Method for obtaining smooth surface by epitaxial lateral overgrowth

By embedding cone-shaped hillocks in a growth-limiting mask and removing the device using a polymer film, the surface roughness problem in the epitaxial lateral overgrowth method is solved, achieving smooth surfaces and efficient production of III-nitride layers.

CN113287205BInactive Publication Date: 2024-10-22RGT UNIV OF CALIFORNIA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980087480.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-31
Filing Date
2019-10-31
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When the existing technology uses the epitaxial lateral overgrowth method to manufacture non-polar and semi-polar GaN substrates, cone-shaped hillocks are prone to appear, resulting in surface roughness, affecting optical gain uniformity and device reliability. Moreover, the growth conditions are narrow and difficult to batch. Production.

Method used

By embedding cone-shaped hillocks in a growth-limiting mask, preventing its lateral expansion, materials such as SiO2 are used to grow in the III-nitride layer, ensuring a smooth surface and removed from the substrate by a polymer film. device.

Benefits of technology

It achieves an extremely smooth surface of the III nitride layer, improves the optical performance and production yield of the device, and avoids process fluctuations and reliability problems caused by surface roughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113287205B_ABST
    Figure CN113287205B_ABST
Patent Text Reader

Abstract

A method for obtaining a smooth surface of an epi layer by epitaxial lateral overgrowth. The method does not use a miscut orientation, nor does it suppress the appearance of pyramidal hillocks, but rather embeds the pyramidal hillocks into the epi layer. A growth limiting mask is used to limit the expansion of the pyramidal hillocks in the lateral direction. Due to the disappearance of the pyramidal hillocks, the surface of the epi layer becomes extremely smooth.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of 35 U.S.C. Section 119(e) of the following co-pending and commonly assigned applications:

[0003] U.S. Provisional Application Serial No. 62 / 753,225, filed on October 31, 2018 by Takeshi Kamikawa and Srinivas Gandrothula, entitled “METHODOF OBTAINING A SMOOTH SURFACE WITH EPITAXIAL LATERAL OVERGROWTH,” attorney docket No. G&C 30794.0693USP1 (UC 2019-166-1);

[0004] This application is incorporated herein by reference.

[0005] This application is related to the following co-pending and co-assigned applications:

[0006] PCT International Patent Application No. PCT / US18 / 31393, filed on May 7, 2018, by Takeshi Kamikawa, Srinivas Gandrothula, Hongjian Li, and Daniel A. Cohen, and entitled “METHOD OF REMOVING A SUBSTRATE,” and attorney docket number 30794.0653WOU1 (UC 2017-621-2), which claims the benefit under 35 U.S.C. § 119(e) of co-pending and commonly assigned U.S. Provisional Patent Application No. 62 / 502,205, filed on May 5, 2017, by Takeshi Kamikawa, Srinivas Gandrothula, Hongjian Li, and Daniel A. Cohen, and entitled “METHOD OF REMOVING A SUBSTRATE,” and attorney docket number 30794.0653USP1 (UC 2017-621-2). 2017-621-1);

[0007] PCT International Patent Application No. PCT / US18 / 51375, filed on September 17, 2018 by Takeshi Kamikawa, Srinivas Gandrothula, and Hongjian Li, and entitled “METHOD OF REMOVING A SUBSTRATE WITH A CLEAVING TECHNIQUE,” and attorney docket number 30794.0659WOU1 (UC2018-086-2), claims the benefit under 35 U.S.C. § 119(e) of co-pending and commonly assigned U.S. Provisional Patent Application No. 62 / 559,378, filed on September 15, 2017 by Takeshi Kamikawa, Srinivas Gandrothula, and Hongjian Li, and entitled “METHOD OF REMOVING A SUBSTRATE WITH A CLEAVING TECHNIQUE,” and attorney docket number 30794.0659WOU1 (UC2018-086-2). TECHNIQUE), case number 30794.0659USP1 (UC 2018-086-1);

[0008] PCT International Patent Application No. PCT / US19 / 25187, filed on April 1, 2019, by Takeshi Kamikawa, Srinivas Gandrothula, and Hongjian Li, and entitled “METHOD OF FABRICATING NONPOLAR AND SEMIPOLAR DEVICES USINGEPITAXIAL LATERAL OVERGROWTH,” attorney docket number 30794.0680WOU1 (UC 2018-427-2), claims the benefit under 35 U.S.C. § 119(e) of co-pending and commonly assigned U.S. Provisional Patent Application Serial No. 62 / 650,487, filed on March 30, 2018, by Takeshi Kamikawa, Srinivas Gandrothula, and Hongjian Li, and entitled “METHOD OF FABRICATING NONPOLAR AND SEMIPOLAR DEVICES USINGEPITAXIAL LATERAL OVERGROWTH,” attorney docket number 30794.0680WOU1 (UC 2018-427-2). NONPOLAR AND SEMIPOLAR DEVICES USING EPITAXIAL LATERALOVERGROWTH), case number G&C 30794.0680USP1 (UC 2018-427-1);

[0009] PCT International Patent Application No. PCT / US19 / 32936, filed on May 17, 2019 by Takeshi Kamikawa and Srinivas Gandrothula, and entitled “METHOD FOR DIVIDING A BAR OF ONE OR MORE DEVICES,” and attorney docket number 30794.0681WOU1 (UC 2018-605-2), claims the benefit under 35 U.S.C. § 119(e) of co-pending and commonly assigned U.S. Provisional Application Serial No. 62 / 672,913, filed on May 17, 2018 by Takeshi Kamikawa and Srinivas Gandrothula, and entitled “METHOD FOR DIVIDING A BAR OF ONE OR MORE DEVICES,” and attorney docket number G&C 30794.0682USP1 (UC 2018-606-2). 2018-605-1); and

[0010] PCT International Patent Application No. PCT / US19 / 34686, filed on May 30, 2019 by Srinivas Gandrothula and Takeshi Kamikawa, and entitled “METHOD OF REMOVING SEMICONDUCTING LAYERS FROM A SEMICONDUCTING SUBSTRATE,” Attorney Docket No. 30794.0682WOU1 (UC 2018-614-2), claims the benefit under 35 U.S.C. § 119(e) of co-pending and commonly assigned U.S. Provisional Application Serial No. 62 / 677,833, filed on May 30, 2018 by Srinivas Gandrothula and Takeshi Kamikawa, and entitled “METHOD OF REMOVING SEMICONDUCTING LAYERS FROM A SEMICONDUCTING SUBSTRATE,” filed on May 30, 2019 by Srinivas Gandrothula and Takeshi Kamikawa, and entitled “METHOD OF REMOVING SEMICONDUCTING LAYERS FROM A SEMICONDUCTING SUBSTRATE,” filed on May 30, 2019 by Srinivas Gandrothula and Takeshi Kamikawa, and entitled “METHOD OF REMOVING SEMICONDUCTING LAYERS FROM A SEMICONDUCTING SUBSTRATE), case number G&C 30794.0682USP1 (UC 2018-614-1);

[0011] All of these applications are incorporated herein by reference. Background of the Invention Technical Field

[0013] The present invention relates to a method for obtaining a smooth surface of an epi layer by epitaxial lateral overgrowth (ELO).

[0014] 2. Description of the Prior Art

[0015] Some device manufacturers have used non-polar and semi-polar gallium nitride (GaN) substrates to produce laser diodes (LD) and light-emitting diodes (LED) for lighting, optical storage, etc. Non-polar and semi-polar GaN substrates are used to avoid large thermoelectric and piezoelectric fields, which can lead to significant improvements in emission efficiency. However, epitaxial growth of III-nitrides along non-polar and semi-polar directions is more difficult than growth along the polar c-plane direction.

[0016] According to U.S. Patent Application Publication No. 2017 / 0092810A1, many pyramidal hillocks were observed on the surface of non-polar m-plane III-nitride films after epitaxial growth. This is a problem when manufacturing LD or LED structures on the surface because the surface roughness may cause uneven optical gain and fluctuations in device processes. This may also reduce the yield of device processes. In addition, the reliability of LD is affected by hillocks and large surface roughness. See, for example, Applied Physics Letters 91, 191906 (2007).

[0017] It is known that pyramidal hillocks deteriorate the roughness of the surface of the GaN substrate. In order to prevent pyramidal hillocks from appearing on the surface of the epi layer, a method of controlling the mis-cut orientation of the GaN substrate by more than 1 degree and growing the epi layer using a nitrogen carrier gas has been used.

[0018] However, the growth conditions for obtaining a smooth surface are very narrow and have strict limitations. One problem is that the surface morphology is affected by the off-angle orientation, and it is known that GaN wafers have a large in-plane distribution of off-angle orientations. This causes the surface morphology of the epi layer to change in different parts of the substrate, which reduces the yield during mass production. See, for example, Physica Status Solidi (a), Volume 214 (Volume 214), Issue 8 (Issue 8), 1600829 (2017).

[0019] In addition, a hillock facet dependence of the leakage current under reverse bias conditions was observed, where the leakage current distribution is caused by carrier and oxygen concentrations. The leakage current distribution is a problem when manufacturing devices such as LDs, LEDs, and power devices such as Schottky barrier diodes (SBDs) or metal oxide semiconductor field effect transistors (MOSFETs). Summary of the invention

[0020] In order to overcome the limitations of the above-mentioned prior art, and to overcome other limitations that will become apparent after reading and understanding this specification, the present invention discloses a method for obtaining a smooth surface of an epi layer by epitaxial lateral overgrowth, wherein the method does not use a miscut orientation, nor does it suppress the appearance of pyramidal hillocks, but instead embeds the pyramidal hillocks in the epi layer. A growth limiting mask is used to limit the expansion of the pyramidal hillocks in the lateral direction. Due to the disappearance of the pyramidal hillocks, the surface of the final epi layer is extremely smooth. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Referring now to the drawings, wherein like reference numerals designate corresponding parts throughout:

[0022] Figure 1 is a schematic cross-sectional view illustrating a device structure manufactured according to one embodiment of the present invention.

[0023] Figure 2 Both photoluminescence (PL) images and differential interference contrast (DIC) microscopy measurement images of a patterned sample and a non-patterned sample according to one embodiment of the present invention are included.

[0024] 3(a) and 3(b) are images showing that a pyramidal hillock is confined within an opening region according to an embodiment of the present invention.

[0025] Figure 4(a) shows scanning electron microscope (SEM) images of the 1st and 3rd rows and PL images of the 2nd and 4th rows of the surface of the epi layer according to an embodiment of the present invention, wherein each column represents a different mis-cut orientation angle of the substrate, i.e., 0°, -0.45°, -0.61° and -1.0° mis-cut of the non-polar (10-10) substrate and -15° mis-cut of the semi-polar (20-2-1) substrate.

[0026] FIG. 4( b ) is an image of a 1° mis-orientation angle according to one embodiment of the present invention.

[0027] Figure 5 (a) Figure 5 (b) Figure 5 (c) Figure 5 (d) and Figure 5 (e) is a schematic diagram illustrating a buried pyramidal hillock during initial growth according to one embodiment of the present invention.

[0028] 6( a ) and 6 ( b ) are PL and DIC images, respectively, of the back side of the epi layer after being removed from the (10-10) substrate according to one embodiment of the present invention.

[0029] FIG. 7( a ) is a SEM image of an island-shaped Group III nitride semiconductor layer oriented along an m-plane according to one embodiment of the present invention.

[0030] 7( b ) shows four images of an island-shaped III-nitride semiconductor layer with different shear orientations marked with 0°, −0.45°, −0.6°, and −1.0° along the (1-100) m plane according to an embodiment of the present invention.

[0031] Figure 8 is a cross-sectional side view of a III-nitride semiconductor laser diode device according to one embodiment of the present invention, taken along a direction perpendicular to an optical resonator.

[0032] 9(a) and 9(b) are schematic diagrams of strips of a device according to an embodiment of the present invention.

[0033] 10(a) and 10(b) are schematic diagrams illustrating how divided support regions are formed at periodic lengths along strips of a device according to one embodiment of the present invention.

[0034] 11(a), 11(b), 11(c), 11(d) and 11(e) are schematic diagrams illustrating how to use a polymer film to remove strips of a device from a substrate according to one embodiment of the present invention.

[0035] 12( a ) and 12 ( b ) are SEM images showing a surface of a substrate and a surface of a strip of a device according to one embodiment of the present invention.

[0036] 13(a) and 13(b) are schematic diagrams illustrating how a growth confinement mask is used to fabricate strips of a device on a substrate in accordance with one embodiment of the present invention.

[0037] 14( a ) and 14 ( b ) are SEM images at different magnifications of the surface of a substrate according to an embodiment of the present invention.

[0038] Figures 15(a), 15(b), 15(c), 15(d), 15(e) and 15(f) are schematic diagrams illustrating how to divide strips of a device according to an embodiment of the present invention.

[0039] 16(a) and 16(b) are schematic diagrams illustrating how a growth limit mask is used to fabricate strips of a device on a substrate according to one embodiment of the present invention.

[0040] Fig.17 is a schematic diagram illustrating how facets are coated on a device according to one embodiment of the present invention.

[0041] 18(a), 18(b), and 18(c) are schematic diagrams illustrating how wire bonding and probes are attached to a device according to one embodiment of the present invention.

[0042] 19(a) and 19(b) are schematic diagrams illustrating how to divide a heat sink into separate devices according to an embodiment of the present invention.

[0043] 20( a ) and 20 ( b ) are schematic diagrams illustrating a testing apparatus for a device according to an embodiment of the present invention.

[0044] Fig.21 is a schematic diagram illustrating how to package a device according to one embodiment of the present invention.

[0045] Fig. 22 is a schematic diagram illustrating how to package a device according to one embodiment of the present invention.

[0046] 23(a) and 23(b) are schematic diagrams illustrating how a growth confinement mask is used to fabricate strips of a device on a substrate according to one embodiment of the present invention.

[0047] 24( a ) and 24 ( b ) are schematic diagrams illustrating a layer bending region of a device according to an embodiment of the present invention.

[0048] 25(a) and 25(b) are schematic diagrams illustrating a polymer film used to remove a strip of a device from a substrate according to an embodiment of the present invention.

[0049] 26( a ) and 26 ( b ) are images showing facets of an island-shaped Group III nitride semiconductor layer after shearing according to one embodiment of the present invention.

[0050] Figure 27(a), Figure 27(b), Figure 27(c), Figure 27(d), Figure 27(e) , 27(f) and 27(g) are schematic diagrams illustrating how to obtain an ELO structure according to an embodiment of the present invention.

[0051] Fig.28 is an image showing a smooth surface of an ELO structure embedded with pyramidal hillocks according to one embodiment of the present invention.

[0052] Fig.29 is a flowchart illustrating a method of manufacturing a Group III nitride semiconductor device according to one embodiment of the present invention. DETAILED DESCRIPTION

[0053] In the following description of the preferred embodiments, reference is made to specific embodiments in which the invention may be practiced. It should be understood that other embodiments may be utilized and structural changes may be made without departing from the scope of the present invention.

[0054] Overview

[0055] The present invention describes a method for obtaining a smooth surface of one or more III-nitride layers (such as GaN layers) using epitaxial lateral overgrowth. In one example, the method is used to manufacture a light emitting diode, a laser diode, a Schottky barrier diode, or a metal oxide semiconductor field effect transistor.

[0056] This method is not affected by the mis-cut orientation in the surface morphology. In addition, this method does not suppress the occurrence of pyramidal hillocks, but embeds the pyramidal hillocks into the epi layer by preventing the expansion of the pyramidal hillocks, wherein a growth restriction mask is used to prevent the expansion of the pyramidal hillocks in the lateral direction. It is believed that the pyramidal hillocks are gradually embedded in the epi layer. Therefore, due to the disappearance of the pyramidal hillocks, the surface of the epi layer is very smooth.

[0057] Figure 1 is a cross-sectional view illustrating a device structure manufactured according to one embodiment of the present invention.

[0058] In this example, a III-nitride based substrate 101, such as a bulk GaN substrate 101, is provided, and a growth restriction mask 102 is formed on or over the substrate 101. In the growth restriction mask 102, stripe-shaped opening regions 103 are defined.

[0059] No-growth regions 104 are obtained when the ELO III-nitride layer 105 grown from adjacent opening regions 103 in the growth limit mask 102 is not agglomerated on top of the growth limit mask 102. Preferably, the growth conditions are optimized so that the lateral width of the ELO III-nitride layer 105 on its wing regions is 20 μm.

[0060] Additional III-nitride semiconductor device layers 106 are deposited on or over ELO III-nitride layer 105 and may include an active region 106a, an electron blocking layer (EBL) 106b, and a cladding layer 106c, among other layers.

[0061] The thickness of ELO Group III nitride layer 105 is important because it determines the width of one or more planar surface regions 107 and layer bow regions 108 located at its edges adjacent to no growth region 104. The width of planar surface regions 107 is preferably at least 5 μm, and more preferably 10 μm or more, and most preferably 20 μm or more.

[0062] The ELO III-nitride layer 105 and the additional III-nitride semiconductor device layer 106 are referred to as island-shaped III-nitride semiconductor layers 109, wherein the no-growth region 104 separates adjacent island-shaped III-nitride semiconductor layers 109. The distance between the island-shaped III-nitride semiconductor layers 109 adjacent to each other is the width of the no-growth region 104, which is typically 20 μm or less, preferably 5 μm or less, but is not limited to these values.

[0063] Each island-shaped III-nitride semiconductor layer 109 can be processed into a separate device 110. The device 110 is processed on the flat surface area 107 and / or the opening area 103, and the device 110 can be a light emitting diode, a laser diode, a Schottky barrier diode, or a metal oxide semiconductor field effect transistor. In addition, the shape of the device 110 generally includes a stripe.

[0064] In this embodiment, the occurrence of the pyramidal hillocks 111 is not suppressed, but the pyramidal hillocks 111 are gradually embedded in the ELO III-nitride layer 105, which prevents the pyramidal hillocks 111 from expanding. The growth limiting mask 102 also limits the expansion of the pyramidal hillocks 111 in the lateral direction. Therefore, the surface of the ELO III-nitride layer 105 is extremely smooth due to the disappearance of the pyramidal hillocks 111.

[0065] Cone-shaped hillock

[0066] Figure 2 FIG. 4 illustrates the reason why no pyramidal hillocks 111 appear on the surface of the epi layers 105 , 106 or 109 .

[0067] Figure 2 Photoluminescence (PL) images and differential interference contrast (DIC) microscopy measurement images of patterned and non-patterned samples of GaN layers, where the samples were co-loaded into a metal organic chemical vapor deposition (MOCVD) chamber and grown simultaneously. The PL and DIC images show the same location on the sample.

[0068] The PL image shows that the yellow luminescence intensity of the GaN layer is poor. The GaN layer emits a broad luminescence spectrum due to the concentration of n-type dopants such as Si, O, etc. A region with a high concentration of n-type dopants emits brighter yellow luminescence than a region with a low concentration of n-type dopants.

[0069] As described above, the GaN layer generally includes a pyramidal hillock, which typically includes four facets tilted toward the

[0001] , [1-210], [000-1] and [-12-10] directions, respectively. Each facet is different in its incorporation of n-type dopants. Therefore, the n-type dopant concentration of each facet is different, which results in a difference in the intensity of yellow luminescence. Therefore, the presence of a pyramidal hillock can be identified by PL measurement.

[0070] On the other hand, the DIC image measures the surface roughness of the GaN layer. Specifically, the DIC image can only detect information on the surface of the GaN layer.

[0071] Figure 2 The non-patterned samples in are the result of the conventional method for preparing epi wafers without treatment, while Figure 2 The patterned sample in is the result of the method of the present invention.

[0072] There are a large number of pyramidal hillocks in the non-patterned samples, which Figure 2 In this case, a pyramidal hillock can be identified in both the PL image and the DIC image at the same position, indicating that the pyramidal hillock is emerging on the surface of the epi layer.

[0073] On the other hand, in the patterned sample, pyramidal hillocks can be identified using only the PL image, but the pyramidal hillocks do not appear on the surface of the epi layer shown in the DIC image. The reason for this is that the pyramidal hillocks are embedded in the epi layer.

[0074] like Figure 3(a)-Figure 3(b) As shown, the pyramidal hillock is generally confined by the SiO2 growth limiting mask 102 to the region of the ELO III-nitride layer 105 within the opening region 103, rather than extending across the entire epi layer 105. In these examples, the width and misalignment orientation of the opening region 103 of each sample are defined as 16.2 μm and -0.45 degrees in FIG. 3(a), and 11 μm and 0 degrees in FIG. 3(b). Note that the location of the pyramidal hillock is not always at the center of the opening region 103, and the shape of the pyramidal hillock is asymmetric.

[0075] From this, it can be considered that the pyramidal hillock appears in the opening region 103 at the beginning of growth. In addition, it is considered that the reason why the pyramidal hillock does not expand outside the opening region 103 is that the size of the pyramidal hillock is limited by the growth limiting mask 102.

[0076] FIG4( a) shows scanning electron microscope (SEM) images of the 1st and 3rd rows of the epi layer surface and PL images of the 2nd and 4th rows, each column representing a different mis-cut orientation angle of the substrate, i.e., 0°, -0.45°, -0.61°, and -1.0° mis-cut for a non-polar (10-10) substrate and -15° mis-cut for a semi-polar (20-2-1) substrate. The SEM images show that there are no pyramidal hillocks on the epi layer surface in each mis-cut orientation. On the other hand, the PL images show a large number of pyramidal hillocks in the opening area. As mentioned above, these pyramidal hillocks are embedded in the epi layer. The smaller the mis-cut orientation angle, the greater the number of pyramidal hillocks. Regardless of the number of pyramidal hillocks, the surface morphology of each mis-cut orientation is extremely smooth.

[0077] As shown in Figure 4(b), a pyramidal hillock may appear at a 1° misorientation angle, depending on the growth conditions, the crystal quality of the substrate, or the surface condition. The effectiveness of this method does not depend on the misorientation angle.

[0078] Figure 5 (a)- Figure 5 (e) is a schematic diagram illustrating how the pyramidal hillocks 111 are buried through the open regions 103 in the growth restriction mask 102 during the growth of the ELO III-nitride layer 105 on the substrate 101 according to the present invention.

[0079] exist Figure 5 (a) and Figure 5 In (b), a pyramidal hillock 111 appears in the opening region 103, and its width wp is as follows: Figure 5 (b) as shown.

[0080] exist Figure 5 In (c), the width wp of the pyramidal hillock 111 is equal to the width of the opening region 103. In this case, the width wp of the pyramidal hillock 111 cannot extend beyond the opening region 103.

[0081] exist Figure 5 In (d), the height hp of the pyramidal hillock 111 appears to be limited by the width wp of the opening region 103 in the growth limiting mask 102 and is related to Figure 5 (c) The height of the pyramidal hillock 111 is maintained at the same level regardless of the further growth of the epi layer 105. However, the area around the pyramidal hillock 111 continues to grow as the epi layer 105 grows, and thus, the pyramidal hillock 111 is gradually embedded in the epi layer 105.

[0082] Finally, if Figure 5 As shown in (e), the pyramidal hillocks 111 are completely embedded in the epi layer 105. In addition, the surface morphology of the epitaxial layer 105 is very smooth and is not affected by the presence of the pyramidal hillocks 111.

[0083] 6(a) and 6(b) are PL and DIC images, respectively, of the back side of the ELO III-nitride layer 105 after the ELO III-nitride layer 105 is removed from the (10-10) substrate 101, where the substrate 101 does not have a mis-cut orientation. The DIC measurement image does not show the pyramidal hillock 111, but the PL image does show the pyramidal hillock 111, indicating that the pyramidal hillock 111 is embedded in the ELO III-nitride layer 105.

[0084] Even though the ELO III-nitride layer 105 is a homogeneous epitaxial layer, the ELO III-nitride layer 105 is easily removed from the substrate 101, and there is no heterogeneous interface between the ELO III-nitride layer 105 and the surface of the substrate 101. However, using the growth limiting mask 102, the ELO III-nitride layer 105 can be removed from the III-nitride substrate 101 in a fast and easy manner.

[0085] For example, the growth limiting mask 102 may be a dielectric film or a metal, such as SiO2, SiN, HfO2, Al2O3, MgF, W, Mo, Pt, Ir, Os, etc. The bonding strength of the interface between the growth limiting mask 102 and any subsequent ELO III-nitride layer 105 grown on the mask 102 is weak. The bonding area, which is the width of the opening area 103, is controlled to be larger or smaller than the size of the device 110.

[0086] In addition, the method can use shearing along the m-plane of the substrate 101, which is the easiest plane to shear among the GaN planes. In addition, the edges of the growth limiting mask 102 provide shearing points and shearing interfaces for removing the substrate 101 from the ELO III-nitride layer 105. Hydrofluoric acid (HF), buffered HF (BHF) or other etchants can also be used to at least partially dissolve the growth limiting mask 102 before removing the substrate 101 from the ELO III-nitride layer 105. Finally, a polymer and / or adhesive tape can be used to remove the substrate 101 from the ELO III-nitride layer 105.

[0087] Preparation method

[0088] The following describes steps for fabricating device 110 according to one embodiment of the present invention.

[0089] Step 1: directly or indirectly forming a growth restriction mask 102 having a plurality of opening regions 103 on a substrate 101 , wherein the substrate 101 is a III-nitride substrate or a heterogeneous substrate.

[0090] Step 2: A plurality of island-shaped group III nitride semiconductor layers 109 are grown on the substrate 101 using the growth restriction mask 102 so that the growth extends in a direction parallel to the stripe-shaped opening regions 103 of the growth restriction mask 102 .

[0091] Step 3: The device 110 is manufactured on the flat surface region 107 by a conventional method. For example, a ridge structure, a p-electrode, a p-pad, etc. are provided at a predetermined position on the island-shaped group III nitride semiconductor layer 109 .

[0092] Step 4: Form a support structure on the device 110 for shearing at the side facets.

[0093] Step 5: Dissolve the growth limit mask 102 at least partially by wet etching.

[0094] Step 6: Removing the strips of devices 110 from the substrate 101 .

[0095] 6.1. Attaching polymer film to the strips of device 110 .

[0096] 6.2. Apply pressure to the polymer film and substrate 101 .

[0097] 6.3. Modifying (eg, lowering) the temperature of the membrane and substrate 101 while applying pressure.

[0098] 6.4. The difference in thermal coefficient between the polymer film and the material of the substrate 101 is exploited to remove the strips of the device 110 .

[0099] Step 7: Dispose an n-electrode in the isolated region of the device 110 .

[0100] Step 8: Breaking the strip of devices 110 into one or more devices 110 or chips.

[0101] Step 9: Mount the device 110 on a heat sink.

[0102] Step 10: Coat the facets of device 110 using a coating bar.

[0103] Step 11: Divide the coating strips.

[0104] Step 12: Screening devices 110.

[0105] Step 13: Mounting the device 110 on / into a package.

[0106] These steps are described in more detail below.

[0107] Step 1: Forming a Growth Limiting Mask

[0108] like Figure 1As shown, an epitaxial GaN layer 105 is grown by ELO on an m-plane GaN substrate 101 patterned with SiO2. The substrate 101 may be of other planes, and a foreign substrate 101 may also be used on which a GaN template is grown. The patterned SiO2 (which serves as a growth restriction mask 102) includes a stripe-shaped opening region 103 with a width of 2-180 μm and an interval of 150 μm, wherein the SiO2 stripes are arranged along the <0001> The ELO GaN layer 105 does not coalesce on top of the growth limit mask 102 .

[0109] Step 2: Growing III-nitride semiconductor layer

[0110] MOCVD can be used for the epitaxial growth of the III-group nitride semiconductor layers 105, 106, 109. Trimethyl gallium (TMGa), trimethyl indium (TMIn) and triethyl aluminum (TMAl) are used as the III-group element sources. Ammonia (NH3) is used as the raw gas for supplying nitrogen. Hydrogen (H2) and nitrogen (N2) are used as carrier gases for the III-group element sources (it is important to include hydrogen in the carrier gas to obtain a smooth surface epi layer). Salt water and bis(cyclopentadienyl) magnesium (Cp2Mg) are used as n-type and p-type dopants.

[0111] The following growth conditions were used:

[0112] The growth pressure is 60 to 760 Torr. In order to obtain a wide width of the island-shaped Group III nitride based semiconductor layer 109, the pressure is preferably 100 to 300 Torr.

[0113] The growth temperature is generally 900-1200°C.

[0114] The V / III ratio ranges from 1000 to 30000, preferably from 3000 to 10000. The TMG ranges from 2 to 20 sccm, and the NH3 ranges from 3 to 10 slm.

[0115] • The carrier gas may comprise hydrogen alone or a mixture of hydrogen and nitrogen.

[0116] To obtain a smooth surface, the growth conditions for each plane need to be optimized by conventional methods.

[0117] After growing for about 2-8 hours, the thickness of the ELO III-nitride layer 105 is about 8-50 μm, and the width of the strip 901 is about 20-150 μm, wherein the width of the strip 901 is the width of the island III-nitride semiconductor layer 109 .

[0118] like Figure 7(a)-Figure 7(b)As shown, the method obtains an island-shaped III-nitride semiconductor layer 109 having a smooth top surface without a pyramidal hillock 111 or a concave portion and having various mis-cut orientations. Specifically, FIG. 7( a) shows an SEM image of an island-shaped III-nitride semiconductor layer 109 oriented along the m-plane, and FIG. 7( b) shows four images of an island-shaped III-nitride semiconductor layer 109 with different mis-cut orientations marked with 0°, -0.45°, -0.6°, and -1.0° along the (1-100) m-plane.

[0119] Step 3: Device Process

[0120] As set forth in step 2, after the III-nitride semiconductor device layer 106 has been grown on the ELO III-nitride layer 105, a flat region 107 is formed for each device 110. These flat regions 107 are separated from one another so that the MOCVD growth stops before they coalesce.

[0121] III-nitride semiconductor device layer

[0122] Figure 8 is a cross-sectional side view of a III-nitride semiconductor laser diode device 110 fabricated along a direction perpendicular to the optical resonator.

[0123] Device 110 is fabricated by conventional methods on a flat surface region 107, with ridge structures, p-electrodes, n-electrodes, pads, etc. disposed at predetermined locations on an island-shaped Group III nitride semiconductor layer 109. (The curved region 108 is not depicted in this figure.)

[0124] The laser diode device 110 includes the following III-nitride semiconductor device layers 106 grown on an ELO GaN-based layer 105 deposited on a growth confinement mask 102, stacked one on top of the other in the order mentioned: n-Al 0.06 GaN cladding layer 801 , n-GaN waveguide layer 802 , InGaN / GaN multiple quantum well (MQW) active layer 803 , AlGaN EBL layer 804 , p-GaN waveguide layer 805 , ITO cladding layer 806 , SiO 2 current limiting layer 807 and p-electrode 808 .

[0125] The optical resonator includes a ridge stripe structure, wherein the ridge stripe structure is composed of an ITO cladding layer 806, a SiO2 current limiting layer 807 and a p-electrode 808. The optical resonator provides optical confinement in the horizontal direction. The width of the ridge stripe structure is on the order of 1.0 to 30 μm, and is typically 10 μm.

[0126] Conventional methods such as photolithography and dry etching can be used to fabricate the ridge stripe structure. The ridge depth (from the surface to the ridge bottom) is in the p-GaN waveguide layer 805. The ridge depth is predetermined before performing dry etching based on simulations or previous experimental data.

[0127] In one embodiment, the p-electrode 808 may include one or more of the following materials: Pd, Ni, Ti, Pt, Mo, W, Ag, Au, etc. For example, the p-electrode 808 may include Pd-Ni-Au (thickness is 3-30-300 nm). These materials may be deposited by electron beam evaporation, sputtering, thermal evaporation, etc. In addition, the p-electrode 808 is typically deposited on the ITO coating 806.

[0128] Step 4: Forming support structures for shearing at the side facets and flat surface areas.

[0129] As shown in Figures 9(a) and 9(b), the goal of this step is to form a support structure for cutting the strip 901 of the device 110 before removing the strip 901 from the substrate 101. The divided support area 902 is formed with a periodic length, where each period is determined by the length of the device 110. For example, in the case of the laser diode device 110, one period is set to 300-1200 μm.

[0130] Each division support region 902 is a line scribed by a diamond tip scriber or a laser scriber, as shown in FIG9( a); or a groove formed by dry etching such as RIE (reactive ion etching) or ICP (inductively coupled plasma), as shown in FIG9( b); but is not limited to these methods. The division support region 902 may be formed on both sides of the strip 901 or on one side of the strip 901. The depth of the division support region 902 is preferably 1 μm or more.

[0131] In both cases, the strip 901 can be divided into separate devices 110 at the dividing support region 902 because the dividing support region 902 is more fragile than any other portion. The dividing support region 902 avoids breaking the strip 901 at an undesirable position, making it possible to accurately determine the length of the device 110.

[0132] The divided support region 902 is formed at the flat surface region 107 and the layer bending region 108 in a manner avoiding the current injection region 903 and the p-electrode 808 in the ridge structure, but it may cover at least a portion of the SiO 2 current limiting layer 807 .

[0133] like Figure 9(a) and 9(b) As shown, the divided support area 902 is formed at the first facet 904 and optionally at the second facet 905, which are easy to handle because they are flat areas. The third facet 906 can be avoided.

[0134] 10( a ) and 10 ( b ) also illustrate how divided support regions 902 may be formed at periodic lengths along strips 901 of device 110 , in accordance with one embodiment of the present invention.

[0135] Step 5: Dissolve the growth limit mask by wet etching.

[0136] The method may further comprise the step of removing at least a portion of the growth limit mask 102 , or preferably substantially all of the growth limit mask 102 , or most preferably all of the growth limit mask 102 , by means of a wet etchant.

[0137] The growth limiting mask 102 is removed by using a chemical solution such as HF or BHF. This process allows the device 110 to be easily removed from the GaN substrate 101. In addition, it is best to perform this process before removing the epi layers 105, 106, 109 from the substrate 101. In addition, it is best to perform this process before processing the device 110 (step 3).

[0138] Step 6: Remove the device strip from the substrate

[0139] From here, use Figure 11(a)-11(e) The process of removing the strip 901 of the device 110 from the substrate 101 is explained.

[0140] Step 6.1 includes attaching a polymer film 1101 to the strip 901 of the device 110, as shown in FIG11(a). In this embodiment, the polymer film 1101 includes a base film 1102, an adhesive 1103, and a backing film 1104.

[0141] Step 6.2 includes applying pressure 1105 to the polymer film 1101 and the substrate 101 using a plate 1106, as shown in FIG11( b). The goal of applying pressure 1105 is to place the polymer film 1101 between the strips 901 of the device 110. The polymer film 1101 is softer than the strips 901 of the device 110, so the polymer layer 1101 can easily surround the strips 901 of the device 110. Preferably, the polymer film 1101 is heated to soften it, which makes it easy for the polymer film 1101 to cover the strips 901 of the device 110.

[0142] Step 6.3 comprises reducing the temperature of the polymer film 1101 and the substrate 101 while maintaining the applied pressure 1105. However, it is not necessary to apply the pressure 1105 during the temperature change.

[0143] Step 6.4 includes removing strips 901 of device 110 by taking advantage of the difference in thermal coefficients between polymer film 1101 and substrate 101 .

[0144] As shown in FIG11(c), the polymer film 1101 shrinks as the temperature decreases. Therefore, as shown in FIG11(d), the bottom of the polymer film 1101 is lower than the top of the strip 901 of the device 110.

[0145] As shown in FIG11( c), the polymer film 1101 can apply pressure 1105 in a horizontal direction at the side facets of the strips 901 of the device 110, exposing shear points 1107 and causing the strips 901 of the device 110 to tilt downward 1108. This pressure 1105 applied from the side facets allows the strips 901 of the device 110 to be effectively removed from the substrate 101. During low temperatures, the polymer film 1101 maintains the pressure 1105 applied from the top of the polymer film 1101 to the strips 901 of the device 110.

[0146] Various methods can be used to reduce the temperature. For example, the substrate 101 and the polymer film 1101 can be placed in liquid N2 (e.g., at 77°K) while applying pressure 1105. The temperature of the substrate 101 and the polymer film 1101 can also be controlled with a piezoelectric converter. In addition, the plate 1106 that applies pressure 1105 to the polymer film 1101 can be cooled to a low temperature before and / or during contact with the polymer film 1101. By doing so, due to the large thermal expansion coefficient, the polymer film 1101 is cooled and pressure 1105 can be applied to the strip 901 of the device 110.

[0147] When the temperature is lowered, the substrate 101 and the polymer film 1101 may be wetted by atmospheric humidity. In this case, the temperature may be lowered in a dry gas atmosphere or a dry N2 atmosphere, which prevents the substrate 101 and the polymer film 1101 from becoming wet.

[0148] Thereafter, as shown in FIG11( d), the temperature is raised to, for example, room temperature, and pressure 1105 is no longer applied to the polymer film 1101. At that time, the strip 901 of the device 110 can be removed from the substrate 101, and then the polymer film 1101 is separated from the substrate 101, as shown in FIG11( e). When the polymer film 1101, particularly the polymer film 1101 having the adhesive 1103, is used, the strip 901 of the device 110 can be removed in an easy and quick manner using the polymer film 1101.

[0149] Remove Bar

[0150] By taking advantage of the different thermal expansion coefficients between the polymer film 1101 and the semiconductor material of the device 110 to remove the strip 901, horizontal pressure can be uniformly applied to the entire substrate 101. Therefore, the strip 901 of the device 110 can be removed from the substrate 101 without damaging the strip 901. This has been demonstrated by the high yields obtained.

[0151] Figure 12(a) and12(b) is a SEM image of the strip 901, showing the surface of the substrate 101 in FIG. 12(a) and the surface of the strip in FIG. 12(b).

[0152] The strip 901 of the device 110 is in the shape of a rectangle with long sides and short sides, such as Figure 13(a) and 13(b) As shown. As shown in FIG. 11( c ), pressure is applied to the strip 901 of the device 110 having such a shape from the vertical direction and in the horizontal direction relative to the long side of the strip 901. By doing so, an effective influence can be given to the shear point, which removes the strip 901 of the device 110 from the substrate 101. Before attaching the polymer film to the strip 901 of the device 110, the growth limiting mask 102 is preferably removed from the substrate 101 by wet etching or the like. Eliminating the growth limiting mask 102 leaves room for applying pressure at the shear point below the strip 901 of the device 110, which can cause the strip 901 of the device 110 to tilt downward as shown in FIG. 11( c ).

[0153] Shearing at the separation region of the m-plane surface

[0154] 14(a) and 14(b) are SEM images of the surface of substrate 101 at different magnifications, which is a non-polar (1-100) III-nitride substrate 101 without mis-cut orientation. As shown in FIG14(a) and FIG14(b), a very smooth surface of substrate 101 is obtained after removing strip 901 using the m-plane facets for shearing. In this case, the surface of the obtained strip 901 can be used as the facet of the VCSEL that emits light.

[0155] Step 7: Fabrication of n-electrode in the separation area of ​​the device

[0156] After removing the strip 901 from the substrate 101 , the strip 901 remains attached to the polymer film 1101 , as shown in FIG. 15( a ), with the strip 901 positioned on the film 1101 in an upside-down manner.

[0157] 15( b) shows the back side of the strip 901 in both a schematic diagram and an SEM image, which has a separation region 1501 between the divided support regions 902. The separation region 1501 directly contacts the substrate 101 or an underlying layer, but is not on the growth limiting mask 102. A shear blade 1502 is used at the divided support region 902.

[0158] Then, as shown in FIG. 15( c ), an n-electrode 1504 may be provided on the back side of the device 110 using a metal mask 1503 .

[0159] In the case where the n-electrode 1504 on the back side of the strip 901 is formed after the strip 901 is removed from the substrate 101, the n-electrode 1504 is preferably formed on the separation region 1501. The separation region 1501 is kept in a good surface state so that a low contact resistivity is obtained for the n-electrode 1504. The present invention keeps the region 1501 clean until the island-shaped Group III nitride semiconductor layer 109 is removed.

[0160] The n-electrode 1504 may also be disposed on the top surface of the strip 901 , which is the same surface made for the p-electrode 808 .

[0161] Typically, the n-electrode 1504 includes the following materials: Ti, Hf, Cr, Al, Mo, W, Au. For example, the n-electrode 1504 may include Ti-Al-Pt-Au (thickness of 30-100-30-500 nm), but is not limited to these materials. The deposition of these materials may be performed by electron beam evaporation, sputtering, thermal evaporation, etc.

[0162] Step 8: Break the strips of device into chips

[0163] After providing the n-electrode 1504, the plurality of strips 901 arranged laterally are divided into a plurality of devices 110, as shown in Fig. 15(d). As shown in Fig. 15(b), the dividing support region 902 helps to divide the strips 901 into devices 110. Although shearing is used, a breaking method or other methods may also be used.

[0164] As shown in FIG16(a), it is possible that the plurality of strips 901 arranged transversely are sheared and broken into separate devices 110 at the dividing support region 902. In addition, as shown in FIG16(b), it is also possible to shear the plurality of strips 901 arranged transversely and longitudinally on the dividing support region 902. In addition, the dividing support region 902 may be provided on both sides 1601 or one side 1602 of the strip 901.

[0165] Step 9: Mount the Device on the Heat Sink

[0166] After step 8, the divided strips 901 remain on the polymer film 1101. In one embodiment, the polymer film 1101 is an ultraviolet (UV) sensitive dicing tape exposed to UV light, which can reduce the adhesive strength of the film 1101, as shown in FIG15(e). This makes it easy to remove the device 110 from the film 1101.

[0167] In this step, a heat sink 1505 including AlN is prepared. Au-Sn solder 1506 is disposed on the heat sink 1505, the heat sink 1505 is heated to a temperature exceeding the melting temperature of the solder 1506, and the device 110 on the polymer film 1101 is bonded to the heat sink 1505 using the Au-Sn solder 1506. The device 110 can be mounted on the heat sink 1505 in two ways: (1) with the n-electrode 1504 side facing down or (2) with the p-electrode 808 side facing down. FIG. 15( e) shows the device 110 mounted to the heat sink 1505 using the solder 1506 with the n-electrode 1504 side facing down. The grooves 1507 in the heat sink 1505 separate the devices 110, wherein the grooves 1507 are used to divide the heat sink 1505, as described in more detail below.

[0168] Step 10: Coating the Facets of the Laser

[0169] The next step in device processing includes coating the facets 904 of the device 110. When the laser diode device 110 is lasing, light in the device 110 that penetrates through the facets 904 of the device 110 to the outside of the device 110 is absorbed by the non-radiative recombination centers at the facets 904, causing the facets 904 to continue to increase in temperature. Therefore, the temperature increase may cause catastrophic optical damage (COD) to the facets 904.

[0170] The facet 904 coating can reduce non-radiative recombination centers. In order to prevent COD, a dielectric layer (such as AlN, AlON, Al2O3, SiN, SiON, SiO2, ZrO2, TiO2, Ta2O5, etc.) must be used to coat the facet 904. In general, the coating film is a multilayer structure including the above materials. The structure and thickness of the layer are determined by the predetermined reflectivity.

[0171] In the present invention, the strip 901 of the device 110 can already be divided in step 8 to obtain the shear facets 904 for a plurality of devices 110. Therefore, it is necessary to perform a method of coating the facets 904 on a plurality of devices 110 simultaneously in a simple manner. In one embodiment, the device 110 is mounted on the heat sink 1505 in a horizontally offset manner, for example, toward one side of the heat sink 1505, as shown in FIG. 15( f). Then, as shown in FIG. Fig.17 As shown, the device 110 and the heat sink 1505 are placed on a spacer plate 1701 , and a plurality of spacer plates 1701 are stored in a coating holder 1702 .

[0172] Note that it is not always necessary to use the spacer plate 1701, and the heat sink plate 1505 can be used alone. Alternatively, the heat sink plate 1505 can be mounted on another strip or plate, which is then placed on the spacer plate 1701.

[0173] By doing so, the facets 904 of multiple devices 110 can be coated simultaneously. In one embodiment, the facet 904 coating is performed at least twice - once for the front facets 904 of the device 110 and once for the back facets 904 of the device 110. The length of the heat sink 1505 can be sized to be approximately the cavity length of the laser diode device 110, which makes it quick and easy to perform the facet 904 coating twice.

[0174] Once the spacer plate 1701 is set in the coating holder 1702, the two facets 904 of the device 110 can be coated without setting the spacer plate 1701 in the coating holder 1702 again. In one embodiment, the first coating is performed on the front facet 904 that emits the laser, and the second coating is performed on the rear facet 904 that reflects the laser. Before the second coating is performed in the facility for depositing the coating film, the coating holder 1702 is turned over. This substantially reduces the preparation time for the process.

[0175] Step 11: Divide the Coating Strips

[0176] As shown in FIG. 18( a), wire bonds 1801 and 1802 are attached to device 110, and heat sink 1505 is then divided at groove 1507, for example, between one or more devices 110. FIG. 18( b) is a top view of FIG. 18( a), showing the relative placement and position of device 110, groove 1507, and bonds 1801, 1802. FIG. 18( c) shows the use of a breakaway probe 1803 and wire bonds 1804 with device 110.

[0177] Figure 19(a) and 19(b) It is further shown how the heat sink 1505 can be divided to separate the devices 110, which can occur before or after the attachment of the wire bonds 1801, 1802. By doing so, it is easy to separate the devices 110 after the coating process has been completed.

[0178] Step 12: Screening Devices

[0179] This step distinguishes defective devices 110 from non-defective devices 110. First, various characteristics of the device 110 are inspected under given conditions; for example, output power, voltage, current, resistivity, FFP (far field pattern), slope efficiency, etc. At this point, the device 110 has been mounted on the heat sink 1505, so it is easy to inspect these characteristics.

[0180] exist Figure 20(a) and 20(b)1 shows a test device 2001, in which probes 2002, 2003 contact the p-electrode 808 and the solder 1506 having electrical continuity with the n-electrode 1504. Then, defect-free devices 110 can be selected and screened through an aging test (life test).

[0181] In one embodiment, it is preferred that the test apparatus 2001 comprises a box or other container so that the aging test can be performed in the device 110 sealed in a dry gas or nitrogen atmosphere. In addition, the heating stage 2004 can be used to maintain the temperature of the device 110 during the screening test, such as 60 degrees, 80 degrees, etc. The photodetector 2005 can be used to measure the optical output power 2006, which identifies a non-defective device 110 with a constant output power, or identifies a defective device 110.

[0182] In particular, in the case of the III-nitride laser diode device 110, it is known that the laser diode 110 deteriorates when it is oscillated in a humidity-containing atmosphere. This degradation is caused by humidity and siloxane in the gas, so it is necessary to seal the III-nitride laser diode device 110 in a dry gas during the aging test.

[0183] Therefore, if Fig.21 As shown, when the III-nitride laser diode device 2100 is purchased from a manufacturer, the chip 2101 itself (i.e., the device 110) is mounted on a stem 2102 and sealed in a dry gas using a TO-CAN package 2103, wherein the package 2103 includes a window 2104 for light emission.

[0184] Generally, screening or burn-in testing is performed before shipping in order to screen out defective devices 110. For example, screening conditions are performed according to the specifications of the laser diode device 110, such as high temperature and high power.

[0185] Furthermore, the burn-in test can be performed with the device 110 mounted on / into the package 2100, and the package 2100 is sealed in dry air and / or dry nitrogen before screening. This fact limits the flexibility of packaging and mounting of the laser device.

[0186] In the prior art, if defective production occurs, the defective product is discarded with the entire TO-CAN package 2100, which is a huge loss for production. This makes it difficult to reduce the production cost of the laser diode device 110. It is necessary to detect the defective device 110 in an earlier step.

[0187] In the present invention, using a heat sink 1505 to coat the facet 904 of the device 110 (on which multiple devices 110 can be mounted in a low-level position) and then using grooves 1507 to divide the heat sink 1505 and the device 110 after the coating process allows the device 110 as a sub-mount with the heat sink 1505 to be inspected in a screening test in a dry air or nitrogen atmosphere.

[0188] When the screening test is performed, the device 110 already has two contacts, namely, the p-electrode 808 and the solder 1506 on the heat sink 1505, or in the case of flip chip bonding, the n-electrode 1504 and the solder 1506 on the heat sink 1505. In addition, when the device 110 only includes the device 110 and the heat sink 1505, the present invention can use the screening test to select defective products. Therefore, in the case of discarding defective products, the present invention can reduce more losses than the prior art, which is of great value.

[0189] In the case of screening high-power laser diode devices 110, it may be preferred that the heat sink 1505 has two parts of solder 1506 that are arranged without electrical continuity. One part of the solder 1506 is connected to the p-electrode 808 through a lead (not shown), and the other part of the solder 1506 is connected to the n-electrode 1504 through a lead (not shown). In addition, it may be preferred to connect the p-electrode 808 and the n-electrode 1504 to the solder part 1506 through two or more leads, for example, as shown in FIG. 18(c), which shows the p-electrode 808 connected to the solder 1506 through two or more leads. In this way, the probe 1803 used to apply current to the device 110 can avoid directly contacting the p-electrode 808 (or the n-electrode 1504), which is critical in the case of screening high-power laser diode devices 110. Specifically, the probe 1803 may damage the contacted part, especially in the case of applying a high current density.

[0190] Step 13: Mounting the Device on / Into the Package

[0191] like Fig. 22 As shown, the device 110 (including the heat sink 1505) can be mounted in the package 2201 using solder or another metal to bond the device 110 at the bottom of the package 2201. The pins 2202 of the package 2201 are connected to the device 110 through the wires 2203. By doing so, a current from an external power source can be applied to the device 110.

[0192] This is more preferable than using metals such as Au-Au, Au-In, etc. for bonding between the package body 2201 and the heat sink 1505. This method requires flatness at the surface of the package body 2201 and at the back of the heat sink 1505. However, without solder, this configuration achieves high thermal conductivity and low temperature bonding, which is a great advantage for device processing.

[0193] Thereafter, a cover 2204 may surround the package 2201. In addition, a phosphor 2205 may be provided outside and / or inside the package 2201, wherein a window 2206 allows light to be emitted out of the package 2201. By doing so, the package 2201 may be used as a light bulb or headlight of a car.

[0194] As presented herein, these processes provide an improved method for obtaining laser diode devices 110. In addition, once the device 110 is removed from the substrate 101, the substrate 101 can be recycled multiple times. This achieves the goals of environmentally friendly production and low-cost modules. These devices 110 can be used as lighting devices such as light bulbs, data storage equipment, optical communication equipment such as Li-Fi, etc.

[0195] It is difficult to package a plurality of different types of laser devices 110 in one package 2201. However, since the aging test can be performed without packaging, this method can overcome this problem. Therefore, it is easy to mount different types of devices 110 in one package 2201.

[0196] Manufacturing LED devices

[0197] Although the above description relates to manufacturing the laser diode device 110, the same method can also be used to manufacture the LED device 110 until step 3. Specifically, the method can manufacture two types of LEDs: a type 1 LED having two electrodes (both a p-electrode and an n-electrode) on one side of the chip, or a type 2 LED having electrodes on both sides of the chip.

[0198] In the case of a type 1 LED, a p-electrode and an n-electrode are formed on the top surface of the device in step 3. Then, the method is the same from step 4 to step 9. Steps 10-11 are omitted, but steps 12-13 may be performed.

[0199] In the case of the type 2 LED, almost the same method as the type 1 LED is used except that an ITO electrode is formed on the p-GaN contact layer.

[0200] Definition of terms

[0201] III-Nitride-Based Substrates

[0202] As long as the III-nitride based substrate 101 can grow the III-nitride semiconductor layers 105 , 106 , 109 through the growth confinement mask 102 , any GaN substrate 101 sliced ​​on the {1-100} plane or other planes and from bulk GaN and AlN crystals can be used.

[0203] Heterogeneous Substrate

[0204] In addition, the present invention can use a foreign substrate 101 on which a III-nitride semiconductor template is deposited, wherein the foreign substrate 101 is a foreign substrate 101 such as sapphire, Si, GaAs, SiC, etc., and the template is GaN or other III-nitride semiconductor. Typically, the template is grown to a thickness of about 2-6 μm, and then a growth limiting mask 102 is set on the template.

[0205] Growth restriction mask

[0206] The growth restriction mask 102 typically includes a dielectric layer such as SiO2, SiN, SiON, Al2O3, AlN, AlON, MgF, ZrO2, etc., or a refractory metal or noble metal such as W, Mo, Ta, Nb, Rh, Ir, Ru, Os, Pt, etc. The growth restriction mask 102 may be a stacked structure selected from the above materials. A plurality of stacked layer structures selected from the above materials may also be used.

[0207] In one embodiment, the thickness of the growth limiting mask 102 is about 0.05-3 μm. The width of the mask is preferably greater than 20 μm, and more preferably, the width is greater than 40 μm.

[0208] The growth limit mask 102 may be deposited by sputtering or electron beam evaporation or PECVD (Plasma Enhanced Chemical Vapor Deposition), ion beam deposition (IBD); but not limited to these methods.

[0209] As shown in Fig. 13(a) and Fig. 13(b), the growth limiting mask 102 includes a plurality of stripe-shaped opening regions 103, which are periodically arranged at intervals p1 and p2 extending in the second direction in a first direction parallel to the 11-20 direction of the III-nitride semiconductor substrate 101 oriented in the (1-100) plane and in a second direction parallel to the 0001 direction of the III-nitride semiconductor substrate 101. The length a of the opening region 103 is, for example, 200 to 35000 μm; the width b is, for example, 2 to 180 μm; the interval p1 of the opening region 102 is, for example, 20 to 180 μm, and the interval p2 is, for example, 200 to 35000 μm; the width of the mask portion is 60 μm; and the distance between the opening regions 103 and the opening regions 103 in the 1-100 direction is 100 μm.

[0210] Another version of the growth restriction mask 102 is shown in Figures 23(a) and 23(b). The growth restriction mask 102 also includes a plurality of stripe-shaped opening regions 103, each stripe-shaped opening region being used to form strips 901 of devices 110, wherein the devices are separated laterally by no-growth regions and the strips 901 are separated longitudinally by dividing support regions 902.

[0211] III-nitride based semiconductor layers

[0212] The ELO III-nitride layer 105 , the III-nitride semiconductor device layer 106 , and the island III-nitride semiconductor layer 110 are typically GaN layers, but may include In, Al, and / or B as well as other impurities such as Mg, Si, Zn, O, C, H, and the like.

[0213] The III-nitride semiconductor device layer 106 generally includes more than two layers, including at least one of an n-type layer, an undoped layer, and a p-type layer. The III-nitride semiconductor device layer 106 specifically includes a GaN layer, an AlGaN layer, an AlGaInN layer, an InGaN layer, and the like.

[0214] In the case where the device 110 has a plurality of Group III nitride semiconductor layers 105 , 106 , 109 , the distance between island-shaped Group III nitride-based semiconductor layers 109 adjacent to each other is generally 30 μm or less, preferably 10 μm or less, but is not limited to these numbers.

[0215] Epitaxial lateral overgrowth

[0216] The crystallinity of the ELO III-nitride layer 105 laterally grown on the growth limiting mask 102 from the stripe-shaped opening region 103 of the growth limiting mask 102 is very high, and the III-nitride-based semiconductor layers 105, 106, 109 made of high-quality semiconductor crystals can be obtained.

[0217] In addition, two advantages can be obtained by using ELO with a III-nitride substrate 101. One advantage is that high-quality III-nitride semiconductor layers 105, 106, 109, such as having a very low defect density, can be obtained compared to using a sapphire substrate 101. Another advantage is that by using similar or identical materials for both the epitaxial layers 105, 106, 109 and the substrate 101, strain in the epitaxial layers 105, 106, 109 can be reduced. Moreover, due to similar or identical thermal expansion, this method can reduce the amount of bending of the substrate 101 during epitaxial growth. As described above, the effect is that the production yield can be very high in order to improve the uniformity of temperature.

[0218] On the other hand, a heterogeneous substrate 101 such as sapphire (m-plane, c-plane), LiAlO, SiC, Si, etc. can be used together with the III-nitride template layer. The advantage of using a heterogeneous substrate 101 such as sapphire, Si, etc. is low cost, which is important for mass production. In addition, since the bonding strength at the shear point is weak, it is easy to remove the heterogeneous structure 101.

[0219] When a plurality of island-shaped III-nitride semiconductor layers 109 are grown and separated from one another (i.e., formed in isolation), the tensile stress or compressive stress is confined to the island-shaped III-nitride semiconductor layers 109, and the effect of the tensile stress or compressive stress does not affect other III-nitride semiconductor layers.

[0220] Furthermore, since the growth limiting mask 102 and the ELO group III nitride layer 105 are not chemically bonded, stress in the ELO group III nitride layer 105 may be relaxed by sliding caused at the interface between the growth limiting mask 102 and the ELO group III nitride layer 105 .

[0221] Moreover, there are gaps between the island-shaped III-nitride semiconductor layers 109 as the no-growth regions 104, resulting in the substrate 101 having rows of island-shaped III-nitride semiconductor layers 109, which are flexible and thus easily deformed and can be bent when an external force is applied. Therefore, even if a slight warp, bend, or deformation occurs in the substrate 101, this can be easily corrected by a small external force, thereby avoiding the occurrence of cracks. Therefore, the substrate 101 can be handled by a vacuum chuck, which makes the manufacturing process of the semiconductor device 110 easier to implement.

[0222] In addition, an island-shaped III-nitride semiconductor layer 109 made of high-quality semiconductor crystals can be grown by suppressing the bending of the substrate 101. Furthermore, even when the III-nitride semiconductor layers 105, 106, 109 are very thick, the occurrence of cracks, etc. can be suppressed, so that a large-area semiconductor device 110 can be easily realized.

[0223] Flat surface area

[0224] The flat surface regions 107 are between the curved regions 108. Furthermore, the flat surface regions 107 are on the growth limiting mask 102.

[0225] The manufacturing of semiconductor device 110 is mainly performed on flat surface area 107. The width of flat surface area 107 is preferably at least 5 μm, and more preferably 10 μm or more. Flat surface area 107 has high uniformity of thickness of each semiconductor layer 105, 106, 109 in flat surface area 107.

[0226] No growth area

[0227] No-growth region 104 defines the distance between island-shaped Group III nitride-based semiconductor layers 109 adjacent to each other, and is typically 20 μm or less, and preferably 5 μm or less, but is not limited to these values.

[0228] Layer bending area

[0229] 24(a) and 24(b) show the layer bending region 108. If a non-polar or semi-polar substrate 101 is used, there may be a first facet 2401 in the flat surface region 107 (which is the main region for forming the ridge structure), a second facet 2402 in the layer bending region 108, and possibly a third facet 2403.

[0230] If the layer bending region 108 including the active layer 106b remains in the LED device 110, a portion of light emitted from the active layer 106b is reabsorbed. Therefore, at least a portion of the active layer 106b in the layer bending region 108 is preferably removed by etching.

[0231] If the layer bending region 108 including the active layer 106b remains in the laser diode device 110, the laser mode may be affected by the layer bending region 108 due to the low refractive index (eg, InGaN layer). Therefore, at least a portion of the active layer 106b in the layer bending region 108 is preferably removed by etching.

[0232] Two etches can be performed to remove the active layer 106b, wherein a first etch is performed to remove the active layer 106b in the region of the second facet 2402 before removing the epi layers 105, 106, 109 from the substrate 101, and a second etch is performed to remove the active layer 106b in the region of the third facet 2403 after removing the epi layers 105, 106, 109 from the substrate 101.

[0233] The emission region formed by the active layer 106b is a current injection region. In the case of the laser diode device 110, the emission region is a ridge structure. In the case of an LED, the emission region is a region for forming a p-contact electrode.

[0234] For both LDs and LEDs, the edge of the emission region should be at least 1 μm or more from the edge of the layer bending region 108, and more preferably 5 μm.

[0235] From another perspective, the defect density of the epitaxial layer of the flat surface region 107 except the opening region 103 is smaller than that of the epitaxial layer of the opening region 103. Therefore, it is more preferred that the ridge stripe structure should be formed in the flat surface region 107 included on the wing region.

[0236] Devices

[0237] Device 110 may include, for example, Schottky diodes, light emitting diodes, semiconductor lasers, photodiodes, transistors, etc., but is not limited to these devices. The present invention is particularly useful for micro-LEDs and laser diodes, such as edge-emitting lasers and vertical cavity surface-emitting lasers (VCSELs), especially semiconductor lasers that require shear facets.

[0238] Polymer film

[0239] The polymer film 1101 is used to remove the island-shaped III-nitride semiconductor layer 109 from the III-nitride-based substrate 101 or the GaN template used with the heterogeneous substrate 101. In the present invention, a dicing tape including a commercially available UV-sensitive dicing tape can be used as the polymer film 1101. For example, the structure of the polymer film 1101 may include three layers 1102, 1103, 1104 or double layers 1103, 1104, as shown in Figures 25(a) and 25(b), respectively, but not limited to those examples. For example, the base film 1102 material having a thickness of about 80 μm can be made of polyvinyl chloride (PVC). For example, the back film 1103 material having a thickness of about 38 μm can be made of polyethylene terephthalate (PET). For example, the adhesive layer 1104 having a thickness of about 15 μm can be made of an acrylic UV-sensitive adhesive.

[0240] When the polymer film 1101 is a UV-sensitive dicing tape and is exposed to UV light, the viscosity of the film 1101 is drastically reduced. After the island-shaped Group III nitride semiconductor layer 109 is removed from the substrate 101, the polymer film 1101 is exposed by UV light, which makes it easy to remove.

[0241] Heat sink

[0242] The heat sink 1505 is preferably made of AlN, SiC, Si, Cu, CuW, or the like, and the solder is preferably Au—Sn, Su—Ag—Cu, Ag paste, or the like.

[0243] Different embodiments

[0244] Various embodiments for fabricating the III-nitride device 110 are described below.

[0245] First embodiment

[0246] In the first embodiment, the substrate 101 used is an m-plane III-nitride substrate 101 without mis-cut orientation. As shown in FIG7(a) and FIG7(b) (0°), the ELO III-nitride layer 105 is uniform and has a very smooth surface.

[0247] The ELO layer was measured by PL measurement. As shown in FIG3(b), it can be seen that the pyramidal hillock 111 is almost completely contained in the opening region 103.

[0248] Then, as shown in Figure 4(a) and Figure 12, use Figure 11(a)-11(e) The method shown removes the island-shaped group III nitride semiconductor layer 109 .

[0249] After removal, PL and DIC images of FIG. 12( a) and FIG. 12( b) are made of the ELO III-nitride layer 105. As shown in FIG. 12( a) and FIG. 12( b), the ELO III-nitride layer after removal contains pyramidal hillocks 111, and its back surface is not affected by the pyramidal hillocks 111. By doing so, the ELO III-nitride layer 105 and the device 110 are not affected by the pyramidal hillocks 111. The ability to embed the pyramidal hillocks 111 in the epi layer 105 provides an important new method for obtaining a smooth surface of the epi layer 105.

[0250] Then, the island-shaped III-nitride semiconductor layer 109 is divided into devices 110. FIG26(a) and FIG26(b) show facets 904 of the island-shaped III-nitride semiconductor layer 109 after shearing, wherein the obtained facets 904 are atomically smooth.

[0251] The island-shaped semiconductor layer 109 can be processed by the above method (ie, steps 1 to 13). By doing so, the laser diode device 110 can be obtained.

[0252] Second embodiment

[0253] In the second embodiment, if Figure 27(a)-Figure 27(g) As shown, ELO structures are obtained. These structures are suitable for LED devices 110.

[0254] In the Type 2 design, as shown in FIG. 27( a), the growth limiting mask 102 has several sub-masks 2701. The length and width dimensions of each sub-mask 2701 vary from 30 μm to 300 μm. In each sub-mask 2701, the growth limiting mask 102 has an opening region 103 with a width of 3 μm to 7 μm and a spacing of 7 μm to 3 μm. The ELO III-nitride layer 105 grown in each sub-mask 2701 is coalesced, and care is taken to prevent coalescence between adjacent sub-masks 2701.

[0255] In the Type 3 design, as shown in FIG. 27( b ), the growth restriction mask 102 has opening regions 103 with a width of 3 μm to 7 μm at intervals of 7 μm to 3 μm, which are patterned throughout the growth restriction mask 102 , wherein the growth restriction mask 102 stripes are perpendicular to the <11-20> axis for semi-polar and non-polar III-nitride-based substrates 101 , and are along the non-polar direction for C-plane III-nitride-based substrates 101 .

[0256] As shown in Fig. 27(b), the ELO III-nitride layer 105 grown from the opening region 103 in the growth limiting mask 102 is agglomerated on top of the growth limiting mask 102 covering the entire surface. Then, by etching in the region 2703, the ELO III-nitride layer 105 is divided into sub-masks 2701 blocks 2702 as shown in Fig. 27(c). The sub-masks 2701 blocks 2702 are enlarged in Fig. 27(d).

[0257] A cross-sectional side view of the resulting structure including the substrate 101, the growth limiting mask 102, the opening region 103, and the island-shaped III-nitride semiconductor layer 109 is shown in FIG27(e). As shown in FIG27(f), a ridge process may be performed to form an LD device 110, which may include a cladding layer 806, a current limiting layer 807, and a p-electrode 808. Otherwise, as shown in FIG27(g), a ridge process is not required to form the LED device 110, and the cladding layer 806 and the p-electrode 808 are deposited.

[0258] In this case, if Fig.28 As shown, a smooth surface can be obtained. The present invention also embeds a pyramidal hillock 111.

[0259] Third embodiment

[0260] The third embodiment is almost the same as the first embodiment except that the ELO Group III nitride layer 105 is not removed.

[0261] The process of this embodiment is the same as step 1 to step 5 as described above. After step 5, the back side of substrate 101 opposite to ELO III group nitride layer 105 is polished until the thickness of substrate 101 is less than 120 μm. Then, n-electrode 1504 is provided on the back side of substrate 101, wherein the back side of substrate 101 is laser scribed to divide it into strips 901. Substrate 101 is divided into strips 901 by a conventional breaking method, wherein strips 901 are coated as shown in step 10, and then strips 901 are broken into devices 110. Next, device 110 is mounted on heat sink 1505. Finally, device 110 is mounted on stem 2102, as shown in FIG. Fig.21 shown.

[0262] In this case, the pyramidal hillocks 111 may also be embedded in the ELO III-nitride layer 105 .

[0263] Process Steps

[0264] Fig.29 1 is a flow chart illustrating a method for manufacturing a III-nitride semiconductor device 110, wherein an island-shaped III-nitride semiconductor layer 109 is grown on a substrate 101 using a growth limiting mask 102 and epitaxial lateral overgrowth, and the epitaxial lateral overgrowth is stopped before the island-shaped III-nitride semiconductor layer 109 is coalesced.

[0265] Block 2901 represents the step of providing a base substrate 101. In one embodiment, the base substrate 101 is a III-nitride based substrate 101, such as a GaN based substrate 101, or a foreign substrate or a foreign substrate 201.

[0266] Block 2902 represents an optional step of depositing an intermediate layer or template layer on the substrate 101. In one embodiment, the template layer is a Group III-nitride based layer, such as a GaN based layer.

[0267] Block 2903 represents the step of forming a growth restriction mask 102 on or above the substrate 101, ie, on the substrate 101 itself or on a template layer. The growth restriction mask 102 is patterned to include a plurality of open regions 103 in a stripe shape.

[0268] Block 2904 represents the step of growing one or more III-nitride based layers 105 on or over the growth limit mask 102 using epitaxial lateral overgrowth, wherein the epitaxial lateral overgrowth of the III-nitride layers 105 extends in a direction parallel to the opening regions 103 of the growth limit mask 102, and the epitaxial lateral overgrowth stops before the III-nitride layers 105 coalesce on the growth limit mask 102. In one embodiment, the ELO III-nitride layers 105 are ELOGaN based layers 105.

[0269] Block 2905 represents the step of growing one or more additional III-nitride semiconductor device layers 106 on the ELO III-nitride layer 105. These additional III-nitride semiconductor device layers 106 together with the ELO III-nitride layer 105 form one or more island-shaped III-nitride semiconductor layers 109, which may be shaped as strips 901.

[0270] Block 2906 represents a step of manufacturing a device 110 from an island-shaped III-nitride semiconductor layer 109 on the flat surface region 107 by a conventional method, wherein a ridge structure, a p-electrode, a p-pad, etc. are disposed at a predetermined position on the island-shaped III-nitride semiconductor layer 109, and the device 110 may include a laser diode device 110 or a light emitting diode device 110. This step may also include forming a support structure for shearing at a side facet of the device 110.

[0271] Block 2907 represents the steps of applying polymer / adhesive film 1101 to strip 901 of device 110, applying pressure to film 1101 from one or more sides, changing the temperature of film 1101, and / or peeling film 1101 with device 110 from substrate 101 after applying pressure and / or changing temperature, wherein after peeling, at least a portion of island-shaped III-nitride semiconductor layer 109 may remain with substrate 101. This step may also include dissolving growth limiting mask 102 by wet etching.

[0272] Block 2908 represents the step of cutting the strip 901 into one or more devices 110 or chips.

[0273] Block 2909 represents the steps of mounting the device 110 onto the heat sink 1505, mounting the heat sink 1505 onto the spacer plate 1701, storing the spacer plate in the coating holder 1702, and then coating the facets 904 of the laser device 110 using the coating holder 1702. This step may also include dividing the spacer plate 1701 into individual devices 110.

[0274] Block 2910 represents the steps of screening the devices 110 and then mounting the devices 110 on / into a package.

[0275] The resulting products of the method include one or more III-nitride based semiconductor devices 110 fabricated according to the method, and a substrate 101 that has been removed from the device 110 and is available for recycling and reuse, as described and illustrated herein.

[0276] Naming conventions

[0277] As used herein, the term "Group III nitride" or "Group III nitride" or "nitride" refers to a group III nitride having a chemical formula B w Al x Ga y In zAny compound or material related to a (B, Al, Ga, In)N semiconductor of N, where 0≤w≤1, 0≤x≤1, 0≤y≤1, 0≤z≤1, and w+x+y+z=1. As used herein, these terms are intended to be broadly interpreted to include the corresponding nitrides of the single species B, Al, Ga and In, as well as binary, ternary and quaternary compounds of such Group III metal species. Thus, these terms include, but are not limited to, compounds of AlN, GaN, InN, AlGaN, AlInN, InGaN and AlGaInN. When two or more (B, Al, Ga, In)N components are present, all possible compounds, including stoichiometric and non-stoichiometric ratios (relative molar fractions of each (B, Al, Ga, In)N component species present in the compound), can be employed within the broad scope of the present invention. In addition, compounds and materials within the scope of the present invention may also include a certain amount of dopants and / or other impurity materials and / or other inclusion materials.

[0278] The invention also covers the selection of specific crystal orientations, directions, terminations and polarities of group III nitrides. When Miller indices are used to identify crystal orientations, directions, terminations and polarities, the use of curly brackets {} indicates a set of symmetric equivalent planes represented by parentheses (). The use of brackets [] indicates a direction, while the use of brackets <> indicates a set of symmetric equivalent directions.

[0279] Many III-nitride devices are grown in a polar orientation, i.e. the c-plane {0001} of the crystal, but this leads to the undesirable quantum confined Stark effect (QCSE) due to the presence of strong piezoelectric polarization and spontaneous polarization. One way to reduce polarization effects in III-nitride devices is to grow the devices in a non-polar or semi-polar orientation of the crystal.

[0280] The term "non-polar" includes {11-20} planes (collectively referred to as a planes) and {10-10} planes (collectively referred to as m planes). Such planes contain equal numbers of Group III atoms and nitrogen atoms in each plane and are charge neutral. Subsequent non-polar layers are equivalent to each other, so the bulk crystal will not be polarized along the growth direction.

[0281] The term "semipolar" may be used to refer to any plane that cannot be classified as a c-plane, an a-plane, or an m-plane. In crystallographic terms, a semipolar plane is any plane with at least two non-zero h, i, or k Miller indices and a non-zero l Miller index. Subsequent semipolar layers are equivalent to each other, so the crystal will have a decreasing polarization along the growth direction.

[0282] in conclusion

[0283] This results in a description of a preferred embodiment of the present invention. The foregoing details of one or more embodiments of the present invention have been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the present invention to the precise form disclosed. In view of the above teachings, many modifications and variations may be made. The scope of the present invention is intended to be limited not by this specific description but by the appended claims.

Claims

1. A method for manufacturing a semiconductor device, comprising: A device comprising a plurality of Group III nitride semiconductor layers is manufactured, wherein: growing at least one of the plurality of Group III nitride semiconductor layers from an opening region in the growth limit mask on or over the substrate and atop the growth limit mask using epitaxial lateral overgrowth, At least one of the plurality of Group III nitride semiconductor layers includes at least one pyramidal hillock embedded therein, forming the pyramidal hillock in the opening region of the growth limit mask during epitaxial lateral overgrowth of at least one of the plurality of Group III nitride semiconductor layers, The epitaxial lateral overgrowth is performed until at least one of the plurality of Group III nitride semiconductor layers is completely embedded in the pyramidal hillock to produce a smooth epitaxial layer surface, During the epitaxial lateral overgrowth, at least one of the plurality of Group III nitride semiconductor layers from adjacent opening regions does not coalesce atop the growth limit mask, At least one of the plurality of Group III nitride semiconductor layers has one or more flat surface regions and layer bending regions at its edge, and One or more Group III-nitride semiconductor device layers are grown on or over the planar surface region.

2. The method according to claim 1, wherein: The growth limiting mask limits the expansion of the pyramidal hillock in a lateral direction.

3. The method according to claim 1, wherein: The plurality of Group III nitride semiconductor layers are grown on or over a foreign substrate, and a Group III nitride template is deposited on or over the foreign substrate prior to the plurality of Group III nitride semiconductor layers.

4. The method according to claim 1, wherein: The plurality of Group III nitride semiconductor layers are removed from the Group III nitride substrate.

5. The method according to claim 4, wherein: The plurality of Group III nitride semiconductor layers are removed from the Group III nitride substrate by: applying a film to the Group III nitride semiconductor layer; applying pressure to the membrane; changing the temperature of the film and the substrate; as well as After applying pressure and changing the temperature, the film having the Group III nitride semiconductor layer is peeled off from the substrate.

6. A device manufactured by the method of claim 1.

7. A semiconductor device comprising: A plurality of Group III nitride semiconductor layers, wherein: growing at least one of the plurality of Group III nitride semiconductor layers from an opening region in the growth limit mask on or over the substrate and atop the growth limit mask using epitaxial lateral overgrowth, At least one of the plurality of Group III nitride semiconductor layers includes at least one pyramidal hillock embedded therein, forming the pyramidal hillocks in the opening regions of the growth limit mask during epitaxial lateral overgrowth of at least one of a plurality of III-nitride based semiconductor layers, The epitaxial lateral overgrowth is performed until at least one of the plurality of Group III nitride semiconductor layers is completely embedded in the pyramidal hillock to produce a smooth epitaxial layer surface, During the epitaxial lateral overgrowth, at least one of the plurality of Group III nitride semiconductor layers from adjacent opening regions does not coalesce atop the growth limit mask, At least one of the plurality of Group III nitride semiconductor layers has one or more flat surface regions and layer bending regions at its edge, and One or more Group III-nitride semiconductor device layers are grown on or over the planar surface region.

8. The device according to claim 7, wherein The growth limiting mask limits the expansion of the pyramidal hillock in a lateral direction.

9. The device according to claim 7, wherein The plurality of Group III nitride semiconductor layers are grown on or over a Group III nitride substrate.

10. The device according to claim 7, wherein The plurality of Group III nitride semiconductor layers are grown on or over a foreign substrate, and a Group III nitride template is deposited on or over the foreign substrate prior to the plurality of Group III nitride semiconductor layers.

11. The device according to claim 7, wherein The plurality of Group III nitride semiconductor layers are removed from the Group III nitride substrate.

12. A method of manufacturing the device according to claim 7.