Polystyrene resin composition
By adding specific hindered phenolic compounds and inorganic fillers to the polystyrene resin composition and optimizing the ratio of polyamide and SPS, the existing technology problems of reduced performance and insufficient fluidity in hot and humid environments have been solved, and high performance has been achieved. Tensile strength and heat resistance, suitable for manufacturing complex shaped molded products.
Patent Information
- Application Number
- CN201980086051.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-12-25
AI Technical Summary
The performance of existing polystyrene-based resin compositions is reduced due to the precipitation of copper compounds in hot and humid environments, and the long-term heat resistance and fluidity are not optimized enough, which poses challenges especially when manufacturing large-scale complex-shaped molded products.
A resin composition containing polystyrene-based resin with syndiotactic structure, polyamide, compatibilizer, specific hindered phenolic compound and inorganic filler is formulated in a specific ratio to improve long-term heat resistance and fluidity , the specific ingredients include polyamide, SPS, compatibilizer, hindered phenol compound and glass filler. The ratio of polyamide and SPS is optimized to improve mechanical strength and heat resistance.
The polystyrene-based resin composition has excellent long-term heat resistance and fluidity, good mechanical properties, high tensile strength and tensile elongation retention, and is suitable for manufacturing complex-shaped molded products.
Smart Images

Figure BDA0003130805220000181
Abstract
Description
Technical Field
[0001] The present invention relates to a polystyrene resin composition. Background Art
[0002] It is known that polystyrene resins having a syndiotactic structure (hereinafter sometimes referred to as SPS) have excellent mechanical strength, heat resistance, electrical properties, water absorption dimensional stability, chemical resistance, etc., and are expected to have a wide range of uses. Among them, due to the excellent chemical resistance, heat resistance, electrical properties and water absorption dimensional stability of SPS, its use in electrical / electronic equipment materials, vehicle / electronic components, home appliances, various machine parts, industrial materials, etc. has attracted attention.
[0003] It is known that by mixing SPS and polyamide, a resin composition having excellent balance of strength, toughness, heat resistance, chemical resistance, molding processability, etc. can be obtained. For example, Patent Document 1 discloses a styrene resin composition obtained by mixing SPS resin, polyamide and specific polyphenylene ether in a specific ratio.
[0004] Patent Document 2 discloses a polystyrene resin composition containing an SPS resin, polyamide, a specific compatibilizer, etc., and a specific copper compound, and reports that the heat aging resistance is further improved.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 03-126744
[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 08-319385 Summary of the invention
[0009] Problems to be solved by the invention
[0010] Although the polystyrene resin composition disclosed in Patent Document 2 has improved heat aging resistance, it is necessary to use a halide as a copper compound in order to obtain sufficient heat aging resistance. Copper halide precipitates halide on metal parts adjacent to the molded body, especially in a hot and humid environment, causing problems such as reduced product performance.
[0011] On the other hand, polyamide resin compositions containing phenolic antioxidants and sulfur-based antioxidants have also been proposed, but they are not yet sufficient for practical use in terms of long-term heat resistance and various physical properties. In addition, in terms of manufacturing large molded products or molded products with complex shapes by injection molding, it is also necessary to optimize the fluidity.
[0012] Solution to the problem
[0013] The present inventors have conducted intensive research to obtain a resin composition having long-term heat resistance and excellent fluidity, comprising a polystyrene resin having a syndiotactic structure. As a result, it was found that a resin composition comprising SPS, polyamide, a compatibilizer, a specific hindered phenol compound and an inorganic filler, and comprising SPS and the specific hindered phenol compound in a specific ratio can solve the above-mentioned problems. That is, the present invention relates to the following scheme.
[0014] [1] A polystyrene resin composition comprising:
[0015] (A) polyamide, (B) a polystyrene resin having a syndiotactic structure, (C) a compatibilizer having a polar group capable of reacting with the polyamide (A) and having compatibility with the polystyrene resin (B), (D) at least one hindered phenol compound selected from the group consisting of N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)] and 2',3'-bis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]hydrazine, and (E) an inorganic filler,
[0016] In 100 wt% of the total of the components (A) to (E), the polystyrene resin (B) accounts for 10.0 wt% to 30.0 wt% and the hindered phenol compound (D) accounts for 0.3 wt% to 1.0 wt%.
[0017] [2] The polystyrene resin composition according to [1] above, wherein the amount of the polyamide (A) is x wt%, the amount of the polystyrene resin (B) is y wt%, and x>y, based on 100 wt% of the total of the components (A) to (E).
[0018] [3] The polystyrene resin composition according to [1] or [2], wherein the amount of the polyamide (A) in 100% by weight of the total of the components (A) to (E) is 40.0% by weight or more and 80.0% by weight or less.
[0019] [4] The polystyrene resin composition according to any one of [1] to [3] above, wherein the amount of the compatibilizer (C) in the total amount of 100 wt % of the components (A) to (E) is 1.0 wt % or more and 10.0 wt % or less.
[0020] [5] A polystyrene resin composition according to any one of [1] to [4] above, wherein the amount of the inorganic filler (E) in the total 100 wt % of the components (A) to (E) is 25.0 wt % or more and 50.0 wt % or less.
[0021] [6] The polystyrene resin composition according to any one of [1] to [5], wherein the hindered phenol compound (D) is N,N′-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)].
[0022] [7] The polystyrene resin composition according to any one of [1] to [6] above, wherein the inorganic filler (E) is a glass filler.
[0023] [8] A molded article comprising the polystyrene resin composition according to any one of [1] to [7].
[0024] Effects of the Invention
[0025] According to the present invention, a polystyrene resin composition having excellent long-term heat resistance and excellent fluidity can be obtained. The polystyrene resin composition of the present invention has excellent mechanical properties and excellent long-term heat resistance such as high tensile strength retention and high tensile elongation retention. DETAILED DESCRIPTION
[0026] As a result of intensive studies, the present inventors have found that the above-mentioned problems can be solved by adjusting the ratio of SPS to a specific hindered phenol compound in the composition. This will be described in detail below.
[0027] In the present specification, the description of "XX to YY" means "XX or more and YY or less." In the present specification, the provisions considered as preferred can be arbitrarily adopted, and a combination of preferred provisions is more preferred.
[0028] The polystyrene resin composition of the present invention is characterized by comprising: (A) polyamide, (B) polystyrene resin having a syndiotactic structure, (C) a compatibilizer having a polar group capable of reacting with the polyamide (A) and having compatibility with the polystyrene resin (B), (D) at least one hindered phenol compound selected from N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)] and 2',3'-bis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]hydrazine, and (E) an inorganic filler, wherein the polystyrene resin (B) accounts for 10.0% by weight or more and 30.0% by weight or less, and the hindered phenol compound (D) accounts for 0.3% by weight or more and 1.0% by weight or less of the total 100% by weight of the components (A) to (E). The details are described below.
[0029] <Polyamide (A)>
[0030] As polyamide, all known polyamides can be used.
[0031] Examples of suitable polyamides include polyamide-4, polyamide-6, polyamide-6,6, polyamide-3,4, polyamide-12, polyamide-11, polyamide-6,10, polyamide-4T, polyamide-6T, polyamide-9T, polyamide-10T, and polyamides obtained from adipic acid and meta-xylylenediamine. Among them, polyamide-6,6 is suitable.
[0032] <Polystyrene Resin (B)>
[0033] The polystyrene resin (B) is an SPS having a high syndiotactic structure. In this specification, "syndiotactic" means that the ratio of phenyl rings in adjacent styrene units to be alternately arranged with respect to the plane formed by the main chain of the polymer block (hereinafter referred to as syndiotacticity) is high.
[0034] Regularity can be determined by carbon isotope nuclear magnetic resonance (NMR) 13 C-NMR method) for quantitative identification. 13 The C-NMR method can quantify the existence ratio of multiple consecutive structural units. For example, it can quantify the existence ratio of two consecutive monomer units in the form of a binary, quantify the existence ratio of three monomer units in the form of a ternary, and quantify the existence ratio of five monomer units in the form of a quinary.
[0035] In the present invention, "polystyrene resin having a high degree of syndiotactic structure" refers to polystyrene, poly(hydrocarbon-substituted styrene), poly(halogenated styrene), poly(halogenated alkyl styrene), poly(alkoxy styrene), poly(vinyl benzoate), hydrogenated polymers thereof or mixtures thereof, or copolymers containing them as main components, having a syndiotactic degree of usually 75 mol% or more, preferably 85 mol% or more, in terms of syndiotactic dyad (r), or usually 30 mol% or more, preferably 50 mol% or more in terms of syndiotactic pentad (rrrr).
[0036] Examples of the poly(hydrocarbon-substituted styrene) include poly(methylstyrene), poly(ethylstyrene), poly(isopropylstyrene), poly(tert-butylstyrene), poly(phenyl)styrene, poly(vinylnaphthalene) and poly(vinylstyrene). Examples of the poly(halogenated styrene) include poly(chlorostyrene), poly(bromostyrene) and poly(fluorostyrene), and examples of the poly(halogenated alkylstyrene) include poly(chloromethylstyrene). Examples of the poly(alkoxystyrene) include poly(methoxystyrene) and poly(ethoxystyrene).
[0037] Examples of the comonomer component of the copolymer containing the above-mentioned structural units include monomers of the above-mentioned styrene-based polymers, as well as olefin monomers such as ethylene, propylene, butene, hexene and octene; diene monomers such as butadiene and isoprene; cyclic olefin monomers, cyclic diene monomers, methyl methacrylate, maleic anhydride and acrylonitrile and other polar vinyl monomers.
[0038] Particularly preferred resins among the polystyrene resins include polystyrene, poly(p-methylstyrene), poly(m-methylstyrene), poly(p-tert-butylstyrene), poly(p-chlorostyrene), poly(m-chlorostyrene), and poly(p-fluorostyrene).
[0039] In addition, copolymers of styrene and p-methylstyrene, copolymers of styrene and p-tert-butylstyrene, copolymers of styrene and divinylbenzene, and the like are exemplified.
[0040] The polystyrene resin having a syndiotactic structure of the present invention preferably has a weight average molecular weight of 1×10 4 Above and 1×10 6 If the weight average molecular weight is 1×10 4 On the other hand, if the weight average molecular weight is 1×10 6 There is no problem with the fluidity of the resin during molding.
[0041] In this specification, unless otherwise specified, the weight average molecular weight refers to the value obtained by measuring by gel permeation chromatography at 145° C. using a GPC apparatus (HLC-8321GPC / HT) manufactured by Tosoh Corporation and a GPC column (GMHHR-H(S)HTC / HT) manufactured by Tosoh Corporation, using 1,2,4-trichlorobenzene as an eluent, and converting using a calibration curve of standard polystyrene. In addition, it may be simply referred to as “molecular weight”.
[0042] SPS (B) can be produced, for example, by polymerizing a styrene-based monomer (a monomer corresponding to the above-mentioned styrene-based polymer) using a condensation product of a titanium compound, water and trialkylaluminum (aluminoxane) as a catalyst in an inactive hydrocarbon solvent or in the absence of a solvent (for example, Japanese Patent Publication No. 2009-068022).
[0043] <Compatibilizer (C)>
[0044] As a compatibilizer (C), a compound having a polar group capable of reacting with polyamide (A) and having compatibility with SPS (B) is used. The compatibilizer (C) is formulated for the purpose of improving the compatibility between polyamide (A) and SPS (B), microdispersing the domain, and improving the interfacial strength between the components. The polar group capable of reacting with polyamide (A) refers to a functional group capable of reacting with the polar group possessed by polyamide. As specific examples, anhydride groups, carboxylic acid groups, carboxylic acid ester groups, carboxylic acid halide groups, carboxylic acid amide groups, carboxylate groups, sulfonic acid groups, sulfonic acid ester groups, sulfonyl chloride groups, sulfonamide groups, sulfonate groups, epoxy groups, amino groups, imide groups, oxazoline groups, etc. can be cited.
[0045] The substance having compatibility with SPS (B) refers to a substance containing a chain having compatibility with SPS in the polymer chain. For example, there can be mentioned polymers having syndiotactic polystyrene, atactic polystyrene, isotactic polystyrene, styrene-based polymers, polyphenylene ether, polyvinyl methyl ether, etc. as main chains, block chains or graft chains.
[0046] Specific examples of the compatibilizer (C) include styrene-maleic anhydride copolymer (SMA), styrene-glycidyl methacrylate copolymer, terminal carboxylic acid-modified polystyrene, terminal epoxy-modified polystyrene, terminal oxazoline-modified polystyrene, terminal amine-modified polystyrene, sulfonated polystyrene, styrene-based ionomers, styrene-methyl methacrylate-graft polymers, (styrene-glycidyl methacrylate)-methyl methacrylate-graft copolymers, acid-modified acrylic-styrene-graft polymers. , (styrene-glycidyl methacrylate)-styrene-graft polymer, polybutylene terephthalate-polystyrene-graft polymer, maleic anhydride-modified SPS, fumaric acid-modified SPS, glycidyl methacrylate-modified SPS, amine-modified SPS and other modified styrene polymers, (styrene-maleic anhydride)-polyphenylene ether-graft polymer, maleic anhydride-modified polyphenylene ether, fumaric acid-modified polyphenylene ether, glycidyl methacrylate-modified polyphenylene ether, amine-modified polyphenylene ether and other modified polyphenylene ether polymers, etc. Among them, modified polyphenylene ether and modified SPS are suitable, and maleic anhydride-modified polyphenylene ether and fumaric acid-modified polyphenylene ether are more suitable.
[0047] The modified polyphenylene ether can be obtained by modifying a known polyphenylene ether using a modifier, but if it can be used for the purpose of the present invention, it is not limited to this method. The polyphenylene ether is a known compound, and for this purpose, reference can be made to the specifications of U.S. Patent No. 3,306,874, U.S. Patent No. 3,306,875, U.S. Patent No. 3,257,357 and U.S. Patent No. 3,257,358. The polyphenylene ether is usually prepared by an oxidative coupling reaction using a disubstituted or trisubstituted phenol in the presence of a copper amine complex catalyst. The copper amine complex can use a copper amine complex derived from a primary amine, a secondary amine and a tertiary amine.
[0048] Examples of the polyphenylene ether include poly(2,3-dimethyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-chloromethyl-1,4-phenylene ether), poly(2-methyl-6-hydroxyethyl-1,4-phenylene ether), poly(2-methyl-6-n-butyl-1,4-phenylene ether), poly(2-ethyl-6-isopropyl-1,4-phenylene ether), poly(2-ethyl-6-n-propyl-1,4-phenylene ether), poly(2,3,6-trimethyl-1,4-phenylene ether), poly[2-(4'-methylphenyl)-1,4-phenylene ether], poly(2-bromo-6-phenyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2-phenyl- 4-phenylene ether), poly(2-chloro-1,4-phenylene ether), poly(2-methyl-1,4-phenylene ether), poly(2-chloro-6-ethyl-1,4-phenylene ether), poly(2-chloro-6-bromo-1,4-phenylene ether), poly(2,6-di-n-propyl-1,4-phenylene ether), poly(2-methyl-6-isopropyl-1,4-phenylene ether), poly(2-chloro-6-methyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dibromo-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether) and poly(2,6-dimethyl-1,4-phenylene ether), etc.
[0049] In addition, for example, copolymers derived from two or more phenolic compounds used in the preparation of the above homopolymers can also be used. In addition, graft copolymers and block copolymers of vinyl aromatic compounds such as polystyrene and the above polyphenylene ethers can also be mentioned. In particular, poly (2,6-dimethyl-1,4-phenylene ether) is preferably used.
[0050] As the modifier used in the modification of polyphenylene ether, compounds having olefinic double bonds and polar groups in the same molecule can be cited, specifically, for example, maleic anhydride, maleic acid, fumaric acid, maleic esters, fumaric esters, maleimide and its N-substituted body, maleate, fumarate, acrylic acid, acrylate, acrylamide, acrylate, methacrylic acid, methacrylate, methacrylamide, methacrylate, glycidyl methacrylate, etc. can be cited. Maleic anhydride, fumaric acid and glycidyl methacrylate are particularly preferably used among them. The above-mentioned various modifiers can be used alone or in combination of two or more.
[0051] The modified polyphenylene ether can be obtained, for example, by reacting the above-mentioned polyphenylene ether with a modifier in the presence of a solvent or other resin. The modification method is not particularly limited, and a known method can be used. Specifically, there can be mentioned: a method of reacting by melt kneading at a temperature in the range of 150 to 350°C using a roll mill, a Banbury mixer, an extruder, etc.; a method of heating the reaction in a solvent such as benzene, toluene, xylene, etc.; etc. In addition, in order to facilitate the reaction, it is also effective to allow the presence of free radical generators such as benzoyl peroxide; di-tert-butyl peroxide; dicumyl peroxide; tert-butyl perbenzoate; azobisisobutyronitrile; azobisisovaleronitrile; 2,3-diphenyl-2,3-dimethylbutane in the reaction system. The method of melt kneading in the presence of a free radical generator is particularly preferred.
[0052] As a compatibilizer (C), a modified SPS having a polar group can also be used. The modified SPS can be obtained, for example, by modifying the above-mentioned SPS using a modifier, but if it can be used for the purpose of the present invention, it is not limited to this method. There are no particular restrictions on the SPS used in the modification, but in particular, from the viewpoint of compatibility with other components, a copolymer of styrene and substituted styrene is preferably used. There are no particular restrictions on the composition ratio of the copolymer, but the content of the substituted styrene unit is preferably in the range of 3 to 50 mol%. If the content is 3 mol% or more, the modification is easy, and if it is 50 mol% or less, compatibility with other components can be maintained.
[0053] As particularly preferred substituted styrenes, for example, alkyl styrenes such as methyl styrene, ethyl styrene, isopropyl styrene, tert-butyl styrene, and vinyl styrene, halogenated styrenes such as chlorostyrene, bromostyrene, and fluorostyrene, halogenated alkyl styrenes such as chloromethyl styrene, methoxy styrene, and alkoxy styrenes such as ethoxy styrene can be cited. These substituted styrenes can be used alone or in combination of two or more. If the amount used is 5% by weight or less relative to SPS, the heat resistance of the composition can be maintained, and therefore, the above-mentioned polymer having an atactic structure can also be used.
[0054] As the modifier used in the modification of the above-mentioned SPS, a compound having an olefinic double bond and a polar group in the same molecule can be used. As such a modifier, for example, maleic anhydride, maleic acid, fumaric acid, maleic ester, fumaric ester, maleimide and its N-substituted body, maleate, fumarate, acrylic acid, acrylate, acrylamide, acrylate, methacrylic acid, methacrylate, methacrylamide, methacrylate, glycidyl methacrylate, etc. can be cited. Among them, maleic anhydride, fumaric acid or glycidyl methacrylate are particularly preferably used. These modifiers can be used alone or in combination of two or more.
[0055] Modified SPS can be obtained, for example, by reacting the above-mentioned SPS with a modifier in the presence of a solvent or other resin. There is no particular limitation on the method of modification, and a known method can be used. Specifically, it can be used: a method of reacting by melt kneading at a temperature in the range of 150 to 350°C using a roll mill, a Banbury mixer, an extruder, etc.; or a method of heating the reaction in a solvent such as benzene, toluene, xylene, etc. In order to facilitate these reactions, it is also effective to allow the presence of free radical generators such as benzoyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, tert-butyl perbenzoate, azobisisobutyronitrile, azobisisovaleronitrile, 2,3-diphenyl-2,3-dimethylbutane in the reaction system. The method of melt kneading in the presence of a free radical generator is particularly preferred. Among these modified SPS, maleic anhydride-modified SPS, fumaric acid-modified SPS, and glycidyl methacrylate-modified SPS are preferably used.
[0056] <Hindered Phenol Compound (D)>
[0057] The hindered phenol compound (D) is at least one selected from N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)] and 2',3'-bis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]hydrazine. By including the hindered phenol compound (D), the polystyrene resin composition of the present invention can have excellent long-term heat resistance.
[0058] From the viewpoint of long-term heat resistance and mechanical properties, it is particularly preferable to use N,N′-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)] as the hindered phenol compound (D).
[0059] <Inorganic filler (E)>
[0060] As an inorganic filler (E), in order to improve the adhesion with SPS (B), it is preferred to use an inorganic filler that has been surface treated with a coupling agent. As an inorganic filler, materials in known shapes such as fibrous, granular, and powdery can be used. As fibrous fillers, glass fibers, carbon fibers, whiskers, ceramic fibers, metal fibers, etc. can be cited. Specifically, as whiskers, there are boron, aluminum oxide, silicon dioxide, silicon carbide, etc., as ceramic fibers, there are gypsum, potassium titanate, magnesium sulfate, magnesium oxide, etc., and as metal fibers, there are copper, aluminum, steel, etc. As the shape of the filler, there are cross-shaped, felt-shaped, bundled and cut-shaped, short fibers, filamentous materials, and whiskers. In the case of a bundled and cut-shaped, a filler with a length of 0.05 to 50 mm and a fiber diameter of 5 to 20 μm is preferred. In the case of a cross-shaped or felt-shaped, a filler with a length of more than 1 mm, more preferably more than 5 mm, is preferred.
[0061] Examples of the granular or powdery filler include talc, carbon black, graphite, titanium dioxide, silicon dioxide, mica, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, oxysulfate, tin oxide, aluminum oxide, kaolin, silicon carbide, metal powder, glass powder, glass flakes, and glass beads.
[0062] Among these inorganic fillers, glass fillers such as glass yarn, glass fiber, glass roving, glass mat, glass powder, glass flakes and glass beads are particularly preferred.
[0063] As the coupling agent used for the surface treatment of the inorganic filler, for example, a silane coupling agent, a titanium coupling agent, etc. can be cited. Specific examples of the silane coupling agent include triethoxysilane, vinyl tri(β-methoxyethoxy)silane, γ-methacryloxypropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, β-(1,1-epoxycyclohexyl)ethyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-aminopropyl triethoxysilane, N-phenyl-γ-aminopropyl trimethoxysilane, γ-mercaptopropane The present invention also includes 1,2-dimethyl- ...
[0064] Specific examples of titanium coupling agents include triisostearyl isopropyl titanate, tri(dodecylbenzenesulfonyl) isopropyl titanate, tri(dioctyl pyrophospho) isopropyl titanate, bis(dioctyl phosphite) tetraisopropyl titanate, bis(ditridecyl phosphite) tetraoctyl titanate, tetrakis(1,1-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphite) tetraisopropyl titanate, The present invention also includes bis(dioctyl pyrophosphoryloxy)ethylene titanate, trioctyl isopropyl titanate, dimethacryloyl isostearyl titanate, isostearyl diacryloyl titanate, tri(dioctylphosphoryloxy) isopropyl titanate, tricumylphenyl isopropyl titanate, tri(N-amidoethyl, aminoethyl) isopropyl titanate, dicumylphenyl glycolate titanate, diisostearyl ethylene titanate, etc. Among them, tri(N-amidoethyl, aminoethyl) isopropyl titanate is preferred.
[0065] The surface treatment of the inorganic filler using the coupling agent can be carried out by a commonly known method without particular limitation. For example, the surface treatment can be carried out by a method suitable for the shape of the inorganic filler, i.e., a sizing treatment in which an organic solvent solution or suspension of the coupling agent is applied to the filler as a sizing agent, a dry mixing treatment using a Henschel mixer, a high-speed mixer, a Lödige mixer, a V-type mixer, etc., a treatment based on a spray method, an overall blending method, a dry selection method, etc. Among them, it is preferred to carry out the surface treatment by sizing treatment, dry mixing treatment, or spraying method.
[0066] For example, a glass film-forming substance may be used together with the coupling agent. The film-forming substance is not particularly limited, and examples thereof include polyester, urethane, epoxy, acrylic, vinyl acetate, polyether and other polymers.
[0067] The polystyrene resin composition of the present invention requires that, in the total of 100 wt % of polyamide (A), SPS (B), compatibilizer (C), specific hindered phenol compound (D) and inorganic filler (E), SPS (B) is 10.0 wt % or more and 30.0 wt % or less, and specific hindered phenol compound (D) is 0.3 wt % or more and 1.0 wt % or less. If the amount of SPS (B) and the amount of compound (D) do not satisfy the above ranges, long-term heat resistance is poor, and mechanical strength such as tensile breaking strength and tensile breaking elongation are reduced.
[0068] The amount of polyamide (A) in the total 100 wt% of components (A) to (E) contained in the polystyrene resin composition of the present invention is preferably 40.0 wt% or more and 80.0 wt% or less. When the amount of the polyamide (A) is 40.0 wt% or more, excellent mechanical strength such as high tensile strength at break and tensile elongation at break can be obtained. When the amount of the polyamide (A) is 80.0 wt% or less, excellent hydrolysis resistance is obtained.
[0069] The amount of polyamide (A) in the total 100 wt % of components (A) to (E) is more preferably 42.0 wt % or more, further preferably 45.0 wt % or more, further preferably 47.0 wt % or more, and more preferably 78 wt % or less, further preferably 75.0 wt % or less, further preferably 70 wt % or less.
[0070] As described above, the amount of SPS (B) in the total 100 wt% of the components (A) to (E) contained in the polystyrene resin composition of the present invention is required to be 10.0 wt% or more and 30.0 wt% or less. If the amount of SPS (B) is less than 10.0 wt%, the hydrolysis resistance of the molded product formed by molding the composition is poor, which is not preferred. If the amount of SPS (B) exceeds 30.0 wt%, it has an adverse effect on the mechanical strength, which is not preferred.
[0071] The amount of SPS (B) in the total 100 wt % of components (A) to (E) is preferably 14.0 wt % or more, more preferably 16 wt % or more, further preferably 18 wt % or more, and more preferably 28 wt % or less, more preferably 26 wt % or less, further preferably 24 wt % or less.
[0072] When the amount of polyamide (A) contained in the polystyrene resin composition of the present invention is x weight % and the amount of SPS (B) is y weight %, x>y is preferred. By satisfying the above relationship, excellent mechanical strength can be obtained. The amount of polyamide (A) x (weight %) and the amount of SPS y (weight %) are as described above.
[0073] The amount of the compatibilizer (C) in the total 100 wt % of the components (A) to (E) contained in the polystyrene resin composition of the present invention is preferably 1.0 wt % or more and 10.0 wt % or less. If the amount of the compatibilizer (C) is 1.0 wt % or more, the fuzzing of the pellets and molded products obtained from the composition of the present invention can be suppressed, and the production stability is excellent. If the amount of the compatibilizer (C) is 10.0 wt % or less, the fluidity of the composition can be maintained at a high level.
[0074] The amount of the compatibilizer (C) in the total 100 wt % of the above-mentioned components (A) to (E) is more preferably 1.5 wt % or more, further preferably 2.0 wt % or more, further preferably 2.5 wt % or more, particularly preferably 3.0 wt % or more, and more preferably 8.0 wt % or less, further preferably 6.0 wt % or less, further preferably 4.5 wt % or less, particularly preferably 3.5 wt % or less.
[0075] As mentioned above, the amount of the specific hindered phenol compound (D) in the total 100 wt% of the components (A) to (E) contained in the polystyrene resin composition of the present invention is required to be 0.3 wt% or more and 1.0 wt% or less. If the amount of the hindered phenol compound (D) is less than 0.3 wt%, the long-term heat resistance of the composition is poor, and thus the mechanical strength such as tensile strength at break and tensile elongation at break is reduced. If the amount of the hindered phenol compound (D) exceeds 1.0 wt%, it is not preferred because it may ooze out into the mold during molding, the appearance of the molded product may be poor, and the moldability may be poor.
[0076] The amount of the hindered phenol compound (D) in the total 100 wt % of the above-mentioned components (A) to (E) is preferably 0.35 wt % or more, more preferably 0.38 wt % or more, further preferably 0.41 wt % or more, and is preferably 0.95 wt % or less, more preferably 0.90 wt % or less, further preferably 0.85 wt % or less.
[0077] The amount of the inorganic filler (E) in the total 100 wt% of the components (A) to (E) contained in the polystyrene resin composition of the present invention is preferably 25.0 wt% or more and 50.0 wt% or less. If the amount of the inorganic filler (E) is 25.0 wt% or more, the mechanical strength of the molded product obtained from the composition is excellent. If the amount of the inorganic filler (E) is 50.0 wt% or less, the fluidity is excellent and good moldability can be maintained.
[0078] The amount of the inorganic filler (E) in the total 100 wt % of the above-mentioned components (A) to (E) is more preferably 26.0 wt % or more, further preferably 28.0 wt % or more, further preferably 29.5 wt % or more, and more preferably 45.0 wt % or less, further preferably 40.0 wt % or less, further preferably 35.0 wt % or less, and particularly preferably 30.0 wt % or less.
[0079] <Other ingredients>
[0080] The polystyrene resin composition of the present invention may contain other components such as a commonly used thermoplastic resin, a rubbery elastomer, an antioxidant, a filler, a crosslinking agent, a crosslinking aid, a nucleating agent, a plasticizer, a compatibilizer, a colorant and / or an antistatic agent, within the range not impairing the purpose of the present invention. Some of the above-mentioned other components are exemplified below.
[0081] Examples of the thermoplastic resin include styrene polymers such as atactic polystyrene, isotactic polystyrene, AS resin, and ABS resin; polyesters such as polyethylene terephthalate; polycarbonates; polyphenylene ethers; polysulfones; polyether sulfones; polyamides; polyphenylene sulfide (PPS); polyoxymethylene; acrylic polymers such as polyacrylic acid, polyacrylates; and polymethyl methacrylate; polyolefins such as polyethylene, polypropylene, polybutene, poly-4-methylpentene-1; and ethylene-propylene copolymers; halogen-containing vinyl compound polymers such as polyvinyl chloride, polyvinylidene chloride, and polyvinylidene fluoride; and mixtures thereof.
[0082] As the rubber-like elastic body, various rubber-like elastic bodies can be used. For example, natural rubber, polybutadiene, polyisoprene, polyisobutylene, chloroprene rubber, polysulfide rubber, thiokol rubber, acrylic rubber, urethane rubber, silicone rubber, epichlorohydrin rubber, styrene-butadiene block copolymer (SBR), hydrogenated styrene-butadiene block copolymer (SEB), styrene-butadiene-styrene block copolymer (SBS), hydrogenated styrene-butadiene-styrene block copolymer (SEBS), styrene-isoprene block copolymer (SIR), hydrogenated styrene-isoprene block copolymer (SEP), styrene-isoprene-styrene block copolymer (SIS), hydrogenated styrene-isoprene-styrene block copolymer (SEPS), styrene-butadiene random copolymer, hydrogenated styrene-butadiene ... Diene random copolymers, styrene-ethylene-propylene random copolymers, styrene-ethylene-butene random copolymers, ethylene-propylene rubber (EPR), ethylene propylene diene rubber (EPDM), or acrylonitrile-butadiene-styrene core-shell rubber (ABS), methyl methacrylate-butadiene-styrene core-shell rubber (MBS), methyl methacrylate-butyl acrylate-styrene core-shell rubber (MAS), octyl acrylate-butadiene-styrene core-shell rubber (MABS), alkyl acrylate-butadiene-acrylonitrile-styrene core-shell rubber (AABS), butadiene-styrene core-shell rubber (SBR), siloxane-containing core-shell rubber represented by methyl methacrylate-butyl acrylate siloxane, and other core-shell type particulate elastomers, or rubbers obtained by modifying them.
[0083] Among them, SBR, SBS, SEB, SEBS, SIR, SEP, SIS, SEPS, core-shell rubbers, and rubbers modified therefrom are particularly preferably used.
[0084] Examples of the modified rubber-like elastomer include styrene-butyl acrylate copolymer rubber, styrene-butadiene block copolymer (SBR), hydrogenated styrene-butadiene block copolymer (SEB), styrene-butadiene-styrene block copolymer (SBS), hydrogenated styrene-butadiene-styrene block copolymer (SEBS), styrene-isoprene block copolymer (SIR), hydrogenated styrene-isoprene block copolymer (SEP), styrene-isoprene-styrene block copolymer (SIS), hydrogenated styrene-isoprene-styrene block copolymer (SEPS), styrene-butadiene random copolymer, hydrogenated styrene-butadiene random copolymer, styrene-ethylene-propylene random copolymer, styrene-ethylene-butylene random copolymer, ethylene-propylene rubber (EPR), ethylene propylene diene rubber (EPDM), and the like modified with a modifier having a polar group.
[0085] Among them, it is particularly preferred to use rubbers modified from SEB, SEBS, SEP, SEPS, EPR, and EPDM. Specifically, maleic anhydride-modified SEBS, maleic anhydride-modified SEPS, maleic anhydride-modified EPR, maleic anhydride-modified EPDM, epoxy-modified SEBS, and epoxy-modified SEPS can be mentioned. These rubber-like elastomers can be used alone or in combination of two.
[0086] As fillers, in addition to inorganic fillers (E), organic fillers can also be added. As organic fillers, organic synthetic fibers, natural plant fibers, etc. can be mentioned. As specific examples of organic synthetic fibers, wholly aromatic polyamide fibers, polyimide fibers, etc. can be mentioned. The above-mentioned organic fillers can be used alone or in combination of two or more. Regarding the amount thereof added, it is preferably 1 to 350 parts by weight, and more preferably 5 to 200 parts by weight, relative to 100 parts by weight of the above-mentioned resin composition. If it is more than 1 part by weight, the effect of the filler can be fully obtained. If it is less than 350 parts by weight, the dispersibility will not be deteriorated and the formability will not be adversely affected.
[0087] <molded body>
[0088] The polystyrene resin composition of the present invention is prepared by blending / mixing the components (A) to (E) represented by the SPS resin and the above-mentioned various components as required. The blending and mixing can be carried out by the following method, that is, after pre-mixing using commonly used equipment such as a ribbon mixer, a drum mixer, a Henschel mixer, etc., using a Banbury mixer, a single-screw extruder, a twin-screw extruder, a multi-screw extruder, a kneader, etc.
[0089] The polystyrene resin composition of the present invention after the above-mentioned melt kneading, or the obtained pellets can be used as raw materials to produce various molded bodies by injection molding, injection compression molding, extrusion molding, blow molding, press molding, vacuum forming and foaming molding. In particular, the pellets obtained by melt kneading can be used to manufacture injection molded bodies based on injection molding and injection compression molding.
[0090] The shape of the molded article is not particularly limited, and examples thereof include sheets, films, fibers, nonwoven fabrics, containers, injection molded articles, blow molded articles, etc. The molded article formed by molding the polystyrene resin composition of the present invention is suitable as industrial materials such as electrical / electronic materials (connectors, printed substrates, etc.), industrial structural materials, automobile parts (vehicle-mounted connectors, hub covers, cylinder head covers, etc.), household electrical appliances, various machine parts, pipes, sheets, discs, films, etc.
[0091] Example
[0092] The present invention will be further specifically described by way of examples, but the present invention is not limited by these examples.
[0093] <Forming conditions>
[0094] Each component was blended at the ratio (weight %) described in the table and dry-blended using a Henschel mixer. Next, the resin composition was kneaded using a twin-screw extruder while side-feeding 30 weight % of glass fiber to produce pellets.
[0095] Except for the following evaluation (2) SFL, dumbbell-shaped tensile test pieces (Type A) were prepared using an injection molding machine [SH100A manufactured by Sumitomo Heavy Industries, Ltd.] under molding conditions of a cylinder temperature of 290°C and a mold temperature of 80°C in accordance with JIS K 7139:2009.
[0096] Physical property evaluations in Examples and Comparative Examples were performed as follows.
[0097] (1)MFR
[0098] The melt flow rate (MFR) of the pellets obtained in Examples and Comparative Examples was measured at a measurement temperature of 300° C. and a load of 2.16 kg in accordance with JIS K 7210-1:2014. The unit is g / 10 minutes.
[0099] (2)SFL
[0100] The pellets obtained in the examples and comparative examples were molded using an injection molding machine [manufactured by NIIGATAMACHINETECHNO, MD100] using a spiral flow mold with a barrel temperature of 290°C, a mold temperature of 80°C, a flow path thickness of 1 mm, and a width of 10 mm. The pressure settings were set to 50, 100, and 150 MPa, respectively, and the flow lengths (SFL: Spiral Flow Length) (mm) during the molding were measured.
[0101] (3) Tensile breaking strength and tensile breaking elongation test
[0102] Using the above-mentioned molding conditions, a dumbbell-shaped tensile test piece (Type A) was obtained in accordance with JIS K 7139:2009.
[0103] Next, the test piece was subjected to a tensile test in accordance with ISO 527-1:2012 (2nd edition) using a tensile testing machine (manufactured by Shimadzu Corporation, trade name: Autograph AG5000B) at room temperature with an initial chuck distance of 100 mm and a tensile speed of 5 mm / min to measure the tensile breaking strength (MPa) and tensile breaking elongation (%).
[0104] (4) Heat resistance test
[0105] The heat resistance was evaluated for long-term heat exposure. Specifically, the test piece used in (3) above was placed in an oven at 120°C for 1000 hours for exposure treatment. The test piece was taken out of the oven and subjected to a tensile test to determine the tensile strength retention rate and tensile elongation retention rate before and after the exposure treatment. The tensile test was performed in accordance with ISO527-1:2012 (2nd edition) in the same manner as in (3) above.
[0106] (5) Appearance evaluation
[0107] The dumbbell-shaped test pieces obtained under the above molding conditions were visually observed to evaluate the color tone. A was evaluated as no color change or almost no color change, and B was evaluated as color change.
[0108] Embodiment 1-2
[0109] Each component was blended at the ratio (weight %) shown in the table, and various evaluations were performed under the above-mentioned molding conditions. The components used are as follows.
[0110] Polyamide (A): Nylon 6,6 [Vydyne (registered trademark) 50BWFS manufactured by Ascend Corporation]
[0111] SPS(B): [Weight average molecular weight 200,000, 90ZC manufactured by Idemitsu Kosan Co., Ltd.]
[0112] Compatibilizer (C): Fumaric acid-modified polyphenylene ether [CX-1 manufactured by Idemitsu Kosan Co., Ltd.]
[0113] Hindered phenol compound (D): N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)] [manufactured by BASF Japan Ltd., Irganox 1098]
[0114] Inorganic filler (E): Glass fiber [manufactured by Nippon Electric Glass Co., Ltd., ECS03T-249H]
[0115] Comparative Examples 1 to 5
[0116] The following arbitrary compounds were used instead of the above hindered phenol compound (D), and the components were blended in the ratios shown in the table, and various evaluations were performed under the above molding conditions. Among them, in Comparative Example 5, the amount of the hindered phenol compound (D) was set to the ratios shown in the table, and the components were blended, and various evaluations were performed under the above molding conditions.
[0117] Copper iodide / potassium iodide compound: [manufactured by PolyAd, AL-120FF]
[0118] Pentaerythritol tetrakis{3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate: [manufactured by BASF Japan Ltd., Irganox 1010]
[0119] 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane: [ADEKA STAB AO-80 manufactured by ADEKA Corporation]
[0120] Tetrakis[3-(dodecylthio)propionate]methanetetrayltetramethylene ester: [ADEKA Corporation, ADEKASTAB AO-412S]
[0121] [Table 1]
[0122]
[0123] The examples having the composition of the present invention have excellent mechanical properties, excellent long-term heat resistance such as high tensile strength retention and high tensile elongation retention, and high fluidity. It was found that in Comparative Examples 1 to 4 not having the composition of the present invention and Comparative Example 5 in which the amount of the hindered phenol compound (D) did not meet the range of the present invention, the retention of mechanical properties after the heat resistance test was reduced.
Claims
1. A polystyrene resin composition comprising Component A: Polyamide, Component B: polystyrene resin having a syndiotactic structure, Component C: a compatibilizer having a polar group that can react with the polyamide (Component A) and is compatible with the polystyrene resin (Component B); Component D: at least one hindered phenol compound selected from N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)] and 2',3'-bis[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]hydrazine, and Ingredient E: Inorganic filler, Of the total 100% by weight of the components A to E, The polystyrene resin, namely component B, is 10.0% by weight or more and 30.0% by weight or less, The compatibilizer, i.e., component C, is 1.0% by weight or more and 3.5% by weight or less. The content of the hindered phenol compound, ie, the component D, is 0.3% by weight or more and 1.0% by weight or less.
2. The polystyrene resin composition according to claim 1, in, The amount of the polyamide (component A) in the total of 100% by weight of the components A to E is x% by weight, the amount of the polystyrene resin (component B) is y% by weight, and x>y.
3. The polystyrene resin composition according to claim 1 or 2, in, The amount of the polyamide, namely the component A, in the total 100% by weight of the components A to E is 40.0% by weight or more and 80.0% by weight or less.
4. The polystyrene resin composition according to claim 1 or 2, in, The amount of the polyamide, namely the component A, in the total 100% by weight of the components A to E is 47.0% by weight or more and 70% by weight or less.
5. The polystyrene resin composition according to claim 1 or 2, in, The amount of the polystyrene resin, ie, the component B, in the total 100% by weight of the components A to E is 18% by weight or more and 24% by weight or less.
6. The polystyrene resin composition according to claim 1 or 2, in, The amount of the compatibilizer, namely the component C, in the total 100% by weight of the components A to E is 3.0% by weight or more and 3.5% by weight or less.
7. The polystyrene resin composition according to claim 1 or 2, in, The amount of the hindered phenol compound, ie, the component D, in the total 100% by weight of the components A to E is 0.41% by weight or more and 0.85% by weight or less.
8. The polystyrene resin composition according to claim 1 or 2, in, The amount of the inorganic filler, namely the component E, in the total 100% by weight of the components A to E is 25.0% by weight or more and 50.0% by weight or less.
9. The polystyrene resin composition according to claim 1 or 2, in, The amount of the inorganic filler, namely the component E, in the total 100% by weight of the components A to E is 29.5% by weight or more and 30.0% by weight or less.
10. The polystyrene resin composition according to claim 1 or 2, in, The polyamide, i.e. component A, is a polyamide selected from polyamide-4, polyamide-6, polyamide-6,6, polyamide-3,4, polyamide-12, polyamide-11, polyamide-6,10, polyamide-4T, polyamide-6T, polyamide-9T, polyamide-10T and a polyamide obtained from adipic acid and meta-xylylenediamine.
11. The polystyrene resin composition according to claim 1 or 2, in, In the polystyrene resin component B, the ratio of phenyl rings in adjacent styrene units alternately arranged relative to the plane formed by the main chain of the polymer block is 75 mol% or more in terms of syndiotactic diad r or 30 mol% or more in terms of syndiotactic pentad rrrr.
12. The polystyrene resin composition according to claim 1 or 2, in, The polystyrene resin, component B, is Polystyrene; A poly(hydrocarbon-substituted styrene) selected from the group consisting of poly(methylstyrene), poly(ethylstyrene), poly(isopropylstyrene), poly(tert-butylstyrene), poly(phenyl)styrene, poly(vinylnaphthalene) and poly(vinylstyrene); A poly(halogenated styrene) selected from the group consisting of poly(chlorostyrene), poly(bromostyrene) and poly(fluorostyrene); Poly(haloalkylstyrene) as poly(chloromethylstyrene); A poly(alkoxystyrene) selected from poly(methoxystyrene) and poly(ethoxystyrene); Poly(vinyl benzoate); Hydrogenated polymers or mixtures thereof; or Copolymers with them as main components.
13. The polystyrene resin composition according to claim 12, in, The copolymer components other than the main component are composed of An olefin monomer selected from ethylene, propylene, butene, hexene and octene; A diene monomer selected from butadiene and isoprene; Cyclic olefin monomers; Methyl methacrylate; Maleic anhydride; and A comonomer component selected from the group consisting of polar vinyl monomers such as acrylonitrile.
14. The polystyrene resin composition according to claim 13, in, The cyclic olefin monomer is a cyclic diene monomer.
15. The polystyrene resin composition according to claim 1 or 2, in, The weight average molecular weight of the polystyrene resin (component B) is 1×10 4 Above and 1×10 6 the following.
16. The polystyrene resin composition according to claim 1 or 2, in, The polar group possessed by the compatibilizer, i.e. component C, which is capable of reacting with the polyamide, i.e. component A, is an anhydride group, a carboxylic acid group, a carboxylate group, a carboxylic acid halide group, a carboxamide group, a carboxylate group, a sulfonic acid group, a sulfonic ester group, a sulfonyl chloride group, a sulfonamide group, a sulfonate group, an epoxy group, an amino group, an imide group or an oxazoline group.
17. The polystyrene resin composition according to claim 1 or 2, in, The compatibilizer, component C, is a polymer having a chain selected from syndiotactic polystyrene, atactic polystyrene, isotactic polystyrene, styrene polymers, polyphenylene ether and polyvinyl methyl ether, which is compatible with the polystyrene resin, component B, as a main chain, block chain or graft chain.
18. The polystyrene resin composition according to claim 1 or 2, in, The compatibilizer, i.e., component C, is the following modified styrene polymer or modified polyphenylene ether polymer, Modified styrene polymer: one selected from styrene-maleic anhydride copolymer, styrene-glycidyl methacrylate copolymer, terminal carboxylic acid-modified polystyrene, terminal epoxy-modified polystyrene, terminal oxazoline-modified polystyrene, terminal amine-modified polystyrene, sulfonated polystyrene, styrene ionomer, styrene-methyl methacrylate-graft polymer, (styrene-glycidyl methacrylate)-methyl methacrylate-graft copolymer, acid-modified acrylic-styrene-graft polymer, (styrene-glycidyl methacrylate)-styrene-graft polymer, polybutylene terephthalate-polystyrene-graft polymer, maleic anhydride-modified SPS, fumaric acid-modified SPS, glycidyl methacrylate-modified SPS and amine-modified SPS; Modified polyphenylene ether polymer: one selected from the group consisting of (styrene-maleic anhydride)-polyphenylene ether-graft polymer, maleic anhydride-modified polyphenylene ether, fumaric acid-modified polyphenylene ether, glycidyl methacrylate-modified polyphenylene ether and amine-modified polyphenylene ether.
19. The polystyrene resin composition according to claim 1 or 2, in, The hindered phenol compound, namely component D, is N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)].
20. The polystyrene resin composition according to claim 1 or 2, in, The inorganic filler, i.e., component E, is a fibrous filler, or a granular or powdery filler as described below. Fibrous filler: one selected from glass fiber, carbon fiber, whisker, ceramic fiber and metal fiber; Granular or powdered filler: one selected from talc, carbon black, graphite, titanium dioxide, silicon dioxide, mica, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, oxysulfate, tin oxide, aluminum oxide, kaolin, silicon carbide, metal powder, glass powder, glass flakes and glass microspheres.
21. The polystyrene resin composition according to claim 1 or 2, in, The inorganic filler, namely component E, is a glass filler.
22. The polystyrene resin composition according to claim 1 or 2, in, The inorganic filler, ie, component E, is an inorganic filler surface-treated with a coupling agent.
23. The polystyrene resin composition according to claim 22, in, The coupling agent is a silane coupling agent or a titanium coupling agent as described below, Silane coupling agent: selected from triethoxysilane, vinyl tri(β-methoxyethoxy)silane, γ-methacryloxypropyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, β-(1,1-epoxycyclohexyl)ethyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, N-β-(aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-aminopropyl triethoxysilane, N-phenyl-γ-aminopropyl trimethoxysilane, γ-mercaptopropyl trimethoxysilane One of oxysilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyl-tri(2-methoxy-ethoxy)silane, N-methyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, 3-ureapropyltrimethoxysilane, 3-4,5-dihydroimidazolepropyltriethoxysilane, hexamethyldisilazane, N,N-bis(trimethylsilyl)urea and 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine; Titanium coupling agent: selected from triisostearyl isopropyl titanate, tri(dodecylbenzenesulfonyl) isopropyl titanate, tri(dioctyl pyrophosphoryl) isopropyl titanate, bis(dioctyl phosphite) tetraisopropyl titanate, bis(ditridecyl phosphite) tetraoctyl titanate, tetra(1,1-diallyloxymethyl-1-butyl)bis(ditridecyl) phosphite titanate, bis(dioctyl pyrophosphoryl) hydroxy One of acetate titanate, bis(dioctylpyrophosphoryloxy)ethylene titanate, trioctanoyl isopropyl titanate, dimethacryloyl isostearyl titanate, isostearyl diacryloyl titanate, tri(dioctylphosphoryloxy) isopropyl titanate, tricumylphenyl isopropyl titanate, tri(N-amidoethyl, aminoethyl) isopropyl titanate, dicumylphenyl glycolate titanate and diisostearyl ethylene titanate.
24. The polystyrene resin composition according to claim 1 or 2, in, The composition further contains one or more components selected from the group consisting of a thermoplastic resin, a rubbery elastomer, an antioxidant, a filler, a crosslinking agent, a crosslinking aid, a nucleating agent, a plasticizer, a compatibilizer, a colorant, and an antistatic agent.
25. The polystyrene resin composition according to claim 1 or 2, in, It further contains one or more components selected from the following thermoplastic resin, the following rubbery elastomer, and the following filler, Thermoplastic resin: a styrene polymer selected from atactic polystyrene, isotactic polystyrene, AS resin and ABS resin; polyester as polyethylene terephthalate; polycarbonate; polyether selected from polyphenylene ether, polysulfone and polyethersulfone; condensation polymer selected from polyamide, polyphenylene sulfide and polyoxymethylene; acrylic polymer selected from polyacrylic acid and polyacrylate; polyolefin selected from polyethylene, polypropylene, polybutene, poly-4-methylpentene-1 and ethylene-propylene copolymer; halogen-containing vinyl compound polymer selected from polyvinyl chloride, polyvinylidene chloride and polyvinylidene fluoride; and mixtures thereof. Rubber-like elastomers: from natural rubber; polybutadiene; polyisoprene; polyisobutylene; chloroprene rubber; polysulfide rubber; ethylsulfide rubber; acrylic rubber; urethane rubber; silicone rubber; epichlorohydrin rubber; styrene-butadiene block copolymer; hydrogenated styrene-butadiene block copolymer; styrene-butadiene-styrene block copolymer; hydrogenated styrene-butadiene-styrene block copolymer; styrene-isoprene block copolymer; hydrogenated styrene-isoprene-styrene block copolymer; hydrogenated styrene-isoprene-styrene block copolymer; styrene-butadiene random copolymer; hydrogenated styrene random copolymer of styrene-ethylene-propylene; random copolymer of styrene-ethylene-butylene; ethylene-propylene rubber; ethylene-propylene diene rubber; a core-shell type particulate elastomer selected from acrylonitrile-butadiene-styrene core-shell rubber, methyl methacrylate-butadiene-styrene core-shell rubber, methyl methacrylate-butyl acrylate-styrene core-shell rubber, octyl acrylate-butadiene-styrene core-shell rubber, alkyl acrylate-butadiene-acrylonitrile-styrene core-shell rubber, butadiene-styrene core-shell rubber and core-shell rubber containing silicone; and one selected from the group consisting of rubbers obtained by modifying these, Filler: One organic filler selected from the group consisting of organic synthetic fibers selected from wholly aromatic polyamide fibers and polyimide fibers, and natural plant fibers.
26. The polystyrene resin composition according to claim 25, in, The polyacrylate is polymethyl methacrylate.
27. The polystyrene resin composition according to claim 25, in, The amount of the organic filler is 1 part by weight or more and 350 parts by weight or less relative to 100 parts by weight of the polystyrene resin composition. It should be noted that the organic filler is not included in 100 parts by weight of the polystyrene resin composition. 28 . A molded article comprising the polystyrene resin composition according to claim 1 .
29. The molded product according to claim 28, which is produced by injection molding, injection compression molding, extrusion molding, blow molding, press molding, vacuum forming or foaming molding.
30. The molded article according to claim 28 or 29, which is a sheet, a film, a fiber, a nonwoven fabric, a container, an injection molded article or a blow molded article.
31. The molded article according to claim 28 or 29, which is an electrical / electronic material, an industrial structural material, a home appliance, a machine part, a tube, a sheet, a disk or a film.
32. The molded article according to claim 31, in, The mechanical component is an automobile component.
Citation Information
Patent Citations
Styrene-based resin composition
JP1991126744A
Polystyrene-based resin composition and its molding
JP1996319385A
Styrene-based polymer and its molded article
JP2009068022A
Copolymers of polyphenylene ethers
US3257357A
2, 6-dichloro-1, 4-polyphenylene ether
US3257358A