according to claim 1 , wherein the benzyl ether phenolic resin has a hydroxyl value of 550 to 850 mg KOH / g according to DIN 53240. 11 . The benzyl ether phenolic resin according to claim 1 , wherein the benzyl ether phenolic resin has a hydroxyl value of 560 to 750 mg KOH / g according to DIN 53240.
12. The benzyl ether phenolic resin according to claim 1, wherein the benzyl ether phenolic resin has a weight average molecular weight of 500-1100 g / mol in the absence of phenol and monomer addition products.
13. The benzyl ether phenolic resin according to claim 1, wherein the benzyl ether phenolic resin has a weight average molecular weight of 550-1000 g / mol in the absence of phenol and monomer addition products.
14. The benzyl ether phenolic resin according to claim 1, wherein the benzyl ether phenolic resin has a weight average molecular weight of 560 to 980 g / mol in the absence of phenol and monomer addition products.
15. A benzyl ether phenolic resin, wherein the benzyl ether phenolic resin comprises free phenol and free hydroxybenzyl alcohol, and the weight ratio of the free phenol to the free hydroxybenzyl alcohol is 1: greater than 1.2 in total, and the benzyl ether phenolic resin comprises less than 2.5 wt % of free phenol and 1 to 26 wt % of free hydroxybenzyl alcohol, each relative to the weight of the benzyl ether phenolic resin.
16. The benzyl ether phenolic resin according to claim 15, wherein the weight ratio of the free phenol to the free hydroxybenzyl alcohol is in the range of 1: greater than 1.2 up to 1:
30.
17. The benzyl ether phenolic resin according to claim 15, wherein the weight ratio of the free phenol to the free hydroxybenzyl alcohol is in the range of 1:1.3 up to 1:20 in total.
18. The benzyl ether phenolic resin according to claim 15, wherein the weight ratio of the free phenol to the free hydroxybenzyl alcohol is in the range of 1:1.6 up to 1:15 in total.
19. The benzyl ether phenolic resin according to claim 15, wherein the weight ratio of the free phenol to the free hydroxybenzyl alcohol is in the range of 1:1.8 up to 1:13 in total.
20. A binder for hardening a mold material mixture, comprising at least: - a polyol component, wherein the polyol component is a benzyl ether phenolic resin according to any one of claims 1 to 19; - an isocyanate component comprising one or more isocyanate compounds having at least 2 isocyanate groups per molecule.
21. The adhesive according to claim 20, comprising a solvent, and the solvent of the polyol component contains less than 10 wt% of an aromatic solvent.
22. The adhesive according to claim 20, wherein the adhesive is used as a kit comprising one or more of the isocyanate compounds as one component and the benzyl ether type phenol resin as another component separated from each other.
23. The adhesive according to claim 20, wherein the adhesive comprises -8 to 70 wt% of the benzyl ether phenolic resin; or - 13 to 78 wt% of one or more of said isocyanate compounds; or - 2-57 wt % of a solvent for the benzyl ether type phenolic resin and the isocyanate compound.
24. The adhesive according to claim 20, wherein the adhesive comprises -10 to 62 wt% of the benzyl ether phenolic resin; or - 17 to 70 wt% of one or more of said isocyanate compounds; or - 3-53 wt% of a solvent for the benzyl ether type phenolic resin and the one or more isocyanate compounds.
25. A mold material mixture, comprising at least: -Refractory mold base materials; and - The adhesive according to any one of claims 20 to 24.
26. The mold material mixture according to claim 25, wherein the refractory mold base material is selected from one or more members of the group consisting of olivine, refractory clay, bauxite, hollow aluminum silicate spheres, glass beads, glass particles, silicon dioxide, zircon sand, and chrome ore sand.
27. The mold material mixture according to claim 26, wherein the silicon dioxide is in the form of quartz sand.
28. A method for producing a mould body for use as a casting mould or core, comprising (i) producing a mould material mixture as claimed in any one of claims 25 to 27; (ii) introducing the mould material mixture into a mould tool; (iii) hardening the mould material mixture in the mould tool with at least one tertiary amine to obtain a self-supporting mould body; and (iv) The hardened mould body is subsequently separated from the mould tool and optionally further hardened, thereby obtaining a solidified mould body.
29. The method according to claim 28, wherein for producing a mold material mixture, the adhesive is used as a kit consisting of at least one or more of the isocyanate compounds as one component and at least the benzyl ether type phenolic resin as another component separated from each other.
30. The method of claim 28, wherein the tertiary amine is selected from one or more members of the group consisting of trimethylamine, dimethylethylamine, dimethyl-n-propylamine, dimethyl-isopropylamine, diethylmethylamine, triethylamine, tri-n-propylamine, tri-isopropylamine, tri-n-butylamine, tri-isobutylamine, 4-(C1-C4 alkyl)pyridine, tris[(3-dimethylamino)propyl]amine, arylpyridine, pyridine, 2-methoxypyridine, pyridazine, 3-chloropyridine, N-methylimidazole, N-ethylimidazole, 4,4'-bipyridine, 1,4-thiazine, and 1-methylbenzimidazole.
31. The method of claim 30, wherein the arylpyridine comprises one or more of the following: phenylpyridine, isoquinoline, acridine, quinoline, and 4-phenylpropylpyridine.