Organic film forming material, pattern forming method, and polymer
By using a combination of polymers with specific structures and organic solvents, the problems of easy peeling and insufficient solvent resistance of organic film materials at high temperatures have been solved, resulting in organic films with high heat resistance and solvent resistance, which improves the patterning ability and yield in the semiconductor manufacturing process.
Patent Information
- Application Number
- CN202110190159.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-19
- Filing Date
- 2021-02-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-02-18
AI Technical Summary
In the existing technology, there are problems in the semiconductor device manufacturing process, such as the organic film material being easy to peel off at high temperatures, insufficient solvent resistance, poor filling characteristics and planarization characteristics, resulting in insufficient patterning ability and difficulty in achieving high integration and high speed.
A polymer with a specific structure is used as an organic film forming material. Combined with organic solvents and surfactants, an organic film is formed through a multilayer photoresist method. The imide structure is used to improve heat resistance and adhesion, and high-boiling-point solvents are added to improve thermal fluidity and landfill characteristics.
It achieves high heat resistance, solvent resistance, filling properties and planarization properties of organic films, improves patterning ability, is suitable for organic film materials in multilayer resist methods, and enhances the manufacturing yield of semiconductor devices.
Smart Images

Figure CN113281964B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an organic film-forming material used in, for example, a semiconductor device manufacturing step, a pattern forming method based on a multilayer resist method using the material, and a polymer used in the organic film-forming material. Background Art
[0002] In the past, the high integration and high speed of semiconductor devices were achieved by miniaturizing the pattern size by shortening the wavelength of the light source in the photolithography technology (optical lithography) using light exposure, which is a general technology. In order to form such a fine circuit pattern on the semiconductor device substrate (processed substrate), a method of processing the processed substrate by dry etching is usually used, using a photoresist film formed with a pattern as an etching mask. However, in reality, there is no dry etching method that can obtain complete etching selectivity between the photoresist film and the processed substrate, so in recent years, a multilayer resist method is generally used for substrate processing. This method is as follows: an intermediate film with an etching selectivity different from that of the photoresist film (hereinafter referred to as the resist upper film) is interposed between the resist upper film and the processed substrate, and after the resist upper film obtains a pattern, the resist upper film pattern is used as a dry etching mask, and the pattern is transferred to the intermediate film by dry etching, and then the intermediate film is used as a dry etching mask, and the pattern is transferred to the processed substrate by dry etching.
[0003] As one of the multilayer resist methods, there is a three-layer resist method that can be implemented using a general resist composition used in a single-layer resist method. This method is to form an organic lower film (hereinafter referred to as an organic film) by coating and calcining an organic lower film material composed of a composition containing an organic resin on a processed substrate, and to form a silicon-containing film (hereinafter referred to as a silicon-containing resist lower film) by coating and calcining a resist lower film material composed of a composition containing a silicon-containing resin thereon, and to form a general organic photoresist film (hereinafter referred to as a resist upper film) thereon. After the resist upper film is patterned, if dry etching using fluorine-based gas plasma is performed, the organic resist upper film can obtain a good etching selectivity ratio relative to the silicon-containing resist lower film, so the resist upper film pattern can be transferred to the silicon-containing resist lower film. According to this method, even if a resist upper film that does not have sufficient film thickness required for directly processing a processed substrate or a resist upper film that does not have sufficient dry etching resistance required for processing a processed substrate is used, since the silicon-containing resist lower film is generally of equal or less film thickness than the resist upper film, the pattern can still be easily transferred to the silicon-containing resist lower film. Then, by using the silicon-containing resist lower film with the transferred pattern as a dry etching mask and transferring the pattern to an organic film by dry etching using oxygen or hydrogen gas plasma, the pattern can be transferred to an organic film with sufficient dry etching resistance required for processing a substrate. The organic film pattern with the transferred pattern is dry-etched using fluorine gas, chlorine gas, etc., and the pattern can be transferred to the substrate.
[0004] On the other hand, the miniaturization in the manufacturing steps of semiconductor devices has gradually approached the inherent limit of the wavelength of the light source used for optical lithography. Therefore, in recent years, some people have studied the high integration of semiconductor devices that do not rely on miniaturization. As for one of the methods, some people have studied semiconductor devices with complex structures such as multi-gate structures, and some of them have been put into practical use. When forming such a structure using a multilayer resist method, an organic film material that can fill the holes, trenches, fins and other tiny patterns formed on the processed substrate with a film without gaps, or fill the height difference, pattern-dense parts and non-patterned areas with a film and flatten (planarization) can be used. By using such an organic film material to form a flat organic film surface on a high-low difference substrate, the film thickness variation of the silicon-containing resist lower film and the resist upper film formed thereon can be suppressed, and the focus margin of optical lithography and the tolerance reduction in the subsequent processing steps of the processed substrate can be suppressed. In this way, semiconductor devices can be manufactured with a good yield. On the other hand, in the single-layer resist method, in order to fill the processed substrate with height differences and patterns, the thickness of the upper resist film will be thickened, which will cause the pattern to collapse after exposure and development, and the pattern shape to deteriorate due to reflection from the substrate during exposure. The pattern formation margin during exposure becomes narrower, making it difficult to manufacture semiconductor devices with a good yield.
[0005] As mentioned above, the organic film material needs to be processed by dry etching to form a pattern with a high aspect ratio, so the organic film is required to have not only the above-mentioned filling-flattening performance but also high dry etching resistance. In addition, the silicon-containing resist underlayer film on the organic film is also required to have high dry etching resistance. Therefore, compared with the silicon-containing resist underlayer film formed by spin coating, inorganic hard masks formed by CVD, ALD, etc. with high dry etching resistance are mostly selected as silicon-containing resist underlayer films. The temperature when forming the hard mask is usually above 300°C, so the organic film is also required to have high heat resistance that can withstand such a temperature. In addition, when the inorganic hard mask is formed by CVD or ALD, there is a possibility of peeling off from the substrate, so it is also required to have close adhesion to the processed substrate. It is important for organic film materials with excellent process margin to have these properties.
[0006] As for the known organic film materials, condensation resins formed by using carbonyl compounds such as ketones and aldehydes and aromatic alcohols as condensing agents for phenolic and naphthol compounds are known. For example, the fluorene bisphenol novolac resins recorded in Patent Document 1, the bisphenol compounds and novolac resins recorded in Patent Document 2, the novolac resins of adamantane phenol compounds recorded in Patent Document 3, and the bisnaphthol compounds and novolac resins recorded in Patent Document 4 can be exemplified. These bisphenol compounds and novolac resins are hardened by the cross-linking reaction caused by the action of oxygen in the air, and are formed into films with solvent resistance for the coating film materials used in the subsequent steps. Although they are excellent in hardening properties, the bisphenols as raw materials have room for improvement in heat resistance.
[0007] Prior art literature
[0008] Patent Literature
[0009] [Patent Document 1] Japanese Patent Application Publication No. 2005-128509
[0010] [Patent Document 2] Japanese Patent Application Publication No. 2006-293298
[0011] [Patent Document 3] Japanese Patent Application Publication No. 2006-285095
[0012] [Patent Document 4] Japanese Patent Application Publication No. 2010-122656
[0013] [Patent Document 5] Japanese Patent Application Publication No. 2013-137334
[0014] [Patent Document 6] Japanese Patent Application Publication No. 2010-122297 Summary of the invention
[0015] Problem that the invention aims to solve
[0016] The present invention is made to solve the above-mentioned problems and aims to provide an organic film forming material that can form an organic film with excellent solvent resistance, heat resistance, filling characteristics, flattening characteristics and pattern forming ability, a pattern forming method using the organic film forming material, and a polymer contained in the organic film forming material.
[0017] Solutions for solving problems
[0018] In order to achieve the above-mentioned object, the present invention provides an organic film-forming material characterized by comprising a polymer having a structure represented by the following general formula (1A) as a partial structure and an organic solvent.
[0019] [Chemistry 1]
[0020]
[0021] In the above general formula (1A), W1 represents a tetravalent organic group, W2 represents a single bond or a connecting group represented by the following formula (1B), R1 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, n1 represents an integer of 0 or 1, and n2 and n3 satisfy the relationship of 0≤n2≤6 and 0≤n3≤6 and 1≤n2+n3≤6.
[0022] [Chemistry 2]
[0023]
[0024] R2 and R3 are each independently hydrogen or an organic group having 1 to 30 carbon atoms. The organic group R2 and the organic group R3 may be bonded within the molecule to form a cyclic organic group.
[0025] Such an organic film-forming material can form an organic film that has heat curing properties like novolac resin, and has excellent heat resistance and good adhesion to the substrate because the main chain is composed of a skeleton containing an imide group. In addition, the organic film-forming material of the present invention can form an organic film that is excellent in solvent resistance, filling properties, planarization properties, and pattern forming ability.
[0026] The organic group W1 in the above general formula (1A) is preferably represented by the following formula (1C).
[0027] [Chemistry 3]
[0028]
[0029] W3 in the above formula (1C) is a single bond or a divalent organic group. The benzene ring in the above formula (1C) may have a substituent, and the substituent on the benzene ring may be bonded to the organic group in W3 to form a cyclic organic group.
[0030] It is preferred that the main chain has the above-mentioned partial structure from the viewpoint of exhibiting excellent heat resistance.
[0031] Alternatively, the organic group W1 in the general formula (1A) is preferably represented by any one of the following formulas (1D).
[0032] [Chemistry 4]
[0033]
[0034] The aromatic ring in the above formula may have a substituent.
[0035] Having the above-mentioned partial structure is preferred from the viewpoint of improving heat resistance, solubility in solvents, and thermal fluidity.
[0036] The linking group W2 in the above general formula (1A) is preferably represented by the following formula (1E).
[0037] [Chemistry 5]
[0038] W2=--CH2--(1E)
[0039] It is preferred from the viewpoint of hardenability that the main chain has the above-mentioned partial structure.
[0040] The Mw (weight average molecular weight) of the above-mentioned polymer is preferably 1,000 to 10,000.
[0041] When the organic film-forming material contains a polymer having an Mw in this range, outgassing during baking can be suppressed without impairing solubility in an organic solvent.
[0042] The polymer is more preferably a novolac resin having a partial structure represented by the general formula (1A).
[0043] The organic film-forming material containing such a polymer can form an organic film having further excellent solvent resistance.
[0044] The organic solvent is preferably a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
[0045] According to such an organic film-forming material, by adding a high-boiling-point solvent to the above-described polymer to impart thermal fluidity to the film, an organic film-forming material having both higher-level filling properties and planarization properties can be obtained.
[0046] Furthermore, the above-described organic film-forming material preferably contains one or more of a surfactant and a plasticizer.
[0047] If the organic film-forming material contains such a component, it can be made into an organic film-forming material which is more excellent in coating property and filling / planarization characteristics.
[0048] Furthermore, the present invention provides a pattern forming method, characterized in that: an organic film is formed on a workpiece using the organic film forming material of the present invention, a silicon-containing resist underlayer film is formed on the organic film using a silicon-containing resist underlayer film material, a resist upper layer film is formed on the silicon-containing resist underlayer film using a photoresist composition, a circuit pattern is formed on the resist upper layer film, the silicon-containing resist underlayer film is etched using the patterned resist upper layer film as a mask to transfer the pattern to the silicon-containing resist underlayer film, the organic film is etched using the silicon-containing resist underlayer film to which the pattern is transferred as a mask to transfer the pattern to the organic film, and further, the workpiece is etched using the organic film to which the pattern is transferred as a mask to form a pattern on the workpiece.
[0049] In addition, the present invention provides a pattern forming method, which is characterized by: forming an organic film on a workpiece using the organic film forming material of the present invention, forming a silicon-containing resist underlayer film on the organic film using a silicon-containing resist underlayer film material, forming an organic anti-reflective film on the silicon-containing resist underlayer film, forming a resist upper layer film using a photoresist composition on the organic anti-reflective film, and forming a four-layer film structure, forming a circuit pattern on the resist upper layer film, etching the organic anti-reflective film and the silicon-containing resist underlayer film using the patterned resist upper layer film as a mask, transferring the pattern to the organic anti-reflective film and the silicon-containing resist underlayer film, etching the organic film using the silicon-containing resist underlayer film with the pattern transferred as a mask, transferring the pattern to the organic film, and further etching the workpiece using the organic film with the pattern transferred as a mask to form a pattern on the workpiece.
[0050] In addition, the present invention provides a pattern forming method, which is characterized by: forming an organic film on a workpiece using the organic film forming material of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film and a silicon oxide nitride film on the organic film, forming a resist upper film on the inorganic hard mask using a photoresist composition, forming a circuit pattern on the resist upper film, etching the inorganic hard mask using the patterned resist upper film as a mask, transferring the pattern to the inorganic hard mask, etching the organic film using the patterned inorganic hard mask as a mask, transferring the pattern to the organic film, and further etching the workpiece using the patterned organic film as a mask to form a pattern on the workpiece.
[0051] In addition, the present invention provides a pattern forming method, which is characterized by: forming an organic film on a workpiece using the organic film forming material of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film and a silicon oxide nitride film on the organic film, forming an organic anti-reflective film on the inorganic hard mask, forming a resist upper film on the organic anti-reflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper film, etching the organic anti-reflective film and the inorganic hard mask using the patterned resist upper film as a mask, transferring the pattern to the organic anti-reflective film and the inorganic hard mask, etching the organic film using the patterned inorganic hard mask as a mask, transferring the pattern to the organic film, and further etching the workpiece using the patterned organic film as a mask to form a pattern on the workpiece.
[0052] The organic film-forming composition of the present invention can be preferably used in various pattern forming methods such as three-layer resist processing using a silicon-containing resist underlayer film or an inorganic hard mask, and four-layer resist processing using an organic antireflection film in addition to these. In the manufacturing process of a semiconductor device, if a circuit pattern is formed using such a pattern forming method of the present invention, a semiconductor device can be manufactured with a good yield.
[0053] At this time, the inorganic hard mask is preferably formed by a CVD method or an ALD method.
[0054] In the pattern forming method of the present invention, for example, an inorganic hard mask can be formed by such a method.
[0055] In this case, the circuit pattern forming method of the resist upper layer film preferably forms the circuit pattern by optical lithography using light with a wavelength of 10 nm to 300 nm, direct drawing using an electron beam, nanoimprinting, or a combination thereof.
[0056] In the formation of the aforementioned circuit pattern, the circuit pattern is preferably developed using an alkali developer or an organic solvent.
[0057] In the pattern forming method of the present invention, such a circuit pattern forming method and a developing method can be preferably used.
[0058] Furthermore, the aforementioned object to be processed is preferably a semiconductor device substrate, or a semiconductor device substrate on which any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed.
[0059] The aforementioned workpiece preferably contains silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0060] According to the pattern forming method of the present invention, the above-mentioned object to be processed can be processed to form a pattern.
[0061] The present invention also provides a polymer having a structure represented by the following general formula (1A) as a partial structure.
[0062] [Chemistry 6]
[0063]
[0064] In the above general formula (1A), W1 represents a tetravalent organic group, W2 represents a single bond or a connecting group represented by the following formula (1B), R1 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, n1 represents an integer of 0 or 1, and n2 and n3 satisfy the relationship of 0≤n2≤6 and 0≤n3≤6 and 1≤n2+n3≤6.
[0065] [Chemistry 7]
[0066]
[0067] R2 and R3 are each independently hydrogen or an organic group having 1 to 30 carbon atoms. The organic group R2 and the organic group R3 may be bonded within the molecule to form a cyclic organic group.
[0068] The polymer of the present invention, when used as a component of an organic film-forming material, can form an organic film having heat resistance, adhesion to a substrate, and filling / planarization properties.
[0069] In the polymer of the present invention, the organic group W1 in the general formula (1A) is preferably represented by the following formula (1C).
[0070] [Chemistry 8]
[0071]
[0072] W3 in the above formula (1C) is a single bond or a divalent organic group. The benzene ring in the above formula (1C) may have a substituent, and the substituent on the benzene ring may be bonded to the organic group in W3 to form a cyclic organic group.
[0073] It is preferred that the polymer has the above-mentioned partial structure in the main chain from the viewpoint of exhibiting heat resistance.
[0074] Or in the polymer of the present invention, the organic group W1 in the general formula (1A) is preferably represented by any one of the following formulas (1D).
[0075] [Chemistry 9]
[0076]
[0077] The aromatic ring in the above formula may have a substituent.
[0078] It is preferred that the polymer has the above-mentioned partial structure from the viewpoint of imparting solvent solubility and thermal fluidity.
[0079] The linking group W2 in the above general formula (1A) is preferably represented by the following formula (1E).
[0080] [Chemistry 10]
[0081] W2=--CH2--(1E)
[0082] It is preferred that the polymer has the above-mentioned partial structure from the viewpoint of imparting hardenability.
[0083] The Mw (weight average molecular weight) of the above-mentioned polymer is preferably 1,000 to 10,000.
[0084] When the organic film-forming material contains a polymer having an Mw in this range, outgassing during baking can be suppressed without impairing solubility in an organic solvent.
[0085] The polymer is more preferably a novolac resin having a partial structure represented by the general formula (1A).
[0086] The organic film-forming material containing such a polymer can form an organic film having further excellent solvent resistance.
[0087] Effects of the Invention
[0088] As described above, the present invention can provide a polymer useful as a component of an organic film forming material for forming an organic film having excellent heat resistance, excellent solvent resistance, excellent embedding characteristics, excellent planarization characteristics, and excellent adhesion to a substrate, and an organic film forming material containing the polymer. In addition, the organic film forming material has excellent heat resistance / solvent resistance / embedding characteristics / planarization characteristics / adhesion to a substrate, does not impair other characteristics such as etching resistance, and is an organic film forming material having excellent pattern forming ability, so it is extremely useful as a resist underlayer film material in a multilayer resist process such as a two-layer resist process, a three-layer resist process using a silicon-containing underlayer film or an inorganic hard mask, or a four-layer resist process using a silicon-containing underlayer film or an inorganic hard mask and an organic antireflection film, or a planarization material for semiconductor device manufacturing.
[0089] Furthermore, if it is an organic film forming method using the organic film forming material of the present invention, it can fully harden on the processed substrate and form a flat organic film. Furthermore, if it is a pattern forming method of the present invention, it can form a fine pattern with high precision on the processed substrate in a multilayer resist process. BRIEF DESCRIPTION OF THE DRAWINGS
[0090] [ Figure 1 ](A) to (F) are explanatory diagrams of an example of a pattern forming method utilizing a three-layer resist process according to the present invention.
[0091] [ Figure 2 ](G) to (I) are explanatory diagrams of the landfill characteristic evaluation method in the examples and comparative examples.
[0092] [ Figure 3 ](J) to (K) are explanatory diagrams of the planarization characteristic evaluation method in the examples and comparative examples. DETAILED DESCRIPTION
[0093] The present invention relates to an organic underlayer film (organic film) material used in a multilayer resist step for microfabrication in the manufacturing steps of semiconductor devices, etc., an organic film forming material that is effective as a flattening material for semiconductor device manufacturing, etc., and a pattern forming method using the organic film forming material that is suitable for exposure to extreme ultraviolet rays, KrF excimer laser (248nm), ArF excimer laser (193nm), F2 laser (157nm), Kr2 laser (146nm), Ar2 laser (126nm), soft X-rays (EUV), electron beams (EB), ion beams, X-rays, etc., and a polymer that is useful as a component of the aforementioned organic film forming material.
[0094] As described above, an organic film-forming material that can form an organic film having excellent solvent resistance, heat resistance, filling properties, planarization properties, and pattern forming ability is desired.
[0095] As a result of diligent research on the above-mentioned issues, the inventors of the present application discovered that an organic film forming material comprising a polymer having a partial structure containing an imide structure represented by the following general formula (1A) can form an organic film material that has excellent heat resistance, excellent solvent resistance, a high degree of filling characteristics, a high degree of planarization characteristics, excellent pattern forming ability and excellent adhesion to the substrate, thereby completing the present invention.
[0096] That is, the present invention is an organic film-forming material characterized by containing a polymer having a structure represented by the following general formula (1A) as a partial structure and an organic solvent.
[0097] [Chemistry 11]
[0098]
[0099] In the above general formula (1A), W1 represents a tetravalent organic group, W2 represents a single bond or a connecting group represented by the following formula (1B), R1 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, n1 represents an integer of 0 or 1, and n2 and n3 satisfy the relationship of 0≤n2≤6 and 0≤n3≤6 and 1≤n2+n3≤6.
[0100] [Chemistry 12]
[0101]
[0102] R2 and R3 are each independently hydrogen or an organic group having 1 to 30 carbon atoms. The organic group R2 and the organic group R3 may be bonded within the molecule to form a cyclic organic group.
[0103] The present invention will be described in detail below, but the present invention is not limited thereto. In the formulae shown below, dotted lines represent bonds between groups or atomic groups represented by the respective formulae in the general formula (1A) and other groups or atomic groups.
[0104] <Polymer for forming organic film>
[0105] The polymer of the present invention is a polymer having a structure represented by the following general formula (1A) as a partial structure.
[0106] [Chemistry 13]
[0107]
[0108] In the above general formula (1A), W1 represents a tetravalent organic group, W2 represents a single bond or a connecting group represented by the following formula (1B), R1 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, n1 represents an integer of 0 or 1, and n2 and n3 satisfy the relationship of 0≤n2≤6 and 0≤n3≤6 and 1≤n2+n3≤6.
[0109] [Chemistry 14]
[0110]
[0111] R2 and R3 are each independently hydrogen or an organic group having 1 to 30 carbon atoms. The organic group R2 and the organic group R3 may be bonded within the molecule to form a cyclic organic group.
[0112] By making a closed-loop imide structure as in the general formula (1A) above in advance, there will be no desorption reaction of water and the like generated as a by-product when the imide precursor such as amic acid is closed, the shrinkage of the film is suppressed, and the planarization characteristics of the organic film will not be damaged. By making a stable imide structure in advance, the decomposition caused by the equilibrium reaction of the imide compound precursor can be suppressed, and the storage stability is also excellent. As for the substituent represented by OR1, it can also be appropriately selected according to the use purpose. A hydroxyl group can be selected to impart solubility, an alkyloxy group can be selected to impart fluidity, and an alkenyl group, an alkynyloxy group, etc. can be selected to impart hardening properties under inert gas. In addition, by appropriately selecting the structure of the connecting group part represented by W2, various physical properties such as etching resistance and optical properties can be adjusted. In addition, in addition to contributing to heat resistance, the imide structure also contributes to improving the adhesion to the substrate. By improving the adhesion, the film peeling when an inorganic hard mask obtained by using a CVD method or an ALD method is formed directly above the organic film can be prevented, and an organic film with excellent process margin can be formed.
[0113] Other organic film materials having an imide structure include polyimides described in Patent Documents 5 and 6. These polyimides have excellent adhesion and heat resistance, but due to their rigid structure, they lack solvent solubility and have problems with versatility. In addition, polyimide itself has no curing properties, so it is necessary to add components such as a crosslinking agent and an acid generator as a crosslinking catalyst, which may damage the heat resistance of the polyimide itself.
[0114] On the other hand, the organic film-forming polymer of the present invention can exhibit appropriate solvent solubility due to the partial structure represented by the above general formula (1A) containing an aromatic ring portion having an OR1 group in addition to the imide structure, and can exhibit excellent solvent resistance and heat resistance after curing.
[0115] The partial structure of the imide ring containing W1 in the general formula (1A) above can be exemplified by the following, and these aromatic rings may also have substituents, and the substituents can be exemplified by an alkyl group having 1 to 10 carbon atoms, an alkynyl group and an alkenyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, a nitro group, a halogen group, a nitrile group, an alkoxycarbonyl group having 1 to 10 carbon atoms, and an alkanoyloxy group having 1 to 10 carbon atoms. Among them, those having a naphthalene ring with n1=1 are preferred from the viewpoint of heat resistance.
[0116] [Chemistry 15]
[0117]
[0118] [Chemistry 16]
[0119]
[0120] The substituent represented by OR1 on the aromatic ring can be exemplified by the following, and n4 in the following formula represents an integer of 1 to 9. When R1 in the above general formula has an aryl group, it may also have a substituent such as a hydroxyl group, a trifluoromethyl group, an alkyl group having 1 to 10 carbon atoms, an alkynyl group and an alkenyl group having 3 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkynyloxy group and an alkenyloxy group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, a nitro group, a halogen group, a nitrile group, an alkoxycarbonyl group having 1 to 10 carbon atoms, and an alkanoyloxy group having 1 to 10 carbon atoms. Among them, a propargyloxy group is preferred from the viewpoint of curability.
[0121] [Chemistry 17]
[0122]
[0123] The organic group W1 in the general formula (1A) can be exemplified by the following, and these aromatic rings may also have substituents, and the substituents can be exemplified by: hydroxyl, trifluoromethyl, alkyl having 1 to 10 carbon atoms, alkynyl and alkenyl having 3 to 10 carbon atoms, alkyloxy having 1 to 10 carbon atoms, alkynyloxy and alkenyloxy having 3 to 10 carbon atoms, aryl having 6 to 10 carbon atoms, nitro, halogen, nitrile, alkoxycarbonyl having 1 to 10 carbon atoms, and alkanoyloxy having 1 to 10 carbon atoms.
[0124] [Chemistry 18]
[0125]
[0126] [Chemistry 19]
[0127]
[0128] [Chemistry 20]
[0129]
[0130] [Chemistry 21]
[0131]
[0132] [Chemistry 22]
[0133]
[0134] [Chemistry 23]
[0135]
[0136] In the organic film-forming polymer of the present invention, it is preferable that the organic group W1 in the general formula (1A) is represented by the following formula (1C).
[0137] [Chemistry 24]
[0138]
[0139] W3 in the above formula (1C) is a single bond or a divalent organic group. The benzene ring in the above formula (1C) may have a substituent, and the substituent on the benzene ring may be bonded to the organic group in W3 to form a cyclic organic group.
[0140] As for W3, specific examples include single bonds or the following. These aromatic rings may also have substituents, such as hydroxyl, trifluoromethyl, alkyl having 1 to 10 carbon atoms, alkynyl and alkenyl having 3 to 10 carbon atoms, alkyloxy having 1 to 10 carbon atoms, alkynyloxy and alkenyloxy having 3 to 10 carbon atoms, aryl having 6 to 10 carbon atoms, nitro, halogen, nitrile, alkoxycarbonyl having 1 to 10 carbon atoms, alkanoyloxy having 1 to 10 carbon atoms, etc. The dotted line in the figure below indicates the atomic bonds on the aromatic ring.
[0141] [Chemistry 25]
[0142]
[0143] It is preferred that the main chain has the above-mentioned partial structure from the viewpoint of exhibiting excellent heat resistance.
[0144] Or the organic film-forming polymer of the present invention is preferably a polymer in which the organic group W1 in the general formula (1A) is represented by any one of the following formulas (1D). In particular, in view of solvent solubility and fluidity, it is preferred to have one or more of a hexafluoroisopropylidene group, an ether bond, a fluorene structure, and a dihydroindene structure.
[0145] [Chemistry 26]
[0146]
[0147] The aromatic ring in the above formula may have a substituent.
[0148] If the partial structure is as described above, it is preferred from the viewpoint of improving heat resistance, solubility in solvents, and thermal fluidity. Among the above, as for the connecting group of the main chain, the structure having a hexafluoroisopropylidene group, the structure having an ether bond, and the structure having a fluorene structure are particularly preferred. The ether bond functions as a soft connecting group and can impart thermal fluidity and solvent solubility. Similarly, the hexafluoroisopropylidene group and the fluorene structure become substituents with large steric hindrance in the main chain, and the coagulation of the molecules of the imide group is suppressed, so that the same effect as the ether bond can be obtained. Thereby, the landfill characteristics / flattening characteristics can be improved without compromising the heat resistance.
[0149] In the organic film-forming polymer of the present invention, W2 represented by the above general formula (1B) can be exemplified by a single bond or the following.
[0150] [Chemistry 27]
[0151]
[0152] In the organic film-forming polymer of the present invention, when the linking group W2 in the general formula (1A) is represented by the following formula (1E), it is particularly preferred from the viewpoints of curability, raw material availability, and ease of polymer production.
[0153] [Chemistry 28]
[0154] W2=--CH2--(1E)
[0155] The Mw (weight average molecular weight) of the polymer is preferably 1000 to 10000, more preferably 1000 to 5000. The weight average molecular weight can be determined as a polystyrene-equivalent weight average molecular weight (Mw) by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent.
[0156] If the molecular weight is within this range, solubility in organic solvents can be ensured, and sublimates generated during baking can be suppressed. In addition, the thermal fluidity of the polymer for forming an organic film is good, so when it is mixed with the composition, it can well fill the fine structure formed on the substrate, and not only that, it can also form an organic film with a flat substrate as a whole.
[0157] The polymer is more preferably a novolac resin having a partial structure represented by the general formula (1A).
[0158] The above polymer which is a novolac resin can be represented by the above general formula (1A) wherein W2 is a linking group represented by the above general formula (1B).
[0159] The organic film-forming material containing such a polymer can form an organic film having further excellent solvent resistance.
[0160] [Method for producing polymer]
[0161] The means for obtaining the polymer used in the organic film forming material of the present invention include, for example, the polycondensation reaction of the imide compound represented by the following partial structure of the general formula (1A) with an aldehyde compound or a ketone compound. However, the case where W2 is a single bond is excluded. R1, R2, R3, n1, n2, n3 and W1 in the following formula are the same as those described above. When one or both of R2 and R3 are hydrogen atoms, it represents polycondensation with aldehyde, and in other cases, it represents polycondensation with ketone.
[0162] [Chemistry 29]
[0163]
[0164] The imide compound used in the polycondensation can be obtained by thermal imidization or chemical imidization (STEP2) after obtaining the intermediate amic acid compound (STEP1) by the reaction of the amine compound and tetracarboxylic anhydride shown below. The amine compound or tetracarboxylic anhydride can also be used alone or as a mixture of two or more. These can be appropriately selected and combined according to the required characteristics. W1, W2, and R1 in the following formula are the same as above.
[0165] [Chemistry 30]
[0166]
[0167] The amide acid of the intermediate represented by STEP1 can usually be prepared in an organic solvent at room temperature or under cooling or heating as needed. Examples of the solvent used include: alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, propylene glycol, diethylene glycol, glycerol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether; ethers such as diethyl ether, dibutyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, 1,4-dioxane; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, trichloroethylene; hexane, heptane, benzene, toluene, xylene, isocyanate, chlorinated solvents such as ... Hydrocarbons such as propylbenzene; nitriles such as acetonitrile; ketones such as acetone, methyl ethyl ketone, isobutyl methyl ketone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol methyl ether acetate, and γ-butyrolactone; aprotic polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric triamide, etc., which can be used alone or in combination of two or more.
[0168] The synthesis of these may also use a base catalyst as needed, and the base catalyst may include: inorganic base compounds such as sodium bicarbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, potassium phosphate, etc.; organic bases such as triethylamine, diisopropylethylamine, N,N-dimethylaniline, pyridine, 4-dimethylaminopyridine, etc., and these may be used alone or in combination of two or more.
[0169] As for the reaction method, there are the following methods: adding the amine compound and the tetracarboxylic anhydride to the solvent at one time; dispersing or dissolving the amine compound and the tetracarboxylic anhydride respectively, or mixing and dispersing or dissolving the obtained ones, dropping and adding; after dispersing or dissolving any one of the amine compound and the tetracarboxylic anhydride in the solvent, dropping and adding the other one dispersed or dissolved in the solvent. In addition, when adding a variety of amine compounds and tetracarboxylic anhydrides respectively, the method of pre-mixing and reacting them can be listed, and they can also be reacted individually in sequence. When using a catalyst, the following methods can be listed: adding the amine compound or the tetracarboxylic anhydride at one time; pre-dispersing or dissolving the catalyst and then dropping it. The reaction solution of the amic acid compound of the intermediate obtained can continue the imidization step of STEP2, or it can be diluted with an organic solvent in order to remove the unreacted raw materials, catalysts, etc. present in the system, and then separated and washed or crystallized with a poor solvent, and the reaction intermediate is recovered in the form of powder.
[0170] The imidization step shown in STEP 2 can be synthesized by thermal imidization or chemical imidization. These methods can be appropriately selected according to the thermal stability of the substituent of the target imide compound and the reactivity of the introduced substituent with the reagent used in the chemical imidization.
[0171] In the case of thermal imidization, the reaction solution of the amic acid obtained in step 1 or when recovered as powder is dissolved in a soluble solvent, a solvent capable of azeotropy with water is added, and the mixture is heated to 100°C to 250°C to carry out imidization by dehydration ring-closure reaction while removing the generated water.
[0172] The solvents that can be used at this time include: esters such as γ-butyrolactone, N-methyl-2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, N,N-dimethylformamide and other polar solvents; benzene, toluene, xylene, mesitylene and other non-polar solvents, etc. It is preferred to use these solvents alone or in mixture and heat them, and dehydrate them while distilling the water generated by the ring closure to the outside of the system.
[0173] In the case of chemical imidization, the reaction solution of the imide precursor obtained in step 1 or when recovered as powder is dissolved in a soluble solvent in advance, and then a base catalyst and an acid anhydride as a dehydrating agent are added and heated to carry out imidization.
[0174] The base catalyst used in chemical imidization can be exemplified by pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc., wherein pyridine has the appropriate alkalinity required for the reaction to proceed, so it is preferred. The dehydrating agent can be exemplified by acetic anhydride, trimellitic anhydride, pyromellitic anhydride, trifluoroacetic anhydride, polyphosphoric acid, phosphorus pentoxide, phosphorus pentachloride, thionyl chloride, etc., and acetic anhydride is preferably used from the viewpoint of purification after the reaction. In addition, the base catalyst and the dehydrating agent can be used alone or in the form of a mixture of two or more, and these can be appropriately controlled by appropriately adjusting the catalyst amount, the dehydrating amount, the reaction temperature, and the reaction time in response to the required performance of the compound as the purpose, to appropriately control the imidization rate.
[0175] The solvent used at this time is not particularly limited as long as it is a solvent inactive in the above reaction, and examples thereof include: ethers such as diethylene glycol diethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, and 1,4-dioxane; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; hydrocarbons such as hexane, heptane, benzene, toluene, xylene, and cumene; nitriles such as acetonitrile; ketones such as acetone, methyl ethyl ketone, isobutyl methyl ketone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol methyl ether acetate, and γ-butyrolactone; aprotic polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric triamide, and the like, and these can be used alone or in combination.
[0176] The reaction solution of the obtained intermediate imide compound can be further subjected to the polycondensation reaction described above, or it can be diluted with an organic solvent to remove unreacted raw materials, catalysts, etc. present in the system, and then separated and washed or crystallized with a poor solvent to recover the reaction intermediate in the form of powder.
[0177] In the polycondensation reaction using the imide compound obtained by the above-described method, the imide compound, aldehyde compound and ketone compound may be used alone or as a mixture of two or more, or an aldehyde compound and a ketone compound may be used in combination.
[0178] These can be appropriately selected and combined according to required properties.
[0179] The polycondensation reaction can be generally carried out in an organic solvent in the presence of an acid catalyst at room temperature or under cooling or heating as required. As the acid catalyst used, inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropolyacids; organic acids such as oxalic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid; and Lewis acids such as aluminum trichloride, aluminum ethoxide, aluminum isopropoxide, boron trifluoride, boron trichloride, boron tribromide, tin tetrachloride, tin tetrabromide, dibutyltin dichloride, dibutyldimethoxide, dibutyltin oxide, titanium tetrachloride, titanium tetrabromide, titanium methoxide (IV), titanium ethoxide (IV), titanium isopropoxide (IV), and titanium oxide (IV).
[0180] The solvent used may be exemplified by alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, propylene glycol, diethylene glycol, glycerol, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ethers such as diethyl ether, dibutyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, and 1,4-dioxane; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; hydrocarbons such as hexane, heptane, benzene, toluene, xylene, and cumene; nitriles such as acetonitrile; ketones such as acetone, methyl ethyl ketone, and isobutyl methyl ketone; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; and aprotic polar solvents such as dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric triamide. These may be used alone or in combination of two or more.
[0181] As for the reaction method, the following methods can be cited: adding the imide compound, the aldehyde compound or the ketone compound, and the catalyst at once; after dispersing or dissolving the imide compound and the aldehyde compound or the ketone compound, adding the catalyst at once or diluting with a solvent and adding dropwise; or after dispersing or dissolving the catalyst, adding the nitrogen-containing compound and the imide compound or the ketone compound at once or diluting with a solvent and adding dropwise. After the reaction is completed, it can be used directly as an organic membrane material, or it can be diluted with an organic solvent to remove unreacted raw materials, catalysts, etc. in the system, and then separated, washed, and recovered.
[0182] The organic solvent used at this time is not particularly limited as long as it can dissolve the compound and separate into two layers when mixed with water. Examples include: hydrocarbons such as hexane, heptane, benzene, toluene, and xylene; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; ketones such as methyl ethyl ketone, methyl amyl ketone, cyclohexanone, and methyl isobutyl ketone; ethers such as diethyl ether, diisopropyl ether, methyl tert-butyl ether, and ethyl cyclopentyl methyl ether; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; and mixtures thereof. The washing water used at this time is usually deionized water or ultrapure water. The number of washing times may be one or more. Even if washing is performed more than 10 times, the corresponding washing effect may not be obtained, so it is preferably about 1 to 5 times.
[0183] In order to remove unreacted raw materials or acidic components in the system during liquid separation and washing, an alkaline aqueous solution can also be used for washing. Specific examples of the base include: alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, ammonia, and organic ammonium.
[0184] In addition, in order to remove unreacted raw materials, metal impurities or alkaline components in the system during liquid separation and washing, an acidic aqueous solution can also be used for washing. As the acid, specifically, inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropoly acids; organic acids such as oxalic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid can be listed.
[0185] The above-mentioned liquid separation and washing using the alkaline aqueous solution and the acidic aqueous solution may be performed alone or in combination. From the viewpoint of removing metal impurities, the liquid separation and washing are preferably performed in the order of the alkaline aqueous solution and the acidic aqueous solution.
[0186] After the above-mentioned separation and washing using alkaline aqueous solution or acidic aqueous solution, it is also possible to continue washing with neutral water. The washing number only needs to be performed once or more, preferably about 1 to 5 times. Neutral water can use the above-mentioned deionized water, ultrapure water, etc. The washing number can be once or more, but if the number is less, there may be a situation where the alkaline component and the acidic component cannot be removed. Even if washing is performed more than 10 times, the corresponding washing effect may not be obtained, so it is preferably about 1 to 5 times.
[0187] In addition, the reaction product after the liquid separation operation can also be recovered in the form of powder by concentrating the solvent to dryness or performing crystallization operation under reduced pressure or normal pressure. In order to improve the operability when preparing the organic membrane material, it can also be prepared in advance into a solution state with an appropriate concentration. At this time, the concentration is preferably 0.1 to 50% by weight, and more preferably 0.5 to 30% by weight. If it is such a concentration, the viscosity is not easy to increase, so it can prevent damage to the operability, and the amount of solvent will not be too large, so it is economical.
[0188] The solvent in this case is not particularly limited as long as it can dissolve the compound. Specific examples include ketones such as cyclohexanone and methyl-2-pentyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; and esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate. These may be used alone or in combination of two or more.
[0189] The preparation of organic film compounds can combine imide compounds, aldehyde compounds, and ketone compounds according to the required performance. The side chain structure that contributes to the improvement of planarization characteristics and the rigid aromatic ring structure that contributes to etching resistance and heat resistance can be combined in any proportion. The organic film material using these compounds can achieve both filling / planarization characteristics and etching resistance in a high-dimensional manner.
[0190] In addition, as another method for obtaining the compound used for the organic film material, the following hydroxyl-containing imide compound and aldehyde compound or ketone compound can be used to obtain an intermediate by polycondensation in the same manner as described above (STEP 1), and then the hydroxyl group can be converted into R1 (STEP 2). In the following formula, n1, n2, n3, W1, R1, R2, and R3 are the same as described above.
[0191] [Chemistry 31]
[0192]
[0193] If the reaction can introduce the above-mentioned substituent, it is not particularly limited, and examples thereof include substitution reactions using halides, toluenesulfonates, or mesylates with a base catalyst, etc. In the following formula, X represents a halogen, a toluenesulfonyl group, or a mesylate group, and n1, n2, n3, W1, R1, R2, and R3 are the same as those described above.
[0194] [Chemistry 32]
[0195]
[0196] Examples of the base catalyst used in the substitution reaction include inorganic base compounds such as sodium bicarbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, and potassium phosphate; and organic amine compounds such as triethylamine, pyridine, and N-methylmorpholine. These may be used alone or in combination of two or more.
[0197] The solvent used at this time is not particularly limited as long as it is a solvent that is inactive in the above reaction. For example, ether solvents such as diethyl ether, tetrahydrofuran, and dioxane, aromatic solvents such as benzene, toluene, and xylene, acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., which can be used alone or in combination.
[0198] The reaction method and recovery method of the compound may be the same as those mentioned above.
[0199] In the preparation of the polymer used in the organic film material obtained by this method, various halides, toluenesulfonates and mesylates can be used alone or in combination according to the required performance. For example, substituents that contribute to the improvement of adhesion to the substrate, the filling / planarization characteristics, and substituents that improve the hardening performance can be introduced in any proportion. Therefore, the organic film material using these polymers can take into account both the filling / planarization characteristics and the etching resistance in a high dimension.
[0200] In addition, as a method for obtaining the polymer used for the organic film material of the present invention when W2 is a single bond, oxidative coupling polymerization with dehydrogenation using the following imide compound can be cited. In the following formula, R1, n1, n2, n3, and W1 are the same as those described above.
[0201] [Chemistry 33]
[0202]
[0203] Oxidative coupling polymerization can be carried out in an organic solvent in the presence of a catalyst at room temperature or under cooling or heating as needed while supplying oxygen. Examples of the catalyst used include di-μ-hydroxy-bis[(N,N,N',N'-tetramethylethylenediamine)copper(II)] chloride, di-μ-hydroxy-bis(N,N,N',N'-tetramethylpropylenediamine)copper(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetraethylethylenediamine)copper(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetraethylethylenediamine)copper(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetraethylethylenediamine)copper(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetraethylethylenediamine)copper(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetramethyl-1,6-hexanediamine)copper(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetramethyl-1,8-naphthalenediamine)copper(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetramethylethylenediamine)titanium(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetramethylethylenediamine)cerium(II)] chloride, di-μ-hydroxy-bis[(N,N,N',N'-tetramethylethylenediamine)iron] chloride, etc.
[0204] Examples of the solvent used include: alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, propylene glycol, diethylene glycol, glycerol, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ethers such as diethyl ether, dibutyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, and 1,4-dioxane; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; hydrocarbons such as hexane, heptane, benzene, toluene, xylene, and cumene; nitriles such as acetonitrile; ketones such as acetone, methyl ethyl ketone, and isobutyl methyl ketone; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; aprotic polar solvents such as dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric triamide, and the like, and these can be used alone or in combination of two or more.
[0205] The reaction method and recovery method of the compound may be the same as those mentioned above.
[0206] As described above, the organic film-forming polymer of the present invention can provide an organic film-forming composition (material) capable of forming an organic film having excellent heat resistance, excellent solvent resistance, high filling property / high planarization property, and excellent adhesion to a substrate.
[0207] <Organic film forming material>
[0208] The present invention also provides an organic film-forming material, which is a material for organic film formation, comprising the organic film-forming polymer of the present invention and an organic solvent. The organic film-forming material of the present invention may also be referred to as an organic film-forming composition. In addition, in the organic film-forming material of the present invention, the organic film-forming polymer of the present invention may be used alone or in combination of two or more.
[0209] The organic solvent that can be used in the organic film-forming material of the present invention is not particularly limited as long as it can dissolve the polymer (base polymer) of the present invention, that is, any component such as the acid generator, crosslinking agent, other additives, etc. described below. Specifically, a solvent having a boiling point of less than 180° C. such as the solvents described in paragraphs (0091) to (0092) of Japanese Patent Application Laid-Open No. 2007-199653 can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and a mixture of two or more thereof can be preferably used.
[0210] Such a material can be applied by spin coating, and since it contains the organic film-forming polymer of the present invention as described above, it can be an organic film-forming material that can form an organic film having excellent heat resistance, excellent solvent resistance, adhesion, and high filling / planarization properties.
[0211] In addition, in the organic film forming material of the present invention, as for the organic solvent, a high boiling point solvent having a boiling point of 180°C or higher (a mixture of a solvent having a boiling point of less than 180°C and a solvent having a boiling point of 180°C or higher) may be added to the above-mentioned solvent having a boiling point of less than 180°C. The high boiling point organic solvent is not limited to hydrocarbons, alcohols, ketones, esters, ethers, chlorine-based solvents, etc. as long as it can dissolve the organic film forming compound. Specific examples include: 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanediol, 2-ethyl-1,3-hexanediol, Diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol Monomethyl ether, triethylene glycol-n-butyl ether, triethylene glycol butyl methyl ether, triethylene glycol diacetate, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, propylene glycol Glycol diacetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol methyl n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, 1,6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, dibutyl adipate, etc., which can be used alone or in combination.
[0212] The boiling point of the high boiling point solvent can be appropriately selected according to the temperature at which the organic film composition is subjected to heat treatment. The boiling point of the added high boiling point solvent is preferably 180°C to 300°C, more preferably 200°C to 300°C. If it is such a boiling point, there is no risk of volatilization too quickly during baking (heat treatment) due to too low a boiling point, and sufficient thermal fluidity can be obtained. In addition, if it is such a boiling point, there is no risk of the boiling point being too high and not volatilizing after baking and remaining in the film, and there is no risk of adversely affecting the film properties such as etching resistance.
[0213] When the high boiling point solvent is used, the amount of the high boiling point solvent blended is preferably 1 to 30 parts by mass relative to 100 parts by mass of the solvent having a boiling point of less than 180° C. If the blended amount is such, there is no risk that the blended amount is too small and sufficient thermal fluidity cannot be imparted during baking, or that the blended amount is too large and remains in the film, resulting in deterioration of film properties such as etching resistance.
[0214] Such an organic film-forming material can provide thermal fluidity by adding a high-boiling-point solvent to the organic film-forming polymer, thereby providing an organic film-forming composition having higher filling / planarizing properties.
[0215] In order to further promote the curing reaction, an acid generator may be added to the organic film forming material of the present invention. Acid generators may generate acid by thermal decomposition or by light irradiation, and both may be added. Specifically, materials described in paragraphs (0061) to (0085) of Japanese Patent Publication No. 2007-199653 may be added, but the present invention is not limited thereto.
[0216] The acid generator may be used alone or in combination of two or more. The amount of the acid generator added is preferably 0.05 to 50 parts, more preferably 0.1 to 10 parts, based on 100 parts of the polymer.
[0217] The organic film-forming material of the present invention may contain a surfactant to improve coating properties during spin coating. For example, the surfactant described in (0142) to (0147) of JP-A-2009-269953 may be used.
[0218] In addition, in the organic film forming material of the present invention, a crosslinking agent may be added in order to improve the hardening property and further suppress the cross-mixing with the upper film. The crosslinking agent is not particularly limited, and various known crosslinking agents can be widely used. As an example, polynuclear phenol hydroxymethyl or methoxymethyl type crosslinking agents, melamine crosslinking agents, glycoluril crosslinking agents, benzoguanamine crosslinking agents, urea crosslinking agents, β-hydroxyalkylamide crosslinking agents, isocyanurate crosslinking agents, aziridine crosslinking agents, oxazoline crosslinking agents, and epoxy crosslinking agents can be illustrated.
[0219] As melamine-based crosslinking agents, specifically, hexamethoxymethylated melamine, hexabutoxymethylated melamine, alkoxy and / or hydroxyl-substituted products thereof, and partial self-condensates thereof can be exemplified. As polynuclear phenol-based methoxymethyl-type crosslinking agents, tetrahydroxymethylated and tetramethoxymethylated products of bisphenols such as bisphenol A and bisphenol F, hexamethoxymethylated products of triphenols such as trisphenol methane, trisphenol ethane, 1,1,1-tris(4-hydroxyphenyl)ethane, tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene, and partial condensates thereof can be exemplified. As glycoluril-based crosslinking agents, specifically, tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, alkoxy and / or hydroxyl-substituted products thereof, and partial self-condensates thereof can be exemplified. As benzoguanamine crosslinking agents, specifically, tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. As urea crosslinking agents, specifically, dimethoxymethylated dimethoxyethylene urea, its alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. As β-hydroxyalkylamide crosslinking agents, specifically, N,N,N',N'-tetrakis (2-hydroxyethyl) adipamide can be exemplified. As isocyanurate crosslinking agents, specifically, triglycidyl isocyanurate and triallyl isocyanurate can be exemplified. As aziridine crosslinking agents, specifically, 4,4'-bis (ethyleneiminocarbonylamino) diphenylmethane, 2,2-bishydroxymethylbutanol-tris [3- (1-aziridine) propionate]. Specific examples of the oxazoline crosslinking agent include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis-4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tert-butyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymers. Specific examples of the epoxy crosslinking agent include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0220] In addition, in order to further improve the planarization / burying characteristics, a plasticizer may be added to the organic film forming material of the present invention. The plasticizer is not particularly limited, and various known plasticizers can be widely used. As an example, low molecular weight compounds such as phthalates, adipic acid esters, phosphates, trimellitic acid esters, and citrates, polyethers, polyesters, and polymers such as polyacetal polymers described in Japanese Patent Application Laid-Open No. 2013-253227 can be illustrated.
[0221] In the organic film forming material of the present invention, as an additive for imparting the embedding / planarizing property similarly to the plasticizer, for example, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a thermally decomposable polymer having a weight loss rate of 40% by mass or more at 30° C. to 250° C. and a weight average molecular weight of 300 to 200,000 can be preferably used. The thermally decomposable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a).
[0222] [Chemistry 34]
[0223]
[0224] In the formula, R6 is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. Y1 is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.
[0225] [Chemistry 35]
[0226]
[0227] In the formula, R 6a Y is an alkyl group having 1 to 4 carbon atoms. a It is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, and may have an ether bond. n represents the average number of repeating units, and is 3 to 500.
[0228] As described above, the organic film forming material of the present invention has excellent heat resistance, excellent solvent resistance, adhesion to the substrate, and high-level filling / planarization properties. Therefore, the organic film forming material of the present invention is extremely useful as an organic film material for a multilayer resist method such as a two-layer resist method, a three-layer resist method using a silicon-containing resist underlayer film or a silicon-containing inorganic hard mask, and a four-layer resist method using a silicon-containing resist underlayer film or a silicon-containing inorganic hard mask and an organic antireflection film.
[0229] <Organic film formation method>
[0230] By using the organic film-forming material of the present invention, an organic film that functions as, for example, an organic underlayer film of a multilayer resist film used in photolithography or a planarizing film (organic planarizing film) for semiconductor manufacturing can be formed.
[0231] The heating film forming step for forming the organic film as the organic lower film can use a single-stage baking, a double-stage baking, or a multi-stage baking of more than three stages, but a single-stage baking or a double-stage baking is economically preferred. The film formation using a single-stage baking is preferably carried out at a temperature of 100°C to 600°C for 5 to 3600 seconds, preferably at a temperature of 150°C to 500°C for 10 to 7200 seconds. By performing heat treatment under such conditions, the flattening and cross-linking reactions caused by heat flow can be promoted. In the multilayer resist method, a coating-type silicon-containing resist lower film and a CVD hard mask are sometimes formed on the obtained film. When a coating-type silicon-containing resist lower film is used, it is preferable to form the film at a temperature higher than the temperature at which the silicon-containing resist lower film is formed. Usually, the silicon-containing resist lower film is formed at a temperature of 100°C to 400°C, preferably at a temperature of 150°C to 350°C. When the organic film is formed at a temperature higher than this temperature, dissolution of the organic film formed with the silicon-containing resist underlayer film forming composition can be prevented, and an organic film that does not mix with the composition can be formed.
[0232] When a CVD hard mask is used, it is preferable to form the organic film at a temperature higher than the temperature at which the CVD hard mask is formed. The temperature at which the CVD hard mask is formed may be, for example, 150° C. to 500° C.
[0233] On the other hand, in the film formation using two-stage baking, for the first stage baking, considering the influence of corrosion of the substrate caused by oxygen in the air, the upper limit of the processing temperature in the air is preferably below 300°C and below 250°C for 10 to 600 seconds. As for the baking temperature of the second stage, it is preferably higher than the baking temperature of the first stage, and is performed at a temperature below 600°C, preferably below 500°C, for 10 to 7200 seconds. The multilayer resist method sometimes forms a coating-type silicon-containing resist lower film and a CVD hard mask on the obtained film. When using a coating-type silicon-containing resist lower film, it is preferable to form the film at a temperature higher than the temperature at which the silicon-containing resist lower film is formed. Usually, the silicon-containing resist lower film is formed at a temperature of 100°C to 400°C, preferably 150°C to 350°C. When the organic film is formed at a temperature higher than this temperature, dissolution of the organic film by the silicon-containing resist underlayer film forming composition can be prevented, and an organic film that is not mixed with the composition can be formed.
[0234] When a CVD hard mask is used in the two-step baking, it is preferable to form the organic film at a temperature higher than the temperature at which the CVD hard mask is formed. The temperature at which the CVD hard mask is formed may be, for example, 150° C. to 500° C.
[0235] In addition, the method for forming an organic film using the material for forming an organic film of the present invention can use, for example, a substrate to be processed having a structure or a height difference of 30 nm or more. As described above, the material for forming an organic film of the present invention has excellent filling / flattening properties, so even if the substrate to be processed has a structure or a height difference (concave and convex) of 30 nm or more, a flat hardened film can be formed. That is, the method for forming an organic film using the material for forming an organic film of the present invention is particularly useful when forming a flat organic film on such a substrate to be processed.
[0236] The thickness of the organic film to be formed can be appropriately selected, and is preferably 30 to 20,000 nm, and particularly preferably 50 to 15,000 nm.
[0237] Furthermore, the above-mentioned method for forming an organic film can be applied to both the case of forming an organic film for an organic underlayer film and the case of forming an organic film for a planarizing film using the organic film-forming material of the present invention.
[0238] The organic film forming material of the present invention can be applied to, for example, the following organic film forming method: a method for forming an organic film that can flatten the surface of a height difference substrate used in the manufacturing step of a semiconductor device, by spin-coating the above-mentioned organic film forming composition of the present invention on a processed substrate, heat-treating the substrate coated with the organic film forming composition in air at a temperature of not less than 50° C. and not more than 250° C. for 10 to 600 seconds, and then heat-treating it in an inert gas at a temperature of not less than 250° C. for 10 to 7200 seconds to form a cured film.
[0239] In the method for forming an organic film, first, the organic film forming material of the present invention is spin-coated (spin-coated) on the substrate to be processed. By using the spin coating method, good filling characteristics can be obtained. After spin coating, baking (heat treatment) is performed to promote flattening and cross-linking reactions caused by heat flow. In addition, by this baking, the solvent in the material can be evaporated, so when the resist upper film and the silicon-containing resist lower film are formed on the organic film, mixing can also be prevented.
[0240] <Pattern Formation Method>
[0241] [Three-layer resist method using a silicon-containing resist underlayer film]
[0242] The present invention provides a pattern forming method, which is characterized by: forming an organic film on a workpiece using the organic film forming material of the present invention, forming a silicon-containing resist underlayer film on the organic film using a silicon-containing resist underlayer film material, forming a resist upper layer film on the silicon-containing resist underlayer film using a photoresist composition, forming a circuit pattern on the resist upper layer film, etching the silicon-containing resist underlayer film using the pattern-formed resist upper layer film as a mask, transferring the pattern to the silicon-containing resist underlayer film, etching the organic film using the silicon-containing resist underlayer film with the pattern transferred thereto as a mask, transferring the pattern to the organic film, and further etching the workpiece using the organic film with the pattern transferred thereto as a mask to form a pattern on the workpiece.
[0243] As for the object to be processed, it is preferred to use a semiconductor device substrate, or a semiconductor device substrate on which a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film are formed. More specifically, there is no particular limitation, and Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al and other substrates, and the above-mentioned metal films are formed on the substrates as the processed layer, etc.
[0244] As for the processed layer, various Low-k films and barrier films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, etc. can be used, and the thickness can usually be formed to 50 to 10,000nm, especially 100 to 5,000nm. In addition, when forming the processed layer, different materials can be used for the substrate and the processed layer.
[0245] In addition, the metal constituting the processed body is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0246] Furthermore, as the object to be processed, it is preferable to use a substrate to be processed having a structure with a height of 30 nm or more or a height difference.
[0247] When an organic film is formed on a workpiece using the material for forming an organic film of the present invention, the above-mentioned method can be used.
[0248] Then, a resist underlayer film (silicon-containing resist underlayer film) is formed on the organic film using a resist underlayer film material containing silicon atoms. The silicon-containing resist underlayer film material is preferably a polysiloxane-based underlayer film material. By providing the silicon-containing resist underlayer film with an antireflection effect, reflection can be suppressed. In particular, for 193nm exposure, if a material containing a large number of aromatic groups and having a high etching selectivity with the substrate is used as the organic film forming material, the k value increases and the substrate reflection becomes high, but by providing the silicon-containing resist underlayer film with an absorption that can become an appropriate k value, reflection can be suppressed and the substrate reflection can be reduced to less than 0.5%. As a silicon-containing resist underlayer film with an antireflection effect, an anthracene-containing pendant structure or polysiloxane structure can be preferably used for 248nm and 157nm exposure, and a polysiloxane containing a light-absorbing group containing a phenyl group or a silicon-silicon bond in a pendant structure or polysiloxane structure and cross-linked by acid or heat can be preferably used for 193nm exposure.
[0249] Then, a resist upper film is formed on the silicon-containing resist lower film using a resist upper film material composed of a photoresist composition. The resist upper film material can be positive or negative, and can use the same resist composition as commonly used. It is preferred that the resist upper film material be spin-coated and then pre-baked at 60 to 180° C. for 10 to 300 seconds. Thereafter, exposure is performed according to the usual method, and post-exposure baking (PEB) and development are further performed to obtain a resist upper film pattern. In addition, the thickness of the resist upper film is not particularly limited, and is preferably 30 to 500 nm, and particularly preferably 50 to 400 nm.
[0250] Then, a circuit pattern (resist upper film pattern) is formed on the resist upper film. The circuit pattern is preferably formed by photolithography using light with a wavelength of 10 nm to 300 nm, direct drawing using an electron beam, nanoimprinting, or a combination thereof.
[0251] In addition, the exposure light may include high-energy rays with a wavelength of less than 300nm, specifically, far ultraviolet rays, KrF excimer laser (248nm), ArF excimer laser (193nm), F2 laser (157nm), Kr2 laser (146nm), Ar2 laser (126nm), 3 to 20nm soft X-rays (EUV), electron beams (EB), ion beams, X-rays, etc.
[0252] In the formation of the circuit pattern, it is preferable to develop the circuit pattern using an alkali developer or an organic solvent.
[0253] Then, the silicon-containing resist lower film is etched using the resist upper film having the circuit pattern as a mask, and the pattern is transferred to the silicon-containing resist lower film. The etching of the silicon-containing resist lower film using the resist upper film pattern as a mask is preferably performed using a fluorocarbon gas. Thus, a silicon-containing resist lower film pattern is formed.
[0254] Then, the organic film is etched using the silicon-containing resist lower film with the transferred pattern as a mask, and the pattern is transferred to the organic film. The silicon-containing resist lower film has a higher etching resistance to oxygen or hydrogen than to organic matter, so the etching of the organic film using the silicon-containing resist lower film pattern as a mask is preferably performed using an etching gas mainly composed of oxygen or hydrogen. In this way, an organic film pattern can be formed.
[0255] Then, the object to be processed is etched using the organic film with the transferred pattern as a mask to transfer the pattern to the object to be processed. The etching of the processed substrate (processed layer) can be performed according to the usual method. For example, if the processed substrate is a SiO2, SiN, or silicon dioxide-based low dielectric constant insulating film, etching is performed mainly using a fluorine (flon) gas. If it is p-Si, Al, or W, etching is performed mainly using a chlorine or bromine gas. When the substrate processing is performed using etching using a fluorine gas, the pattern of the lower film of the silicon-containing resist will be stripped off at the same time as the substrate processing. On the other hand, when the substrate processing is performed using etching using a chlorine or bromine gas, in order to strip off the pattern of the lower film of the silicon-containing resist, dry etching stripping using a fluorine gas is required after the substrate processing.
[0256] The organic film obtained by using the organic film-forming material of the present invention can be excellent in etching resistance when etching the workpiece as described above.
[0257] [Four-layer resist method using a silicon-containing resist underlayer film and an organic antireflective film]
[0258] The present invention provides a pattern forming method, which is characterized by: forming an organic film on a workpiece using the organic film forming material of the present invention, forming a silicon-containing resist underlayer film on the organic film using a silicon-containing resist underlayer film material, forming an organic antireflection film on the silicon-containing resist underlayer film, forming a resist upper layer film using a photoresist composition on the organic antireflection film, and forming a four-layer film structure, forming a circuit pattern on the resist upper layer film, etching the organic antireflection film and the silicon-containing resist underlayer film using the pattern-formed resist upper layer film as a mask, transferring the pattern to the organic antireflection film and the silicon-containing resist underlayer film, etching the organic film using the silicon-containing resist underlayer film with the pattern transferred as a mask, transferring the pattern to the organic film, and further etching the workpiece using the organic film with the pattern transferred as a mask to form a pattern on the workpiece.
[0259] This method can be performed in the same manner as the above-mentioned three-layer resist method using the silicon-containing resist underlayer film, except that an organic antireflection film (BARC) is formed between the silicon-containing resist underlayer film and the resist upper layer film.
[0260] The organic anti-reflection film can be formed by spin coating using a known organic anti-reflection film material.
[0261] [Three-layer resist method using an inorganic hard mask]
[0262] Furthermore, as a pattern forming method using the three-layer resist method of the organic film forming composition of the present invention, the present invention provides a pattern forming method, characterized in that: an organic film is formed on a workpiece using the organic film forming material of the present invention, an inorganic hard mask selected from a silicon oxide film, a silicon nitride film and a silicon oxide nitride film is formed on the organic film, a resist upper film is formed on the inorganic hard mask using a photoresist composition, a circuit pattern is formed on the resist upper film, the inorganic hard mask is etched using the patterned resist upper film as a mask to transfer the pattern to the inorganic hard mask, the organic film is etched using the patterned inorganic hard mask as a mask to transfer the pattern to the organic film, and further, the workpiece is etched using the patterned organic film as a mask to form a pattern on the workpiece.
[0263] This method can be performed in the same manner as the above-mentioned three-layer resist method using the silicon-containing resist underlayer film, except that an inorganic hard mask is formed on the organic film instead of the silicon-containing resist underlayer film.
[0264] The inorganic hard mask selected from silicon oxide film, silicon nitride film, and silicon oxide nitride film (SiON film) can be formed by CVD method, ALD method, etc. The method of forming silicon nitride film is described in, for example, Japanese Patent Publication No. 2002-334869 and International Publication No. 2004 / 066377. The film thickness of the inorganic hard mask is preferably 5 to 200 nm, more preferably 10 to 100 nm. It is best to use SiON film with high effect as an anti-reflective film as the inorganic hard mask. The substrate temperature when forming the SiON film is 300 to 500°C, so the lower film needs to withstand a temperature of 300 to 500°C. The organic film formed using the organic film forming composition of the present invention has high heat resistance and can withstand high temperatures of 300 to 500°C, so it can be a combination of an inorganic hard mask formed by CVD method or ALD method and an organic film formed by spin coating method.
[0265] [Four-layer resist method using inorganic hard mask and organic anti-reflective film]
[0266] Furthermore, in the present invention, as a pattern forming method by a four-layer resist method using the organic film forming composition of the present invention, the present invention provides a pattern forming method, characterized in that: an organic film is formed on a workpiece using the organic film forming material of the present invention, an inorganic hard mask selected from a silicon oxide film, a silicon nitride film and a silicon oxide nitride film is formed on the organic film, an organic antireflection film is formed on the inorganic hard mask, and a resist upper layer film is formed on the organic antireflection film using a photoresist composition, thereby preparing A 4-layer film structure is formed, a circuit pattern is formed on the resist upper film, the organic anti-reflective film and the inorganic hard mask are etched using the patterned resist upper film as a mask, the pattern is transferred to the organic anti-reflective film and the inorganic hard mask, the organic film is etched using the patterned inorganic hard mask as a mask, the pattern is transferred to the organic film, and further, the object to be processed is etched using the patterned organic film as a mask to form a pattern on the object to be processed.
[0267] This method can be performed in the same manner as the above-mentioned three-layer resist method using an inorganic hard mask, except that an organic antireflection film (BARC) is formed between the inorganic hard mask and the resist upper layer film.
[0268] In particular, when a SiON film is used as an inorganic hard mask, the two-layer antireflection film of the SiON film and the BARC can suppress reflection even in immersion exposure with a high NA exceeding 1.0. Another advantage of forming a BARC is that it has the effect of reducing the tailing of the resist upper film pattern directly above the SiON film.
[0269] Here, an example of the pattern forming method using the three-layer resist method of the present invention is shown in Figure 1(A) to (F). In the case of the three-layer resist method, Figure 1 As shown in (A), an organic film 3 is formed on a processing layer 2 formed on a substrate 1 using the organic film-forming composition of the present invention, a silicon-containing resist lower layer film 4 is formed, and a resist upper layer film 5 is formed thereon. Figure 1 As shown in (B), the exposed portion 6 of the resist upper layer film 5 is exposed and PEB (post-exposure baking) is performed. Figure 1 (C) is shown, and development is performed to form a resist upper film pattern 5a. Figure 1 As shown in (D), the resist upper film pattern 5a is used as a mask, and the silicon-containing resist lower film 4 is dry-etched using a fluorine-based gas to form a silicon-containing resist lower film pattern 4a. Figure 1 As shown in (E), after removing the resist upper film pattern 5a, the organic film 3 is subjected to oxygen plasma etching using the silicon-containing resist lower film pattern 4a as a mask to form an organic film pattern 3a. Figure 1 As shown in FIG. 2(F), after removing the silicon-containing resist lower film pattern 4a, the processed layer 2 is etched using the organic film pattern 3a as a mask to form a pattern 2a.
[0270] When forming an inorganic hard mask, the silicon-containing resist lower film 4 may be replaced with an inorganic hard mask, and when forming an anti-reflection film (BARC), the BARC may be formed between the silicon-containing resist lower film 4 and the resist upper film 5. The etching of the BARC may be performed continuously before the etching of the silicon-containing resist lower film 4, or the etching of the silicon-containing resist lower film 4 may be performed only after the etching of the BARC, and then the etching device may be changed.
[0271] As described above, according to the pattern forming method of the present invention, a fine pattern can be formed on a substrate to be processed with high precision using a multilayer resist method.
[0272] Example
[0273] Hereinafter, the present invention will be described in more detail by citing synthesis example, comparative synthesis example, embodiment and comparative example, but the present invention is not limited thereto. In addition, with regard to molecular weight and dispersity, the weight average molecular weight (Mw) and number average molecular weight (Mn) calculated using polystyrene obtained by gel permeation chromatography (GPC) using tetrahydrofuran as eluent are obtained, and dispersity (Mw / Mn) is obtained.
[0274] Synthesis Example Synthesis of polymers for organic membrane materials
[0275] The imide compounds (A1) to (A6) used as intermediates of polymers for organic film-forming materials are synthesized using tetracarboxylic anhydrides (B1) to (B3) and amine compounds (C1) to (C6) shown below.
[0276] Tetracarboxylic anhydride:
[0277] [Chemistry 36]
[0278]
[0279] Amine compounds:
[0280] [Chemistry 37]
[0281]
[0282] [Synthesis Example 1] Synthesis of Imidide Compound (A1)
[0283] [Chemistry 38]
[0284]
[0285] 150 g of N-methylpyrrolidone was added to 30.00 g of tetracarboxylic anhydride (B1), and a uniform solution was prepared at an internal temperature of 40°C under a nitrogen environment. Then, 14.74 g of an amine compound (C1) was added, and the mixture was reacted at an internal temperature of 40°C for 3 hours to obtain an amide acid solution. 200 g of o-xylene was added to the obtained amide acid solution, and the mixture was reacted for 9 hours at an internal temperature of 150°C while removing the generated low-boiling substances and generated water from the system, and dehydration imidization was performed. After the reaction was completed, the mixture was cooled to room temperature and crystallized in 1000 g of diisopropyl ether. The precipitated crystals were filtered and separated, washed twice with 500 g of diisopropyl ether and recovered. The recovered crystals were vacuum dried at 70°C to obtain compound (A1).
[0286] [Synthesis Examples 2 to 6] Synthesis of Imidide Compounds (A2) to (A6)
[0287] Compounds (A2) to (A6) shown in Table 1 were obtained under the same reaction conditions as in Synthesis Example 1 except that the tetracarboxylic anhydride and amine compound shown in Table 1 were used.
[0288] [Table 1]
[0289]
[0290] The synthesis of polymers (P1) to (P9) for organic film forming materials uses the above intermediate imide compounds (A1) to (A6) and the following (D1) to (D3) as aldehyde components. However, D1 is used in the form of a 37% formalin aqueous solution.
[0291] [Chemistry 39]
[0292]
[0293] [Synthesis Example P1] Synthesis of polymer (P1)
[0294] [Chemistry 40]
[0295]
[0296] 15.00 g of the imide compound (A1), 1.36 g of the aldehyde compound (D1), and 60 g of 2-methoxy-1-propanol were mixed under nitrogen atmosphere at an internal temperature of 80°C to form a uniform solution, and then 1.5 g of a 20% p-toluenesulfonic acid solution in 2-methoxy-1-propanol was slowly added, and the mixture was stirred at an internal temperature of 110°C for 8 hours. After cooling to room temperature, 200 g of methyl isobutyl ketone was added, and the organic layer was washed 5 times with 50 g of pure water, and then dried under reduced pressure. 50 g of THF was added to the residue, and the polymer was reprecipitated with 200 g of hexane. The precipitated polymer was filtered and dried under reduced pressure to obtain a polymer (P1).
[0297] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. The results are as follows.
[0298] (P1): Mw=2820, Mw / Mn=1.72
[0299] [Synthesis Examples P2 to P9] Synthesis of Polymers (P2) to (P9)
[0300] Polymers (P2) to (P9) shown in Table 2 were obtained under the same reaction conditions as in Synthesis Example P1 except that the imide compounds and aldehyde compounds shown in Table 2 were used. The structural formula, weight average molecular weight (Mw) and dispersity (Mw / Mn) of the obtained polymers are shown in Tables 3 and 4.
[0301] [Table 2]
[0302]
[0303] [Synthesis Example P10] Synthesis of polymer (P10)
[0304] [Chemistry 41]
[0305]
[0306] 40 g of N-methyl-2-pyrrolidone was added to 8.00 g of polymer (P6) and 5.78 g of potassium carbonate, and a uniform dispersion was prepared at an internal temperature of 50°C under a nitrogen environment. 4.94 g of propargyl bromide was slowly added dropwise, and the mixture was reacted at an internal temperature of 50°C for 24 hours. 150 g of methyl isobutyl ketone and 50 g of pure water were added to the reaction solution to make it uniform, and the separated water layer was removed. Furthermore, the organic layer was washed 6 times with 50 g of 3% nitric acid aqueous solution and 50 g of pure water, and then the organic layer was dried under reduced pressure. 40 g of THF was added to the residue to prepare a uniform solution, and then crystallized with 150 g of methanol. The precipitated crystals were filtered and separated, washed twice with 60 g of methanol and recovered. The recovered crystals were vacuum dried at 70°C to obtain a polymer (P10).
[0307] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. The results are as follows.
[0308] (P10): Mw=3670, Mw / Mn=1.44
[0309] [Synthesis Example P11] Synthesis of polymer (P11)
[0310] [Chemistry 42]
[0311]
[0312] 40 g of N-methyl-2-pyrrolidone was added to 8.00 g of polymer (P8) and 4.72 g of potassium carbonate, and a uniform dispersion was prepared at an internal temperature of 50°C under a nitrogen environment. 4.04 g of propargyl bromide was slowly added dropwise, and the mixture was reacted at an internal temperature of 50°C for 24 hours. 150 g of methyl isobutyl ketone and 50 g of pure water were added to the reaction solution and homogenized, and then the separated water layer was removed. Furthermore, the organic layer was washed 6 times with 50 g of 3% nitric acid aqueous solution and 50 g of pure water, and then the organic layer was dried under reduced pressure. 40 g of THF was added to the residue to prepare a uniform solution, and then crystallized with 150 g of methanol. The precipitated crystals were filtered and separated, washed twice with 60 g of methanol and recovered. The recovered crystals were vacuumed at 70°C to obtain a polymer (P11).
[0313] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. The results are as follows.
[0314] (P11): Mw=3740, Mw / Mn=1.55
[0315] [Synthesis Example P12] Synthesis of polymer (P12)
[0316] [Chemistry 43]
[0317]
[0318] 8.0 g of the imide compound (A6) and 0.10 g of di-u-hydroxy-bis[(N,N,N',N'-tetramethylethylenediamine)copper(II)] chloride were added to a flask and dissolved with 50 g of N-methylpyrrolidone. The mixture was reacted at room temperature in an open atmosphere for 48 hours, diluted with 200 g of methyl isobutyl ketone, and then 50 g of a 5 wt% aqueous hydrochloric acid solution was added to stop the reaction. The separated water layer was removed, and the organic layer was further washed twice with 50 g of a 2 wt% aqueous ammonia solution, twice with 50 g of a 3 wt% aqueous nitric acid solution, and five times with 50 g of pure water, and then the organic layer was dried under reduced pressure. 50 ml of THF was added to the residue, and the polymer was reprecipitated with 200 ml of hexane. The precipitated polymer was filtered and dried under reduced pressure to obtain a polymer (P12).
[0319] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. The results are as follows.
[0320] (P12): Mw=3860, Mw / Mn=1.42
[0321] [Comparative Synthesis Example 1] Synthesis of Polymer (R1)
[0322] [Chemistry 44]
[0323]
[0324] 120 g of NMP (N-methyl-2-pyrrolidone) was added to 20.00 g of tetracarboxylic anhydride (B3) and 5.42 g of 9,9-bis(4-aminophenyl)fluorene, and the mixture was reacted for 3 hours at an internal temperature of 40°C under a nitrogen environment. 2.90 g of aniline as a capping agent was added to the obtained polyamic acid intermediate solution, and the mixture was further reacted for 3 hours at an internal temperature of 40°C to obtain a polyimide precursor solution. 2.46 g of pyridine was added to the obtained reaction solution, and 7.63 g of acetic anhydride was further slowly added dropwise, and the mixture was reacted for 4 hours at an internal temperature of 60°C for imidization. After the reaction was completed, the mixture was cooled to room temperature, 400 g of methyl isobutyl ketone was added, the organic layer was washed twice with 100 g of a 3% nitric acid aqueous solution, and then washed 6 times with 100 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF (tetrahydrofuran) was added to the residue to prepare a uniform solution, and then crystallized with 400 g of methanol. The precipitated crystals were filtered out, washed twice with 300 g of methanol, and recovered. The recovered crystals were vacuum dried at 70° C. to obtain a polymer (R1).
[0325] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. The results are as follows.
[0326] (R1): Mw=3520, Mw / Mn=1.46
[0327] [Comparative Synthesis Example 2] Synthesis of Polymer (R2)
[0328] [Chemistry 45]
[0329]
[0330] 90.1 g of 9,9-fluorene-bis-naphthol, 10.5 g of 37% formalin solution, and 270 g of 2-methoxy-1-propanol were made into a uniform solution under a nitrogen atmosphere at a liquid temperature of 80°C, and then 18 g of 20% p-toluenesulfonic acid 2-methoxy-1-propanol solution was slowly added, and stirred at a liquid temperature of 110°C for 8 hours. After cooling to room temperature, 600 g of methyl isobutyl ketone was added, and the organic layer was washed 5 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 320 g of THF was added to the residue, and the polymer was reprecipitated with 1350 g of hexane. The precipitated polymer was filtered and dried under reduced pressure to obtain a polymer (R2).
[0331] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. The results are as follows.
[0332] Mw=3,700、Mw / Mn=2.82
[0333] [Comparative Synthesis Example 3] Synthesis of Polymer (R3)
[0334] [Chemistry 46]
[0335]
[0336] 78.8 g of 2,7-dipropargyloxynaphthalene, 21.6 g of 37% formalin solution, and 250 g of 1,2-dichloroethane were made into a uniform solution under a nitrogen atmosphere at a liquid temperature of 70°C, and then 5 g of methanesulfonic acid was slowly added and stirred at a liquid temperature of 80°C for 12 hours. After cooling to room temperature, 500 g of methyl isobutyl ketone was added, and the organic layer was washed 5 times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 300 mL of THF was added to the residue, and the polymer was reprecipitated with 2,000 mL of hexane. The precipitated polymer was filtered and dried under reduced pressure to obtain a polymer (R3).
[0337] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. The results are as follows.
[0338] Mw = 2,720, Mw / Mn = 1.55.
[0339] The structural formula, weight average molecular weight (Mw) and dispersity (Mw / Mn) of the polymers (P1) to (P12) obtained above are shown in Tables 3 and 4. In addition, Mw and Mw / Mn of the polymers (R1) to (R3) used in Comparative Examples are also shown in Table 5.
[0340] [Table 3]
[0341]
[0342] [Table 4]
[0343]
[0344] [Table 5]
[0345]
[0346] Preparation of organic film-forming materials (UDL-1 to 15, comparative examples UDL1 to 3)
[0347] Among the above polymers (P1) to (P12) and (R1) to (R3), the materials shown in Table 6 below were used to prepare organic film-forming materials (UDL-1 to 15, comparative examples UDL-1 to 3). In addition, in the preparation of organic film-forming materials UDL13 to 15, (S1) 1,6-diacetoxyhexane: boiling point 260°C, (S2) γ-butyrolactone: boiling point 204°C, and (S3) tripropylene glycol monomethyl ether: boiling point 242°C were used as high boiling point solvents. The polymers were dissolved in propylene glycol monomethyl ether acetate (PGMEA) containing 0.1% by mass of FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) and cyclohexanone (CyHO) in the ratios shown in Table 6, and filtered using a 0.1 μm fluororesin filter to prepare organic film-forming materials (UDL-1 to 15, comparative examples UDL-1 to 3). The organic film-forming materials UDL13 to 15 were prepared by adding a high boiling point solvent to PGMEA and CyHO together with a polymer.
[0348] [Table 6]
[0349]
[0350] Example 1 Solvent Resistance Measurement (Examples 1-1 to 1-15, Comparative Examples 1-1 to 1-3)
[0351] The organic film forming materials (UDL-1 to 15, comparative UDL-1 to 3) prepared above were coated on a silicon substrate, baked at 350°C in the atmosphere for 60 seconds, and then the film thickness was measured. PGMEA solvent was dispensed thereon, left for 30 seconds and spin-dried, and then baked at 100°C for 60 seconds to evaporate PGMEA, and the film thickness was measured to determine the difference in film thickness before and after the PGMEA treatment. These results are shown in Table 7.
[0352] [Table 7]
[0353]
[0354] As shown in Table 7, in Examples 1-1 to 1-15 using the organic film forming material of the present invention, the residual film rate after PGMEA treatment is more than 98%, and it can be seen that a curing reaction occurs due to heat treatment, showing sufficient solvent resistance. In addition, compared with the case of using an oxidative coupling polymer as in Example 1-12, Examples 1-1 to 1-11, 13 to 15 show slightly better results in solvent resistance. From this result, it can be seen that due to the condensation reaction with the aldehyde component, the polymer that has been phenolic varnish resinized undergoes a curing reaction more efficiently. In addition, when the polyimide of Comparative Example 1-1 is used, because there is no part that contributes to the curing reaction, the residual film rate after PGMEA treatment is less than 80%, and solvent resistance is not shown. From these results, it can be seen that the organic film forming polymer of the present invention is endowed with sufficient curability required to show excellent solvent resistance, and is endowed with more improved curability by phenolic varnishization. In addition, since the polymers R2 and R3 which are novolac resins were used in Comparative Examples 1-2 and 1-3, it is considered that the solvent resistance of the same level as that of Examples 1-1 to 1-15 was exhibited.
[0355] Example 2 Evaluation of heat resistance properties (Examples 2-1 to 2-15, Comparative Examples 2-1 to 2-3)
[0356] The above organic film materials (UDL-1 to 15, comparative UDL-1 to 3) were coated on a silicon substrate, respectively, and baked at 350°C for 60 seconds in the atmosphere to form a 200 nm coating film, and the film thickness A was measured. The substrate was further calcined at 450°C for 10 minutes under a nitrogen flow with an oxygen concentration of 0.2% or less, and the film thickness B was measured. The ratio (%) of the film thickness B to the film thickness A was calculated as the residual film rate. These results are shown in Table 8.
[0357] [Table 8]
[0358]
[0359] As shown in Table 8, in Examples 2-1 to 2-15 using the organic film-forming material of the present invention, the film thickness reduction did not reach 2% even after calcination at 450°C under a nitrogen flow, which is a result that the film thickness changes little even after high-temperature baking. Among them, in Examples 2-5, 2-6, 2-8 to 2-15 using polymers having a naphthalene ring structure, the film loss was reduced to less than 1%, which shows that the heat resistance is better. On the other hand, in Comparative Example 2-1 using a polyimide structure that does not contribute to cross-linking, the film thickness reduction exceeded 10%, which is a result of poor heat resistance. In addition, in Comparative Example 2-3 with low heat resistance of the main chain, about 20% of the film loss occurred, and in Comparative Example 2-2 using a phenolic varnish resin with a rigid structure without an imide structure, about 4% of the film thickness reduction also occurred. From this result, it can be seen that the polymer having an imide skeleton of the present invention has excellent heat resistance.
[0360] Example 3 Evaluation of landfill characteristics (Examples 3-1 to 3-15, Comparative Examples 3-1 to 3-3)
[0361] like Figure 2 As shown, the above-mentioned organic film forming materials (UDL-1 to 15, comparative UDL-1 to 3) were coated on a SiO2 wafer substrate having a dense hole pattern (hole diameter 0.16μm, hole depth 0.50μm, center distance between two adjacent holes 0.32μm), and baked at 350°C for 60 seconds in the atmosphere using a hot plate to form an organic film. Similarly, after baking at 350°C for 60 seconds in the atmosphere, it was baked at 450°C for 60 seconds under a nitrogen flow with an oxygen concentration of less than 0.2% to form an organic film. The substrate used is as follows Figure 2 (G) (top view) and (H) (cross-sectional view) show a base substrate 7 (SiO2 wafer substrate) with a dense hole pattern. The cross-sectional shape of each wafer substrate obtained was observed using a scanning electron microscope (SEM) to confirm whether the organic film was filled inside the pores without pores (voids) under each calcination condition. The results are shown in Table 9. When an organic film-forming material with poor filling characteristics was used, pores were generated inside the pores in this evaluation. When an organic film-forming material with good filling characteristics was used, as shown in this evaluation, Figure 2 As shown in (I), the organic film 8 is filled inside the pores without any voids.
[0362] [Table 9]
[0363]
[0364] As shown in Table 9, Examples 3-1 to 3-15 using the organic film forming material of the present invention can fill the hole pattern without generating voids, and it can be confirmed that they have good filling characteristics. On the other hand, some calcination conditions in Comparative Examples 3-1 to 3-3 were confirmed to generate voids and had poor filling characteristics. In Comparative Examples 3-1 to 3-2, it is presumed that the polymer itself has low fluidity, so the filling performance at the time of baking at 350°C is insufficient. In Comparative Example 3-3, it is presumed that there is no problem with the fluidity of the polymer, but due to insufficient heat resistance, voids are generated by baking at 450°C.
[0365] Example 4 Evaluation of planarization characteristics (Examples 4-1 to 4-15, Comparative Examples 4-1 to 4-3)
[0366] The organic film forming materials (UDL-1 to 15, comparative UDL-1 to 3) were coated on the surfaces having the giant isolated trench pattern ( Figure 3 (J), a base substrate 9 (SiO2 wafer substrate) with a groove width of 10 μm and a groove depth of 0.10 μm) was baked at 350°C in the atmosphere for 60 seconds, and then baked at 450°C for 60 seconds in a nitrogen flow with an oxygen concentration of less than 0.2% to form an organic film. The height difference of the organic film 10 between the groove part and the non-groove part was observed using an NX10 atomic force microscope (AFM) manufactured by Park Systems. Figure 3 (k) in delta10). The results are shown in Table 10. In this evaluation, the smaller the height difference, the better the planarization characteristics. In addition, in this evaluation, a trench pattern with a depth of 0.10 μm was planarized using an organic film material with a film thickness of about 0.2 μm, and strict evaluation conditions were used to evaluate the quality of the planarization characteristics.
[0367] [Table 10]
[0368]
[0369] As shown in Table 10, in Examples 4-1 to 4-15 using the organic film forming material of the present invention, the height difference of the organic film between the groove part and the non-groove part is small compared to Comparative Examples 4-1 to 4-3, and it can be confirmed that the flattening characteristics are excellent. In addition, it can be seen that in Examples 4-13 to 4-15 to which a high boiling point solvent is added, the flattening characteristics are further improved due to the addition of the high boiling point solvent. In Comparative Example 4-3, as shown in the results of the heat resistance evaluation shown in Table 8, the heat resistance is poor, so the film loss caused by high temperature baking is large, the film thickness difference between the upper part of the height difference and the lower part of the height difference increases, and the flattening characteristics deteriorate, resulting in the above-mentioned results. In addition, in Comparative Examples 4-1 and 4-2, as shown in the results of the filling characteristic evaluation test, poor filling occurs at the time of baking at 350°C, so it is presumed that the poor flattening characteristics are caused by insufficient fluidity itself.
[0370] Example 5 Pattern Formation Test 1 (Examples 5-1 to 5-15, Comparative Examples 5-1 to 5-3)
[0371] The above-mentioned organic film forming materials (UDL-1 to 15, comparative UDL-1 to 3) were coated on a silicon wafer substrate formed with a 300nm SiO2 film, and calcined at 350°C for 60 seconds in the atmosphere to form an organic film with a thickness of 200nm. A CVD-SiON hard mask was formed thereon, and an organic anti-reflection film material (ARC-29A: manufactured by Nissan Chemical Co., Ltd.) was further coated and baked at 210°C for 60 seconds to form an organic anti-reflection film with a thickness of 80nm. A single-layer resist for ArF as a resist upper film material was coated thereon and baked at 105°C for 60 seconds to form a photoresist film with a thickness of 100nm. A wet protection film material (TC-1) was coated on the photoresist film and baked at 90°C for 60 seconds to form a protection film with a thickness of 50nm.
[0372] As for the resist upper film material (single-layer resist for ArF), it is prepared by dissolving a polymer RP1), an acid generator (PAG1), and a basic compound (Amine1) in a solvent containing 0.1 mass % of a surfactant FC-430 (manufactured by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 11, and filtering using a 0.1 μm fluororesin filter.
[0373] [Table 11]
[0374]
[0375] The polymer RP1), the acid generator (PAG1), and the basic compound (Amine1) used in the resist upper layer film material (single-layer resist for ArF) are shown below.
[0376] [Chemistry 47]
[0377]
[0378] The wet protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent at the ratio shown in Table 12, and filtering the solution through a 0.1 μm fluororesin filter.
[0379] [Table 12]
[0380]
[0381] The polymer (PP1) used in the wet protection film material (TC-1) is shown below.
[0382] [Chemistry 48]
[0383]
[0384] Then, exposure was performed using an ArF immersion exposure device (manufactured by Nikon Co., Ltd.; NSR-S610C, NA1.30, σ0.98 / 0.65, 35-degree dipole s-polarized illumination, 6% half-step phase shift mask), baked (PEB) at 100°C for 60 seconds, and developed with a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a 55nm 1:1 positive line and space pattern.
[0385] Then, using a Tokyo Electron etching device Telius, dry etching was performed using the resist pattern as a mask to etch the organic anti-reflective film and the CVD-SiON hard mask to form a hard mask pattern, and the obtained hard mask pattern was used as a mask to etch the organic film to form an organic film pattern, and the obtained organic film pattern was used as a mask to etch the SiO2 film. The etching conditions are as follows.
[0386] Transfer conditions of resist pattern to SiON hard mask.
[0387] Chamber pressure: 10.0Pa
[0388] RF power: 1,500W
[0389] CF4 gas flow rate: 75sccm
[0390] O2 gas flow rate: 15sccm
[0391] Time: 15 seconds
[0392] Transfer conditions for transferring the hard mask pattern to the organic film.
[0393] Chamber pressure: 2.0Pa
[0394] RF power: 500W
[0395] Ar gas flow rate: 75sccm
[0396] O2 gas flow rate: 45sccm
[0397] Time: 120 seconds
[0398] Transfer conditions for organic film pattern transfer to SiO2 film.
[0399] Chamber pressure: 2.0Pa
[0400] RF power: 2,200W
[0401] C5F 12 Gas flow rate: 20sccm
[0402] C2F6 gas flow rate: 10sccm
[0403] Ar gas flow rate: 300sccm
[0404] O2 gas flow rate: 60sccm
[0405] Time: 90 seconds
[0406] Table 13 shows the results of observing the pattern cross section using an electron microscope (S-4700) manufactured by Hitachi, Ltd.
[0407] [Table 13]
[0408]
[0409] As shown in the results in Table 13, in Examples 5-1 to 5-15 using the organic film forming material of the present invention, it was confirmed that the resist upper film pattern was finally well transferred to the substrate, and the organic film material of the present invention is suitable for use in microfabrication using a multilayer resist method. On the other hand, in Comparative Examples 5-1 and 5-3, due to insufficient heat resistance, the film was exposed to high temperatures when forming a CVD-SiON hard mask, so defects occurred in the film and a pattern could not be formed.
[0410] Example 6 Pattern Formation Test 2 (Examples 6-1 to 6-15, Comparative Examples 6-1 to 6-3)
[0411] The above-mentioned organic film forming materials (UDL-1 to 15, comparative UDL-1 to 3) were coated on SiO2 wafer substrates having a trench pattern (trench width 10 μm, trench depth 0.10 μm), and the coating film was formed in the same manner as in the pattern forming test 1, and patterning and dry etching were performed, and the shape of the final pattern was observed. The results are shown in Table 14.
[0412] [Table 14]
[0413]
[0414] As shown in the results in Table 14, in Examples 6-1 to 6-15 using the organic film forming material of the present invention, it was confirmed that the resist upper film pattern was finally well transferred to the substrate, and the organic film material of the present invention is suitable for use in micro-processing using a multilayer resist method. On the other hand, in Comparative Examples 6-1 and 6-3, similarly to Pattern Formation Test 1, patterns could not be formed due to insufficient heat resistance. In Comparative Example 6-2, although heat resistance and solvent resistance were ensured, the pattern was poorly buried, so pattern collapse occurred during pattern processing, and ultimately a good pattern could not be obtained.
[0415] From the above, it can be seen that if the organic film forming material of the present invention contains the organic film forming polymer of the present invention, it has excellent solvent resistance, high heat resistance that can withstand high temperature conditions above 400°C, a high degree of filling characteristics, excellent planarization characteristics, and excellent adhesion. Therefore, it is extremely useful as an organic film forming material used in a multilayer resist method. Furthermore, if the pattern forming method of the present invention uses the organic film forming material, even if the processed body is a substrate with a height difference, a fine pattern can be formed with high precision.
[0416] The present invention is not limited to the above-described embodiments. The above-described embodiments are illustrative, and those having substantially the same configuration and achieving the same effects as the technical concept described in the claims of the present invention are all within the technical scope of the present invention.
[0417] Description of Reference Numerals
[0418] 1:Substrate
[0419] 2: Processing layer
[0420] 2a: Pattern (pattern formed on the processed layer)
[0421] 3: Organic film
[0422] 3a: Organic film pattern
[0423] 4: Silicon-containing resist lower layer film
[0424] 4a: Silicon-containing resist lower film pattern
[0425] 5: Resist upper film
[0426] 5a: Resist upper film pattern (resist pattern)
[0427] 6: Exposure part
[0428] 7: Base substrate with dense hole pattern
[0429] 8: Organic film
[0430] 9: Base substrate with large isolated trench patterns
[0431] 10: Organic film
[0432] delta10: height difference between the organic film 10 in the trench part and the non-ditch part
Claims
1. An organic film-forming material, Its characteristics are: A polymer containing a structure represented by the following general formula (1A) as a partial structure, and an organic solvent; In the above general formula (1A), W 1 represents a 4-valent organic group, W 2 represents a single bond or a linking group represented by the following formula (1B), R 1 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, n1 represents an integer of 0 or 1, and n2 and n3 satisfy the relationship of 0≤n2≤6 and 0≤n3≤6 and 1≤n2+n3≤6; R 2 and R 3 Each independently represents hydrogen, an organic group having 1 to 30 carbon atoms, and the organic group R 2 With organic group R 3 It can also form cyclic organic groups by bonding within the molecule; When n1 is 0, W 1 Any one of the following expressions: When n1 is 1, W 1 Any one of the following expressions:
2. The organic film-forming material according to claim 1, in, The linking group W in the above general formula (1A) 2 It is represented by the following formula (1E); 3. The organic film-forming material according to claim 1 or 2, in, The weight average molecular weight of the polymer is 1,000 to 10,000.
4. The organic film-forming material according to claim 1 or 2, in, The polymer is a novolac resin having a partial structure represented by the above-mentioned general formula (1A).
5. The organic film-forming material according to claim 1 or 2, in, The organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180° C. and one or more organic solvents having a boiling point of 180° C. or higher. 6 . The organic film-forming material according to claim 1 , further comprising at least one of a surfactant and a plasticizer.
7. A pattern forming method, characterized in that: forming an organic film on a workpiece using the organic film-forming material according to any one of claims 1 to 6, forming a silicon-containing resist underlayer film on the organic film using a silicon-containing resist underlayer film material, forming a resist upper film on the silicon-containing resist lower film using a photoresist composition, forming a circuit pattern on the upper layer of the resist, Using the patterned resist upper film as a mask, the silicon-containing resist lower film is etched to transfer the pattern to the silicon-containing resist lower film. Using the silicon-containing resist lower layer film with the transferred pattern as a mask, the organic film is etched to transfer the pattern to the organic film. Furthermore, the object to be processed is etched using the organic film to which the pattern is transferred as a mask to form a pattern on the object to be processed.
8. A pattern forming method, characterized in that: forming an organic film on a workpiece using the organic film-forming material according to any one of claims 1 to 6, forming a silicon-containing resist underlayer film on the organic film using a silicon-containing resist underlayer film material, forming an organic anti-reflective film on the silicon-containing resist underlayer film, A photoresist composition is used to form a resist upper film on the organic anti-reflection film to form a 4-layer film structure. forming a circuit pattern on the upper layer of the resist, Using the patterned resist upper film as a mask, the organic anti-reflection film and the silicon-containing resist lower film are etched to transfer the pattern to the organic anti-reflection film and the silicon-containing resist lower film. Using the silicon-containing resist lower layer film with the transferred pattern as a mask, the organic film is etched to transfer the pattern to the organic film. Furthermore, the object to be processed is etched using the organic film to which the pattern is transferred as a mask to form a pattern on the object to be processed.
9. A pattern forming method, characterized in that: forming an organic film on a workpiece using the organic film-forming material according to any one of claims 1 to 6, forming an inorganic hard mask film selected from a silicon oxide film, a silicon nitride film and a silicon oxide nitride film on the organic film, forming a resist upper layer film on the inorganic hard mask using a photoresist composition, forming a circuit pattern on the upper layer of the resist, Using the patterned resist upper film as a mask, the inorganic hard mask is etched to transfer the pattern to the inorganic hard mask. Using the inorganic hard mask film having the pattern formed thereon as a mask, the organic film is etched to transfer the pattern to the organic film. Furthermore, the object to be processed is etched using the patterned organic film as a mask to form a pattern on the object to be processed.
10. A method for forming a pattern, Its characteristics are: forming an organic film on a workpiece using the organic film-forming material according to any one of claims 1 to 6, forming an inorganic hard mask film selected from a silicon oxide film, a silicon nitride film and a silicon oxide nitride film on the organic film, forming an organic anti-reflection film on the inorganic hard mask, A photoresist composition is used to form a resist upper film on the organic anti-reflection film to form a 4-layer film structure. forming a circuit pattern on the upper layer of the resist, Using the patterned resist upper film as a mask, the organic anti-reflection film and the inorganic hard mask are etched to transfer the pattern to the organic anti-reflection film and the inorganic hard mask. Using the inorganic hard mask film having the pattern formed thereon as a mask, the organic film is etched to transfer the pattern to the organic film. Furthermore, the object to be processed is etched using the patterned organic film as a mask to form a pattern on the object to be processed.
11. The pattern forming method according to claim 9 or 10, in, The inorganic hard mask is formed by a CVD method or an ALD method.
12. The pattern forming method according to any one of claims 7 to 10, in, The resist upper layer film patterning method forms a pattern by optical lithography using light with a wavelength of 10 nm to 300 nm, direct writing using an electron beam, nanoimprinting, or a combination thereof.
13. The pattern forming method according to any one of claims 7 to 10, in, The patterning method of the resist upper layer film includes alkali development or development using an organic solvent.
14. The pattern forming method according to any one of claims 7 to 10, in, The object to be processed is a semiconductor device substrate, a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film or a metal oxide nitride film.
15. The pattern forming method according to any one of claims 7 to 10, in, The workpiece includes silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
16. A polymer having a structure represented by the following general formula (1A) as a partial structure; In the above general formula (1A), W 1 represents a 4-valent organic group, W 2 represents a single bond or a linking group represented by the following formula (1B), R 1 represents a hydrogen atom or a monovalent organic group having 1 to 10 carbon atoms, n1 represents an integer of 0 or 1, and n2 and n3 satisfy the relationship of 0≤n2≤6 and 0≤n3≤6 and 1≤n2+n3≤6; R 2 and R 3 Each independently represents hydrogen, an organic group having 1 to 30 carbon atoms, and the organic group R 2 With organic group R 3 It can also form cyclic organic groups by bonding within the molecule; When n1 is 0, W 1 Any one of the following expressions: When n1 is 1, W 1 Any one of the following expressions:
17. The polymer according to claim 16, in, The linking group W in the above general formula (1A) 2 It is represented by the following formula (1E); 18. The polymer according to claim 16 or 17, which has a weight average molecular weight of 1,000 to 10,000.
19. The polymer according to claim 16 or 17, which is a novolac resin having a partial structure represented by the general formula (1A).