Solid-state batteries

By designing the aluminum-lithium alloy structure and sulfide-based electrolyte material of the negative electrode layer in the lithium-ion battery, the problem of the reduction of the discharge capacity of the aluminum-lithium alloy material in the lithium-ion battery is solved, and the battery is high Durability and high energy density.

CN113224377BActive Publication Date: 2024-11-29HONDA MOTOR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110061840.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-18
Publication Date
2024-11-29
Estimated Expiration
2041-01-18

Smart Images

  • Figure CN113224377B_ABST
    Figure CN113224377B_ABST
Patent Text Reader

Abstract

The problem to be solved by the present invention is to reduce the internal resistance in a solid battery having a LiAl-based negative electrode composite. In order to solve the above problem, the present invention is a solid battery 1, which includes a positive electrode layer 20, a negative electrode layer 30, and a solid electrolyte layer 40 arranged between the positive electrode layer 20 and the negative electrode layer 30, and the negative electrode layer 30 includes an aluminum layer 31 connected to the solid electrolyte layer 40, and an aluminum-lithium alloy layer 33.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer. Background Art

[0002] In the past, negative electrodes containing aluminum-lithium alloys were considered to have high capacity, but when used in general lithium-ion batteries using organic solvents, the durability of lithium-ion batteries is considered to be reduced because LiAl is ionized and dissolved or micronized in the solvent due to repeated charge and discharge (for example, see Non-Patent Document 1). Therefore, even if aluminum-lithium alloys are used as negative electrodes of lithium-ion batteries, it is difficult to utilize the original properties of aluminum-lithium alloys.

[0003] On the other hand, aluminum-lithium alloys are expected to be used as materials for the negative electrode of solid batteries that do not use organic solvents, etc. For example, a technology has been proposed that forms a negative electrode layer of a solid battery by press-molding a sulfide-based solid electrolyte material and a powdered aluminum-lithium alloy (see, for example, Non-Patent Document 1).

[0004] [Prior technical literature]

[0005] (Patent Document)

[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-154267

[0007] (Non-patent literature)

[0008] Non-patent document 1: LY Beaulieu et al., "Colossal Reversible Volume Changes in Lithium Alloys", Electrochemical and Solid-State Letters, 4(9), A137-A140 (2001) Summary of the invention

[0009] [Problems to be solved by the invention]

[0010] However, when a powdery aluminum-lithium alloy is used, the discharge capacity tends to decrease if charge and discharge are repeated.

[0011] An object of the present invention is to provide a solid battery whose discharge capacity is unlikely to decrease even when charge and discharge are repeated.

[0012] [Technical means to solve the problem]

[0013] (1) The present invention relates to a solid battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer arranged between the positive electrode layer and the negative electrode layer, wherein the negative electrode layer comprises a first aluminum layer connected to the solid electrolyte layer, and an aluminum-lithium alloy layer.

[0014] According to the invention of (1), the first aluminum layer 31 is connected to the solid electrolyte layer 40, so when the solid battery 1 is discharged, even if the lithium in the aluminum-lithium alloy layer 33 moves to the solid electrolyte layer 40 side, it will be alloyed with the aluminum in the aluminum layer 31 before reaching the solid electrolyte layer 40. Therefore, lithium is not likely to flow out from the solid electrolyte layer 40 side due to discharge, and the discharge capacity of the solid battery 1 is not likely to decrease even if charge and discharge are repeated.

[0015] (2) The solid battery according to (1), wherein X in the composition ratio of lithium to aluminum in the negative electrode layer LiXAl1-X (0≤X≤1) is 0.1≤X≤0.5.

[0016] According to the invention of (2), the total amount of aluminum can be ensured to increase the energy density and reduce the internal resistance of the solid battery.

[0017] (3) A solid battery according to (1) or (2), wherein, on the surface of the negative electrode layer on the side of the solid electrolyte layer, the ratio of the reflection intensity I220 of LiAl to the reflection intensity I110 of Al in X-ray diffraction measurement using CuKα rays is 0.1≤I220 / I110≤10.

[0018] According to the invention of (3), the aluminum layer on the solid electrolyte layer side of the negative electrode layer is fully alloyed, and the negative electrode lithium can be easily released to the positive electrode side without being absorbed by aluminum during discharge, thereby reducing the internal resistance of the solid battery.

[0019] (4) The solid battery according to any one of (1) to (3), wherein the negative electrode layer has a thickness of 10 to 400 μm.

[0020] According to the invention of (4), by making the film thickness of the negative electrode layer 30 within an appropriate range, it is possible to further suppress the reduction of aluminum and lithium from the negative electrode layer 30 due to charge and discharge. Thus, it is possible to provide a solid battery 1 whose discharge capacity is less likely to decrease even after repeated charge and discharge.

[0021] (5) The solid battery according to any one of (1) to (4), wherein the negative electrode layer further comprises a second aluminum layer, and the aluminum-lithium alloy layer is arranged between the first aluminum layer and the second aluminum layer.

[0022] According to the invention of (5), by configuring the aluminum layer into two layers, the total amount of aluminum in the negative electrode layer can be maintained and the internal resistance of the solid battery can be reduced. The reason is that a thinner first aluminum layer on the solid electrolyte layer side can be formed, which can easily release the negative electrode lithium during discharge.

[0023] (6) The solid battery according to any one of (1) to (5), wherein the solid electrolyte layer is composed of a sulfide-based solid electrolyte material.

[0024] According to the invention of (6), unlike the case where an aluminum-lithium alloy is used as the negative electrode of a lithium ion battery using an organic solvent, in a sulfide-based solid battery, there is no situation where the aluminum-lithium alloy is ionized and dissolved in the solid electrolyte, and high durability can be maintained. Thus, a sulfide-based solid battery can be provided whose discharge capacity is not easily reduced even if charge and discharge are repeated. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a diagram schematically showing a cross section of a solid battery according to a first embodiment of the present invention.

[0026] Figure 2 It is a figure which shows the X-ray diffraction spectrum chart of Comparative Example 1 immediately after charge and discharge.

[0027] Figure 3 It is a figure which shows the X-ray diffraction spectrum chart of Example 1 immediately after charge and discharge.

[0028] Figure 4 It is a figure which shows the X-ray diffraction spectrum chart of Example 2 immediately after charge and discharge.

[0029] Figure 5 It is a graph showing changes in direct current resistance (DCR) at each composition ratio of Examples 1 and 2 and Comparative Example 1.

[0030] Figure 6 This is a graph showing changes in charge and discharge efficiency at each composition ratio of Examples 1 and 2 and Comparative Example 1.

[0031] Figure 7 This is a graph showing changes in discharge capacity at each composition ratio of Examples 1 and 2 and Comparative Example 1.

[0032] Figure 8 It is a diagram schematically showing a cross section of a solid battery according to a second embodiment of the present invention. DETAILED DESCRIPTION

[0033] Below, while referring to the attached Figure 1 The first embodiment of the present invention will be described in detail. Figure 11 is an explanatory diagram showing a cross section of a solid battery according to a first embodiment of the present invention. Figure 1 As shown, the solid battery 1 includes a battery body 10, a negative electrode current collector 50, and a positive electrode current collector 60. In the embodiment, the solid battery refers to a solid battery in which the entire battery is solidified.

[0034] The negative electrode collector 50 and the positive electrode collector 60 are conductive plate-like members that sandwich the battery body 10 from both sides. The negative electrode collector 50 has a function of collecting electricity from the negative electrode layer 30 , and the positive electrode collector 60 has a function of collecting electricity from the positive electrode layer 20 .

[0035] The electrode collector material used for the negative electrode collector 50 is not particularly limited as long as it is a conductive material, and examples thereof include copper, nickel, stainless steel, vanadium, manganese, iron, titanium, cobalt, zinc, etc. Among them, copper and nickel are preferred because of their excellent conductivity and excellent current collection. The shape and thickness of the negative electrode collector 50 are not particularly limited as long as they are sufficient to collect current from the negative electrode layer 30.

[0036] Examples of the electrode collector material used for the positive electrode collector 60 include vanadium, aluminum, stainless steel, gold, platinum, manganese, iron, titanium, etc. Among them, aluminum is preferred. The shape and thickness of the positive electrode collector 60 are not particularly limited as long as they can collect current from the positive electrode layer 20.

[0037] The battery body 10 includes a positive electrode layer 20 functioning as a positive electrode, a negative electrode layer 30 functioning as a negative electrode, and a conductive solid electrolyte layer 40 located between the positive electrode layer 20 and the negative electrode layer 30 .

[0038] The positive electrode layer 20 is formed by pressing a material containing a positive electrode active material and a sulfide-based solid electrolyte. Examples of the positive electrode active material include layered positive electrode active materials such as LiCoO2, LiNiO2, LiCo1 / 3Ni1 / 3Mn1 / 3O2, LiVO2, and LiCrO2; spinel-type positive electrode active materials such as LiMn2O4, Li(Ni0.25Mn0.75)2O4, LiCoMnO4, and Li2NiMn3O8; and olivine-type positive electrode active materials such as LiCoPO4, LiMnPO4, and LiFePO4.

[0039] The sulfide-based solid electrolyte material used for the positive electrode layer 20 usually contains a metal element (M) as an ion capable of conducting, and sulfur (S). Examples of the above-mentioned M include Li, Na, K, Mg, Ca, etc., among which Li is preferred. In particular, the sulfide-based solid electrolyte material preferably contains Li, A (A is at least one selected from the group consisting of P, Si, Ge, Al, and B), and S. Furthermore, the above-mentioned A is preferably P (phosphorus). Furthermore, the sulfide-based solid electrolyte material may contain halogens such as Cl, Br, and I. The reason is that by containing halogens, ion conductivity can be improved. In addition, the sulfide-based solid electrolyte material may contain oxygen (O).

[0040] Examples of sulfide-based solid electrolyte materials having Li ion conductivity include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3- LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-ZmSn (where m and n are positive numbers. Z is any one of Ge, Zn, and Ga.), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-LiXMOy (where X and y are positive numbers. M is any one of P, Si, Ge, B, Al, Ga, and In.), etc. In addition, the above-mentioned record of "Li2S-P2S5" means a sulfide-based solid electrolyte material, which is formed using a raw material composition containing Li2S and P2S5, and the same applies to other records.

[0041] In addition, when the sulfide-based solid electrolyte material is formed using a raw material composition comprising Li2S and P2S5, the ratio of Li2S to the total amount of Li2S and P2S5 is, for example, preferably in the range of 70mol% to 80mol%, more preferably in the range of 72mol% to 78mol%, and further preferably in the range of 74mol% to 76mol%. The reason is that a sulfide-based solid electrolyte material having an original composition or an approximate composition thereof can be made, and a sulfide-based solid electrolyte material with higher chemical stability can be made. Here, generally speaking, the original (ortho) composition refers to the composition with the highest degree of hydration in the oxoacid (oxoacid) obtained by hydrating the same oxide. In this state, the crystal composition with the most Li2S added to the sulfide is called the original composition. In the Li2S-P2S5 system, Li3PS4 conforms to the original composition. In the case of Li2S-P2S5 sulfide solid electrolyte materials, the ratio of Li2S and P2S5 in the original composition can be obtained as Li2S:P2S5=75:25 on a molar basis. In addition, when Al2S3 or B2S3 is used to replace P2S5 in the above raw material composition, the preferred range is the same. In the Li2S-Al2S3 system, Li3AlS3 conforms to the original composition, and in the Li2S-B2S3 system, Li3BS3 conforms to the original composition.

[0042] In addition, when the sulfide-based solid electrolyte material is formed using a raw material composition containing Li2S and SiS2, the ratio of Li2S to the total amount of Li2S and SiS2 is, for example, preferably in the range of 60mol% to 72mol%, more preferably in the range of 62mol% to 70mol%, and further preferably in the range of 64mol% to 68mol%. The reason is that a sulfide-based solid electrolyte material having an original composition or a composition approximate thereto can be made, and a sulfide-based solid electrolyte material with higher chemical stability can be made. In the Li2S-SiS2 system, Li4SiS4 conforms to the original composition. In the case of a Li2S-SiS2-based sulfide-based solid electrolyte material, the ratio of Li2S and SiS2 of the original composition can be obtained as Li2S:SiS2=66.6:33.3 on a molar basis. In addition, when GeS2 is used to replace SiS2 in the above-mentioned raw material composition, the preferred range is the same. In the Li2S-GeS2 system, Li4GeS4 conforms to the original composition.

[0043] In addition, when the sulfide-based solid electrolyte material is formed using a raw material composition containing LiX (X = Cl, Br, I), the proportion of LiX is, for example, preferably in the range of 1 mol% to 60 mol%, more preferably in the range of 5 mol% to 50 mol%, and further preferably in the range of 10 mol% to 40 mol%.

[0044] In addition, the sulfide-based solid electrolyte material may be sulfide glass, crystallized sulfide glass, or a crystalline material obtained by a solid phase method. In addition, for example, sulfide glass can be obtained by mechanical grinding (ball mill, etc.) of the raw material composition. In addition, for example, crystallized sulfide glass can be obtained by heat treating sulfide glass at a temperature above the crystallization temperature. In addition, when the sulfide-based solid electrolyte material is a Li ion conductor, the Li ion conductivity at room temperature is, for example, preferably 1×10-5S / cm or more, and more preferably 1×10-4S / cm or more.

[0045] Furthermore, the positive electrode layer 20 may further contain a conductive material, a binder, and a solid electrolyte in addition to the above-mentioned sulfide-based solid electrolyte and positive electrode active material.

[0046] The negative electrode layer 30 is a member including a first aluminum layer 31 connected to the solid electrolyte layer 40, a second aluminum layer 32 connected to the negative electrode current collector 50, and an aluminum-lithium alloy layer 33 disposed between the first aluminum layer 31 and the second aluminum layer 32. The aluminum-lithium alloy layer 33 may include a non-alloyed lithium layer.

[0047] The first aluminum layer 31 and the second aluminum layer 32 are layers containing aluminum as a main component. The aluminum-lithium alloy layer 33 is a plate-shaped, foil-shaped, or film-shaped layer, and is formed when the solid battery 1 is charged, when the solid battery 1 is discharged, when aluminum and lithium are pressed and formed, and when the solid battery 1 is manufactured by the following joining process. In addition, in this specification, the aluminum-lithium alloy layer 33 is not limited to a layer containing aluminum-lithium alloy as a main component, and also includes a portion that is a starting point for forming an aluminum-lithium alloy.

[0048] In the present embodiment, the negative electrode layer 30 is composed of only the first aluminum layer 31, the second aluminum layer 32, and the aluminum-lithium alloy layer 33. The negative electrode layer 30 is formed by, for example, pressing plate-shaped (foil-shaped, film-shaped) aluminum and lithium. Thus, a negative electrode layer 30 is formed, which includes the first aluminum layer 31, the second aluminum layer 32, and the aluminum-lithium alloy layer 33. In addition, the negative electrode layer 30 can also be formed by evaporating lithium on plate-shaped (foil-shaped, film-shaped) aluminum by sputtering or the like.

[0049] The first aluminum layer 31 is configured to be connected to the solid electrolyte layer 40. Here, when the solid battery 1 is discharged, the lithium in the aluminum-lithium alloy layer 33 moves to the solid electrolyte layer 40 side, but a part of the lithium is alloyed with the aluminum in the first aluminum layer 31 before reaching the solid electrolyte layer 40, thereby being retained in the negative electrode layer 30. Therefore, as long as the film thickness of the first aluminum layer 31 is thick, it is not easy to release lithium from the solid electrolyte layer 40 side of the first aluminum layer 31 during discharge.

[0050] The second aluminum layer 32 is arranged in a manner connected to the negative electrode current collector 50. By dividing the aluminum layer into two layers, the total amount of aluminum in the entire negative electrode layer can be maintained and the internal resistance of the solid battery 1 can be reduced. The reason is that the first aluminum layer 31 on the solid electrolyte 40 layer side can be formed thinner, and the negative electrode lithium can be easily released during discharge.

[0051] The molar ratio and mass ratio of lithium to aluminum in the negative electrode layer 30 are not particularly limited, but in the present embodiment, the composition ratio of lithium to aluminum in the negative electrode layer 30 is LiXAl1-X (0≤X≤1) 0.1≤X≤0.5. Thus, the total amount of aluminum can be ensured to increase the energy density and reduce the internal resistance of the solid battery.

[0052] The film thickness of the negative electrode layer 30 is not particularly limited, but is preferably 10 to 400 μm, and more preferably 20 to 200 μm. In addition, in the stage before charge and discharge, the total film thickness of the first aluminum layer 31 and the second aluminum layer 32 is, for example, 5 to 200 μm, and preferably 10 to 100 μm. In addition, in the stage before charge and discharge, the film thickness of the first aluminum layer 31 is, for example, 5 to 100 μm, and preferably 25 to 50 μm. In addition, in the stage before charge and discharge, the film thickness of the aluminum-lithium alloy layer 33 is, for example, 5 to 200 μm, and preferably 10 to 100 μm.

[0053] By setting the thickness of the negative electrode layer 30 within an appropriate range, it is possible to suppress the reduction of aluminum and lithium from the negative electrode layer 30 due to charge and discharge. In addition, by setting the thickness of the first aluminum layer 31 within an appropriate range, it is possible to suppress the reduction of lithium from the negative electrode layer 30 during discharge.

[0054] The solid electrolyte layer 40 is a plate-shaped member formed of a sulfide-based solid electrolyte material. The sulfide-based solid electrolyte material is not particularly limited, but the same sulfide-based solid electrolyte material as that used for the positive electrode layer 20 can be used.

[0055] In addition, the manufacturing method of the solid battery 1 of the present embodiment includes a joining process, wherein the up-down direction is set as the stacking direction, and the lithium layer is stacked on the second aluminum layer 32, the first aluminum layer 31 is stacked on the aforementioned lithium layer, the solid electrolyte layer 40 is stacked on the first aluminum layer 31, and the positive electrode layer 20 is stacked on the solid electrolyte layer 40, and then the obtained stack is joined, thereby obtaining the solid battery 1.

[0056] As such a joining process, for example, the negative electrode collector 50, the second aluminum layer 32, the lithium layer, the aluminum layer 31 (negative electrode layer 30), the solid electrolyte layer 40, the positive electrode layer 20, and the positive electrode collector 60 are stacked in order and pressed. By pressing the stacked body in a state where the first aluminum layer 31 and the second aluminum layer 32 are arranged above and below the lithium layer, the lithium layer reacts with the first aluminum layer 31 and the second aluminum layer 32 to form an aluminum-lithium alloy layer 33. By pressing in a state where the lithium layer is sandwiched between two aluminum layers, aluminum-lithium alloying is performed well. Accordingly, a solid battery 1 is manufactured, which includes a positive electrode layer 20, a negative electrode layer, and a solid electrolyte layer 40, and the negative electrode layer includes a first aluminum layer 31, an aluminum-lithium alloy layer 33 and a second aluminum layer 32. In addition, when the lithium layer is not completely alloyed, a lithium layer may remain in the aluminum-lithium alloy layer 33.

[0057] [Example]

[0058] Next, the present invention will be described in detail based on Examples and Comparative Examples, but the present invention is not limited to these Examples.

[0059] A positive electrode composite was prepared by mixing a ternary positive electrode active material (LiCO1 / 3Ni1 / 3Mn1 / 3O2) coated with LiNbO3, a solid electrolyte, and a conductive additive in respective mass ratios of 75, 22, and 3 wt%. 15 mg of this positive electrode composite and 100 mg of solid electrolyte were weighed and pressed with a uniaxial press at a molding pressure of 10 ton / cm2 to obtain a laminate of a positive electrode layer 20 and a solid electrolyte layer 40. A negative electrode layer according to Comparative Example 1 and Examples 1 and 2 shown below was arranged on the opposite side of the positive electrode layer 20 of the solid electrolyte 400 to prepare a solid battery. After the initial charge and discharge test and the DC resistance test, the solid electrolyte layer 40 and the negative electrode layer were peeled off, and an X-ray diffraction measurement was performed from the solid electrolyte layer 40 side.

[0060] <Comparative Example 1>

[0061] Aluminum foil and lithium foil having a thickness of 100 μm were overlapped and pressed at 0.5 ton / cm2 to prepare the negative electrode layer of Comparative Example 1. The negative electrode layer of Comparative Example 1 consisted of an aluminum layer, an aluminum-lithium alloy layer, and a lithium layer from the solid electrolyte layer side.

[0062] <Example 1>

[0063] The first aluminum foil with a thickness of 50 μm, the lithium foil, and the second aluminum foil with a thickness of 50 μm were stacked in sequence and pressed at 0.5 ton / cm2 to form the negative electrode layer of Example 1. The negative electrode layer of Example 1 is composed of an aluminum layer, an aluminum-lithium alloy layer, and an aluminum layer from the solid electrolyte layer side.

[0064] <Example 2>

[0065] The first aluminum foil with a thickness of 75 μm, the lithium foil, and the second aluminum foil with a thickness of 25 μm were stacked in sequence and pressed at 0.5 ton / cm2 to form the negative electrode layer of Example 2. The negative electrode layer of Example 2 is composed of an aluminum layer, an aluminum-lithium alloy layer, and an aluminum layer from the solid electrolyte layer side.

[0066] The thickness of the lithium foil was changed to produce a plurality of negative electrodes of Comparative Example 1 and Examples 1 and 2, and the negative electrodes with the composition ratio of Li to Al changed were tested. The detailed configuration of each example is shown in the following Table 1. In Table 1, the first Al foil represents the first aluminum foil, and the second Al foil represents the second aluminum foil.

[0067] [Table 1]

[0068]

[0069]

[0070] A solid battery equipped with the negative electrodes of Comparative Example 1 and Examples 1 and 2 was prepared. These solid batteries were charged and discharged, and after charging and discharging, X-ray diffraction measurement was performed on the negative electrode of Example 1 from the positive electrode side (solid electrolyte layer side). The measurement was performed using an X-ray diffraction apparatus (UltIma-3 manufactured by Rigaku Corporation) in an inert environment using CuKα rays. At this time, the divergence longitudinal limiting slit was set to 10 mm, the scattering slit was set to open, and the measurement was performed with 2θ in the range of 20° to 80°. Figure 2 The X-ray diffraction measurement results of Comparative Example 1 are shown. Figure 3 The X-ray diffraction measurement results of Example 1 are shown. Figure 4The results of X-ray diffraction measurement of Example 2 are shown. In addition, regarding the composition ratio of Li to Al in the negative electrode layer, LiXAl1-X, X=0.13 and 0.44 were shown.

[0071] When observing Figures 2 to 4 When the peak showing the maximum intensity of Al, that is, the diffraction peak at the (1 1 0) plane (2θ=44.58±0.2°), and the peak showing the maximum intensity of LiAl, that is, the diffraction peak at the (2 2 0) plane (2θ=39.96±0.2°) were detected. Compared with the comparative example, the peak of LiAl detected in Examples 1 and 2 is relatively larger than the peak of Al, which shows that aluminum alloying has progressed on the solid electrolyte side of the negative electrode layer. Compared with Example 1, Example 2 detects a further larger peak of LiAl, which is larger than the peak of Al. That is, the thinner the thickness of the first aluminum layer on the solid electrolyte side, the greater the ratio of LiAl to Al.

[0072] In addition, the results of measuring the ratio I220 / I110 of the intensity I110 of the diffraction peak of Al at the (1 1 0) plane and the intensity I220 of the diffraction peak of LiAl at the (2 2 0) plane for each example shown in Table 1 are shown in Table 2. I220 / I110 is preferably 0.1≤I220 / I110≤10. More preferably, it is 5.9≤I220 / I110≤9.0. Since the aluminum layer on the solid electrolyte layer side of the negative electrode layer is fully alloyed, the negative electrode lithium can be easily released to the positive electrode side without being absorbed by aluminum during discharge, thereby reducing the internal resistance of the solid battery.

[0073] [Table 2]

[0074]

[0075]

[0076] Figure 5 The results of the DC resistance test are shown in Table 3. The DC resistance is measured under the condition of 10 seconds discharge at 0.1C to 5.0C at 25°C. The DC resistance of the solid batteries according to Examples 1 and 2 is smaller than that of the comparative example. In particular, when the Li ratio X is small and the Al ratio is high, it is observed that the resistance is significantly reduced relative to the comparative example. In the solid battery of Example 2 set to X=0.24, the DC resistance is reduced by about 72% compared with the comparative example, which is a significant improvement.

[0077] [Table 3]

[0078] Comparative Example Example 1 Example 2 <![CDATA[Li X Al 1-X ]]> <![CDATA[DC Resistance (Ω·cm 2 )]]> <![CDATA[DC Resistance (Ω·cm 2 )]]> <![CDATA[DC resistance (Ω·cm 2 )]]> X=0.44 49.28 33.74 51.08 X=0.38 79.32 56.78 60.23 X=0.32 109.87 85.84 47.36 X=0.24 202.24 110.26 56.29 X=0.13 210.39 140.95 97.33

[0079] Figure 6 , 7The results of the initial capacity test are shown in Tables 4 and 5. The initial capacity test was performed at 25°C and 0.1C (=0.186 mA / cm2). Figure 6 As shown in FIG. 1 , when the Li ratio X is small and the Al ratio is high, the charge and discharge efficiency of Examples 1 and 2 is further improved compared to the Comparative Example. Figure 7 As shown, the discharge capacity is equal to or higher than that of the comparative example. In particular, in Example 2, when the Li ratio X is small and the Al ratio is high, the discharge capacity is greatly improved.

[0080] [Table 4]

[0081]

[0082]

[0083] [Table 5]

[0084] <![CDATA[Li X Al 1-X ]]> Charge and discharge efficiency (%) Charge and discharge efficiency (%) Charge and discharge efficiency (%) X=0.44 79.5 74.4 81 X=0.38 81.4 76.2 80.1 X=0.32 81.2 80.7 80.8 X=0.24 64.1 64.5 80.9 X=0.13 53.7 63.1 63.5

[0085] The first embodiment of the present invention has been described above, but the present invention is not limited to the above embodiment. Next, a second embodiment of the present invention will be described.

[0086] Figure 8 1 is a diagram schematically showing the cross-sectional structure of a solid battery 11 according to a second embodiment of the present invention. The negative electrode layer 130 of the solid battery 11 is a member including: a first aluminum layer 31 connected to a solid electrolyte layer 40, and an aluminum-lithium alloy layer 34 disposed between the negative electrode current collector 50 and the first aluminum layer 31. The aluminum-lithium alloy layer 34 of this embodiment is aluminum-lithium alloyed in its entirety up to the second aluminum layer 32 in the first embodiment, and the composition ratio of Li to Al in the negative electrode layer 130 is the same as that in the first embodiment.

[0087] The aluminum-lithium alloy layer 34 of this embodiment is formed until the negative electrode current collector 50, and is formed with a larger aluminum ratio than the aluminum-lithium alloy layer 33 according to the first embodiment. Thus, a thinner first aluminum layer can be formed, and the total amount of aluminum in the negative electrode layer can be increased, thereby improving energy density.

[0088] In this embodiment, the negative electrode layer 130 preferably has the same film thickness as the negative electrode layer 30 of the first embodiment, a composition ratio of Li to Al LiXAl1-X (0≤X≤1), and a ratio of the reflection intensity I220 of LiAl to the reflection intensity I110 of Al in the X-ray diffraction measurement using CuKα rays on the surface of the solid electrolyte layer 40 side I220 / I110, which can produce the same effect as the solid battery 1 according to the first embodiment.

[0089] Reference numerals

[0090] 1.11: Solid-state batteries

[0091] 10, 100: Battery body

[0092] 20: Positive electrode layer

[0093] 30, 130: Negative electrode layer

[0094] 31: 1st aluminum layer

[0095] 32: Second aluminum layer

[0096] 33: Aluminum-lithium alloy layer

[0097] 34: Aluminum-lithium alloy layer

[0098] 40: Solid electrolyte layer

[0099] 50: Negative electrode collector

[0100] 60: Positive electrode collector

Claims

1. A solid battery comprising a positive electrode layer, a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, The negative electrode layer comprises a first aluminum layer connected to the solid electrolyte layer, an aluminum-lithium alloy layer, and a second aluminum layer connected to the negative electrode current collector, wherein the aluminum-lithium alloy layer is disposed between the first aluminum layer and the second aluminum layer. The thickness of the first aluminum layer is 75 μm, the thickness of the second aluminum layer is 25 μm, in, The composition ratio of lithium to aluminum in the negative electrode layer is Li X Al 1-X where X is 0.1≤X≤0.

5.

2. The solid state battery according to claim 1, in, The reflection intensity I of LiAl on the surface of the negative electrode layer on the solid electrolyte layer side in X-ray diffraction measurement using CuKα rays is 220 Reflection intensity relative to Al I 110 The ratio I 220 / I 110 0.1≤I 220 / I 110 ≤10.

3. The solid battery according to claim 1, in, The negative electrode layer has a thickness of 10 to 400 μm.

4. The solid state battery according to claim 1, in, The solid electrolyte layer is composed of a sulfide-based solid electrolyte material.

Citation Information

Patent Citations

  • All-solid battery, and manufacturing method thereof

    JP2014154267A

  • Solid-state battery and method for producing solid-state battery

    WO2019151376A1