Microstructure and method for producing microstructure

By forming a microporous structure with excellent straight tube properties in the titanium oxide anodized film, the blockage problem caused by the non-standard tube of titanium oxide microporous in the prior art is solved, and efficient material permeability in the sensor is achieved.

CN113396247BActive Publication Date: 2024-12-03FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202080012497.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-02-14
Filing Date
2020-01-09
Publication Date
2024-12-03
Estimated Expiration
2040-01-09

AI Technical Summary

Technical Problem

The existing titanium oxide microporous anodized films are prone to clogging when passing through due to the non-linear tube structure in chemical sensors or biosensors, and lack suitable microporous structures.

Method used

By forming a plurality of micropores with excellent straight tube properties in the thickness direction of the titanium or titanium alloy anodized film, the density ratio of the micropores on the surface and back is more than 80% and less than 120%, and the anodizing treatment and removal process are used to form a throughput through. Pore ​​structure, preferably cathode electrolysis, chemical conversion or ultrasonic treatment is used to remove the anodic oxide film.

Benefits of technology

It realizes reducing clogging when substances pass through in chemical sensors or biosensors, and improves the straight tube properties of micropores, making it suitable for high-sensitivity chemical or biosensor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113396247B_ABST
    Figure CN113396247B_ABST
Patent Text Reader

Abstract

The present invention provides a microstructure having micropores with excellent straightness and a method for manufacturing the microstructure. The microstructure is composed of an anodic oxide film of titanium or a titanium alloy. The microstructure has a plurality of micropores penetrating in the thickness direction of the anodic oxide film, and when the density of the micropores on the surface of the anodic oxide film is set to A and the density of the micropores on the back of the anodic oxide film is set to B, the ratio A / B of the density A of the micropores on the surface to the density B of the micropores on the back is 80% or more and 120% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a microstructure composed of an anodic oxide film of titanium or a titanium alloy and a method for manufacturing the microstructure, and in particular to a microstructure having straight micropores penetrating in the thickness direction of the anodic oxide film and a method for manufacturing the microstructure. Background Art

[0002] In recent years, microstructures having a plurality of through holes provided in a substrate have been utilized in various fields such as the field of nanotechnology, and various applications thereof are expected.

[0003] For example, when a microstructure is made of titanium oxide, titanium oxide has the characteristics of a semiconductor and can form a dummy micron microstructure by anodic oxidation. Therefore, a microstructure using titanium oxide can be expected to be used as a highly sensitive chemical sensor or biosensor in the field of metamaterials.

[0004] As a microstructure using titanium oxide, for example, Patent Document 1 describes nanotube-shaped titanium dioxide having an aspect ratio of 6 or more, which is obtained by anodic oxidation of titanium metal or an alloy containing titanium as a main component. The nanotube diameter is described as 5 to 500 nm.

[0005] In non-patent document 1, as a microstructure using titanium oxide, a microstructure composed of a plurality of TiO2 nanotubes is described. In non-patent document 1, it is described that a microstructure composed of a plurality of TiO2 nanotubes is manufactured by anodization. In addition, in non-patent document 1, it is described that a microstructure composed of a plurality of TiO2 nanotubes is used for a membrane, a photocatalyst, a solar cell, an electronic device, and the like.

[0006] Previous technical literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-263580

[0009] Non-patent literature

[0010] Non-patent literature 1: Angew. Chem. Int. Ed. 2011, 50, 2904-2939. Summary of the invention

[0011] Technical issues to be solved by the invention

[0012] As described in the above-mentioned Patent Document 1 and Non-Patent Document 1, it is well known that titanium oxide can form micropores by anodic oxidation. However, the micropores of titanium oxide are usually not straight tubes from the surface to the bottom surface. Therefore, when the titanium oxide anodic oxide film having micropores is used as a chemical sensor or a biosensor, when a substance, especially a liquid, is allowed to pass through and used, the non-straight micropores become the cause of clogging, etc. Therefore, the titanium oxide anodic oxide film having micropores in the past is not necessarily suitable for use in chemical sensors or biosensors.

[0013] An object of the present invention is to provide a microstructure having micropores with excellent straightness and a method for producing the microstructure.

[0014] Means for solving technical problems

[0015] In order to achieve the above-mentioned purpose, the first method of the present invention provides a microstructure, which is composed of an anodized film of titanium or titanium alloy, wherein the microstructure has a plurality of micropores penetrating in the thickness direction of the anodized film, and when the density of the micropores on the surface of the anodized film is set to A and the density of the micropores on the back side of the anodized film is set to B, the ratio A / B of the density A of the micropores on the surface to the density B of the micropores on the back side is greater than 80% and less than 120%.

[0016] The thickness of the anodized film is preferably 0.1 to 10 μm.

[0017] Preferably, the average diameter of the micropores is 17 to 200 nm.

[0018] A second embodiment of the present invention provides a method for manufacturing a microstructure, wherein the microstructure has a plurality of micropores penetrating in the thickness direction of an anodized film, and the manufacturing method has an anodized film forming step, in which an anodized treatment step of anodizing a substrate composed of titanium or a titanium alloy to form an anodized film and a removal step of removing the anodized film are sequentially performed at least once, and an anodized treatment step is performed after the removal step to form an anodized film having a plurality of micropores.

[0019] Preferably, after the anodized film forming step, there is a substrate removing step of removing the substrate present at the bottom side of the micropores, and the micropores are penetrated in the thickness direction of the anodized film by the substrate removing step.

[0020] The removal step is preferably a step of removing the anodic oxide film by cathode electrolysis. Also, the removal step is preferably a step of removing the anodic oxide film by chemical conversion treatment. Also, the removal step is preferably a step of removing the anodic oxide film by ultrasonic treatment.

[0021] Effects of the Invention

[0022] According to the present invention, a microstructure having micropores with excellent straightness can be obtained. In addition, a microstructure having micropores with excellent straightness can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic plan view showing an example of a microstructure according to an embodiment of the present invention.

[0024] Figure 2 is along Figure 1 The microstructure is shown in a cross-sectional view taken along the cutting line IB-IB.

[0025] Figure 3 This is a schematic diagram for explaining a method of calculating the density of micropores in the microstructure according to the embodiment of the present invention.

[0026] Figure 4 This is a schematic diagram for explaining a method of calculating the density of micropores in the microstructure according to the embodiment of the present invention.

[0027] Figure 5 This is a schematic cross-sectional view showing one step of a method for producing a microstructure according to an embodiment of the present invention.

[0028] Figure 6 This is a schematic cross-sectional view showing one step of a method for producing a microstructure according to an embodiment of the present invention.

[0029] Figure 7 This is a schematic cross-sectional view showing one step of a method for producing a microstructure according to an embodiment of the present invention.

[0030] Figure 8 This is a schematic cross-sectional view showing one step of a method for producing a microstructure according to an embodiment of the present invention.

[0031] Fig. 9 This is a schematic cross-sectional view showing one step of a method for producing a microstructure according to an embodiment of the present invention. DETAILED DESCRIPTION

[0032] Hereinafter, the microstructure and the method for producing the microstructure of the present invention will be described in detail based on the preferred embodiments shown in the drawings.

[0033] In addition, the drawings described below are exemplary drawings for explaining the present invention, and the present invention is not limited to the drawings shown below.

[0034] In addition, the "to" indicating a numerical range below includes the numerical values ​​described on both sides. For example, c is a numerical value α1 to a numerical value β1, which means that the range of ε is a range including the numerical values ​​α1 and β1, and when expressed in mathematical notation, α1≤ε≤β1.

[0035] "Specific numerical values" include the error range generally allowed in the corresponding technical field unless otherwise specified. Also, "the same" includes the error range generally allowed in the corresponding technical field.

[0036] [Microstructure]

[0037] Figure 1 is a schematic plan view showing an example of a microstructure according to an embodiment of the present invention, Figure 2 It is a cross-sectional view taken along the cutting line IB-IB of the microstructure shown in FIG. 1 .

[0038] Figure 1 The microstructure 10 shown is composed of an anodized film 12 of titanium or a titanium alloy. The microstructure 10 has a plurality of micropores 14 penetrating in the thickness direction Dt of the anodized film 12. The anodized film 12 is provided with a plurality of micropores 14 penetrating in the thickness direction Dt.

[0039] In the microstructure 10, when the density of the micropores 14 on the surface 12a of the anodized film 12 is set to A and the density of the micropores 14 on the back side 12b of the anodized film 12 is set to B, the ratio A / B of the density A of the micropores on the surface of the anodized film 12 to the density B of the micropores on the back side of the anodized film 12 is greater than 80% and less than 120%.

[0040] In the present invention, the surface of the anodized film is defined as a surface without a substrate, and the back surface of the anodized film is defined as a surface with a substrate.

[0041] exist Figure 1 In the microstructure 10 shown, the titanium or titanium alloy anodized film 12 has a plurality of micropores 14 penetrating in the thickness direction Dt, and the above ratio is 80% or more, and the micropores 14 are through-holes with excellent straightness. Therefore, for example, when used as a chemical sensor or a biosensor, when a substance, especially a liquid, is allowed to pass through, since the micropores 14 are straight tubes, clogging caused by the micropores 14 can be suppressed, and it is suitable for use in chemical sensors or biosensors.

[0042] Hereinafter, the microstructure will be described in more detail.

[0043] 〔Ratio of density〕

[0044] Figure 3 and Figure 4This is a schematic diagram for explaining a method of calculating the density of micropores in the microstructure according to the embodiment of the present invention.

[0045] Using a scanning electron microscope, images of three viewing fields are obtained for the surface 12a and the back surface 12b of the anodized film 12. For example, Figure 3 The image of the surface 12a of the anodized film 12 is shown, and the Figure 4 An image of the back side 12b of the anodized film 12 is shown.

[0046] For the surface 12a and the back side 12b of the anodized film 12, the number of micropores is visually obtained for each field of view. The density of the micropores in each field of view is obtained based on the area of ​​each field of view. Furthermore, the average value of the density of the micropores in the three fields of view is obtained. The average value of the density of the micropores in the three fields of view of the surface 12a of the anodized film 12 is used as the density A of the micropores 14 on the surface 12a of the anodized film 12. The average value of the density of the micropores in the three fields of view of the back side 12b of the anodized film 12 is used as the density B of the micropores 14 on the back side 12b of the anodized film 12.

[0047] As described above, the ratio A / B of the density A of the micropores 14 on the surface 12a of the anodized film 12 to the density B of the micropores 14 on the back side 12b of the anodized film 12 is greater than 80% and less than 120%. That is, the ratio A / B is 80%≤A / B≤120%. If the ratio A / B is within the above range of 80% to 120%, it means that there are fewer cases where the micropores branch and the micropores are formed obliquely, and that the straightness of the micropores is high. In addition, the closer the ratio A / B is to 100%, the more straight micropores 14 there are, and the better the straightness. The ratio A / B is preferably 90%≤A / B≤110%, more preferably 95%≤A / B≤105%, and particularly preferably 98%≤A / B≤102%.

[0048] 〔Titanium or titanium alloy〕

[0049] The microstructure is composed of an anodic oxide film 12 of titanium or a titanium alloy. Therefore, titanium and titanium alloys are not particularly limited as long as they can be anodized. As titanium, for example, pure titanium specified in JIS (Japanes e Industrial Standards: Japanese Industrial Standards) H 4600: 2012 can be used. And as a titanium alloy, for example, α-β titanium alloy (Ti-6Al-4V) and β titanium alloy (Ti-15V-3Cr-3Sn-3Al) can be used.

[0050] The substrate composed of titanium or titanium alloy is not particularly limited, and may be various components such as titanium plate or titanium alloy plate, or titanium film or titanium alloy film. In addition, a structure in which a titanium film or titanium alloy film formed by evaporation or sputtering is formed on various supports such as silicon wafer, quartz, glass, etc. is also included in the above-mentioned substrate. Furthermore, a structure in which a titanium film or titanium alloy film is laminated on a resin substrate is also included in the substrate.

[0051] <Degreasing treatment>

[0052] The surface of the titanium or titanium alloy substrate on the side to be subjected to the anodizing treatment step is preferably subjected to a degreasing treatment in advance.

[0053] The degreasing treatment uses acids, alkalis, organic solvents, etc. to dissolve and remove organic components such as dust, grease, resin, etc. attached to the surface of the titanium or titanium alloy substrate. It is carried out for the purpose of preventing defects in the subsequent treatments caused by organic components.

[0054] The degreasing treatment can be performed using a conventionally known degreasing agent. Specifically, for example, the degreasing treatment can be performed using various commercially available degreasing agents using a predetermined method.

[0055] Among them, the following methods can be preferably exemplified.

[0056] A method of bringing an organic solvent such as alcohol (e.g., methanol), ketone, gasoline, volatile oil into contact with the surface of a substrate at room temperature (organic solvent method); a method of bringing a solution containing a surfactant such as soap or neutral detergent into contact with the surface of a substrate at a temperature between room temperature and 80°C, followed by washing with water (surfactant method); a method of bringing a sulfuric acid aqueous solution having a concentration of 10 to 200 g / L (liter) into contact with the surface of a substrate at a temperature between room temperature and 70°C for 30 to 80 seconds, followed by washing with water; a method of bringing a sodium hydroxide aqueous solution having a concentration of 5 to 20 g / L into contact with the surface of a substrate at room temperature for about 30 seconds, while using the surface of the substrate as a cathode and applying a current density of 1 to 10 A / dm 2 A method of electrolyzing by passing a direct current of 100 to 500 g / L of nitric acid aqueous solution for neutralization; "making various known anodizing electrolytes contact the surface of the substrate at room temperature, while using the surface of the substrate as a cathode and applying a current density of 1 to 10 A / dm 2A method of electrolysis by passing a direct current or an alternating current; a method of contacting an alkaline aqueous solution with a concentration of 10 to 200 g / L with the surface of the substrate at 40 to 50°C for 15 to 60 seconds, and then contacting with an aqueous nitric acid solution with a concentration of 100 to 500 g / L for neutralization; a method of contacting an emulsion prepared by mixing a surfactant, water, etc. in diesel, kerosene, etc. with the surface of the substrate at a temperature of room temperature to 50°C, and then washing with water (emulsification degreasing method); a method of contacting a mixed solution of sodium carbonate, phosphates, surfactants, etc. with the surface of the substrate at a temperature of room temperature to 50°C for 30 to 180 seconds, and then washing with water (phosphate method).

[0057] The degreasing treatment is preferably a method that can remove the fat components on the surface of the titanium or titanium alloy substrate and hardly dissolves the titanium or titanium alloy substrate. From this viewpoint, an organic solvent method, a surfactant method, an emulsification degreasing method, and a phosphate method are preferred.

[0058] 〔Thickness of anodic oxide film〕

[0059] If the thickness h of the anodized film 12 (reference Figure 2 ) becomes more than 0.1μm, the shape of the pores formed into micropores remains in a stable state. If it is less than 10μm, the reaction time is short, the surface is difficult to dissolve in the electrolyte, and the micropore shape is easy to maintain. For this reason, the thickness h of the anodized film 12 is preferably 0.1-10μm, and more preferably 0.2-5μm.

[0060] about Figure 2 The thickness h of the anodized film 12 shown is obtained by cutting the anodized film 12 and obtaining a photographic image of the cross section at a magnification of 200,000 times using a scanning electron microscope. In the photographic image of the anodized film 12, the contour shape of the anodized film 12 is obtained, and the area corresponding to the thickness h is measured at 10 points to obtain the measured value. The average value of the measured values ​​at the 10 points is calculated, and the average value is used as the thickness h of the anodized film 12.

[0061] 〔Average diameter of micropores〕

[0062] In view of the conditions for stably forming micropores, the average diameter d of the micropores 14 (refer to Figure 1 and Figure 2 ) is preferably 17 to 200 nm, more preferably 30 to 100 nm.

[0063] about Figure 1 and Figure 2The average diameter d of the micropores 14 shown is obtained by photographing the surface of the anodized film 12 from above at a magnification of 100 to 10,000 times using a scanning electron microscope. In the photographic image, at least 20 micropores connected in a ring shape are extracted, and their diameters are measured as the opening diameter, and their average value is calculated as the average diameter.

[0064] In addition, regarding the magnification, the magnification within the above range can be appropriately selected so as to obtain a photographic image capable of extracting more than 20 micropores. In addition, the opening diameter measures the maximum value of the distance between the ends of the micropore portion. That is, the shape of the opening of the micropore is not limited to a substantially circular shape, and therefore, when the shape of the opening is non-circular, the maximum value of the distance between the ends of the micropore portion is taken as the opening diameter. Therefore, for example, even in the case of a micropore in which two or more micropores are integrated, they are regarded as one micropore, and the maximum value of the distance between the ends of the micropore portion is taken as the opening diameter.

[0065] Next, a method for producing a microstructure will be described.

[0066] [Method for producing microstructure]

[0067] The method for manufacturing a microstructure is not particularly limited as long as it has an anodic oxidation treatment. For example, it is a method for manufacturing a microstructure having a plurality of micropores penetrating in the thickness direction of an anodic oxide film, which has an anodic oxide film forming step, in which an anodic oxidation treatment step of anodizing a substrate composed of a titanium plate or a titanium alloy plate to form an anodic oxide film and a removal step of removing the anodic oxide film are sequentially performed at least once, and an anodic oxidation treatment step is performed after the removal step to form an anodic oxide film having a plurality of micropores. In addition, after the anodic oxide film forming step, there is a substrate removal step of removing the substrate present at the bottom side of the micropores, and the micropores are penetrated in the thickness direction of the anodic oxide film by the substrate removal step.

[0068] Hereinafter, a method for producing a microstructure will be described using the drawings.

[0069] Figures 5 to 9 Schematic cross-sectional views showing a method for manufacturing a microstructure according to an embodiment of the present invention in order of steps.

[0070] The method for producing the microstructure described below is Figure 1 and Figure 2 An example of a method for manufacturing the microstructure 10 shown in FIG. Figures 5 to 9 In, with Figure 1 and Figure 2 The same components of the microstructure 10 shown are denoted by the same reference numerals, and detailed description thereof will be omitted.

[0071] In the method for manufacturing a microstructure, first, Figure 5 As shown, a substrate 20 composed of a titanium plate or a titanium alloy plate is prepared.

[0072] The substrate 20 may be selected according to the final microstructure 10 (see Fig. 9 The size and thickness are appropriately determined by the thickness of the anodized film 12 of the substrate 20, the processing device, etc. The substrate 20 is, for example, a rectangular plate.

[0073] Next, the surface 20a (reference Figure 5 ) is anodized. Thus, the surface 20a (reference Figure 5 ) is anodized, such as Figure 6 As shown, an anodic oxide film 22 is formed having a plurality of micropores 14 extending in the thickness direction Dt of the substrate 20 and a barrier layer 25 present at the bottom of the plurality of micropores 14. The step of forming the anodic oxide film 22 by anodizing as described above is called an anodizing treatment step.

[0074] Then, if Figure 7 As shown, the substrate 20 is removed Figure 6 The step of removing the anodic oxide film 22 from the substrate 20 is referred to as a removal step.

[0075] Next, the substrate 20 is subjected to anodizing treatment again. Figure 8 As shown in FIG. 1 , an anodized film 12 having a plurality of micropores 14 extending in the thickness direction Dt is formed. Figure 8 The substrate 20 is present on the bottom side of the micropores 14 in the anodized film 12 shown.

[0076] As described above, at least one anodizing step for forming the anodized film 12, anodizing the substrate 20 to form the anodized film 22, and a removal step for removing the anodized film 22 are sequentially performed, and the anodizing step is performed after the removal step, which is the anodized film forming step. The anodizing step and the removal step are not limited to one time, and can also be performed multiple times, but the anodizing step is performed after the removal step.

[0077] After the anodic oxide film forming step, Figure 8 In the anodized film 12 having a plurality of micropores 14 shown in FIG. 1 , the substrate 20 existing at the bottom side of the micropores 14 is removed so that the micropores 14 penetrate in the thickness direction Dt of the anodized film 12. That is, the barrier layer 25 existing at the bottom of the micropores 14 is included. Figure 8The substrate 20 on the opposite side of the surface 12 a of the anodized film 12 having the plurality of micropores 14 is removed so that the micropores 14 penetrate the anodized film 12 in the thickness direction Dt, thereby making the micropores 14 through-holes.

[0078] Therefore, if Fig. 9 As shown, an anodic oxide film 12 of a titanium plate or a titanium alloy plate having a plurality of penetrating micropores 14 is formed to obtain a microstructure 10. The micropores 14 have a ratio of 80%.

[0079] In addition, the process of removing the substrate 20 present at the bottom side of the micropore 14 in order to make the micropore 14 into a through hole is called a substrate removal process. The substrate removal process is a process of removing the substrate 20 including the barrier layer 25 present at the bottom of the micropore 14 in order to make the micropore 14 into a through hole.

[0080] Furthermore, the step of penetrating the micropores 14 in the thickness direction Dt of the anodized film 12 is referred to as a penetration step.

[0081] Hereinafter, the method for producing the microstructure will be described in more detail.

[0082] <Anodizing treatment>

[0083] As the electrolyte solution (electrolyte) for anodizing, when titanium or titanium alloy is subjected to anodic polarization, it is necessary to be able to dissolve the dissolving power of titanium or titanium alloy, and the electrolyte solution preferably includes ions containing halogen atoms. The ions containing halogen atoms mentioned here refer to any ions of atoms containing fluorine, chlorine, bromine, and iodine, specifically, fluoride ion, chloride ion, bromide ion, iodide ion, chlorate ion, bromate ion, iodate ion, chlorite ion, bromite ion, hypochlorite ion, hypobromite ion, hypoiodite ion, etc. can be cited. These ions can be used alone or as a mixture of two or more.

[0084] As the electrolyte solution containing these ions, specifically, an aqueous solution of an acid or salt that forms these ions can be used. The concentration is preferably 0.001 to 50% by volume, more preferably 0.005 to 10% by volume, and further preferably 0.01 to 5% by volume, based on the acid or salt. In addition, as described above, the electrolyte solution containing ions containing halogen atoms used for anodizing treatment is called a halide aqueous solution.

[0085] As the electrolyte solution for anodizing treatment, an aqueous solution of ammonium fluoride is particularly preferred. In addition, an organic solvent can be used. As the organic solvent, an alcohol or glycol can be used. The amount of the organic solvent added is preferably 0 to 99.5%, more preferably 50 to 99%, and most preferably 80 to 99% relative to the amount of the electrolyte solution. In addition, ethylene glycol is particularly preferred as the organic solvent.

[0086] The anodic oxidation treatment is usually carried out at an applied voltage of 5 to 200 V, preferably 10 to 100 V, and a current density of 0.2 to 500 mA / cm 2 , preferably 0.5 to 100 mA / cm 2 The temperature is set to 1 minute to 24 hours, preferably 5 minutes to 10 hours.

[0087] Furthermore, the temperature of the electrolyte solution during the anodizing treatment is preferably 0 to 50°C, more preferably 0 to 40°C.

[0088] The electrolyte solution may contain a water-soluble titanium compound. The water-soluble titanium compound is usually hydrolyzed in an aqueous solution to generate titanium oxide. Therefore, by containing a water-soluble titanium compound, titanium oxide is further hydrolyzed on the surface of the titanium oxide generated by anodic oxidation, thereby preventing the titanium oxide from dissolving again in the electrolyte solution and increasing the aspect ratio of the titanium oxide.

[0089] As water-soluble titanium compounds, titanium alkoxides such as titanium isopropoxide, titanium trichloride, titanium tetrachloride, titanium fluoride, ammonium tetrafluorotitanate, titanium sulfate, titanyl sulfate, etc. can be cited, but are not limited to these. The concentration is preferably 0.001 to 1000, more preferably 0.01 to 50, and further preferably used in the range of 0.04 to 5 relative to the ion containing the halogen atom in terms of molar ratio.

[0090] Furthermore, the electrolyte solution may contain an acidic compound of a different type from the acid or salt that forms the ion containing the halogen atom. By containing the acidic compound, the reaction rate can be controlled, for example, the anodic oxidation rate can be accelerated or suppressed.

[0091] As such acidic compounds, in addition to the acid of the aforementioned halide or its oxide ion, sulfuric acid, nitric acid, acetic acid, hydrogen peroxide, oxalic acid, phosphoric acid, chromic acid, glycerophosphoric acid, etc. can be cited, but it is not limited to these. The concentration thereof is preferably used in the range of 0.001 to 1000, more preferably 0.01 to 50, and further preferably 0.04 to 5 in terms of molar ratio relative to the ion containing the halogen atom.

[0092] Furthermore, the electrolyte solution may contain titanium oxide fine particles. By containing titanium oxide fine particles, the generated titanium oxide can be prevented from being dissolved again in the electrolyte solution, and the aspect ratio of the titanium oxide can be increased.

[0093] As titanium oxide particles, titanium oxide particles with a particle size of 0.5 to 100 nm are preferred, and titanium oxide particles with a particle size of 2 to 30 nm are more preferred. Specifically, titanium oxide particles prepared from titanium ore by a liquid phase method, titanium oxide particles synthesized by a gas phase method, a sol-gel method, and a liquid phase deposition method can be cited. Here, the gas phase method refers to a method of producing titanium oxide by calcining the hydrous titanium oxide obtained by heating and hydrolyzing titanium ore with a strong acid such as sulfuric acid at 800°C to 850°C. The liquid phase method refers to a method of producing titanium oxide by contacting titanium chloride with oxygen and hydrogen. The sol-gel method refers to a method of producing titanium oxide by hydrolyzing titanium alkoxide in an alcohol aqueous solution to generate a sol, then adding a hydrolysis catalyst to the sol and leaving it to gel, and calcining the gelled product. The liquid phase deposition method refers to a method of obtaining titanium oxide by hydrolyzing titanium fluoride, ammonium tetrafluorotitanate, or titanyl sulfate.

[0094] <Anodic oxide film removal>

[0095] Anodic oxide film removal As long as the anodic oxide film can be removed, the removal method is not particularly limited. For example, chemical conversion treatment can be preferably used in the removal of the anodic oxide film, because the anodic oxide film can be uniformly removed. When the anodic oxide film is removed by chemical conversion treatment, the solution used is preferably a halide aqueous solution used in the above-mentioned electrolyte solution. The concentration of the halide aqueous solution is preferably 1 to 50% by mass. The temperature of the halide aqueous solution is preferably 25 to 60°C.

[0096] Furthermore, an aqueous solution of an inorganic acid such as sulfuric acid, phosphoric acid, nitric acid, chromium, or a mixture thereof (hereinafter referred to as an acid aqueous solution) can be used for the removal of the anodic oxide film. The concentration of the acid aqueous solution is preferably 1 to 50% by mass. The temperature of the acid aqueous solution is preferably 25 to 60°C.

[0097] In addition, an aqueous alkali solution can also be used, preferably an aqueous solution of at least one alkali selected from the group consisting of sodium hydroxide, potassium hydroxide and lithium hydroxide. The concentration of the aqueous alkali solution is preferably 0.1 to 40% by mass. The temperature of the aqueous alkali solution is preferably 20 to 35°C. Specifically, for example, 10 g / L of ammonium fluoride aqueous solution at 30°C, 50 g / L of sulfuric acid aqueous solution at 40°C, 0.5 g / L of sodium hydroxide aqueous solution at 30°C, or 35 g / L of sodium hydroxide aqueous solution at 30°C can be preferably used.

[0098] The immersion time in the halide aqueous solution, acid aqueous solution or alkali aqueous solution is preferably 3 to 120 minutes, more preferably 10 to 90 minutes, and even more preferably 15 to 60 minutes.

[0099] Ultrasonic treatment can be preferably used in the removal of the anodic oxide film, because the anodic oxide film can be removed uniformly and in a short time. In this case, a substrate ultrasonic device is used. Starting from immersing the substrate in the above-mentioned liquid, the ultrasonic application time in the ultrasonic treatment is preferably 1 to 60 minutes, more preferably 3 to 45 minutes, and further preferably 5 to 30 minutes.

[0100] Cathodic electrolysis can also be preferably used in the removal of the anodic oxide film, because the anodic oxide film can be removed uniformly and in a short time, and the substrate will not be dissolved. Cathodic electrolysis is a technology that utilizes the following phenomenon: when removing the anodic oxide film, if the substrate is fixed on the cathode and a voltage is applied, hydrogen is generated on the surface of the substrate, thereby causing the film to peel off. The voltage during the removal of the anodic oxide film is preferably 1 to 60V, more preferably 2 to 20V, and most preferably 3 to 10V.

[0101] <Base Material Removal>

[0102] After the anodized film is formed, the substrate removal existing at the bottom side of the micropores is not particularly limited, and various methods can be used. For example, by removing the substrate from the back side 20b Figure 8 The substrate 20 shown can be removed by grinding or polishing. In addition to removing the substrate 20 by physical action such as grinding or polishing, the substrate 20 can also be removed by dissolving, for example. For dissolving, for example, a dilute hydrofluoric acid aqueous solution can be used.

[0103] The present invention is basically configured as described above. Although the microstructure and the method for producing the microstructure of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various improvements or changes can be made without departing from the spirit of the present invention.

[0104] Example

[0105] Below, examples are given to further specifically describe the present invention. The materials, reagents, usage amounts, amounts of substances, ratios, processing contents, processing steps, etc. shown in the following examples can be appropriately changed as long as they do not depart from the purpose of the present invention. Therefore, the scope of the present invention should not be interpreted restrictively by the specific examples shown below.

[0106] In this example, the thickness of each microstructure of Examples 1 to 3 and Comparative Example 1 was measured, and the ratio of micropores was determined.

[0107] In addition, in this example, the straightness of the micropores was evaluated by using the permeability using a test liquid which will be described in detail later. The microstructures of Examples 1 to 3 and Comparative Example 1 were evaluated for permeability.

[0108] <Thickness of fine structure>

[0109] The microstructure was set to the average thickness of the titanium substrate.

[0110] <Ratio of Micropores>

[0111] The surface of the microstructure was photographed using FE-SEM (field emission scanning electron microscope) at a magnification of 50,000 times to obtain photographic images of three fields of view. The number of micropores was obtained per field of view. The average value of the three fields of view was used as the density A of the micropores on the surface to obtain the number of micropores per unit area on the surface.

[0112] For the back side of the microstructure, photographic images of three viewing fields were obtained in the same manner as for the surface of the microstructure. The number of micropores was calculated for each viewing field. The number of micropores per unit area on the back side was calculated using the average value of the three viewing fields as the density B of the micropores on the back side.

[0113] The ratio of the density A of the micropores on the surface to the density B of the micropores on the back surface was determined (A / B×100(%)).

[0114] <Permeability>

[0115] As described above, permeability is an index for evaluating the straightness of micropores. A test liquid, which will be described in detail later, is used for the evaluation of permeability.

[0116] For permeability, a test liquid was prepared in which titanium oxide particles (TT0-51: particle size 10 to 30 nm) manufactured by ISHIHARA SANGYO KAISHA, LTD. were dispersed in water as fine particles. A predetermined amount of the test liquid was dripped onto the microstructures of Examples 1 to 3 and Comparative Example 1, respectively. The ratio of the number of particles contained in the permeated test liquid to the number of particles contained in the test liquid was measured. The more particles contained in the permeated test liquid, the better the permeability.

[0117] The test liquid that passed through the microstructure was dried and the mass of the remaining particle components was measured. The mass of the remaining particle components was taken as the number of particles that passed through. The ratio of the mass of the particles added when making the test liquid to the mass of the remaining particle components was calculated. In addition, if the mass of the added particles is the same as the mass of the remaining particle components, the permeability is 100%.

[0118] Next, Examples 1 to 3 and Comparative Example 1 will be described.

[0119] (Example 1)

[0120] A titanium substrate (JIS H 4600, titanium purity: 99.5%) having an average thickness of 0.2 mm and a size of 25 mm×100 mm was used.

[0121] The titanium substrate was subjected to the following steps (a) to (d) to produce a microstructure.

[0122] (a) First Anodic Oxide Film Forming Step

[0123] An anodizing treatment was performed using an electrolyte solution (3.5% by volume of ammonium fluoride, 5% by volume of water, and 95% by volume of ethylene glycol) maintained at a temperature of 5°C, with the titanium substrate as the anode, thereby forming an anodic oxide film on the titanium substrate. In addition, an anodic oxidation treatment was performed using a DC power supply, with the applied voltage set to 60V and the applied time set to 30 minutes. After the anodic oxide film was formed, it was washed with water using a sprayer.

[0124] (b) Anodic oxide film removal process

[0125] After the first anodic oxide film forming step, the substrate was connected to a cathode in a sulfuric acid aqueous solution (1 mol / L) and a voltage of 4 V was applied for 4 minutes to remove the anodic oxide film. After the anodic oxide film was removed, it was washed with water using a sprayer and dried.

[0126] (c) Second Anodic Oxide Film Forming Step

[0127] The second anodic oxide film forming step was carried out in the same manner as the above-mentioned (a) first anodic oxide film forming step to form an anodic oxide film again. Thereafter, the anodic oxide film was washed with water using a sprayer and dried.

[0128] (d) Matrix removal

[0129] A photoresist method was used to form a square pattern with a side of 1 mm on the back of the titanium substrate on the side where the anodic oxide film was not formed, and a dilute hydrofluoric acid aqueous solution was used to dissolve the titanium substrate and the anodic oxide film in contact with the titanium substrate, so that the micropores formed in the anodic oxide film penetrated. Thus, a microstructure having penetrating micropores was produced.

[0130] (Example 2)

[0131] In Example 2, the steps are the same as those in Example 1 except for (b) the anodic oxide film removal step.

[0132] In Example 2, chemical conversion treatment was used in the (b) anodic oxide film removal step. In the (b) anodic oxide film removal step of Example 2, the titanium substrate was immersed in an anodic oxide film removal solution (ammonium fluoride 100 g / L aqueous solution) maintained at a temperature of 30° C. for 20 minutes to perform chemical conversion treatment.

[0133] (Example 3)

[0134] In Example 3, the process is the same as that of Example 1 except that (b) the anodic oxide film removal process is different from that of Example 1.

[0135] In Example 3, ultrasonic treatment was used in the (b) anodic oxide film removal step. In the (b) anodic oxide film removal step of Example 3, the titanium substrate was subjected to ultrasonic treatment for 5 minutes using a BRANSON 3210 tabletop ultrasonic cleaner manufactured by YAMATOSCIENTIFIC CO., LTD.

[0136] (Comparative Example 1)

[0137] In Comparative Example 1, a microstructure was produced by performing (d) a substrate removal step after (a) a first anodic oxide film forming step, as compared to Example 1. In Comparative Example 1, the steps of (b) an anodic oxide film removal step and (c) a second anodic oxide film forming step were not performed.

[0138] [Table 1]

[0139]

[0140] As shown in Table 1, the permeability of Examples 1 to 3 is much better than that of Comparative Example 1. That is, Examples 1 to 3 are microstructures having micropores with better visibility than that of Comparative Example 1.

[0141] According to Examples 1 to 3, the removal of the anodic oxide film is preferably performed in the order of cathode electrolysis, ultrasonic treatment, and chemical conversion treatment.

[0142] Explanation of symbols

[0143] 10-microstructure, 12-anodized film, 12a, 20a-surface, 12b, 20b-back surface, 14-micropores, 20-substrate, 22-anodized film, 25-barrier layer, Dt-thickness direction, d-average diameter, h-thickness.

Claims

1. A microstructure consisting of an anodic oxide film of titanium or a titanium alloy, in, The microstructure is used in a chemical sensor or a biosensor. The microstructure has a plurality of micropores penetrating in the thickness direction of the anodized film, When the density of micropores on the surface of the anodized film is A and the density of micropores on the back side of the anodized film is B, the ratio A / B of the density A of the micropores on the surface to the density B of the micropores on the back side is 80% or more and 120% or less, The titanium alloy is selected from α-β titanium alloy, namely Ti-6Al-4V, and β titanium alloy, namely Ti-15V-3Cr-3Sn-3Al.

2. The microstructure according to claim 1, in, The thickness of the anodized film is 0.1 μm to 10 μm.

3. The microstructure according to claim 1 or 2, in, The average diameter of the micropores is 17nm to 200nm.

4. A method for producing a microstructure having a plurality of micropores penetrating in a thickness direction of an anodized film, The microstructure is used in a chemical sensor or a biosensor. The manufacturing method comprises an anodic oxide film forming step, in which an anodic oxide film forming step and a removal step of removing the anodic oxide film are sequentially performed at least once, and the anodic oxide film is formed by anodizing a substrate composed of titanium or a titanium alloy, and the anodic oxide film is formed by performing the anodic oxide treatment step after the removal step. The method for manufacturing a microstructure includes, after the anodized film forming step, a substrate removing step of removing the substrate present on the bottom side of the micropores. By the substrate removal step, the micropores penetrate the anodized film in the thickness direction. The titanium alloy is selected from α-β titanium alloy, namely Ti-6Al-4V, and β titanium alloy, namely Ti-15V-3Cr-3Sn-3Al.

5. The method for producing a microstructure according to claim 4, in, The removal step is a step of removing the anodic oxide film by using cathode electrolysis.

6. The method for producing a microstructure according to claim 4, in, The removal step is a step of removing the anodic oxide film by chemical conversion treatment.

7. The method for producing a microstructure according to claim 4, in, The removing step is a step of removing the anodic oxide film using ultrasonic treatment.

Citation Information

Patent Citations

  • Titania having shape of nanotube and its producing method

    JP2005263580A

  • Production method of porous structure, and electrophoresis apparatus used therein

    JP2016145389A

  • Method of fabricating photoelectrode and dye-sensitized solar cell, and photoelectrode of dye-sensitized solar cell fabricated by using the same

    KR1020140030475A

  • Titanium oxide NANO tube material and method for manufacturing the same