A method for solvent pre-assisted preparation of perovskite solar cells without charge transport layer

The 2D-3D heterojunction perovskite film is constructed through solvent pre-assisted preparation method to form a structure with type II energy level alignment, which solves the problem of the preparation of charge-free transport layer in perovskite solar cells and achieves high efficiency and low The cost perovskite solar cell process improves the photoelectric conversion efficiency.

CN113421971BInactive Publication Date: 2024-12-06DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110720241.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-28
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The use of electron transport layer and hole transport layer in perovskite solar cells leads to high material costs and unstable equipment, and its existence is non-essential, affecting equipment efficiency.

Method used

Using solvent pre-assisted preparation method, the 2D-3D heterojunction perovskite film is constructed in situ between the 3D perovskite film and the transparent conductive substrate to form a structure with type II energy level alignment to achieve a charge-free transport layer. The preparation of the process simplifies the process and reduces costs.

Benefits of technology

It realizes the efficient preparation of perovskite solar cells without charge transport layer, solves the problems of energy level mismatch and leakage, improves the photoelectric conversion efficiency, and is simple in process and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113421971B_ABST
    Figure CN113421971B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for solvent pre-assisted preparation of perovskite solar cells without charge transport layer. Perovskite materials themselves have the characteristics of bipolar charge transport, which means that electron transport layer and hole transport layer are not necessary for perovskite solar cells. Their use will cause the high price and instability of perovskite solar cells. Eliminating the charge transport layer can save material costs and reduce the coating process of the charge transport layer. The present invention adopts a new solution pre-assisted growth method to prepare 2D perovskite materials in situ between a 3D perovskite film and a transparent electrode to form a 2D-3D heterojunction perovskite material. By adjusting the type and concentration of amine salts, the band gap structure of the 2D perovskite material is accurately controlled so that it forms a type II energy level alignment structure with the 3D perovskite material, thereby transmitting electrons or holes, and preparing a perovskite solar cell without an electron transport layer, a hole transport layer or the simplest perovskite solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of perovskite solar cells and relates to a method for solvent pre-assisted preparation of a perovskite solar cell without a charge transport layer. Background Art

[0002] Perovskite solar cells (PSCs), as the third generation of solar cells, have become a research hotspot in the photovoltaic field, with a certified efficiency of 25.5%. [https: / / www.nrel.gov / pv / cell-efficiency.html ]. Typical perovskite solar cells usually place the light-absorbing layer perovskite material between the electron transport layer (ETL) and the hole transport layer (HTL). During operation, the perovskite material absorbs light to generate electrons and holes. Driven by the self-built field between adjacent layers, electrons and holes are transferred to the electron transport layer and the hole transport layer respectively, and finally transferred to the corresponding electrodes to form photocurrent. The electron transport layer can collect electrons and block holes, and is usually composed of metal oxides, metal sulfides or fullerene derivatives. The hole transport layer can collect holes and block electrons, and usually includes small organic molecules, organic polymers and inorganic compounds.

[0003] Perovskite materials themselves have the characteristics of bipolar charge transport, that is, they transport electrons and holes at the same time, which means that electron transport layers and hole transport layers are not necessary for perovskite solar cells [J.Am.Chem.Soc.,2012,134,17396]. Their use will cause the high price and instability of perovskite solar cells. Eliminating the electron transport layer can save material costs and reduce the coating process of the charge transport layer, which can reduce the manufacturing cost and time by at least one third or even half [Adv.Funct.Mater.,2020,30,2000863]. Studies have been conducted to prepare perovskite solar cells without charge transport layers by passivating transparent conductive substrates [Angew.Chem.,Int.Ed.,2020,59,20980], component engineering or doping [Chem.,2018,4,2405], heterojunction engineering [Nat.Photonics,2016,10,196]. Summary of the invention

[0004] The present invention provides a novel method for solvent pre-assisted preparation of perovskite solar cells without charge transport layer, in situ construction of 2D-3D heterojunction perovskite film, forming a (cascade type) with a certain energy level gradient, transmitting electrons in a type II energy level alignment manner, and preparing a device without charge transport layer. The method simultaneously realizes in situ controllable energy level of heterojunction perovskite materials and improves perovskite quality to solve the leakage problem, with simple process, strong operability and low cost.

[0005] The technical solution is as follows:

[0006] A method for solvent pre-assisted preparation of a perovskite solar cell without a charge transport layer, comprising the following steps:

[0007] The 2D perovskite material is prepared in situ between the 3D perovskite film and the transparent electrode by using solution pre-assisted growth, and a large volume of organic amine salt solution is applied to the surface of the transparent conductive substrate. According to the properties of the energy level regulation of the 2D perovskite material, the band gap structure of the 2D perovskite material is precisely controlled by adjusting the type and concentration of the amine salt, so that it forms a type II energy level alignment structure with the 3D perovskite material to transfer electrons or holes. The preparation of devices without charge transport layer is divided into the following 4 categories:

[0008] ① Device structure without electron transport layer: A 2D perovskite amine salt material with a conduction band position lower than that of the 3D perovskite material is selected and prepared in situ between the 3D perovskite and the transparent conductive substrate. The formed 2D-3D heterojunction material transmits electrons in a type II energy level aligned manner to prepare a device without electron transport layer (ITO / 2D-3DPVK / HTL / CE).

[0009] Preparation scheme 1 is as follows:

[0010] Step (1): Cleaning and processing of transparent conductive substrate

[0011] Step (2), preparation of 2D-3D heterojunction perovskite film

[0012] 1) Preparation of perovskite precursor solution: the composition is ABX 3 The drug is dissolved in a solvent to prepare a solution A with a concentration of 0.7-1.5M, stirred for 2-5 hours at a temperature of 25-35°C, and then filtered through a filter membrane with a pore size of 0.22 μm to obtain a perovskite precursor solution;

[0013] 2) Preparation of a large volume organic amine salt solution: dissolving a 2D perovskite amine salt material having a conduction band position lower than that of a 3D perovskite material in a solvent to obtain a solution B having a concentration of 200-700 mg / mL, stirring the solution at a temperature of 25-35° C. for 2-5 hours, and then filtering the solution with a filter membrane having a pore size of 0.22 μm to obtain a large volume organic amine salt solution;

[0014] 3) Deposition of 2D-3D heterojunction perovskite film: The large volume organic amine salt solution prepared in step 1) and the perovskite precursor solution prepared in step 2) are sequentially coated on a transparent conductive substrate, and due to the reaction between the two solutions, 2D perovskite is formed between the transparent conductive substrate and the 3D perovskite, thereby preparing a 2D-3D heterojunction perovskite film;

[0015] Step (3): Preparation of hole transport layer

[0016] Depositing a hole transport layer on the surface of a 2D-3D heterojunction perovskite film;

[0017] Step (4): Preparation of metal counter electrode

[0018] The device prepared in the above steps is placed into a mask plate, and metal electrodes are evaporated in a vacuum evaporation chamber.

[0019] ②Device structure without hole transport layer: A 2D perovskite amine salt material with a valence band position higher than that of the 3D perovskite material is selected and prepared in situ between the 3D perovskite and the transparent conductive substrate. The 2D-3D heterojunction material transports holes in a type II energy level aligned manner to prepare a device without hole transport layer (ITO / 2D-3DPVK / ETL / CE).

[0020] Preparation scheme 2 is as follows:

[0021] Step (1): Cleaning and treatment of transparent conductive substrate

[0022] Step (2) Preparation of 2D-3D heterojunction perovskite materials

[0023] Preparation of perovskite precursor solution. The composition is ABX 3 The drug is dissolved in a solvent to prepare a solution A with a concentration of 0.7-1.5M, stirred for 2-5 hours at a temperature of 25-35°C, and then filtered with a filter membrane with a pore size of 0.22μm to obtain a perovskite precursor solution.

[0024] Preparation of large volume organic amine salt solution. The 2D perovskite amine salt material with a valence band position higher than that of the 3D perovskite material is dissolved in a solvent to prepare a solution B with a concentration of 200-700 mg / mL, stirred at a temperature of 25-35°C for 2-5 hours, and then filtered with a filter membrane with a pore size of 0.22 μm to obtain a large volume organic amine salt solution.

[0025] Deposition of 2D-3D heterojunction perovskite thin films. A large volume of organic amine salt solution is applied on a transparent conductive substrate and then a perovskite layer is deposited to prepare a 2D-3D heterojunction perovskite thin film.

[0026] Step (3) Preparation of electron transport layer

[0027] Deposition of electron transport layer on the surface of 2D-3D heterojunction perovskite.

[0028] Step (4) Preparation of metal counter electrode

[0029] The device prepared in the above steps is placed into a mask plate, and metal electrodes are evaporated in a vacuum evaporation chamber.

[0030] ③ The simplest carbon-based device structure: A 2D-3D heterojunction perovskite that transports electrons in a type II energy level aligned manner is selected, and carbon materials are used as the hole transport layer and counter electrode to prepare the simplest PSCs, and its device structure is (ITO / 2D-3D PVK / C).

[0031] Preparation scheme three is as follows:

[0032] Steps (1)-(2) are the same as in Preparation Scheme 1.

[0033] Step (3) Preparation of carbon electrode

[0034] Preparation of carbon electrodes.

[0035] ④ The simplest device structure: Select a 2D-3D perovskite material that transports holes in a type II energy level alignment manner, and use a modified anti-solvent method to form another layer of 2D perovskite material on the surface of the 2D-3D perovskite to prepare a 2D-3D-2D heterojunction perovskite film. Adjust the type and concentration of the amine salt in the anti-solvent so that the 3D-2D perovskite material transports electrons in a type II energy level alignment manner on the side close to the counter electrode. The simplest device structure prepared is (ITO / 2D-3D-2D PVK / CE).

[0036] Preparation scheme 4 is as follows:

[0037] Step (1): Cleaning and treatment of transparent conductive substrate

[0038] Step (2) Preparation of 2D-3D-2D heterojunction perovskite materials

[0039] Preparation of perovskite precursor solution. The composition is ABX 3 The drug is dissolved in a solvent to prepare a solution A with a concentration of 0.7-1.5M, stirred for 2-5 hours at a temperature of 25-35°C, and then filtered with a filter membrane with a pore size of 0.22μm to obtain a perovskite precursor solution.

[0040] Preparation of large volume organic amine salt solution. The 2D perovskite amine salt material with a valence band position higher than that of the 3D perovskite material is dissolved in a solvent to prepare a solution B with a concentration of 200-700 mg / mL, stirred at a temperature of 25-35°C for 2-5 hours, and then filtered with a filter membrane with a pore size of 0.22 μm to obtain a large volume organic amine salt solution.

[0041] Preparation of improved anti-solvent solution: The 2D perovskite amine salt material with a conduction band position lower than that of the 3D perovskite material is dissolved in the anti-solvent to prepare a solution C with a concentration of 10-70 mg / mL, stirred at a temperature of 25-35°C for 2-5 hours, and then filtered with a filter membrane with a pore size of 0.22 μm to obtain a modified anti-solvent solution.

[0042] Deposition of 2D-3D-2D heterojunction perovskite thin films. A large volume of organic amine salt solution is applied to a transparent conductive substrate, and then a perovskite layer is deposited. By using a modified anti-solvent solution, a 2D-3D-2D heterojunction perovskite thin film is prepared.

[0043] Step (3) Preparation of metal counter electrode

[0044] The device prepared in the above steps is placed into a mask plate, and metal electrodes are evaporated in a vacuum evaporation chamber.

[0045] The transparent conductive substrate includes a rigid or flexible transparent conductive substrate, which may be a fluorine-doped SnO 2 At least one of transparent conductive glass (FTO), indium tin oxide transparent conductive glass (ITO), aluminum-doped zinc oxide transparent conductive glass (AZO), transparent indium tin oxide conductive film (ITO-PET and ITO-PEN), and transparent cadmium telluride conductive film (CAT-PEN);

[0046] The chemical formula of perovskite is ABX 3 , where A is a monovalent cation, preferably CH 3 NH 3 + NH 2 -CH=NH 2 + , Cs + , Li + , C 4 H 9 NH 3 + , CH 6 N 3 + 、Na + , K + At least one of the following, B is a divalent cation, preferably Pb 2 + , Cs + Sn 2+ ,Ge 2+ 、Co 2+ , Fe 2 + , Mn 2+ , Cu 2+ 、Ni 2+ At least one of, X is Cl - Br - ,I - 、SCN - , BF 4 -At least one of; the solvent for perovskite and bulky organic amine salt can be selected from N, N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide, N-methyl-2-pyrrolidone, etc.; wherein the anti-solvent is preferably at least one of toluene, xylene, chlorobenzene, acetonitrile, acetone, ethyl acetate, ether, n-butanol, ethanol, isopropanol;

[0047] 2D perovskites are divided into RP type and DJ type according to their different structures. The general structural formula is (RNH 3 ) 2 A n-1 B n X 3n+1 and MA n-1 B n X 3n+1 , n is the number of layers of its octahedron, A is usually MA + (CH 3 NH 3 + ), FA + (NH=CHNH 3 + ), Cs + , B is usually Pb 2+ Sn 2+ , X is usually I - Br - , Cl - The 2D perovskite amine salt material is RNH 3 + The bulky organic amine cationic groups represented by M 2+ Representative diamine organic groups, among which the 2D perovskite amine cations with valence band positions higher than those of the 3D perovskite materials include phenylethylamine cations (PEA + ), polyethyleneimine cation (PEI + ) etc.; 2D perovskite amine cations with conduction band positions lower than those of 3D perovskite materials include n-butylamine cations (n-BA + ), 2-thiophenemethylamine cation (ThMA + ), phenylenediamine cation (PDA 2+ ), fluorinated phenylethylamine cation (F-PEA + )wait;

[0048] The 2D and 3D perovskite material deposition methods may include spin coating, spray coating, doctor blade coating, slot die coating, screen printing, etc.;

[0049] The electron transport layer (ETL) is a dense layer of metal oxide, which may be TiO 2 、ZnO、SnO 2 、SnS 2,[6,6]-phenyl-C61-butyric acid methyl ester(PCBM),C 60 , WO x , graphene, Nb 2 O 5 , CdSe, CdS and multi-component Zn 2 SnO 4 、BaSnO 3 、CuInS 2 、SrTiO 3 Or at least one of its dopants; the hole transport layer (HTL) includes organic small molecules, organic polymers and inorganic compounds (such as NiO, CuSCN, etc.).

[0050] Beneficial effects of the present invention: Compared with the prior art, the method of the present invention is not only fast, convenient, simple to operate, and low in cost, but can also simultaneously solve the energy level mismatch and leakage problems of perovskite solar cells without a charge transport layer, optimize the structure of perovskite solar cells, and prepare perovskite solar cells without an electron transport layer with high photoelectric conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a schematic diagram of the preparation of 2D-3D perovskite materials and 2D-3D-2D perovskite materials;

[0052] Figure 2 It is a schematic diagram of the device structure without electron transport layer (ITO / 2D-3D PVK / Spiro-OMeTAD / Au);

[0053] Figure 3 yes Figure 2 Battery performance and mechanism;

[0054] Figure 4 It is a schematic diagram of the device structure without hole transport layer (FTO / 2D-3D PVK / PCBM(BCP) / Au);

[0055] Figure 5 yes Figure 4 Battery performance and mechanism;

[0056] Figure 6 This is the simplest carbon-based device structure: (ITO / 2D-3D PVK / C) schematic diagram;

[0057] Figure 7 yes Figure 6 Battery performance and mechanism;

[0058] Figure 8 This is a schematic diagram of the simplest device structure (FTO / 2D-3D-2D PVK / Au);

[0059] Fig. 9 yes Figure 8 Battery performance and mechanism. DETAILED DESCRIPTION

[0060] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.

[0061] Embodiment 1:

[0062] A method for solvent pre-assisted preparation of a perovskite solar cell without an electron transport layer comprises the following steps:

[0063] Step (1): Cleaning of ITO substrate

[0064] The ITO substrate was cleaned in sequence with detergent, acetone, isopropanol and ethanol in an ultrasonic bath for 20 min each, and then treated with UV-ozone for 15 min.

[0065] Step (2) Preparation of 2D-3D heterojunction perovskite materials

[0066] Preparation of perovskite precursor solution. Cesium iodide, methylamine bromide, lead bromide, methylamine iodide and lead iodide are dissolved in a mixture of N,N-dimethylformamide and dimethyl sulfoxide to obtain solution A; wherein N,N-dimethylformamide and dimethyl sulfoxide are mixed in a volume ratio of 4:1 in the solution; cesium iodide, methylamine bromide, lead bromide, methylamine iodide and lead iodide are mixed in a molar ratio of 0.07:0.21:0.21:1.19:1.31; the concentration is 0.7M; at a temperature of 25°C, solution A is stirred for 2h, and then filtered through a filter membrane with a pore size of 0.22μm to obtain a perovskite precursor solution.

[0067] Preparation of large volume organic amine salt solution. The large volume organic amine salt n-butylammonium iodide was dissolved in dimethyl sulfoxide to prepare a solution B with a concentration of 200 mg / mL, stirred at 25°C for 2 hours, and then filtered with a filter membrane with a pore size of 0.22 μm to obtain a large volume organic amine salt solution.

[0068] Deposition of 2D-3D heterojunction perovskite films. Deposition by spin coating. 15 μL / cm 2 A large volume of organic amine salt solution was dripped onto the transparent conductive substrate ITO, first spin-coated at a low speed of 1000 rpm for 10 seconds, and then 20 μL / cm was dripped at the 5th second of spin coating. 2 Perovskite precursor solution; then spin-coat at a high speed of 4000 rpm for 30 seconds, and add 50 μL / cm 2 Anti-solvent chlorobenzene; immediately after the spin coating is stopped, annealing is performed on a hot plate at a temperature of 75°C for 100 minutes to prepare a 2D-3D heterojunction perovskite film, such as Figure 1shown.

[0069] Step (3) Preparation of Spiro-OMeTAD hole transport layer

[0070] In 1 mL of chlorobenzene solvent, add 1 mol of Spiro-OMeTAD, and add 17.5 μL of Li-TFSI solution and 28.8 μL of 4-tert-butylpyridine as additives to prepare solution C; stir at 30 °C for 4 h, and after all dissolved, filter with a filter membrane with a pore size of 0.22 μm to obtain the Spiro-OMeTAD hole transport layer solution; drip 18 μL / cm 2 The Spiro-OMeTAD solution was spin-coated at 3500 rpm for 30 s to deposit on the perovskite film as a hole transport layer.

[0071] (4) Preparation of metal counter electrodes and battery performance testing

[0072] The device prepared in the above steps is placed into the mask and placed in a vacuum deposition chamber. -4 Pa, first The Au electrode was evaporated to a thickness of Complete the evaporation.

[0073] Device structure such as Figure 2 As shown, the prepared device was exposed to standard simulated sunlight AM1.5 G (100mW / cm 2 ), use standard silicon cells (B5-520) to calibrate the light intensity, and use Keithley2460 instrument to test. The JV test results are as follows Figure 3 shown.

[0074] Embodiment 2:

[0075] A method for solvent pre-assisted preparation of a hole transport layer-free perovskite solar cell comprises the following steps:

[0076] Step (1): Cleaning of FTO substrate

[0077] The FTO substrate was cleaned with detergent, acetone, isopropanol and ethanol in an ultrasonic bath for 20 min each, and then treated with UV-ozone for 15 min.

[0078] Step (2) Preparation of 2D-3D heterojunction perovskite materials

[0079] Preparation of perovskite precursor solution: Lead iodide, iodomethylamine, and iodoformamidine were dissolved in N,N-dimethylformamide to obtain solution A; wherein the molar ratio of lead iodide, iodomethylamine, and iodoformamidine was 1:0.7:0.3; the concentration was 1.5M; at a temperature of 35°C, solution A was stirred for 5 hours, and then filtered through a filter membrane with a pore size of 0.22μm to obtain a perovskite precursor solution.

[0080] Preparation of large volume organic amine salt solution. The large volume organic amine salt phenethylammonium iodide was dissolved in dimethyl sulfoxide to prepare a solution B with a concentration of 700 mg / mL, stirred at 35°C for 5 hours, and then filtered with a filter membrane with a pore size of 0.22 μm to obtain a large volume organic amine salt solution.

[0081] Deposition of 2D-3D heterojunction perovskite films. Deposition by doctor blade coating. 7μL / cm 2 A large volume of organic amine salt solution was dripped onto the transparent conductive substrate ITO and linearly swiped by a glass blade at a speed of 5.5 mm / s; 10 μL / cm 2 A large volume of organic amine salt solution was dripped onto the transparent conductive substrate ITO and linearly swiped by a glass blade at a speed of 10 mm / s; it was immediately annealed on a hot plate at a temperature of 75°C for 100 min to prepare a 2D-3D heterojunction perovskite film.

[0082] Step (3) Preparation of electron transport layer PCBM (BCP)

[0083] PCBM and BCP were dissolved in chlorobenzene and isopropanol, respectively, to prepare solution C with a concentration of 20 mg / mL and solution D with a concentration of 0.5 mg / mL. Solution C and solution D were stirred at 30°C for 6 h, and then filtered with a filter membrane with a pore size of 0.22 μm. 15 μL / cm 2 The PCBM solution was spin coated at 2000 rpm for 30 s and annealed at 75 °C for 10 min to deposit PCBM on the perovskite layer. After cooling to room temperature, 40 μL / cm 2 The BCP solution was spin coated at a speed of 5000 rpm for 30 seconds, and then annealed at a temperature of 75°C for 5 minutes to deposit the BCP layer, thereby completing the preparation of the electron transport layer PCBM (BCP).

[0084] (4) Preparation of metal counter electrodes and battery performance testing

[0085] The device prepared in the above steps is placed into the mask and placed in a vacuum deposition chamber. -4 Pa, first The Au electrode was evaporated to a thickness of Complete the evaporation.

[0086] Device structure such as Figure 4 As shown, the prepared device was exposed to standard simulated sunlight AM1.5 G (100mW / cm 2 ), use standard silicon cells (B5-520) to calibrate the light intensity, and use Keithley2460 instrument to test. The JV test results are as follows Figure 5 shown.

[0087] Embodiment 3:

[0088] A method for solvent pre-assisted preparation of the simplest carbon-based perovskite solar cell comprises the following steps:

[0089] Steps (1)-(2) are the same as in Preparation Scheme 1.

[0090] Step (3) Preparation of carbon electrode

[0091] Conductive carbon paste is coated on the perovskite layer and dried at 85° C. for 90 minutes to obtain the simplest carbon-based perovskite solar cell; the amount of the conductive carbon paste is determined according to user needs.

[0092] Device structure such as Figure 6 As shown, the prepared device was exposed to standard simulated sunlight AM1.5 G (100mW / cm 2 ), use standard silicon cells (B5-520) to calibrate the light intensity, and use Keithley2460 instrument to test. The JV test results are as follows Figure 7 shown.

[0093] Implementation Example 4:

[0094] A method for preparing the simplest perovskite solar cell with solvent pre-assistance comprises the following steps:

[0095] Step (1): Cleaning of FTO substrate

[0096] The FTO substrate was cleaned with detergent, acetone, isopropanol and ethanol in an ultrasonic bath for 20 min each, and then treated with UV-ozone for 15 min.

[0097] Step (2) Preparation of 2D-3D-2D heterojunction perovskite materials

[0098] Preparation of perovskite precursor solution. Lead iodide, iodomethylamine, and chloromethylamine are dissolved in a mixture of N, N-dimethylformamide and dimethyl sulfoxide to obtain solution A; wherein the molar ratio of lead iodide, lead chloride, and iodomethylamine is 0.75:0.25:1; the concentration is 1.3M; wherein N, N-dimethylformamide and dimethyl sulfoxide are mixed in the solution at a volume ratio of 7:3; at a temperature of 30°C, solution A is stirred for 3.5 hours, and then filtered through a filter membrane with a pore size of 0.22μm to obtain a perovskite precursor solution.

[0099] Preparation of large volume organic amine salt solution. The large volume organic amine salt phenethylammonium iodide was dissolved in dimethylacetamide to prepare a solution B with a concentration of 450 mg / mL, stirred at 30°C for 3.5 hours, and then filtered with a filter membrane with a pore size of 0.22 μm to obtain a large volume organic amine salt solution.

[0100] Preparation of improved anti-solvent solution: 2-Thienylmethylammonium iodide was dissolved in anti-solvent ethyl acetate to prepare solution C with a concentration of 35 mg / mL, stirred at 30°C for 3.5 h, and then filtered with a filter membrane with a pore size of 0.22 μm to obtain a modified anti-solvent solution.

[0101] Deposition of 2D-3D-2D heterojunction perovskite films. Deposition by spin coating. 10 μL / cm 2 A large volume of organic amine salt solution was dripped onto the transparent conductive substrate FTO, first spin-coated at a low speed of 2000 rpm for 10 s, and then 15 μL / cm was dripped at the 5th second of spin coating. 2 Perovskite precursor solution; then spin-coat at a high speed of 5000 rpm for 30 seconds, and add 45 μL / cm 2 Improve the anti-solvent solution; immediately anneal on a hot plate at 100°C for 75 minutes after the spin coating is stopped to prepare a 2D-3D-2D heterojunction perovskite film, such as Figure 1 shown.

[0102] Step (3) Preparation of metal counter electrode and battery performance test

[0103] The device prepared in the above steps is placed into the mask and placed in a vacuum deposition chamber. -4 Pa, first The Au electrode was evaporated to a thickness of Complete the evaporation.

[0104] Device structure such as Figure 8 As shown, the prepared device was exposed to standard simulated sunlight AM1.5 G (100mW / cm 2), use standard silicon cells (B5-520) to calibrate the light intensity, and use Keithley2460 instrument to test. The JV test results are as follows Fig. 9 shown.

Claims

1. A method for preparing a perovskite solar cell without a charge transport layer by solvent pre-assisted preparation, It is characterized in that Here are the steps: The 2D perovskite material is prepared in situ between the 3D perovskite film and the transparent electrode by using a solution pre-assisted growth method, and a large volume of organic amine salt solution is applied to the surface of the transparent conductive substrate; according to the energy level regulation properties of the 2D perovskite material, the type and concentration of the amine salt are adjusted to precisely control the band gap structure of the 2D perovskite material so that it forms a type II energy level alignment structure with the 3D perovskite material to transmit electrons or holes; the preparation of devices without charge transport layer is divided into the following 4 categories: device structure without electron transport layer, device structure without hole transport layer, carbon-based simplest device structure and simplest device structure; in, Device structure without electron transport layer: Select 2D perovskite amine salt material with a conduction band position lower than that of 3D perovskite material, and prepare it in situ between the 3D perovskite layer and the transparent conductive substrate. The formed 2D-3D heterojunction material transmits electrons in a type II energy level alignment manner to prepare a device without electron transport layer; The specific steps are as follows: Step (1): Cleaning and processing of transparent conductive substrate Step (2), preparation of 2D-3D heterojunction perovskite film 1) Preparation of perovskite precursor solution: the composition is ABX 3 The drug is dissolved in a solvent to prepare a solution A with a concentration of 0.7-1.5M, stirred for 2-5 hours at a temperature of 25-35°C, and then filtered through a filter membrane with a pore size of 0.22 μm to obtain a perovskite precursor solution; 2) Preparation of a large volume organic amine salt solution: dissolving a 2D perovskite amine salt material having a conduction band position lower than that of a 3D perovskite material in a solvent to obtain a solution B having a concentration of 200-700 mg / mL, stirring the solution at a temperature of 25-35° C. for 2-5 hours, and then filtering the solution with a filter membrane having a pore size of 0.22 μm to obtain a large volume organic amine salt solution; 3) Deposition of 2D-3D heterojunction perovskite film: The large volume organic amine salt solution prepared in step 2) and the perovskite precursor solution prepared in step 1) are sequentially coated on a transparent conductive substrate, and the 2D perovskite is reacted to form a 2D-3D heterojunction perovskite film between the transparent conductive substrate and the 3D perovskite; Step (3): Preparation of electron transport layer Depositing an electron transport layer on the surface of a 2D-3D heterojunction perovskite film; Step (4): Preparation of metal counter electrode The device prepared in the above steps is placed into a mask, and metal electrodes are evaporated in a vacuum evaporation chamber; in, Device structure without hole transport layer: 2D perovskite amine salt material with a higher valence band position than 3D perovskite material is selected and prepared in situ between 3D perovskite and transparent conductive substrate. The 2D-3D heterojunction material transports holes in a type II energy level alignment manner to prepare a device without hole transport layer; The specific steps are as follows: Step (1): Cleaning and treatment of transparent conductive substrate Step (2) Preparation of 2D-3D heterojunction perovskite materials 1) Preparation of perovskite precursor solution: the composition is ABX 3 The drug is dissolved in a solvent to prepare a solution A with a concentration of 0.7-1.5M, stirred for 2-5 hours at a temperature of 25-35°C, and then filtered through a filter membrane with a pore size of 0.22 μm to obtain a perovskite precursor solution; 2) Preparation of a large volume organic amine salt solution: dissolving a 2D perovskite amine salt material having a valence band position higher than that of a 3D perovskite material in a solvent to obtain a solution B having a concentration of 200-700 mg / mL, stirring the solution at a temperature of 25-35° C. for 2-5 hours, and then filtering the solution with a filter membrane having a pore size of 0.22 μm to obtain a large volume organic amine salt solution; 3) Deposition of 2D-3D heterojunction perovskite film: A large volume of organic amine salt solution is applied on a transparent conductive substrate and then a perovskite layer is deposited to prepare a 2D-3D heterojunction perovskite film; Step (3) Preparation of hole transport layer Depositing a hole transport layer on the surface of a 2D-3D heterojunction perovskite film; Step (4) Preparation of metal counter electrode The device prepared in the above steps is placed into a mask, and metal electrodes are evaporated in a vacuum evaporation chamber; in, The simplest carbon-based device structure: 2D-3D heterojunction perovskite that transmits electrons in a type II energy level alignment manner is selected, and carbon materials are used as hole transport layers and counter electrodes to prepare the simplest PSCs, whose device structure is ITO / 2D-3D PVK / C; The specific steps are as follows: Step (1): Cleaning and processing of transparent conductive substrate Step (2), preparation of 2D-3D heterojunction perovskite film 1) Preparation of perovskite precursor solution: the composition is ABX 3 The drug is dissolved in a solvent to prepare a solution A with a concentration of 0.7-1.5M, stirred for 2-5 hours at a temperature of 25-35°C, and then filtered through a filter membrane with a pore size of 0.22 μm to obtain a perovskite precursor solution; 2) Preparation of a large volume organic amine salt solution: dissolving a 2D perovskite amine salt material having a conduction band position lower than that of a 3D perovskite material in a solvent to obtain a solution B having a concentration of 200-700 mg / mL, stirring the solution at a temperature of 25-35° C. for 2-5 hours, and then filtering the solution with a filter membrane having a pore size of 0.22 μm to obtain a large volume organic amine salt solution; 3) Deposition of 2D-3D heterojunction perovskite film: The large volume organic amine salt solution prepared in step 2) and the perovskite precursor solution prepared in step 1) are sequentially coated on a transparent conductive substrate, and the 2D perovskite is reacted to form a 2D-3D heterojunction perovskite film between the transparent conductive substrate and the 3D perovskite; Step (3), preparing a carbon electrode, preparing a carbon electrode; in, The simplest device structure: Select a 2D-3D perovskite material that transports holes in a type II energy level alignment manner, use a modified anti-solvent method to form another layer of 2D perovskite material on the surface of the 2D-3D perovskite, and prepare a 2D-3D-2D heterojunction perovskite film; adjust the type and concentration of the amine salt in the anti-solvent so that the 3D-2D perovskite material transports electrons in a type II energy level alignment manner on the side close to the counter electrode. The simplest device structure prepared is ITO / 2D-3D-2D PVK / CE; The specific steps are as follows: Step (1), cleaning and treating the transparent conductive substrate; Step (2), preparation of 2D-3D-2D heterojunction perovskite material; 1) Preparation of perovskite precursor solution: the composition is ABX 3 The drug is dissolved in a solvent to prepare a solution A with a concentration of 0.7-1.5M, stirred for 2-5 hours at a temperature of 25-35°C, and then filtered through a filter membrane with a pore size of 0.22 μm to obtain a perovskite precursor solution; 2) Preparation of a large volume organic amine salt solution: dissolving a 2D perovskite amine salt material having a valence band position higher than that of a 3D perovskite material in a solvent to obtain a solution B having a concentration of 200-700 mg / mL, stirring the solution at a temperature of 25-35° C. for 2-5 hours, and then filtering the solution with a filter membrane having a pore size of 0.22 μm to obtain a large volume organic amine salt solution; 3) Preparation of improved anti-solvent solution: dissolving the 2D perovskite amine salt material whose conduction band position is lower than that of the 3D perovskite material in the anti-solvent to obtain a solution C with a concentration of 10-70 mg / mL, stirring for 2-5 hours at a temperature of 25-35° C., and then filtering with a filter membrane with a pore size of 0.22 μm to obtain a modified anti-solvent solution; 4) Deposition of 2D-3D-2D heterojunction perovskite film: A large volume of organic amine salt solution is applied on a transparent conductive substrate, and then a perovskite layer is deposited. By using a modified anti-solvent solution, a 2D-3D-2D heterojunction perovskite film is prepared; Step (3) Preparation of metal counter electrode; The device prepared in the above steps is placed into a mask, and metal electrodes are evaporated in a vacuum evaporation chamber; The chemical formula of the perovskite is ABX 3 , where A is a monovalent cation, CH 3 NH 3 + NH 2 -CH=NH 2 + , Cs + , Li + , C 4 H 9 NH 3 + , CH 6 N 3 + 、Na + , K + One of them; B is a divalent cation, which is Pb 2 + , Cs + Sn 2+ ,Ge 2+ 、Co 2+ , Fe 2+ , Mn 2+ , Cu 2 + 、Ni 2+ One of the following; X is Cl - Br - ,I - 、SCN - , BF 4 - The solvent for perovskite and bulky organic amine salt is selected from N, N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide, N-methyl-2-pyrrolidone; the anti-solvent is selected from toluene, xylene, chlorobenzene, acetonitrile, acetone, ethyl acetate, ether, n-butanol, ethanol, isopropanol; The 2D perovskite amine salt material is RNH 3 + The bulky organic amine cationic groups represented by M 2+ The representative diamine organic group, wherein the 2D perovskite amine cation whose valence band position is higher than that of the 3D perovskite material is selected from phenylethylamine cation and polyethyleneimine cation; the 2D perovskite amine cation whose conduction band position is lower than that of the 3D perovskite material is selected from n-butylamine cation, 2-thienylmethylamine cation, phenylenediamine cation and fluorinated phenylethylamine cation.

2. The method according to claim 1, It is characterized in that The transparent conductive substrate comprises a rigid or flexible transparent conductive substrate, which is a fluorine-doped SnO 2 One of transparent conductive glass, indium tin oxide transparent conductive glass, aluminum-doped zinc oxide transparent conductive glass, transparent indium tin oxide conductive film, and transparent cadmium telluride conductive film.

3. The method according to claim 1, It is characterized in that 2D perovskites are divided into RP type and DJ type according to their different structures. The general structural formula is (RNH 3 ) 2 A n-1 B n X 3n+1 and MA n-1 B n X 3n+1 , n is the number of layers of its octahedron, A is MA + (CH 3 NH 3 + ), FA + (NH=CHNH 3 + ), Cs + , B is Pb 2+ Sn 2+ , X is usually I - Br - , Cl - .

4. The method according to claim 3, It is characterized in that The electron transport layer is a dense layer of metal oxide, which is TiO 2 、ZnO、SnO 2 、SnS 2 , [6,6]-phenyl-C61-butyric acid methyl ester, C 60 , WO x , graphene, Nb 2 O 5 , CdSe, CdS and multi-component Zn 2 SnO 4 、BaSnO 3 、CuInS 2 、SrTiO 3 Or at least one of its dopants; the hole transport layer includes organic small molecules, organic polymers and inorganic compounds.

5. The method according to claim 4, It is characterized in that The 2D and 3D perovskite material deposition methods include spin coating, spray coating, doctor blade coating, slot die coating, and screen printing.