Laminated electrolyte membrane, membrane electrode assembly, water electrolysis hydrogen generation device, and method for producing laminated electrolyte membrane
By using hydrocarbon-based polymer electrolyte, fluorine-based polymer electrolyte and polyvinylidene fluoride superimposed electrolyte membrane in a water electrolytic device, the problems of insufficient bonding and oxidation deterioration are solved, the hydrogen barrier properties and mechanical strength are improved, and the Electrolytic efficiency and durability.
Patent Information
- Application Number
- CN202080015697.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-03-19
AI Technical Summary
In the water electrolytic device, the bonding property between the hydrocarbon-based polymer electrolyte membrane and the catalyst layer is insufficient and the oxidation deterioration of the hydrocarbon-based polymer electrolyte membrane at high electrode potentials leads to a decrease in current efficiency and a risk of safety.
The first layer with hydrocarbon-based polymer electrolyte as the main component and the second layer of superimposed electrolyte membrane with fluorine-based polymer electrolyte and polyvinylidene fluoride as the main component are adopted. The bondability is improved through the laminated structure of the mixed region, and the high-level The potential side prevents oxidation and deterioration.
Good bonding between the catalyst layer and the electrolyte membrane and anti-oxidation of the hydrocarbon polymer electrolyte layer are achieved, hydrogen barrier properties and mechanical strength are improved, and electrolytic efficiency and durability of the water electrolytic device are enhanced.
Smart Images

Figure CN113454270B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrolyte membrane used in a water electrolysis device or a fuel cell. Background Art
[0002] Fuel cells are power generation devices that extract electrical energy by electrochemically oxidizing fuels such as hydrogen. In recent years, they have attracted attention as a clean energy supply source. Among fuel cells, polymer electrolyte membrane (PEM) fuel cells have a low standard operating temperature of about 100°C and high energy density, so they are expected to be widely used as power generation devices for relatively small-scale distributed power generation facilities and mobile bodies such as automobiles and ships. In addition, they are also attracting attention as power sources for small mobile devices and mobile devices, so they are expected to replace secondary batteries such as nickel-metal hydride batteries and lithium-ion batteries and be installed in mobile phones and personal computers.
[0003] There are various methods for producing hydrogen used as fuel cell fuel. If water is electrolyzed using surplus electricity generated by renewable energy, electricity can be converted into hydrogen energy without emitting carbon dioxide. There are two ways to produce hydrogen by electrolysis of water: alkaline water electrolysis and polymer electrolyte membrane (PEM) water electrolysis. However, PEM water electrolysis has the advantage of being able to operate at a high current density and flexibly respond to fluctuations in the output of renewable energy.
[0004] The principle of PEM type water electrolysis is shown below.
[0005] 1. Water supplied to the anode is oxidized by applying voltage, generating oxygen, protons, and electrons.
[0006] 2. Protons are conducted to the cathode via ion exchange groups in the electrolyte membrane.
[0007] 3. Electrons are conducted from the anode to the cathode through an external circuit by applying a voltage.
[0008] 4. Protons and electrons combine at the cathode to generate hydrogen.
[0009] As such a polymer electrolyte membrane for a PEM type water electrolysis device, an example of using the following membrane is reported, wherein the membrane uses a fluorine-based polymer electrolyte membrane represented by "Nafion (registered trademark)" manufactured by DuPont (DuPont) of the United States. However, the fluorine-based polymer electrolyte membrane is essentially large in hydrogen permeation, and the hydrogen barrier is insufficient. Therefore, there is a safety issue in the water electrolysis device, such as the decrease in current efficiency caused by the generated hydrogen passing from the cathode to the anode and the mixing of hydrogen and oxygen. Moreover, the fluorine-based polymer electrolyte membrane is a rubber-like material with low fracture strength, so there is a problem that the membrane is easily deformed. Moreover, there is also a problem that when the electrolyte membrane is thickened in order to solve this problem, as the proton conductivity decreases, the electrolysis efficiency of the water electrolysis device decreases.
[0010] To address this problem, it has been proposed to use hydrocarbon-based polymer electrolyte membranes instead of fluorine-based polymer electrolyte membranes (for example, Patent Document 1). Hydrocarbon-based polymer electrolyte membranes have excellent hydrogen barrier properties even in the form of thin films and have high breaking strength, so deformation can be suppressed.
[0011] One of the issues in the application of hydrocarbon-based polymer electrolyte membranes is the bonding between the electrolyte membrane and the catalyst layer. Patent Document 2 proposes an electrolyte membrane with a catalyst layer that improves the bonding between the electrolyte membrane and the catalyst layer by disposing a bonding promotion layer containing a fluorine-based polymer electrolyte and graphitized carbon particles between the electrolyte membrane and the catalyst layer.
[0012] [Prior art literature]
[0013] Patent Literature
[0014] Patent Document 1: Japanese Patent Application Publication No. 2016-216826
[0015] Patent Document 2: Japanese Patent Publication No. 2008-512884 Summary of the invention
[0016] Problems to be solved by the invention
[0017] However, it has been found that the electrolyte membrane with a catalyst layer using a hydrocarbon-based polymer electrolyte membrane has the following two new problems.
[0018] 1) The adhesion between the electrolyte membrane and the adhesion promoting layer is insufficient, and a voltage increase may occur due to peeling.
[0019] 2) The catalyst layer is in electrical contact with the hydrocarbon-based polymer electrolyte membrane. When the electrodes are at a high potential, such as in a water electrolysis device, the hydrocarbon-based polymer electrolyte membrane is oxidatively degraded.
[0020] Means of solving problems
[0021] The present invention for solving the above-mentioned problem is an electrolyte membrane, in which a second layer having a fluorine-based polymer electrolyte and polyvinylidene fluoride as main components is stacked on at least one side of a first layer having a hydrocarbon-based polymer electrolyte as a main component, and the first layer and the second layer are stacked via a region where the components constituting the two layers are mixed (hereinafter referred to as a mixed region).
[0022] Effects of the Invention
[0023] In the electrolyte membrane of the present invention, the first layer and the second layer, and the catalyst layer and the second layer can achieve good bonding, respectively. Furthermore, the hydrocarbon-based polymer electrolyte layer as the first layer can be prevented from contacting the electrode on the high potential side, thereby preventing oxidation degradation. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a cross-sectional photograph obtained by enlarging and photographing a mixed region portion of a laminated electrolyte membrane according to one embodiment of the present invention. DETAILED DESCRIPTION
[0025] Hereinafter, the laminated electrolyte membrane of the present invention will be described in detail.
[0026] 〔Hydrocarbon-based polymer electrolyte〕
[0027] A hydrocarbon-based polymer electrolyte is a hydrocarbon-based polymer having an ionic group. A hydrocarbon-based polymer having an ionic group refers to a polymer having a main chain with hydrocarbon as the main constituent unit and the main chain or side chain is endowed with an ionic group, and the main chain and side chain are substantially not fluorinated. In addition, the meaning of being substantially not fluorinated is that a polymer having a fluorinated portion in a very small part of the main chain or side chain should not be excluded. Specifically, a polymer including a polymer having a fluorine atom content of less than 5% per number average molecular weight of the polymer is called a hydrocarbon-based polymer having an ionic group.
[0028] As a hydrocarbon polymer constituting a hydrocarbon polymer electrolyte, an aromatic hydrocarbon polymer is particularly preferred. Aromatic hydrocarbon polymers are polymers containing a hydrocarbon skeleton having an aromatic ring in the main chain. As a specific example, a polymer having an aromatic ring in the main chain and having a structure selected from polysulfone, polyethersulfone, polyphenylene ether, polyarylether polymer, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene polymer, polyarylene ketone, polyetherketone, polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone. In addition, the polysulfone, polyethersulfone, polyetherketone, etc. mentioned here are general terms for structures having sulfone bonds, ether bonds, and ketone bonds in their molecular chains, including polyetherketoneketone, polyetheretherketone, polyetheretherketoneketone, polyetherketoneetherketoneketone, polyetherketonesulfone, etc. The hydrocarbon skeleton can have multiple structures in these structures. Among these, the most preferred is a polymer having a polyetherketone structure in the main chain, that is, a polyetherketone polymer. Here, the main component means that the mass of the etherketone structure portion regarded as a repeating unit is 50% by mass or more when the mass of the entire polymer is 100% by mass.
[0029] As the ionic group possessed by the hydrocarbon-based polymer electrolyte used in the present invention, any ionic group having proton exchange energy is sufficient. As such ionic groups, sulfonic acid groups, sulfonimide groups, sulfuric acid groups, phosphonic acid groups, phosphoric acid groups, and carboxylic acid groups can be preferably used. The ionic group may contain two or more types in the polymer. Among them, in terms of high proton conductivity, the polymer more preferably has at least a sulfonic acid group, a sulfonimide group, and a sulfuric acid group, and in terms of raw material cost, it is most preferably a sulfonic acid group.
[0030] 〔Fluorine-based polymer electrolyte〕
[0031] Fluorine-based polymer electrolyte refers to a polymer having a main chain with perfluorocarbon as the main constituent unit and the main chain or side chain is endowed with an ionic group. As such a fluorine-based polymer electrolyte, for example, a perfluorocarbon polymer (also containing etheric oxygen atoms) with a sulfonic acid group can be cited. Wherein, preferably a copolymer with a repeating unit based on tetrafluoroethylene and a repeating unit of perfluorocarbon with a sulfonic acid group. As a commercially available product of such a copolymer, it can be cited: Nafion (registered trademark: manufactured by DuPont (DuPont) company), Aquivion (registered trademark: manufactured by Solvay (Solvay) company) etc. with perfluorocarbon sulfonic acid polymers, polytrifluorostyrene sulfonic acid polymers, perfluorocarbon sulfonic acid polymers, trifluorostyrene sulfonic acid polymers, ethylene tetrafluoroethylene-g-styrene sulfonic acid polymers, ethylene-tetrafluoroethylene copolymers, polyvinylidene fluoride-perfluorocarbon sulfonic acid polymers, ethylene-tetrafluoroethylene copolymers, trifluorostyrene etc. are resins of base polymers, etc. From the viewpoint of power generation performance such as heat resistance and chemical stability, a fluorine-based polymer electrolyte composed of a perfluorocarbon sulfonic acid-based polymer is particularly preferred.
[0032] 〔platinum〕
[0033] The laminated electrolyte membrane of the present invention preferably contains platinum. Platinum can be used by reducing platinum or a platinum precursor compound. Examples of platinum precursors include H2Pt(OH)6, PtO2·nH2O, etc. When a platinum precursor is used, it can be easily reduced to platinum by using a reducing agent in a solution containing the platinum precursor. As a reducing agent for the platinum precursor, hydrogen, hydrazine, formaldehyde, formic acid or oxalic acid, methanol, ethanol, 1-propanol, isopropanol, 1-butanol, 2-butanol, and mixtures thereof can be used.
[0034] The particle size of platinum used in the laminated electrolyte membrane is not particularly limited, but platinum with a small particle size is preferably used to reduce the thickness of the hydrogen permeation prevention layer. The particle size of platinum is preferably 1 μm or less, more preferably 100 nm or less, and further preferably 20 nm or less.
[0035] Furthermore, platinum may be contained in any one of the first layer, the second layer, and the third layer described below, but is preferably contained in the second layer or the third layer.
[0036] 〔Polyvinylidene fluoride〕
[0037] The so-called polyvinylidene fluoride, in addition to homopolymers of vinylidene fluoride (i.e., pure polyvinylidene fluoride), copolymers of vinylidene fluoride with other copolymerizable monomers are also included in the meaning of polyvinylidene fluoride mentioned in the present invention. As monomers copolymerizable with vinylidene fluoride, for example, one or more of tetrafluoroethylene, hexafluoropropylene, trifluoroethylene, trichloroethylene or vinyl fluoride can be used. Such polyvinylidene fluoride can be obtained by emulsion polymerization or suspension polymerization.
[0038] Moreover, as the polyvinylidene fluoride used in the second layer, if the molecular weight is large, the entanglement between the molecular chains of the polyvinylidene fluoride and the hydrocarbon-based polymer electrolyte and the fluorine-based polymer electrolyte in the mixed region becomes stronger, and the bonding property is improved. Therefore, the weight average molecular weight of the polyvinylidene fluoride is preferably 300,000 or more, and more preferably 500,000 or more.
[0039] 〔First floor〕
[0040] The laminated electrolyte of the present invention has a layer (first layer) with a hydrocarbon-based polymer electrolyte as the main component. The hydrocarbon-based polymer electrolyte forming the layer is as described above. In addition, here, as the main component, it means that in the part of the first layer other than the mixed area described later, more than 50% by mass of all the components contained in the unit volume are hydrocarbon-based polymer electrolytes, preferably more than 70% by mass, more preferably more than 80% by mass, and particularly preferably substantially composed of hydrocarbon-based polymer electrolytes. In addition, here, "substantially" means that trace amounts, specifically less than 1% by mass, of other components are allowed, and typically means that no other components are contained.
[0041] 〔Second floor〕
[0042] The laminated electrolyte membrane of the present invention has a layer (second layer) with fluorine-based polymer electrolyte and polyvinylidene fluoride as the main component on at least one side of the first layer. In addition, here, as the main component, it means that in the part of the second layer except the mixed area described later, more than 50% by mass of all the components contained in the unit volume are fluorine-based polymer electrolytes and polyvinylidene fluoride, preferably more than 70% by mass, more preferably more than 80% by mass, and particularly preferably substantially composed of fluorine-based polymer electrolytes and polyvinylidene fluoride. In addition, here, "substantially" means that it is allowed to contain trace amounts, specifically less than 1% by mass of other components, and typically refers to not containing other components.
[0043] When in the second layer, the content ratio of the fluorine-based polymer electrolyte is small, the membrane resistance becomes larger. Therefore, when the total mass of the fluorine-based polymer electrolyte and polyvinylidene fluoride is set to 100 mass %, the fluorine-based polymer electrolyte is preferably more than 20 mass %, more preferably more than 60 mass %, and then preferably more than 70 mass %. When the content of the fluorine-based polymer electrolyte becomes more and the content ratio of polyvinylidene fluoride decreases, the bonding property with the first layer decreases. Therefore, when the total mass of the fluorine-based polymer electrolyte and polyvinylidene fluoride is set to 100 mass %, the fluorine-based polymer electrolyte is preferably less than 90 mass %, more preferably less than 80 mass %. By setting to the range, bonding and ion conductivity are taken into account, so as to have an effect on the balance of efficiency and durability. In addition, the weight ratio of the fluorine-based polymer electrolyte and polyvinylidene fluoride is obtained in the part of the second layer except the mixed region described later.
[0044] The present invention can achieve high hydrogen barrier properties and mechanical strength by using the first layer containing a hydrocarbon-based polymer electrolyte as the main electrolyte layer. Therefore, the thickness of the second layer is preferably set to 40% or less, more preferably 30% or less, and further preferably 20% or less relative to the thickness of the first layer. Moreover, if the film thickness of the second layer becomes thinner, the mixed region becomes thinner, and the bonding property between the first layer and the second layer decreases. Therefore, the thickness of the second layer is preferably set to 1% or more, and further preferably 5% or more relative to the thickness of the first layer. In addition, the measurement and determination of the thickness of the first layer and the second layer are described in the embodiment 1. (4) described later.
[0045] 〔Third floor〕
[0046] The laminated electrolyte membrane of the present invention may include a layer (third layer) containing a fluorine-based polymer electrolyte as a main component, which is laminated on the surface of the second layer opposite to the surface on which the first layer is laminated.
[0047] Moreover, the third layer does not contain hydrocarbon-based polymer electrolytes. In addition, here, as the main component, it means that 60% or more of the total components contained in the unit volume of the third layer are fluorine-based polymer electrolytes, preferably 70% or more, more preferably 80% or more, and particularly preferably substantially composed of fluorine-based polymer electrolytes. In addition, here, "substantially" means that trace amounts, specifically less than 1% by mass, of other components (excluding hydrocarbon-based polymer electrolytes) are allowed, and typically means that no other components are contained.
[0048] In the present invention, when the first layer containing a hydrocarbon-based polymer electrolyte is used as the main electrolyte layer, higher hydrogen barrier properties and mechanical strength are achieved. Therefore, the thickness of the third layer is preferably set to 40% or less, more preferably 30% or less, and further preferably 20% or less relative to the thickness of the first layer. As a lower limit, it is preferably set to 0.1% or more relative to the thickness of the first layer.
[0049] [Method for producing laminated electrolyte membrane]
[0050] The laminated electrolyte membrane of the present invention can be produced by the following steps.
[0051] First, as a first step, a first layer having a hydrocarbon-based polymer electrolyte as a main component is formed.
[0052] As an example of a method for forming the first layer, the first layer can be formed by sequentially performing a step of forming a layer in a state where an ionic group contained in a hydrocarbon-based polymer electrolyte forms a salt with a cation of an alkali metal or alkaline earth metal, and a step of exchanging a proton with the cation of the alkali metal or alkaline earth metal that forms a salt with the ionic group. The formation method is described in more detail below. In addition, in this specification, a polymer electrolyte in a state where an ionic group forms a salt with a cation of an alkali metal or alkaline earth metal is described as a "salt-type polymer electrolyte".
[0053] In the method for forming the first layer, there is a step of exchanging the cations of the alkali metal or alkaline earth metal that forms a salt with the ionic group with protons after forming the layer with the salt-type polymer electrolyte. The step of exchanging the cations with the protons is preferably a step of contacting the salt-type polymer electrolyte with an acidic aqueous solution. Moreover, the contact is more preferably a step of immersing the first layer in an acidic aqueous solution. In this step, the protons in the acidic aqueous solution are replaced with the cations that are ionically bonded with the ionic group, and the residual water-soluble impurities, or residual monomers, solvents, residual salts, etc. are removed at the same time. The acidic aqueous solution used is not particularly limited, and it is preferred to use a proton acid such as sulfuric acid, hydrochloric acid, nitric acid, acetic acid, trifluoromethanesulfonic acid, methanesulfonic acid, phosphoric acid, citric acid, etc. The temperature or concentration of the acidic aqueous solution should also be appropriately determined, but from the perspective of productivity, it is preferred to use a sulfuric acid aqueous solution of 3% by mass or more and 30% by mass or less at a temperature of 0°C or more and 80°C or less.
[0054] The solvent used when forming the first layer can be appropriately selected according to the polymer species. As the solvent, for example, N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, cyclopentane, 1,3-dimethyl-2-imidazolidinone, hexamethylphosphoric triamide and other non-protonic polar solvents, γ-butyrolactone, ethyl acetate, butyl acetate and other ester solvents, ethylene carbonate, propylene carbonate and other carbonate solvents, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether and other alkanediol monoalkyl ethers can be preferably used. In addition, a mixed solvent obtained by mixing two or more of these solvents can also be used.
[0055] Furthermore, for the purpose of adjusting the viscosity, various low-boiling-point solvents such as alcohol solvents such as methanol, ethanol, 1-propanol, and isopropanol, ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester solvents such as ethyl acetate, butyl acetate, and ethyl lactate, hydrocarbon solvents such as hexane and cyclohexane, aromatic hydrocarbon solvents such as benzene, toluene, and xylene, halogenated hydrocarbon solvents such as chloroform, dichloromethane, 1,2-dichloroethane, perchloroethylene, chlorobenzene, dichlorobenzene, and hexafluoroisopropanol, ether solvents such as diethyl ether, tetrahydrofuran, and 1,4-dioxane, nitrile solvents such as acetonitrile, nitrated hydrocarbon solvents such as nitromethane and nitroethane, and water may be mixed in the solvent.
[0056] Furthermore, as an example of a method for forming the second layer, there is a method of forming an electrolyte layer having a fluorine-based polymer electrolyte and polyvinylidene fluoride as main components on the formed first layer. When the membrane forming solvent remains in the laminated electrolyte membrane even after drying, it is preferably washed with pure water.
[0057] As the solvent used when forming the second layer, from the viewpoint of forming a mixed region near the interface between the first layer and the second layer and improving bonding, a solvent having high affinity with the first layer components is preferred. Therefore, it is preferred to use an aprotic polar solvent, and it is further preferred to use the solvent used when forming the first layer.
[0058] The peeling force between the first layer and the second layer of the laminated electrolyte membrane of the present invention is preferably 0.3 N or more, more preferably 1.0 N or more, and particularly preferably 2.0 N or more. The upper limit is not particularly limited, but is generally 10.0 N or less. The greater the peeling force, the more the peeling of the first layer and the second layer is suppressed, thereby preventing the performance degradation during the operation of the device.
[0059] 〔Mixed Area〕
[0060] In the laminated electrolyte membrane of the present invention, the first layer and the second layer are laminated via a region (mixed region) where components constituting the two layers are mixed.
[0061] The so-called mixed area, such as Figure 1As shown, it refers to a region sandwiched by a layer formed only of the components constituting the first layer and a layer formed only of the components constituting the second layer, and the length in the thickness direction (for convenience, also referred to as "thickness") is 0.1 μm or more as observed by the method described in the later-described Example 1. (4), and the hydrocarbon-based polymer electrolyte and at least one selected from polyvinylidene fluoride and fluorine-based polymer electrolyte are observed in this region. The thicker the mixed region, the higher the bonding strength between the first layer and the second layer, so the thickness is preferably 0.2 μm or more, more preferably 0.5 μm or more, and further preferably 1.0 μm or more. On the other hand, if the mixed region becomes too thick, the hydrocarbon-based polymer electrolyte is exposed to the surface of the laminated electrolyte membrane, and when used as an electrolyte membrane, the hydrocarbon-based polymer electrolyte in contact with the electrode may be oxidatively degraded. Therefore, the thickness of the mixed region is preferably a thickness that does not expose the hydrocarbon-based polymer electrolyte to the surface, and is a thickness that is less than 80% of the total thickness of the first layer and the second layer.
[0062] The concentration of the polymer electrolyte solution used is preferably 3% to 40% by mass, more preferably 5% to 30% by mass. If the solution viscosity is too low, the retention of the solution is poor, resulting in liquid flow. On the other hand, if the solution viscosity is too high, the surface smoothness of the electrolyte membrane may sometimes deteriorate.
[0063] As a method for casting the polymer electrolyte solution used to form the first layer and the second layer, knife coating, direct roll coating, Meyer bar coating, gravure coating, reverse coating, air knife coating, spray coating, brush coating, dip coating, die coating, vacuum die coating, curtain coating, flow coating, spin coating, screen printing, inkjet coating and the like can be applied.
[0064] Regarding the drying of the solvent, the drying method may be selected from known methods such as heating of the substrate, hot air, infrared heaters, etc. In consideration of decomposition of the polymer electrolyte, the drying temperature is preferably 200° C. or lower, more preferably 130° C. or lower.
[0065] In the stacked electrolyte membrane, for the purpose of improving mechanical strength and thermal stability of ionic groups, improving water resistance, improving solvent resistance, improving free radical resistance, improving coating liquid coating properties, improving storage stability, etc., cross-linking agents or crystallization nucleating agents, plasticizers, stabilizers, release agents, antioxidants, free radical supplements, inorganic microparticles and other additives commonly used in polymer compounds may be added within the scope that does not violate the purpose of the present invention.
[0066] The laminated electrolyte membrane of the present invention can be applied to various uses. For example, it can be applied to medical uses such as artificial skin, filtration uses, ion exchange resin uses such as chlorine-resistant reverse osmosis membranes, various structural materials, electrochemical uses, humidification membranes, anti-fog films, antistatic films, deoxidation membranes, solar cell membranes, and gas barrier membranes. Among them, it can be preferably used for various electrochemical uses. As electrochemical uses, for example, solid polymer fuel cells, redox flow batteries, electrochemical hydrogen pumps, hydrogen purification devices, water electrolysis devices, and chlor-alkali electrolysis devices can be listed, and it can be particularly well used in water electrolysis devices.
[0067] <Electrolyte membrane with catalyst layer, membrane electrode assembly, electrochemical hydrogen pump, water electrolysis hydrogen generator>
[0068] The battery used in the water electrolysis device is a structure in which a catalyst layer, an electrode substrate and a diaphragm are sequentially stacked on both sides of the composite electrolyte membrane of the present invention. Among them, the catalyst layer stacked on both sides of the laminated electrolyte membrane (i.e., the layer structure of catalyst layer / electrolyte membrane / catalyst layer) is called an electrolyte membrane with a catalyst layer (CCM), and the catalyst layer and the gas diffusion substrate stacked on both sides of the electrolyte membrane (i.e., the layer structure of gas diffusion substrate / catalyst layer / electrolyte membrane / catalyst layer / gas diffusion substrate) are called a membrane electrode assembly (MEA).
[0069] As a method for manufacturing CCM, a catalyst layer paste composition for forming a catalyst layer is generally applied to the surface of the electrolyte membrane and dried, or only the catalyst layer is prepared on a substrate and the catalyst layer is transferred to thereby stack the catalyst layer on the electrolyte membrane (transfer method).
[0070] Here, regarding the catalyst layer, the catalyst layer on the anode side is referred to as the anode catalyst layer, and the catalyst layer on the cathode side is referred to as the cathode catalyst layer. In the present invention, it is desirable to configure the second layer between the first layer and the anode catalyst layer. By adopting such a configuration, direct contact between the first layer and the anode catalyst layer is prevented, thereby suppressing oxidative degradation of the components constituting the first layer, thereby preventing a decrease in performance when used in a device such as a fuel cell or a water electrolysis hydrogen generation device.
[0071] In the case of making MEA by pressing, known methods can be applied (for example, the chemical plating method described in Electrochemistry, 1985, 53, p. 269, the hot pressing bonding method of gas diffusion electrodes described in J. Electrochem. Soc., Electrochemical Science and Technology, 1988, 135, 9, p. 2209, etc.). The temperature or pressure during pressing can be appropriately selected according to the thickness, moisture content, catalyst layer or electrode substrate of the electrolyte membrane. Moreover, in the present invention, composite formation can be achieved by pressing even when the electrolyte membrane is dry or absorbs water. As specific pressing methods, roller pressing with a specified pressure or clearance or flat plate pressing with a specified pressure can be listed. From the perspective of industrial productivity or inhibition of thermal decomposition of polymer materials having ionic groups, it is preferably carried out in the range of 0°C to 250°C. From the perspective of electrolyte membrane or electrode protection, the pressure is preferably as weak as possible within the range of maintaining the close contact between the electrolyte membrane and the catalyst layer. In the case of flat pressing, it is preferably a pressure of 10MPa or less. From the perspective of preventing the short circuit of the anode and cathode electrodes, the electrode and the electrolyte membrane are overlapped without the pressing step to implement the composite, and the battery is used as a water electrolysis device. It is also one of the preferred options. In the case of this method, when repeatedly operated as a water electrolysis device, there is a tendency that the degradation of the electrolyte membrane, which is speculated to be the cause of the short circuit, is suppressed, and the durability as a water electrolysis device becomes good. Moreover, in the control of the pressing conditions, in order to obtain a uniform electrolyte membrane with a catalyst layer without wrinkles or peeling, it is preferred to raise the temperature after pressurization, maintain the specified voltage and temperature, maintain the pressure and lower the temperature, and then open the pressure. If the temperature is raised while pressing or the pressure is opened before the temperature is lowered, there is a three-dimensional thermal shrinkage in the state where the interface between the electrolyte membrane and the catalyst layer is not fixed, and the peeling caused by wrinkles or poor adhesion occurs.
[0072] The physical properties required of the power supply of the water electrolysis hydrogen generator include gas-liquid flow path function, good electrical conductivity, acid resistance, oxidation resistance, hydrogen brittleness resistance, heat resistance, processability, etc. Any material can be used as long as it has such physical properties. For example, porous conductive sheets with conductive substances as the main constituent materials can be listed, and as the conductive substances, calcined bodies from polyacrylonitrile, calcined bodies from asphalt, carbon materials such as graphite and expanded graphite, stainless steel, molybdenum, titanium, nickel, zirconium, niobium, tantalum, etc. can be exemplified.
[0073] The anode power supply is preferably an inorganic conductive material that will not be oxidized by the high potential of the anode during water electrolysis, preferably stainless steel, molybdenum, titanium, nickel, zirconium, niobium, tantalum, etc., and particularly preferably titanium. The conductive material is in the form of fibers or particles, etc., and is not particularly limited, but preferably a fibrous conductive inorganic material (inorganic conductive fiber). As a porous conductive sheet using inorganic conductive fibers, any structure of woven or non-woven fabrics can be used. As a woven fabric, plain weave, twill weave, satin weave, pattern weave, jacquard weave (figured brocade), etc. can be used without particular limitation. Moreover, as a non-woven fabric, a non-woven fabric manufactured by a papermaking method, a needle punch method, a spunbond method, a water jetpunch method, a melt-blown method, etc. can be used without particular limitation. Moreover, the porous conductive sheet using inorganic conductive fibers can also be an expanded metal (expanded metal), a perforated metal (perforated metal) or a braid.
[0074] In the porous conductive sheet, conductive particles such as carbon black or conductive fibers such as carbon fibers are preferably added as auxiliary agents to improve conductivity. In addition, the porous conductive sheet is preferably plated with platinum to improve stability.
[0075] Example
[0076] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0077] 1. Evaluation Method
[0078] The measurement conditions of various physical properties are as follows.
[0079] (1) Molecular weight of polymer
[0080] The number average molecular weight and weight average molecular weight of the polymer solution were measured by gel permeation chromatography (GPC). As an integrated device of a UV detector and a differential refractometer, HLC-8022GPC manufactured by Tosoh was used, and as a GPC column, two TSK gelSuperHM-H (inner diameter 6.0 mm, length 15 cm) manufactured by Tosoh were used, and the measurement was performed at a flow rate of 0.2 mL / min through an N-methyl-2-pyrrolidone solvent (N-methyl-2-pyrrolidone solvent containing 10 mmol / L lithium bromide), and the number average molecular weight and weight average molecular weight were calculated based on standard polystyrene conversion.
[0081] (2) Ion exchange capacity (IEC)
[0082] The determination was performed by neutralization titration method. The determination was performed 3 times and the arithmetic mean value was taken.
[0083] 1. After the water on the surface of the measurement sample that has been subjected to proton substitution and fully washed with pure water is wiped off, the sample is vacuum dried at 100° C. for 12 hours or more to determine the dry weight.
[0084] 2. 50 mL of a 5 mass % sodium sulfate aqueous solution was added to the electrolyte, and the solution was allowed to stand for 12 hours to perform ion exchange.
[0085] 3. Titrate the generated sulfuric acid using a 0.01 mol / L sodium hydroxide aqueous solution. Add 0.1 w / v% of a commercially available phenolphthalein solution for titration as an indicator, and the point at which the solution turns light purple is regarded as the end point.
[0086] 4.IEC is calculated by the following formula.
[0087] IEC (meq / g) = [concentration of sodium hydroxide aqueous solution (mmol / ml) x amount added (ml)] / dry weight of sample (g).
[0088] (3) Electrolyte membrane thickness
[0089] The measurement was performed using ID-C112 model manufactured by Mitutoyo Co., Ltd. mounted on Granite Comparator Stand BSG-20 manufactured by Mitutoyo Co., Ltd.
[0090] The membrane thickness is measured by cutting the electrolyte membrane into 10 cm squares, measuring the positions at 5 cm from the end in the MD direction, 1 cm, 3 cm, 5 cm, 7 cm, and 9 cm from the end in the TD direction, and the positions at 5 cm from the end in the TD direction, and 1 cm, 3 cm, 5 cm, 7 cm, and 9 cm from the end in the MD direction, and finding the average value of these 9 points. The average value is defined as the membrane thickness of the electrolyte membrane.
[0091] (4) Confirmation of the mixed region, measurement of its thickness, and determination of the thickness of the first, second, and third layers using a scanning transmission electron microscope (STEM)
[0092] The sample piece of the electrolyte membrane was immersed in a 2 mass % lead acetate aqueous solution as a staining agent and left to stand at 25°C for 48 hours for staining. The stained sample was taken out and embedded in epoxy resin. A 100 nm thin slice was cut at room temperature using an ultramicrotome and observed under the following conditions.
[0093] A. Energy dispersive X-ray (EDX) quantitative line analysis was performed on the cross section of the cut electrolyte membrane sheet from one surface (for convenience, referred to as "surface a") side toward the other surface side, that is, in the thickness direction. The measuring device and measuring conditions are as follows.
[0094] Device: STEM (Scientific Electron Microscope)
[0095] JEM-ARM200F Dual-X (Made in JEOL)
[0096] EDX detector JED2300 (manufactured by JEOL)
[0097] Accelerating voltage: 200 kV.
[0098] B. Focusing on the fluorine atom concentration, in the measurement of item A above, the intensity distribution of the fluorine atom concentration in the thickness direction is determined with the distance from the surface a as the X-axis and the fluorine atom concentration as the Y-axis.
[0099] The above operation was performed for 10 samples, and from the 10 intensity distribution curves obtained, an intensity distribution curve in which the fluorine atom concentration was averaged was obtained with the Y axis being the average value of the fluorine atom concentration (an example is shown in FIG. Figure 1 ). In addition, it goes without saying that all samples were measured from the same surface side. Figure 1 In the figure, the Y axis indicates that the values are larger in the direction of the arrow.
[0100] C. In the intensity distribution curve of the averaged fluorine atomic concentration obtained in the above item B, the minimum fluorine atomic concentration is taken as the portion corresponding to the first layer, and the maximum fluorine concentration is taken as the portion corresponding to the second layer or the third layer. In addition, the corresponding portion can be understood from the stacking order and the SEM photograph image.
[0101] D. When the fluorine atom concentration of the first layer obtained by the above item C is defined as C1 and the fluorine atom concentration of the second layer is defined as C2, the position on the X-axis between the position on the X-axis for obtaining C1 and the position on the X-axis for obtaining C2 and representing the fluorine atom concentration of (C1+C2) / 2 is regarded as the boundary surface between the first layer and the second layer. In addition, when there are multiple positions on the X-axis representing the fluorine atom concentration of (C1+C2) / 2, the position obtained by the arithmetic average of the X-axis coordinate values corresponding to the fluorine atom concentrations is regarded as the boundary surface between the first layer and the second layer.
[0102] Furthermore, when a third layer exists, a surface regarded as a boundary surface between the first layer or the second layer and the third layer is obtained in the same manner.
[0103] E. When the difference between C1 and C2, i.e., |C1-C2|, is set to D, the region between the position on the X-axis where C1 is obtained and the position on the X-axis where C2 is obtained and between the positions on the X-axis indicating the fluorine concentrations of (C1+C2) / 2+0.3×D and (C1+C2) / 2-0.3×D is taken as the mixed region, and the thickness corresponding to (C1+C2) / 2±0.3×D is taken as the thickness of the mixed region. In addition, when there are multiple positions on the X-axis indicating the fluorine concentration of (C1+C2) / 2+0.3×D or (C1+C2) / 2-0.3×D, the position obtained by the arithmetic average of the X-axis coordinate values corresponding to the fluorine atom concentration is taken as the position corresponding to (C1+C2) / 2+0.3×D or (C1+C2) / 2-0.3×D.
[0104] F. The thicknesses of the first layer, the second layer, and the third layer are determined based on the positions of the surfaces regarded as the boundary surfaces of the respective layers determined above and the distances from the surface a.
[0105] (5) Bonding test
[0106] The electrolyte membrane was immersed in pure water at 80° C. for 24 hours, and the first layer and the second layer were observed for peeling. If no peeling was observed, it was indicated as “bonded” in the table, and if peeling was observed, it was indicated as “peeled”.
[0107] (6) Peel test
[0108] 1. Prepare the electrolyte membrane or electrolyte membrane with a catalyst layer to be evaluated and commercially available NR212 (Nafion 50 μm) by cutting each of them into 5 cm×12 cm.
[0109] 2. In the case of an electrolyte membrane with a catalyst layer, the catalyst layer is wiped off with a solvent such as alcohol that does not dissolve the electrolyte membrane.
[0110] 3. A Teflon sheet (3 cm×5 cm) was placed on the upper 3 cm portion of the long side of the electrolyte membrane to be evaluated, and NR212 was overlapped thereon so as to match the position of the electrolyte membrane to be evaluated.
[0111] 4. The electrolyte membranes stacked in step 3 are stacked and heated and pressed at 150° C. and 4.5 MPa for 10 minutes.
[0112] 5. The sample prepared in 4. above was cut into a strip of 1 cm×12 cm to prepare a peeling test piece.
[0113] 6. The electrolyte membrane and NR212 to be evaluated are grasped by the upper and lower chucks of the tensile testing machine, and the stress when the upper chuck is in stroke is measured.
[0114] 7. The average of the stresses between the travel distances of 5 cm and 8 cm was calculated as the peeling force.
[0115] Measuring device: autograph AG-IS (manufactured by Shimadzu Corporation)
[0116] Travel speed: 10mm / min
[0117] Test piece: 1cm wide x 12cm long
[0118] Distance between samples: 2cm
[0119] Test temperature: 23°C, in pure water
[0120] Number of experiments: n=5.
[0121] (7) Fabrication of Catalyst-Layered Electrolyte Membrane (CCM)
[0122] A catalyst ink was prepared by mixing platinum catalyst TEC10E50E manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. and "Nafion (registered trademark)" manufactured by DuPont at a weight ratio of 2:1, and the amount of platinum was 0.3 mg / cm 2 The cathode catalyst layer transfer film A100 was prepared by coating it onto a commercially available Teflon film.
[0123] A catalyst ink prepared by mixing indium oxide catalyst manufactured by Yumico and "Nafion (registered trademark)" manufactured by DuPont at a weight ratio of 2:1 was prepared so that the indium content was 2.5 mg / cm 2 The anode catalyst layer transfer film A200 is prepared by coating it on a commercially available Teflon film. A pair of films is prepared by cutting the anode catalyst layer transfer film A200 and the cathode catalyst layer transfer film A100 into 5 cm squares, respectively, so that they are overlapped oppositely in a manner of clamping the polymer electrolyte membrane to be evaluated. When a stacked electrolyte membrane is used as the polymer electrolyte membrane, the cathode catalyst layer transfer film A100 is arranged on the surface of the first layer side, and the anode catalyst layer transfer film A200 is arranged on the surface of the second layer side or the third layer side. After that, the temperature is raised from the pressurized state, and the heat pressing is performed at 150°C and 5MPa for 3 minutes. After the temperature is reduced to below 40°C under the pressurized state, the pressure is released to obtain an electrolyte membrane with a catalyst layer for a water electrolysis device with A200 as the anode and A100 as the cathode.
[0124] (8) Fabrication of membrane electrode assembly (MEA)
[0125] The electrolyte membrane with a catalyst layer for a water electrolysis device was sandwiched between two commercially available porous titanium sintered body plates to obtain a membrane electrode assembly for a water electrolysis device.
[0126] (9) Water electrolysis performance test
[0127] The membrane electrode assembly for water electrolysis was mounted on a JARI standard cell "Ex-1" (electrode area 25 cm) manufactured by Eiwa Co., Ltd. 2 ), set the battery temperature to 80°C, and the conductivity to 1μScm -1 The following pure water was supplied to one of the electrodes (oxygen generating electrode: anode) at atmospheric pressure and a flow rate of 0.2 L / min.
[0128] The other electrode (hydrogen generating electrode: cathode) was configured to be able to control the pressure by a back pressure valve, and was flushed with 100% RH nitrogen gas to atmospheric pressure before evaluation.
[0129] A Multistat 1480 and a power booster Model PBi500L-5U manufactured by Solatron were used, and the load current was 50 A (current density 2 A / cm 2 ) for output. After the current is maintained at atmospheric pressure for 10 hours, the battery voltage at this time is measured. The lower the battery voltage, the better the water electrolysis efficiency.
[0130] (10) Water electrolysis durability test
[0131] After the test in (9), the load current was further increased to 50 A (current density 2 A / cm 2 ) was maintained for 200 hours, and the battery voltage was measured thereafter. The voltage increase after this endurance test is shown in Table 1. The smaller the voltage increase from the test (9), the better the durability.
[0132] 2. Synthesis example
[0133] [Synthesis Example 1] Synthesis of Block Copolymer b1
[0134] (Synthesis of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane (K-DHBP) represented by the following general formula (G1))
[0135]
[0136] In a 500 ml flask with a stirrer, a thermometer and a distillation tube, 49.5 g of 4,4'-dihydroxybenzophenone, 134 g of ethylene glycol, 96.9 g of trimethyl orthoformate and 0.50 g of p-toluenesulfonic acid monohydrate were placed and dissolved. After that, the mixture was stirred at 78°C to 82°C for 2 hours. Furthermore, the internal temperature was slowly raised to 120°C and heated until the distillation of methyl formate, methanol and trimethyl orthoformate completely stopped. After the reaction solution was cooled to room temperature, it was diluted with ethyl acetate, and the organic layer was washed with 100 mL of 5% potassium carbonate aqueous solution and separated, and the solvent was distilled off. 80 mL of dichloromethane was added to the residue to precipitate crystals, and 52.0 g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane was obtained by filtration and drying.
[0137] (Synthesis of 3,3'-sodium disulfonate-4,4'-difluorobenzophenone represented by the following general formula (G2))
[0138]
[0139] 109.1 g of 4,4'-difluorobenzophenone (Aldrich reagent) was reacted in 150 mL of fuming sulfuric acid (50% SO3) (Wako Pure Chemical Industries, Ltd. reagent) at 100°C for 10 hours. Then, a small amount was added to a large amount of water, and after neutralization with NaOH, 200 g of salt was added to precipitate the synthetic product. The obtained precipitate was filtered out and recrystallized with an ethanol aqueous solution to obtain 3,3'-sodium disulfonate-4,4'-difluorobenzophenone represented by the general formula (G2).
[0140] (Synthesis of the oligomer a1′ not containing an ionic group represented by the following general formula (G3))
[0141] In a 1000mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 16.59g of potassium carbonate (Aldrich reagent, 120mmol), 25.8g of K-DHBP (100mmol), and 20.3g of 4,4'-difluorobenzophenone (Aldrich reagent, 93mmol) were added. After nitrogen substitution, dehydration was performed at 160°C in 300mL of N-methylpyrrolidone (NMP) and 100mL of toluene, and the temperature was raised to remove toluene, and polymerization was performed at 180°C for 1 hour. Reprecipitation was performed using a large amount of methanol to purify, and oligomer a1 (terminal hydroxyl group) containing no ionic group was obtained. The number average molecular weight was 10000.
[0142] In a 500mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark water separator, 1.1g of potassium carbonate (Aldrich reagent, 8mmol) and 20.0g (2mmol) of the oligomer a1 (terminal hydroxyl group) containing no ionic group were added. After nitrogen substitution, dehydration was carried out at 100°C in 100mL of NMP and 30mL of cyclohexane. The cyclohexane was removed by heating, and 4.0g of decafluorobiphenyl (Aldrich reagent, 12mmol) was added and reacted at 105°C for 1 hour. Reprecipitation was carried out using a large amount of isopropanol, thereby purifying to obtain the oligomer a1' (terminal fluorine group) containing no ionic group represented by the following formula (G3). The number average molecular weight is 11000, and the number average molecular weight of the oligomer a1' containing no ionic group is 10400 obtained by subtracting the linker part (molecular weight 630).
[0143]
[0144] (Here, m is a positive integer)
[0145] (Synthesis of the Ionic Group-Containing Oligomer a2 Represented by the Following General Formula (G4))
[0146] In a 1000 mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark water trap, potassium carbonate 27.6 g (Aldrich reagent, 200 mmol), K-DHBP 12.9 g (50 mmol), 4,4'-biphenol 9.3 g (Aldrich reagent, 50 mmol), 3,3'-sodium disulfonate-4,4'-difluorobenzophenone 39.3 g (93 mmol) and 18-crown ether-6 17.9 g (82 mmol of Wako Pure Chemical Industries, Ltd.) were added, and after nitrogen substitution, dehydration was performed at 170°C in NMP 300 mL and toluene 100 mL, and the temperature was raised to remove toluene, and polymerization was performed at 180°C for 1 hour. Reprecipitation was performed using a large amount of isopropanol to purify, and an oligomer a2 (terminal hydroxyl group) containing an ionic group represented by the following formula (G4) was obtained. The number average molecular weight is 16000.
[0147]
[0148] (In formula (G4), M represents sodium or potassium; n is a positive integer)
[0149] (Synthesis of Block Polymer b1 Containing Oligomer a2 as Segment (A1) Containing Ionic Group, Oligomer a1 as Segment (A2) Not Containing Ionic Group, and Octafluorobiphenylene as Linking Site)
[0150] In a 500mL three-necked flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark water separator, 0.56g of potassium carbonate (Aldrich reagent, 4mmol) and 16g (1mmol) of oligomer a2 (terminal hydroxyl group) containing an ionic group were added. After nitrogen substitution, dehydration was carried out at 100°C in 100mL of NMP and 30mL of cyclohexane. The cyclohexane was removed by heating, and 11g (1mmol) of oligomer a1' (terminal fluorine group) containing no ionic group was added. The reaction was carried out at 105°C for 24 hours. Reprecipitation was performed using a large amount of isopropanol to purify the block copolymer b1. The weight average molecular weight is 340,000
[0151] The block copolymer b1 itself was used as a polymer electrolyte membrane. After being immersed in a 10 mass % sulfuric acid aqueous solution at 80°C for 24 hours for proton substitution and deprotection reaction, it was immersed in a large excess of pure water for 24 hours for thorough washing. At this time, the ion exchange capacity determined by neutralization titration was 2.12 meq / g.
[0152] [Synthesis Example 2] Synthesis of Block Copolymer b2
[0153] (Synthesis of a polyethersulfone (PES)-based block copolymer precursor b2′ containing a segment represented by the following formula (G6) and a segment represented by the following formula (G7))
[0154] 1.78 g of anhydrous nickel chloride and 15 mL of dimethyl sulfoxide were mixed and adjusted to 70° C. 2.37 g of 2,2′-bipyridine was added thereto, and the mixture was stirred at the same temperature for 10 minutes to prepare a nickel-containing solution.
[0155] Here, 1.64 g of 2,5-dichlorobenzenesulfonic acid (2,2-dimethylpropyl) ester and 0.55 g of polyethersulfone (Sumitomo Chemical Co., Ltd. manufactured by Sumitomo Chemical Co., Ltd. PES5200P, Mn=40,000, Mw=94,000) represented by the following formula (G5) are dissolved in 5 mL of dimethyl sulfoxide. 1.35 g of zinc powder is added to the solution obtained and adjusted to 70°C. The solution containing nickel is injected thereto and a polymerization reaction is carried out at 70°C for 4 hours. The reaction mixture is added to 60 mL of methanol, and then 60 mL of 6 mol / L hydrochloric acid is added and stirred for 1 hour. The precipitated solid is separated and dried by filtration, and 1.75 g of a block copolymer precursor b2' (polyarylene precursor) containing a segment represented by the following formula (G6) and the following formula (G7) is obtained with a yield of 97%. The weight average molecular weight is 210,000.
[0156]
[0157] (Here, n is independently a positive integer in formula (G5) and formula (G7))
[0158] (Synthesis of a polyethersulfone (PES)-based block copolymer b2 comprising a segment represented by the above formula (G7) and a segment represented by the following formula (G8))
[0159] 0.25 g of block copolymer precursor b2' was added to a mixed solution of 0.18 g of lithium bromide monohydrate and 8 mL of N-methyl-2-pyrrolidone, and reacted at 120°C for 24 hours. The reaction mixture was injected into 80 mL of 6 mol / L hydrochloric acid and stirred for 1 hour. The precipitated solid was separated by filtration. The separated solid was dried to obtain an off-white block copolymer b2 comprising a segment represented by formula (G7) and a segment represented by the following formula (G8). The weight average molecular weight of the obtained polyarylene was 190,000.
[0160] The block copolymer b2 itself was used as a polymer electrolyte membrane, and after being immersed in a 10 mass % sulfuric acid aqueous solution at 80°C for 24 hours for proton substitution, it was immersed in a large excess of pure water for 24 hours for sufficient washing. At this time, the ion exchange capacity determined by neutralization titration was 2.02 meq / g.
[0161]
[0162] [Synthesis Example 3] Synthesis of Block Copolymer b3
[0163] (Synthesis of the hydrophobic oligomer a3 represented by the following formula (G9))
[0164]
[0165] (Here, k is a positive integer)
[0166] In a 1 L three-necked flask equipped with a stirrer, a thermometer, a cooling tube, a Dean-Stark tube, and a three-way stopcock for nitrogen inlet, 51.9 g (0.30 mol) of 2,6-dichlorobenzonitrile, 92.8 g (0.27 mol) of 2,2-bis(4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, and 49.7 g (0.36 mol) of potassium carbonate were weighed.
[0167] After nitrogen replacement, 363 mL of sulfolane and 181 mL of toluene were added and stirred. The flask was immersed in an oil bath and heated to reflux at 150°C. The water generated by the reaction was azeotroped with toluene, and the reaction was performed while removing it outside the system using a Dean-Stark tube. After about 3 hours, almost no water was confirmed to be generated. After slowly increasing the reaction temperature and removing most of the toluene, the reaction was continued at 200°C for 3 hours. Next, 12.9 g (0.076 mol) of 2,6-dichlorobenzonitrile was added and the reaction was continued for 5 hours.
[0168] The obtained reaction solution was left to cool, and then 100 mL of toluene was added for dilution. The precipitate of the inorganic compound produced as a byproduct was filtered out, and the filtrate was put into 2 L of methanol. The precipitated product was filtered out, recovered and dried, and then dissolved in 250 mL of tetrahydrofuran. It was reprecipitated in 2 L of methanol to obtain 109 g of the target oligomer. The number average molecular weight of the oligomer was 8,000.
[0169] (Synthesis of the hydrophilic monomer represented by the following formula (G10))
[0170]
[0171] In a 3L three-necked flask with a stirrer and a cooling tube, 245g (2.1mol) of chlorosulfonic acid was added, followed by 105g (420mmol) of 2,5-dichlorobenzophenone, and the mixture was reacted in an oil bath at 100°C for 8 hours. After a prescribed time, the reaction solution was slowly injected into 1000g of crushed ice and extracted with ethyl acetate. The organic layer was washed with saline and dried with magnesium sulfate, and ethyl acetate was distilled off to obtain pale yellow crude crystals of 3-(2,5-dichlorobenzoyl)benzenesulfonyl chloride. The crude crystals were not purified and were used directly in the next step.
[0172] 41.1 g (462 mmol) of 2,2-dimethyl-1-propanol (neopentyl alcohol) is added to 300 mL of pyridine and cooled to about 10°C. Here, it takes about 30 minutes to slowly add the obtained crude crystals. After the full amount is added, stir for 30 minutes to react. After the reaction, the reaction solution is injected into 1000 mL of hydrochloric acid water to recover the precipitated solid. The obtained solid is dissolved in ethyl acetate, washed with sodium bicarbonate aqueous solution and brine, dried with magnesium sulfate, and then ethyl acetate is distilled off to obtain crude crystals. It is recrystallized with methanol to obtain white crystals of 3-(2,5-dichlorobenzoyl)benzenesulfonic acid neopentyl ester represented by the structural formula.
[0173] (Synthesis of polyarylene block copolymer b3 represented by the following formula (G11))
[0174]
[0175] (Here, k, m, and n are each independently a positive integer)
[0176] In a 1L three-necked flask connected to a stirrer, a thermometer, and a nitrogen inlet tube, under nitrogen, 166 mL of dry N,N-dimethylacetamide (DMAc) was added to a mixture of 15.1 g (1.89 mmol) of the hydrophobic oligomer a3, 39.5 g (98.4 mmol) of 3-(2,5-dichlorobenzoyl)benzenesulfonic acid neopentyl ester, 2.75 g (4.2 mmol) of bis(triphenylphosphine)dichloronickel, 11.0 g (42.1 mol) of triphenylphosphine, 0.47 g (3.15 mmol) of sodium iodide, and 16.5 g (2.53 mmol) of zinc.
[0177] The reaction system was heated under stirring (finally heated to 82°C) and reacted for 3 hours. The viscosity in the system was observed to rise during the reaction. The polymerization reaction solution was diluted with 180mL of DMAc, stirred for 30 minutes, and cerium silica was used as a filter aid for filtration. In a 1L 3-necked flask equipped with a stirrer, 25.6g (295 mmol) of lithium bromide was added to the filtrate in 1 / 3 each time, divided into 3 times and each time with an interval of 1 hour, and it was reacted for 5 hours at 120°C under a nitrogen environment. After the reaction, it was cooled to room temperature and injected into 4L of acetone for coagulation. After filtering and air-drying the coagulant, it was crushed by a mixer and washed with 1N sulfuric acid 1500mL while stirring. After filtering, the product was washed with ion exchange water until the pH of the washing liquid became 5 or more, and then dried at 80°C for one night to obtain the target block copolymer b3. The weight average molecular weight of this block copolymer is 200,000.
[0178] The block copolymer b3 itself was used as a polymer electrolyte membrane, and after being immersed in a 10 mass % sulfuric acid aqueous solution at 80°C for 24 hours for proton substitution, it was immersed in a large excess of pure water for 24 hours for sufficient washing. At this time, the ion exchange capacity determined by neutralization titration was 2.38 meq / g.
[0179] [Synthesis Example 4] Synthesis of random copolymer r1
[0180] (Synthesis of Polyketal Ketone Random Copolymer r1 Comprising Monomer Represented by Formula (G1), 4,4'-difluorobenzophenone and Monomer Represented by Formula (G2))
[0181] In a 500mL three-necked flask with a stirrer, a nitrogen inlet tube, and a Dean-Stark water separator, potassium carbonate 13.82g (Aldrich reagent, 100mmol), K-DHBP 20.66g (80mmol) obtained as the intermediate product of the synthesis example 1, 4,4'-difluorobenzophenone 10.5g (Aldrich reagent, 48mmol) and 3,3'-disulfonic acid sodium-4,4'-difluorobenzophenone 13.5g (32mmol) obtained as the intermediate product of the synthesis example 1 were added, and after nitrogen substitution, dehydration was carried out at 180°C in N-methylpyrrolidone (NMP) 100mL and toluene 50mL, and the temperature was raised to remove toluene, and polymerization was carried out at 230°C for 6 hours. Reprecipitation was performed using a large amount of water to purify and obtain a polyketal ketone random copolymer. The weight average molecular weight is 250,000.
[0182] The random copolymer r1 itself was used as a polymer electrolyte membrane. It was immersed in a 10 mass % sulfuric acid aqueous solution at 80°C for 24 hours for proton substitution and deprotection reaction. It was then immersed in a large excess of pure water for 24 hours for thorough washing. At this time, the ion exchange capacity determined by neutralization titration was 1.51 meq / g.
[0183] [Example 1]
[0184] 20 g of the block copolymer b1 obtained in Synthesis Example 1 was dissolved in 80 g of NMP, and stirred at 20,000 rpm for 1 hour using a stirrer to prepare a transparent polymer electrolyte solution b1 having a polymer concentration of 20% by mass.
[0185] After the obtained polymer electrolyte solution b1 was pressure filtered using a glass fiber filter, the polymer electrolyte solution b1 was cast onto a polyethylene terephthalate (PET) substrate using an applicator and dried at 100°C for 4 hours to obtain a thin film of polymer. After being immersed in a 10 mass % sulfuric acid aqueous solution at 80°C for 24 hours for proton substitution and deprotection reaction, it was immersed in a large amount of excess pure water for 24 hours for thorough washing, and dried at room temperature to obtain a first layer (film thickness 50 μm).
[0186] On one side of the obtained first layer, a rod coater is used to apply Nafion as a fluorine-based polymer electrolyte (the commercially available D2020 solution manufactured by Chemours is used by replacing NMP) and W#9300 (weight average molecular weight>1 million) manufactured by Kureha, which is commercially available as polyvinylidene fluoride, dissolved in NMP to obtain a polymer electrolyte solution A (solid content ratio: fluorine-based polymer electrolyte / polyvinylidene fluoride = 60 mass% / 40 mass%, solid content concentration 10 mass%), and dried at 120°C for 2 hours to form a layer, which is immersed in a large amount of excess pure water for 24 hours and fully washed, and dried at room temperature to make a second layer, thereby obtaining a laminated electrolyte membrane (film thickness 55μm). The thickness of the mixed area of the obtained laminated electrolyte membrane is 1.8μm.
[0187] [Example 2]
[0188] A laminated electrolyte membrane (membrane thickness: 55 μm) was obtained in the same manner as in Example 1 except that 0.1 mass % of platinum fine particles (average particle size: 5 nm) were added to the polymer electrolyte solution A.
[0189] [Example 3]
[0190] A 20 mass % solution of Nafion (D2020 solution commercially available from Chemours) containing 0.2 mass % of platinum particles (average particle size 5 nm) was applied to the surface of the second layer of the stacked electrolyte membrane obtained in Example 1 on the side where the first layer was not provided, using a rod coater, and the mixture was dried at 100°C for 1 hour to produce a third layer, thereby obtaining a stacked electrolyte membrane (membrane thickness 65 μm).
[0191] [Example 4]
[0192] A laminated electrolyte membrane (film thickness 55 μm) was obtained in the same manner as in Example 1 except that commercially available W#7200 (weight average molecular weight = 630,000) manufactured by Kureha was used as polyvinylidene fluoride instead of commercially available W#9300 manufactured by Kureha.
[0193] [Example 5]
[0194] A laminated electrolyte membrane (membrane thickness 55 μm) was obtained in the same manner as in Example 1 except that commercially available W#1100 (weight average molecular weight = 280,000) manufactured by Kureha was used as polyvinylidene fluoride instead of commercially available W#9300 manufactured by Kureha.
[0195] [Example 6]
[0196] A laminated electrolyte membrane (membrane thickness: 55 μm) was obtained in the same manner as in Example 1 except that the solid content ratio of the polymer electrolyte solution A was fluorine-based polymer electrolyte / polyvinylidene fluoride=90 mass % / 10 mass %.
[0197] [Example 7]
[0198] A laminated electrolyte membrane (membrane thickness: 55 μm) was obtained in the same manner as in Example 1 except that the solid content ratio of the polymer electrolyte solution A was fluorine-based polymer electrolyte / polyvinylidene fluoride=20 mass % / 80 mass %.
[0199] [Example 8]
[0200] A laminated electrolyte membrane (membrane thickness 80 μm) was obtained in the same manner as in Example 1 except that the thickness of the second layer was 30 μm.
[0201] [Example 9]
[0202] A laminated electrolyte membrane (membrane thickness: 50.5 μm) was obtained in the same manner as in Example 1 except that the thickness of the second layer was 0.5 μm.
[0203] [Example 10]
[0204] A laminated electrolyte membrane (film thickness: 11 μm) was obtained in the same manner as in Example 1 except that the thickness of the first layer was 10 μm and the thickness of the second layer was 1 μm.
[0205] [Example 11]
[0206] A laminated electrolyte membrane (membrane thickness: 55 μm) was obtained in the same manner as in Example 1 except that the block copolymer b2 obtained in Synthesis Example 2 was used instead of the block copolymer b1.
[0207] [Example 12]
[0208] A laminated electrolyte membrane (membrane thickness: 55 μm) was obtained in the same manner as in Example 1 except that the block copolymer b3 obtained in Synthesis Example 3 was used instead of the block copolymer b1.
[0209] [Example 13]
[0210] A laminated electrolyte membrane (membrane thickness: 55 μm) was obtained in the same manner as in Example 1 except that the random copolymer r1 obtained in Synthesis Example 4 was used instead of the block copolymer b1.
[0211] [Example 14]
[0212] A laminated electrolyte membrane (membrane thickness 55 μm) was obtained in the same manner as in Example 1 except that the solid content ratio of the polymer electrolyte solution A was fluorine-based polymer electrolyte / polyvinylidene fluoride=95% by mass / 5% by mass.
[0213] [Example 15]
[0214] A laminated electrolyte membrane (membrane thickness: 55 μm) was obtained in the same manner as in Example 1 except that the solid content ratio of the polymer electrolyte solution A was fluorine-based polymer electrolyte / polyvinylidene fluoride=5% by mass / 95% by mass.
[0215] [Example 16]
[0216] A laminated electrolyte membrane (film thickness 55 μm) was obtained in the same manner as in Example 1 except that commercially available W#7300 (weight average molecular weight>1,000,000) manufactured by Kureha was used as polyvinylidene fluoride instead of commercially available W#9300 manufactured by Kureha.
[0217] [Comparative Example 1]
[0218] The first single-layer electrolyte membrane (membrane thickness 50 μm) was obtained by the same method as described in the first paragraph of Example 1. The initial performance was relatively good, but the durability was poor, so the longer the use, the more disadvantageous it became.
[0219] [Comparative Example 2]
[0220] A laminated electrolyte membrane (55 μm) was obtained in the same manner as in Example 1 except that a 20 mass% NMP solution of Nafion (a commercially available D2020 solution manufactured by Chemours was replaced with NMP) was used instead of the polymer electrolyte solution A. In the dried laminated electrolyte membrane, the first layer and the second layer peeled off.
[0221] [Comparative Example 3]
[0222] A laminated electrolyte membrane (55 μm) was obtained in the same manner as in Example 1, except that a polymer electrolyte solution B was used instead of the polymer electrolyte solution A, which was prepared by mixing a commercially available Nafion solution, a D2020 solution manufactured by Chemours, a commercially available polyvinylidene fluoride solution, a commercially available KYNAR LATEX RC-10,278 manufactured by Alkema, and a solvent in which water and isopropyl alcohol (IPA) were in a mass ratio of 1:1 in a mass ratio of 2.3:1:4.3.
[0223] The laminated electrolyte membrane produced in this example does not form a mixed region.
[0224] [Comparative Example 4]
[0225] A commercially available Nafion solution, D2020 solution manufactured by Chemours, was cast onto a PET substrate and dried at 100° C. for 1 hour to obtain a first layer (film thickness 50 μm).
[0226] On one side of the obtained first layer, a polymer electrolyte solution B (solid content ratio: block copolymer b1 / polyvinylidene fluoride = 60 mass% / 40 mass%, solid content concentration 10 mass%) obtained by dissolving block copolymer b1 and W#9300 manufactured by Kureha, which is commercially available as polyvinylidene fluoride, in NMP was applied by a rod coater, and dried at 120°C for 2 hours to form a layer. After immersion in a 10 mass% sulfuric acid aqueous solution at 80°C for 24 hours for proton substitution and deprotection reaction, it was immersed in a large amount of excess pure water for 24 hours and fully washed, and dried at room temperature to prepare a second layer, thereby obtaining a laminated electrolyte membrane (film thickness 55 μm). Peeling of the first layer and the second layer occurred in the dried laminated electrolyte membrane.
[0227] [Comparative Example 5]
[0228] A nafion membrane (membrane thickness: 50 μm) was obtained by the same method as described in the previous section of Comparative Example 4. Table 1 shows the constitution and physical properties of the polymer electrolyte membranes used in each of the Examples and Comparative Examples, and the results of the hydrogen compression evaluation and the water electrolysis evaluation.
[0229] Table 1
[0230]
[0231] In the first layer "Polymer Electrolyte" in the table, b1 represents block copolymer b1, b2 represents block copolymer b2, b3 represents block copolymer b3, and r1 represents random copolymer r1.
[0232] This application claims the priority based on Japanese Patent Application No. 2019-063208 filed on March 28, 2019, and all the contents described in the claims and specification attached to the application of this Japanese patent application are incorporated herein by reference.
[0233] Description of the accompanying drawings
[0234] 1: First layer
[0235] 2: Second layer
[0236] 3: Mixed Area
Claims
1. A laminated electrolyte membrane, comprising: a first layer having a hydrocarbon-based polymer electrolyte as a main component and a second layer having a fluorine-based polymer electrolyte and polyvinylidene fluoride as main components laminated on at least one side thereof, wherein the first layer and the second layer are laminated via a region where the constituent components of the two layers are mixed, hereinafter referred to as a mixed region, The thickness of the mixed region is 1.0 μm or more and is 80% or less of the total thickness of the first layer and the second layer, and is thick enough not to expose the hydrocarbon-based polymer electrolyte to the surface. The thickness of the second layer is 1% or more and 40% or less of the thickness of the first layer. 2 . The laminated electrolyte membrane according to claim 1 , wherein a third layer having a fluorine-based polymer electrolyte as a main component is laminated on a surface of the second layer opposite to the first layer. 3 . The laminated electrolyte membrane according to claim 1 , wherein at least one of the first layer and the second layer contains platinum. 4 . The laminated electrolyte membrane according to claim 2 , wherein the first layer and at least one of the second layer and the third layer contain platinum. 5 . The laminated electrolyte membrane according to claim 1 , wherein the content of polyvinylidene fluoride contained in the second layer is 20 to 90% by mass when the total mass of the fluorine-based polymer electrolyte and polyvinylidene fluoride is 100% by mass. 6 . The laminated electrolyte membrane according to claim 1 , wherein the weight average molecular weight of the polyvinylidene fluoride is 300,000 or more. 7 . The laminated electrolyte membrane according to claim 1 , wherein the peeling force between the first layer and the second layer is 0.3 N or more. 8 . The laminated electrolyte membrane according to claim 1 , wherein the hydrocarbon-based polymer electrolyte contains a polyetherketone-based polymer having an ionic group as a main component. 9 . A laminated electrolyte membrane with catalyst layers, comprising: a laminated electrolyte membrane according to claim 1 having an anode catalyst layer on one surface thereof and a cathode catalyst layer on the opposite surface thereof. 10 . The catalyst layer-carrying laminated electrolyte membrane according to claim 9 , wherein a second layer is laminated between the first layer and the anode catalyst layer. 11 . A membrane electrode assembly comprising an anode power supply stacked on an anode catalyst layer of the laminated electrolyte membrane with a catalyst layer according to claim 9 or 10, and a cathode power supply stacked on a cathode catalyst layer.
12. The membrane electrode assembly according to claim 11, wherein the anode power supply is composed of an inorganic conductive material.
13. A water electrolysis type hydrogen generation device, produced by using the laminated electrolyte membrane according to any one of claims 1 to 8.
14. A water electrolysis type hydrogen generation device, produced by using the laminated electrolyte membrane with a catalyst layer according to claim 9 or 10.
15. A water electrolysis type hydrogen generation device, produced by using the membrane electrode assembly according to claim 11 or 12.
16. A method for manufacturing a laminated electrolyte membrane, comprising the following steps a and b, Step a: forming a first layer including a hydrocarbon-based polymer electrolyte, Step b: forming a second layer and a mixed region having a thickness of 1.0 μm or more between the first layer and the second layer by coating a solution A prepared by dissolving a fluorine-based polymer electrolyte and polyvinylidene fluoride in an aprotic polar solvent on the first layer, wherein: The thickness of the mixed region is 80% or less of the total thickness of the first layer and the second layer and is thick enough not to expose the hydrocarbon-based polymer electrolyte to the surface. The thickness of the second layer is 1% to 40% of the thickness of the first layer.