Low cis polybutadiene rubber and preparation method thereof, HIPS and preparation method thereof

By performing anionic solution polymerization reaction in an inert solvent and terminating the reaction, the prepared low cis polybutadiene rubber is used as a toughener for HIPS resin, which solves the difficulty of gloss and impact resistance of HIPS resin in the continuous polymerization process of single reactors. The problems of both consideration have been taken into account, and more balanced performance and halogenation-free process have been achieved.

CN113461857BActive Publication Date: 2024-11-19CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010244096.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-03-31
Publication Date
2024-11-19
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

The HIPS resin obtained by toughening of low cis polybutadiene rubber prepared by the existing single reactor continuous polymerization process is difficult to obtain balanced gloss and impact resistance simultaneously.

Method used

A low cis polybutadiene rubber is used, in which the content of 1,2-polymerized structural unit is 8-20% by weight, the number average molecular weight is 70,000-90,000 g/mol, the molecular weight distribution coefficient is 2.25-2.65, at 100°C At the time of Mooney's viscosity ML1+4 is 40-60, and at 25°C, the viscosity of 5% styrene solution is 40-66 cp. The anionic solution polymerization reaction is carried out in an inert solvent, and inhibited in an organic lithium initiator and gel. In the presence of a agent and a structural regulator, the termination reaction is carried out to prepare a star polymer.

Benefits of technology

The balance of gloss and impact resistance of HIPS resin is achieved, and the problem of difficult to take into account gloss and impact resistance in the continuous polymerization process of single reactor is solved, while avoiding corrosion problems in the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the field of HIPS resin, and discloses a low-cis polybutadiene rubber and a preparation method thereof, and a HIPS resin and a preparation method thereof. The low-cis polybutadiene rubber has a 1,2-polymerization structural unit content of 8-20 wt %; a number average molecular weight of 70,000-90,000 g / mol; a molecular weight distribution coefficient of 2.25-2.65; and a Mooney viscosity ML at 100°C. 1+4 The viscosity of the 5 wt% styrene solution at 25°C is 40-66cp. The low cis polybutadiene rubber is used as a toughening agent to obtain a HIPS resin with more balanced impact resistance and gloss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of synthetic rubber and resin, in particular to low-cis polybutadiene rubber and a preparation method thereof, and HIPS resin and a preparation method thereof. Background Art

[0002] The use of different toughening rubbers will have a significant impact on the performance of HIPS resin. Theoretically, LCBR rubber, high cis polybutadiene rubber, styrene butadiene rubber and styrene-butadiene-styrene thermoplastic elastomer are the types of rubber commonly used in the continuous bulk process to prepare HIPS resin.

[0003] Toughening rubber cannot choose a cross-linked structure because cross-linked rubber cannot undergo a grafting reaction. In the traditional bulk process, high cis polybutadiene rubber is used. High cis polybutadiene rubber has a low glass transition temperature, is easy to relax, and has good impact resistance, but has a tendency to crystallize at low temperatures, which is not conducive to improving low-temperature toughness. For low-temperature toughness HIPS resin, LCBR is the best toughening agent because it has moderate vinyl content, low gel content, and randomly distributed molecular chain cis-trans 1,4 structures.

[0004] According to different processes, LCBR rubber is divided into intermittent polymerization products and continuous polymerization products. Intermittent polymerization process is flexible. After the polymerization, a multifunctional coupling agent is generally used for coupling reaction to balance the product Mooney viscosity and 5% styrene viscosity. In the continuous polymerization process, due to the continuous material transportation, when there is only one reactor, the termination coupling agent cannot be introduced during the polymerization process, otherwise the active chain will be terminated by the coupling agent, and the ideal branched polymerization product cannot be obtained.

[0005] The continuous polymerization products on the market are divided into two categories, namely, single-reactor continuous polymerization process and three-reactor continuous polymerization process. The former is represented by Japan's Asahi Kasei Corporation. No branching agent is added during the polymerization process. Its products are linear structures and cannot achieve a balance between Mooney viscosity and 5% styrene solution viscosity. It is difficult to balance gloss and impact resistance at the same time when modifying HIPS. The latter is represented by Arlanxeo. The polymerization reaction is carried out in the first reactor, the coupling reaction is carried out in the second reactor, and the termination reaction is carried out in the third reactor. This process is long, the investment is large, and the floor space is large. In addition, this type of product uses chlorine-containing silane as a coupling agent. Chloride ions enter the condensed water and colloid particles in the post-processing stage, corroding the post-processing equipment. Summary of the invention

[0006] The purpose of the present invention is to overcome the defect that the HIPS resin toughened with low-cis polybutadiene rubber prepared by the single-reactor continuous polymerization process in the prior art is difficult to obtain a HIPS resin with more balanced gloss and impact resistance, and to provide a continuous star-shaped low-cis polybutadiene rubber as a toughening agent and a preparation method thereof, and a HIPS resin and a preparation method thereof, which can obtain a HIPS resin with more balanced gloss and impact resistance.

[0007] In order to achieve the above-mentioned object, the first aspect of the present invention provides a low-cis polybutadiene rubber, wherein the content of 1,2-polymerized structural units in the low-cis polybutadiene rubber is 8-20% by weight; the number average molecular weight is 70,000-90,000 g / mol; the molecular weight distribution coefficient is 2.25-2.65; the Mooney viscosity ML at 100°C is 0.1-0.2%. 1+4 The viscosity of 5 wt% styrene solution at 25°C is 40-66cp.

[0008] The second aspect of the present invention provides a method for preparing the low-cis polybutadiene rubber, wherein the method comprises:

[0009] (1) in an inert solvent, in the presence of an organic lithium initiator, a gel inhibitor and a structure regulator, 1,3-butadiene and a branched monomer are continuously introduced into a reactor from the bottom of the reactor to perform an anionic solution polymerization reaction until the conversion rate of 1,3-butadiene reaches more than 99%;

[0010] (2) contacting the mixture obtained in step (1) with a terminator to terminate the reaction.

[0011] A third aspect of the present invention provides a method for preparing a HIPS resin, the method comprising:

[0012] (1) providing a low-cis polybutadiene rubber solution, wherein the low-cis polybutadiene rubber solution contains the low-cis polybutadiene rubber obtained by the above method;

[0013] (2) In the presence of a free radical initiator, polymerizing styrene and a toughening agent; wherein the toughening agent comprises the low-cis polybutadiene rubber solution obtained in step (1).

[0014] The fourth aspect of the present invention provides a HIPS resin prepared by the above method.

[0015] The low-cis polybutadiene rubber of the present invention realizes the balanced control of Mooney viscosity and 5% styrene solution viscosity of low-cis polybutadiene rubber (LCBR) continuously polymerized in a single reactor, and as a toughening agent of HIPS resin, the HIPS resin has more balanced gloss and impact resistance. In particular, the viscosity of the 5% by weight styrene solution of the low-cis polybutadiene rubber provided by the present invention at 25° C. is below 66 cp, and the obtained HIPS resin has higher gloss.

[0016] The preparation method of low cis polybutadiene rubber provided by the invention comprises the following steps: adding a branching monomer from the bottom of a reaction container and copolymerizing the monomer with 1,3-butadiene to prepare a star polymer, thereby balancing the relationship between the rubber Mooney viscosity and the viscosity of a 5 wt% styrene solution at 25° C., solving the problem that the impact resistance and glossiness of a HIPS resin prepared by a single reactor continuous polymerization process from a low cis polybutadiene rubber (LCBR) cannot be taken into account at the same time, and at the same time, the process is halogen-free, solving the corrosion problem in the preparation process. DETAILED DESCRIPTION

[0017] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0018] According to the first aspect of the present invention, the present invention provides a low-cis polybutadiene rubber, wherein the content of 1,2-polymerized structural units in the low-cis polybutadiene rubber is 8-20% by weight; the number average molecular weight is 70,000-90,000; the molecular weight distribution coefficient is 2.25-2.65; the Mooney viscosity ML at 100°C is 1+4 The viscosity of 5 wt% styrene solution at 25°C is 40-66cp.

[0019] In the present invention, the butadiene monomers forming the low-cis polybutadiene rubber mainly refer to 1,3-butadiene, unless otherwise specified. The polymerization form of 1,3-butadiene generally includes the 1,2-polymerization form, thereby forming the 1,2-polymerization structural unit (-[CH 2 -CH 2 (CH=CH 2 )]-), including 1,4-polymerized forms, thereby forming 1,4-polymerized structural units (-[CH 2 -CH=CH-CH 2]-). Wherein, the content of the 1,2-polymer structural unit is 8-20% by weight, so that the grafting reaction of the continuous bulk HIPS resin can be guaranteed. When the content of the 1,2-polymer structural unit is less than 8% by weight, it will be unfavorable for the subsequent grafting reaction in the preparation of the subsequent HIPS resin; when the content of the 1,2-polymer structural unit is greater than 20% by weight, cross-linking points are easily formed, which is not conducive to the improvement of impact resistance. Preferably, the content of the 1,2-polymer structural unit in the low-cis polybutadiene rubber is 9-18% by weight, more preferably 10-16% by weight.

[0020] While satisfying the above-mentioned content range of 1,2-polymer structural units, the content of cis-1,4-polymer structural units is preferably 20-40% by weight, more preferably 25-40% by weight, and further preferably 30-40% by weight; the content of trans-1,4-polymer structural units is preferably 40-60% by weight, more preferably 45-60% by weight, and further preferably 50-60% by weight.

[0021] According to the present invention, the low cis polybutadiene rubber is 70,000-90,000 g / mol, and the purpose of such setting is to control the Mooney viscosity and the viscosity of the 5 wt% styrene solution to remain in an appropriate range, so as to better balance the relationship between the Mooney viscosity and the viscosity of the 5 wt% styrene solution; wherein, when the number average molecular weight of the low cis polybutadiene rubber is less than 70,000 g / mol, the Mooney viscosity requirement of the product low cis polybutadiene rubber cannot be met, and the processing performance of the low cis polybutadiene rubber is not good, and the impact strength of the HIPS resin is poor; when the number average molecular weight of the low cis polybutadiene rubber is greater than 90,000 g / mol, the viscosity requirement of the product low cis polybutadiene rubber 5% styrene solution cannot be met, and the gloss of the HIPS resin is not good. Preferably, the number average molecular weight of the low cis polybutadiene rubber is 73,000-88,000 g / mol, and more preferably 75,000-85,000 g / mol.

[0022] The low cis polybutadiene rubber of the present invention has a suitable molecular weight distribution coefficient, which is conducive to controlling the relative proportion of branched rubber and linear rubber to balance the relationship between Mooney viscosity and 5% styrene solution viscosity. When the molecular weight distribution coefficient of low cis polybutadiene rubber is less than 2.25, the product is not branched enough, and the linear product accounts for a large proportion, resulting in a low Mooney viscosity of low cis polybutadiene rubber; when the molecular weight distribution coefficient of low cis polybutadiene rubber is greater than 2.65, the product branched product accounts for a high proportion, and the Mooney viscosity exceeds the upper limit of low cis polybutadiene rubber. Preferably, the molecular weight distribution coefficient is 2.28-2.55, more preferably 2.3-2.55.

[0023] In the present invention, the molecular weight and molecular weight distribution index of low cis polybutadiene rubber are determined by gel permeation chromatography, and the gel permeation chromatography analysis adopts HLC-8320 gel permeation chromatograph of Tosoh Corporation of Japan, the chromatographic column is TSKgel SuperMultiporeHZ-N, TSKgel SuperMultiporeHZ standard column, the solvent is chromatographic pure tetrahydrofuran (THF), narrow distribution polystyrene is used as standard sample, the polymer sample is prepared into a tetrahydrofuran solution with a mass concentration of 1 mg / mL, the injection volume is 10.00 μL, the flow rate is 0.35 mL / min, and the test temperature is 40.0°C.

[0024] According to the present invention, the Mooney viscosity ML of the low cis polybutadiene rubber of the present invention at 100°C is 1+4 The Mooney viscosity of low cis polybutadiene rubber at 100°C is ML 40-60, in order to ensure the processing performance of low cis polybutadiene rubber and better balance the gloss and impact strength of HIPS. 1+4 Less than 40, low cis polybutadiene rubber has poor processing performance and affects the impact resistance of HIPS; Mooney viscosity ML at 100°C 1+4 When the viscosity is higher than 60, the low cis polybutadiene rubber is easy to plasticize during the drying stage, which affects the product quality. Preferably, the Mooney viscosity of the low cis polybutadiene rubber at 100°C is ML 1+4 It is 40-58, more preferably 45-55.

[0025] In the present invention, the Mooney viscosity is measured using a GT-7080-S2 Mooney viscometer produced by Gotech Corporation of Taiwan, China, in accordance with GB / T1232.1 standard, wherein the preheating time is 1 min, the rotation time is 4 min, and the test temperature is 100°C.

[0026] According to the present invention, the viscosity of the 5 wt% styrene solution of the low cis polybutadiene rubber at 25° C. is 40-66 cp, preferably 42-66 cp, and more preferably 44-58 cp. Controlling the viscosity of the 5 wt% styrene solution of the low cis polybutadiene rubber at 25° C. within the above range and preferred range can balance the relationship between the gloss and impact resistance of the obtained HIPS resin.

[0027] The viscosity of 5 wt% rubber styrene solution at 25°C was measured using Beijing Yanshan Petrochemical Company corporate standard Q / SH3155.SXL.C26-2019 and a Finn viscometer was used at a constant temperature of 25°C.

[0028] According to the present invention, the low cis polybutadiene rubber of the present invention can obtain a lower gel content. Preferably, the gel content of the low cis polybutadiene rubber is below 400 ppm, preferably below 200 ppm, and more preferably below 150 ppm. The solvent system and gel inhibitor used in the present invention can effectively avoid the accumulation of active macromolecular chains in the reactor and avoid the generation of gel in the polymerization stage, and the gel content is extremely low.

[0029] In the present invention, the gel content is determined by the weight method tested by Beijing Yanshan Petrochemical Company Enterprise Standard Q / SH3155.SXL.C27-2019. The specific process is as follows: add the polymer sample to styrene, oscillate in an oscillator at a temperature of 25°C for 16 hours to completely dissolve the soluble matter, and prepare a styrene solution containing a polymer content of 5% by weight, and record the mass of the polymer sample as C (in grams); weigh a 400-mesh clean nickel mesh, and record the mass of the clean nickel mesh as B (in grams); then filter the above solution with a nickel mesh; rinse the nickel mesh with styrene after filtration, dry the nickel mesh at 150°C and normal pressure for 30 minutes, weigh it, and record its mass as A (in grams); calculate the gel content according to the following formula:

[0030] Gel content % = [(AB) / C] x 100%.

[0031] According to the present invention, the low-cis polybutadiene rubber of the present invention can obtain lower chromaticity. Preferably, the chromaticity of the low-cis polybutadiene rubber in a 5 wt% styrene solution is lower than 5, preferably below 0, and more preferably below -2.

[0032] The chromaticity was tested using a desktop colorimeter HunterLab ColorFlex from HunterLab, USA, in accordance with the Q / SH3155.SXL.C29-2019 standard; the test conditions were: the colorimetric system adopted was CIELAB, the optical geometry was 45° / 0°, the light source was C light source, the observation angle was 2°, and the sample thickness was approximately 15 mm.

[0033] The second aspect of the present invention provides a method for preparing the low-cis polybutadiene rubber, wherein the method comprises:

[0034] (1) in an inert solvent, in the presence of an organic lithium initiator, a gel inhibitor and a structure regulator, 1,3-butadiene and a branched monomer are continuously introduced into a reactor from the bottom of the reactor to perform an anionic solution polymerization reaction until the conversion rate of 1,3-butadiene reaches more than 99%;

[0035] (2) contacting the mixture obtained in step (1) with a terminator to terminate the reaction.

[0036] According to the present invention, the method for preparing the low-cis polybutadiene rubber adopts a continuous reaction mode. The method can be carried out in a conventional reactor in the art, and the volume of the reactor can be reasonably selected according to the output of the target product and the amount of raw materials. Generally, the volume of the reactor can be 10-10000L.

[0037] The inventors of the present invention have found in their research that aromatic vinyl monomers can be used as branching monomers to copolymerize with 1,3-butadiene to prepare star-shaped polymers, thereby balancing the rubber Mooney viscosity and the viscosity of a 5 wt% styrene solution at 25°C. Furthermore, the inventors of the present invention have also found that the position of adding the branching monomers will affect the molecular weight and molecular weight distribution of the final product, low cis-polybutadiene rubber, thereby affecting the Mooney viscosity of the product and the viscosity of a 5 wt% styrene solution at 25°C, and further affecting the impact resistance and gloss of the HIPS product.

[0038] According to the present invention, 1,3-butadiene and branching monomers are respectively continuously introduced into the reactor from the bottom of the reactor to carry out anionic solution polymerization. The shape of the reactor can be any conventional shape in the art, as long as the branching monomers and 1,3-butadiene undergo branching reaction.

[0039] According to the present invention, the inert solvent refers to an inert solvent that does not participate in the polymerization reaction. The inert solvent can be a C5-C8 cycloalkane and / or a C5-C9 alkane, preferably one or more of cyclohexane, methylcyclopentane, methylcyclohexane, methylpentane, n-hexane, n-heptane and isooctane.

[0040] The amount of the inert solvent used in the present invention can be reasonably selected according to the amount of the monomer and the control requirements of the polymerization temperature, and the amount can vary in a wide range. Based on the total weight of 100g of 1,3-butadiene monomer, the amount of the inert solvent used can be 400-900g.

[0041] According to the present invention, the inert solvent is preferably added from the bottom of the reactor together with 1,3-butadiene, so as to avoid excessive concentration of local monomers and formation of gel, thereby ensuring the quality of LCBR rubber and making the final HIPS product have better comprehensive performance.

[0042] According to the present invention, there is no particular limitation on the organic lithium initiator, and various organic lithium initiators conventionally used in the art for preparing polybutadiene rubber can be used. Preferably, the organic lithium initiator is a compound represented by the formula RLi, wherein R is selected from a C1-C20 alkyl group, a C6-C20 cycloalkyl group or a C6-C20 aryl group, preferably a C1-C10 alkyl group, a C6-C8 cycloalkyl group or a C6-C8 aryl group; more preferably, the organic lithium initiator is one or more of methyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, isobutyl lithium, tert-butyl lithium, cyclohexyl lithium, 4-cyclohexylbutyl lithium, phenyl lithium, triphenylmethyl lithium and 2-naphthyl lithium. Considering the solubility and storage stability of the initiator in an inert solvent, n-butyl lithium and / or sec-butyl lithium are more preferred, and n-butyl lithium is further preferred. The organic lithium initiator is added to the polymerization system in the form of a solution. The solvent of the organic lithium initiator can be one or more of hexane, cyclohexane, heptane, etc., and the concentration is preferably 0.04-0.2 mol·L -1 .

[0043] The amount of the initiator used in the present invention can be reasonably selected according to the amount of the monomer used and the molecular weight of the low cis polybutadiene rubber to be obtained, and the amount can vary within a wide range. Preferably, the molar ratio of 1,3-butadiene to the organic lithium initiator is 750-1300:1, preferably 850-1200:1, and more preferably 900-1100:1.

[0044] According to the present invention, the anionic solution polymerization reaction is carried out in the presence of a structure regulator, and the type of the structure regulator of the present invention can be conventionally selected in the art. Preferably, the structure regulator is potassium alkoxide and / or sodium alkoxide. In order to better balance the relationship between the Mooney viscosity of the low cis-polybutadiene rubber and the viscosity of the 5 wt% styrene solution, preferably, the structure regulator is potassium tert-pentoxide and / or potassium 2-hexoxide, and the above structure regulator has good solubility in hydrocarbon solvents.

[0045] According to the present invention, the amount of the structure regulator can be reasonably selected according to the various performance indicators of the target product. If the amount of the structure regulator is too low, the reactivity ratio of 1,3-butadiene and the branched monomer is large, and the branched monomer is more inclined to homopolymerization, resulting in easier production of gel. In order to suppress the gel content, more gel inhibitors must be added, and there is an upper limit to the amount of gel inhibitor added. If the amount of the structure regulator is too high, the molecular chain is easily deactivated, resulting in a decrease in the conversion rate of 1,3-butadiene. Preferably, the molar ratio of the amount of the structure regulator to the amount of the organic lithium initiator is 0.1-1:1, more preferably 0.1-0.8:1, and further preferably 0.1-0.5:1. In this way, the reactivity ratio of 1,3-butadiene and the branched monomer can be adjusted, so that 1,3-butadiene and the branched monomer are more inclined to ideal copolymerization in step (2), so as to control the branching degree and gel content of the product without seriously deactivating the active chain.

[0046] According to the present invention, the gel inhibitor refers to a substance having a certain chain transfer effect and capable of inhibiting the formation of gel during the polymerization process. The gel inhibitor is one or more of tetramethylethylenediamine / 1,2-butadiene, C4 residue and 1,2-butadiene, preferably 1,2-butadiene. The 1,2-butadiene can be pure 1,2-butadiene or 1,2-butadiene containing some inert components, and can be prepared into a certain concentration for use according to the needs of the equipment.

[0047] According to the present invention, the amount of the gel inhibitor can be reasonably selected according to the gel content index of the target product to meet the requirements of the product. Preferably, the weight ratio of the gel inhibitor to 1,3-butadiene is 1-10:10000, more preferably 5-8:10000.

[0048] According to the present invention, the conditions of the anionic solution polymerization reaction in step (1) are such that the conversion rate of 1,3-butadiene reaches more than 99%. If the polymerization temperature is too low, the conversion rate of the monomer per unit time is low, and the residence time needs to be extended; if the polymerization temperature is too high, gel is easily generated, which affects the quality of the product.

[0049] Preferably, the conditions of the anionic solution polymerization reaction include: temperature of 0-120°C, preferably 40-115°C (e.g. 80-110°C), more preferably 50-110°C; time (i.e. residence time) of 30-90min, preferably 40-80min; gauge pressure of 0.1-2MPa, preferably 0.5-1MPa. The anionic solution polymerization reaction of the present invention can have high controllability, and its polymerization temperature is easy to control, so that the performance of the obtained product is easy to control.

[0050] According to the present invention, the present invention has no particular limitation on the branching monomer, as long as the low cis polybutadiene rubber of the present invention can be obtained. Preferably, the branching monomer is a C10-C16 aromatic vinyl monomer, more preferably one or more of divinylbenzene, dipropylenebenzene and diallylbenzene, and further preferably divinylbenzene. Aromatic vinyl monomers are copolymerized with 1,3-butadiene to prepare star polymers, thereby balancing the relationship between the Mooney viscosity of the low cis polybutadiene rubber and the viscosity of the 5% styrene solution, and a HIPS resin with more balanced gloss and impact resistance can be obtained, while achieving halogen-free process and solving the corrosion problem in the post-processing process.

[0051] The present invention has no particular limitation on the amount of branching monomers, as long as the low cis polybutadiene rubber of the present invention can be obtained with a number average molecular weight in the range of 70,000-90,000 g / mol (preferably 73,000-88,000 g / mol, more preferably 75,000-85,000 g / mol) and a molecular weight distribution coefficient in the range of 100. However, in order to make the obtained low cis polybutadiene rubber have a more suitable branching area, so that the HIPS has higher impact resistance. Preferably, the molar ratio of the branching monomer to the organic lithium initiator is 0.4-1:1, preferably 0.4-0.8:1.

[0052] Wherein, the branched monomer is added to the polymerization system in the form of a solution. Preferably, the solvent of the solution containing the branched monomer is the same as the selection of the aforementioned inert solvent, and the inert solvent can be a C5-C8 cycloalkane and / or a C5-C9 alkane, preferably one or more of cyclohexane, methylcyclopentane, methylcyclohexane, methylpentane, n-hexane, n-heptane and isooctane. The concentration of the branched monomer can be adjusted in a wide range according to the metering pump range of the branched monomer.

[0053] Preferably, steps (1) and (2) are carried out in an inert atmosphere, wherein the inert atmosphere is provided by one or more inactive gases selected from nitrogen, neon and argon.

[0054] According to the present invention, in step (2), the branching reaction can be terminated by using a terminator, thereby obtaining a polymerization solution of low-cis polybutadiene rubber.

[0055] According to the present invention, the method for preparing low-cis polybutadiene rubber of the present invention comprises the step of removing solvent from the mixed solution obtained in step (2) in order to extract low-cis polybutadiene rubber. The method for removing solvent can be a conventional method in the art, such as using steam condensation desolventizing treatment to extract low-cis polybutadiene rubber from the mixed solution.

[0056] Preferably, the terminator is one or more of alcohol, organic acid and carbon dioxide of C1-C4, preferably one or more of isopropyl alcohol, stearic acid, citric acid and carbon dioxide, more preferably carbon dioxide. Carbon dioxide is adopted to carry out termination reaction, carbon dioxide can form carbonate with the metal ion (Li, Mg, Al, Fe, Zn) in the polymerization system, thus avoids the chromogenic reaction of metal ion, and product has lower chroma. Carbon dioxide here can be passed into reaction system in the mode of gas (for example, passing into carbon dioxide gas that gauge pressure is 0.2-1MPa (for example, can be 0.3-0.6MPa)), can also be introduced into reaction system in the form of dry ice aqueous solution (for example concentration is 0.1-5 weight %).

[0057] There is no particular limitation on the amount of carbon dioxide used, and preferably, the molar ratio of carbon dioxide to initiator is 0.5-5:1, preferably 0.6-2:1. This can ensure the pH value of the polymerization system and remove metal ions in low-cis polybutadiene rubber.

[0058] In order to improve the antioxidant property of the obtained low-cis polybutadiene rubber, an antioxidant may be introduced into the low-cis polybutadiene rubber. Preferably, after the termination of step (2), an antioxidant is introduced into the reaction system obtained by termination, so that the obtained polymerization solution of the low-cis polybutadiene rubber contains the antioxidant. After the antioxidant is introduced, the solvent removal step is performed. The antioxidant is not particularly limited in the present invention, and may be any conventional antioxidant in the art. For example, the antioxidant is one or more of 4,6-bis(octylthiomethyl)-o-cresol (trade name: antioxidant 1520), β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (trade name: antioxidant 1076), N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (trade name: antioxidant 4020), N-isopropylphenyl-N'-phenyl-p-phenylenediamine (trade name: antioxidant 4010NA) and N-phenyl-2-naphthylamine (trade name: antioxidant D). Generally speaking, since antioxidant 1520 has two thioether substituents at the 2 and 4 positions and has a dual function (having both the main antioxidant function and the auxiliary antioxidant function), it can play an intramolecular synergistic role, and the use of antioxidant 1520 as an antioxidant system can reduce the amount of the antioxidant system. In addition, the addition of antioxidant 1076 can significantly prevent the breakage of polymer molecular chains. Preferably, it is a combination of antioxidant 1520 and antioxidant 1076, and the weight ratio of antioxidant 1520 to antioxidant 1076 can be 0.5-5:1. More preferably, it is a combination of antioxidant 1520 and antioxidant 1076 in a weight ratio of 1-3:1.

[0059] Preferably, the weight ratio of the antioxidant to 1,3-butadiene is 0.1-0.6:100, preferably 0.2-0.4:100.

[0060] A third aspect of the present invention provides a method for preparing a HIPS resin, wherein the method comprises:

[0061] (1) providing a low-cis polybutadiene solution, wherein the low-cis polybutadiene rubber solution contains the low-cis polybutadiene rubber obtained by the above method;

[0062] (2) In the presence of a free radical initiator, polymerizing styrene and a toughening agent; wherein the toughening agent comprises the low-cis polybutadiene solution obtained in step (1).

[0063] According to the present invention, the solvent in the low-cis polybutadiene polymerization solution is a benzene solvent, and the benzene solvent is one or more of unsubstituted or C1-C4 alkyl-substituted benzene, and the C1-C4 alkyl group can be, for example, one or more of methyl, ethyl, n-propyl, isopropyl and n-butyl. The C1-C4 alkyl-substituted benzene used as the benzene solvent can be single-point substituted or multi-point substituted. Preferably, the benzene solvent is one or more of benzene, toluene, ethylbenzene and xylene, preferably ethylbenzene.

[0064] The amount of the benzene solvent used is sufficient to make the content of low-cis polybutadiene rubber in the low-cis polybutadiene rubber solution be 25-55 wt % or more. Under this condition, the amount of the benzene solvent used is preferably such that the content of butadiene is 30-45 wt %.

[0065] The method of providing the low cis polybutadiene solution in step (1) is preferably to form a solution of the low cis polybutadiene rubber and a benzene solvent. The low cis polybutadiene rubber is the low cis polybutadiene rubber obtained by removing the solvent from the mixed solution obtained after the termination reaction.

[0066] According to the present invention, in step (2) of the method for preparing HIPS resin of the present invention, the HIPS resin can be obtained by using low cis polybutadiene rubber as a toughening agent and polymerizing with styrene. The toughening agent contains a solvent brought by the solution of the above step (1). Preferably, in step (2), the amount of the toughening agent is such that, based on the total weight of styrene and the toughening agent, the content of the benzene solvent is less than 18% by weight, more preferably, the content of the benzene solvent is 6-18% by weight. Preferably, the weight ratio of styrene to the toughening agent on a dry weight basis is 550-2500: 100, more preferably 600-2000: 100, and further preferably 900-1900: 100.

[0067] According to the present invention, the free radical initiator can be various initiators conventionally used in the art for preparing HIPS resin, for example, the free radical initiator can be one or more of thermal decomposition initiators, preferably one or more of peroxide initiators and azobisnitrile compound initiators, more preferably one or more of peroxy-2-ethylhexyl tert-butyl carbonate, diacyl peroxide, peroxydicarbonate, peroxycarboxylic acid ester, alkyl peroxide and azobisnitrile compounds, further preferably one or more of dibenzoyl peroxide, di-o-methylbenzoyl peroxide, tert-butyl peroxybenzoate, diisopropylbenzene peroxide, azobisisobutyronitrile and azobisisoheptonitrile. Preferably, the weight ratio of styrene to the free radical initiator is 2500-12000:1, more preferably 3000-9500:1, more preferably 4000-9000:1, and further preferably 5000-8500:1.

[0068] According to the present invention, preferably, in step (2), the polymerization reaction conditions include: the polymerization reaction conditions include: temperature of 100-150° C., time of 7-9 h. The polymerization reaction can be carried out under stirring, for example, under stirring at 100-400 rpm.

[0069] According to the present invention, in another preferred embodiment of the present invention, in step (2), the conditions of the polymerization reaction include: first reacting at 100-110°C for 1-3h, then reacting at a temperature of 115-125°C for 1-3h (e.g. 1-2h), then reacting at 130-140°C for 1-3h (e.g. 1-2h), and finally reacting at 145-155°C for 1-3h (e.g. 1-2.5h). More preferably, in step (2), the conditions of the polymerization reaction include: first reacting at 105-110°C for 1.5-2.5h, then reacting at a temperature of 120-125°C for 1.5-2.5h, then reacting at 130-135°C for 1.5-2.5h, and finally reacting at 150-155°C for 1.5-2.5h. The polymerization reaction can be carried out under stirring, for example, under stirring at 100-400rpm.

[0070] The present invention also provides HIPS resin prepared by the method.

[0071] Preferably, in the HIPS resin of the present invention, the content of the structural unit of styrene is 85-95% by weight, preferably 90-95% by weight (it can be understood that the remaining content is mainly the structural unit provided by butadiene, that is, the content of the structural unit of butadiene is 5-15% by weight, preferably 5-10% by weight), the number average molecular weight is 60,000-150,000, more preferably 80,000-120,000; the molecular weight distribution coefficient is 2-3.

[0072] The method of the present invention can obtain a HIPS resin product with more balanced gloss and impact resistance. Preferably, the Izod impact strength of the HIPS resin is 10 kJ / m 2 Above, preferably 10.5 kJ / m 2 The surface gloss at 60° is 70 or above, preferably 80 or above. The mechanical properties of HIPS are tested using the British INSTRON 5567 universal material testing machine. The notched cantilever beam impact strength is measured according to GB / T1843-1996 standard (kJ / m 2 ); 60° surface gloss is measured according to ASTM D526 (60°).

[0073] The present invention will be described in detail below through examples.

[0074] In the following examples and comparative examples, the determination methods involved include:

[0075] (1) The monomer conversion rate was determined by the weight method, i.e., the weight percentage of the polymer weight after solvent removal to the theoretical polymer yield.

[0076] (2) Mooney viscosity was measured using a GT-7080-S2 Mooney viscometer produced by Gotech Co., Ltd. in Taiwan, China, in accordance with GB / T1232.1 standard, with a preheating time of 1 min, a rotation time of 4 min, and a test temperature of 100°C.

[0077] (3) The content of 1,2-polymer structural units in low-cis polybutadiene rubber is measured by measuring the vinyl content, using an AVANCEDRX400MHz nuclear magnetic resonance spectrometer (BRUKER) 1 H-NMR) determination, wherein 1 The resonance frequency of H nuclei is 300.13 MHz, the spectrum width is 2747.253 Hz, the pulse width is 5.0 μs, the data point is 16 K, the sample tube diameter is 5 mm, and the solvent is deuterated chloroform CDCl 3 , the sample concentration was 15% (W / V), the test temperature was room temperature, the number of scans was 16 times, and the calibration was based on the chemical shift of tetramethylsilane as 0 ppm.

[0078] (4) The molecular weight and molecular weight distribution were determined using a HLC-8320 gel permeation chromatograph from Tosoh Corporation of Japan. The test conditions included: the chromatographic column was TSKgel SuperMultiporeHZ-N, the standard column was TSKgelSuperMultiporeHZ, the solvent was chromatographic grade THF, the calibration standard was polystyrene, the sample mass concentration was 1 mg / ml, the injection volume was 10.00 μl, the flow rate was 0.35 ml / min, and the test temperature was 40.0°C.

[0079] (5) The viscosity of 5 wt% rubber styrene solution at 25°C was measured using Beijing Yanshan Petrochemical Company corporate standard Q / SH3155.SXL.C26-2019 and a Finn viscometer was used at a constant temperature of 25°C.

[0080] (6) In the present invention, the gel content is determined by the weight method tested by Beijing Yanshan Petrochemical Company Enterprise Standard Q / SH3155.SXL.C27-2019. The specific process is as follows: add the polymer sample to styrene, oscillate in an oscillator at a temperature of 25°C for 16 hours to completely dissolve the soluble matter, and prepare a styrene solution containing a polymer content of 5% by weight, and record the mass of the polymer sample as C (in grams); weigh a 400-mesh clean nickel mesh, and record the mass of the clean nickel mesh as B (in grams); then filter the above solution with a nickel mesh; after filtering, rinse the nickel mesh with styrene, dry the nickel mesh at 150°C and normal pressure for 30 minutes, weigh it, and record its mass as A (in grams); calculate the gel content according to the following formula:

[0081] Gel content % = [(AB) / C] x 100%.

[0082] (7) The chromaticity was tested using a HunterLab ColorFlex desktop colorimeter from HunterLab, USA, in accordance with standard Q / SH3155.SXL.C29-2019. The test conditions were: CIELAB was used as the colorimetric system, the optical geometry was 45° / 0°, the light source was C light source, the observation angle was 2°, and the sample thickness was approximately 15 mm.

[0083] (8) The mechanical properties of HIPS were tested using the British INSTRON 5567 universal material testing machine. The cantilever beam notched impact strength was measured according to GB / T1843-1996 (kJ / m 2 ); 60° surface gloss is measured according to ASTM D526 (60°).

[0084] Experimental device and process: The experiment was carried out in a 16L polymerization reactor (customized by Xiandali Company, with an inner diameter of 20cm), using a bottom-in and top-out feeding method and full-load operation. Solvent, butadiene monomer, branching monomer, gel inhibitor, initiator and structure regulator were added from the bottom of the reactor respectively, and terminator and antioxidant were added to the pipeline at the reactor outlet to obtain polymer glue.

[0085] The pressure in this experiment refers to the gauge pressure.

[0086] Antioxidant 1520 was purchased from Sinopharm Reagent Company; Antioxidant 1076 was purchased from Inokai Reagent Company.

[0087] The organolithium initiators were purchased from J&K Reagent Company and diluted to 0.07 mol·L with hexane. -1 .

[0088] 1,2-Butadiene was purchased from Inotech Reagents and diluted with hexane to a concentration of 1 wt %.

[0089] Potassium tert-pentyl oxide was purchased from J&K Reagent Company and diluted to 0.02 mol·L with hexane. -1 .

[0090] Divinylbenzene (DVB) was purchased from Inotech Reagent Company and diluted to 0.04 mol·L with hexane. -1 .

[0091] Example 1

[0092] This example is used to illustrate the low-cis polybutadiene rubber and the preparation method thereof of the present invention.

[0093] (1) Under nitrogen protection, n-hexane solvent, 1,3-butadiene monomer, DVB monomer, 1,2-butadiene (gel inhibitor), organic lithium initiator and structure regulator (types and amounts are shown in Table 1, and the flow rates listed in the table are all measured based on pure compounds) are continuously added into a 16L reactor from the bottom of the reactor; and anionic solution polymerization is carried out at a specified temperature and reaction pressure (conditions are shown in Table 1).

[0094] (2) A terminator and an antioxidant (the types and amounts are shown in Table 2, and the flow rates listed in the table are all measured based on pure compounds) are added sequentially into the pipeline at the upper outlet of the polymerization, and finally a polymerization solution PB1 of low-cis polybutadiene rubber is obtained, wherein the content of low-cis polybutadiene rubber is 15.8 wt %.

[0095] The polymer solution sample finally obtained was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymer C1 were measured. The results are shown in Table 3.

[0096] Embodiment 2-5

[0097] This example is used to illustrate the low-cis polybutadiene rubber and the preparation method thereof of the present invention.

[0098] The method described in Example 1 is different in that the materials and amounts shown in Table 1 are used for reaction to obtain polymerization solutions PB2-PB5 of low cis polybutadiene rubber, respectively, wherein the content of each low cis polybutadiene rubber is: PB2: 15.8 wt%; PB3: 15.8 wt%; PB4: 15.8 wt%; PB5: 15.8 wt%.

[0099] The final obtained polymerization solution sample was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymers C2-C5 were measured. The results are shown in Table 3.

[0100] Example 6

[0101] This example is used to illustrate the low-cis polybutadiene rubber and the preparation method thereof of the present invention.

[0102] According to the method described in Example 1, the difference is that isopropanol is used as the terminator instead of the carbon dioxide aqueous solution, and the amount used is 0.15g of isopropanol per 100g of 1,3-butadiene, thereby obtaining a polymerization solution PB6 of low-cis polybutadiene rubber, wherein the content of low-cis polybutadiene rubber is 15.8% by weight.

[0103] The final polymerization solution sample was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymer C6 were measured. The results are shown in Table 3.

[0104] Comparative Example 1

[0105] The method described in Example 1 is different in that DVB is not added as a comonomer at the bottom of the reactor, thereby obtaining a polymerization solution DPB1 of low-cis polybutadiene rubber, wherein the content of low-cis polybutadiene rubber is 15.7 wt %.

[0106] The final polymerization solution sample was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymer DC1 were measured. The results are shown in Table 3.

[0107] Comparative Example 2

[0108] The method described in Example 1 is different in that the DVB flow rate is 1.94 g / h, thereby obtaining a polymerization solution DPB2 of low-cis polybutadiene rubber, wherein the content of low-cis polybutadiene rubber is 15.8 wt %.

[0109] The final polymerization solution sample was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymer DC2 were measured. The results are shown in Table 3.

[0110] Comparative Example 3

[0111] The method described in Example 1 is different in that the flow rate of n-butyl lithium during the polymerization process is 2.66 g / h, thereby obtaining a polymerization solution DPB3 of low-cis polybutadiene rubber, wherein the content of low-cis polybutadiene rubber is 15.8 wt %.

[0112] The final polymerization solution sample was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymer DC3 were measured. The results are shown in Table 3.

[0113] Comparative Example 4

[0114] The method described in Example 1 is different in that 1,2-butadiene is not added during the polymerization process. After 6 hours, the polymerization kettle is full of gel and normal polymerization cannot be performed. A polymerization solution DPB4 of low-cis polybutadiene rubber is obtained, wherein the content of low-cis polybutadiene rubber is 15.8 wt %.

[0115] A portion of the final obtained polymerization solution sample was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymer DC4 were measured. The results are shown in Table 3.

[0116] Comparative Example 5

[0117] According to the method described in Example 1, except that potassium tert-pentoxide was not added during the polymerization process, a large amount of gel was generated in the polymerization kettle after 24 hours; a polymerization solution DPB5 of low-cis polybutadiene rubber was obtained, wherein the content of low-cis polybutadiene rubber was 15.8% by weight.

[0118] The final obtained polymerization solution sample was taken out for steam condensation and desolventization treatment, and the structure and performance of the obtained polymer DC5 were measured. The results are shown in Table 3.

[0119] Comparative Example 6

[0120] The method described in Example 1 is different in that the n-hexane solution containing the branching monomer DVB is continuously added to the reactor at a distance of 1 / 2 from the bottom of the reactor to obtain a polymerization solution DPB6 of low-cis polybutadiene rubber, wherein the content of low-cis polybutadiene rubber is 15.7% by weight.

[0121] The final obtained polymerization solution sample was taken out for steam condensation and desolventization treatment. The structure and performance of the obtained polymer DC6 were measured. The results are shown in Table 3.

[0122] Comparative Example 7

[0123] The method described in Example 1 is different in that a n-hexane solution containing a branched monomer DVB is continuously added to the reactor at 5 / 8 of the distance from the bottom of the reactor to obtain a polymerization solution DPB7 of low-cis polybutadiene rubber, wherein the content of low-cis polybutadiene rubber is 15.7% by weight.

[0124] The final obtained polymerization solution sample was taken out for steam condensation and desolventization treatment. The structure and performance of the obtained polymer DC7 were measured. The results are shown in Table 3.

[0125] Table 1

[0126]

[0127] Table 2

[0128]

[0129]

[0130] Table 3

[0131]

[0132] It can be seen from Table 3 that the low cis polybutadiene rubber prepared in the present invention has moderate 5% styrene solution viscosity and Mooney viscosity, low chroma and gel content, and is particularly suitable as a HIPS (or ABS) toughening agent.

[0133] Example 7

[0134] This example is used to illustrate the HIPS resin and its preparation method of the present invention.

[0135] (1) 96 g of the low-cis polybutadiene rubber C1 obtained in Example 1 was mixed with 234 g of ethylbenzene to form a low-cis polybutadiene polymerization solution;

[0136] (2) 330 g of the polymerization solution of the low-cis polybutadiene rubber obtained in step (1) and 1100 g of styrene monomer were mixed, and then 45 g of mineral oil (provided by Beijing Yanshan Petrochemical Company Chemical Plant No. 1, density 0.85-0.88 g / ml, the same below) and 0.1 g of tert-butyl peroxy-2-ethylhexyl carbonate were added and mixed, and the mixture was polymerized at a stirring rate of 300 rpm and a polymerization temperature of 105° C. for 2 h, and then the mixture was heated to 120° C. for polymerization for 2 h; the mixture was heated to 135° C. for polymerization for 2 h at a stirring rate of 100 rpm, and finally the mixture was heated to 150° C. for polymerization for 2 h. The reaction product was subjected to vacuum flash evaporation to remove unreacted monomers and solvent, and HIPS resin P1 was obtained.

[0137] After the HIPS resin was dried, its structure and performance were measured. The results are shown in Table 4.

[0138] Example 8

[0139] This example is used to illustrate the HIPS resin and its preparation method of the present invention.

[0140] (1) 90 g of the low-cis polybutadiene rubber C2 obtained in Example 2 was mixed with 210 g of ethylbenzene to form a low-cis polybutadiene polymerization solution;

[0141] (2) 300 g of the polymerization solution of the low-cis polybutadiene rubber obtained in step (1) and 1100 g of styrene monomer were mixed, and then 50 g of mineral oil and 0.2 g of azobisisobutyronitrile were added and mixed, and the mixture was polymerized at a stirring rate of 350 rpm and a polymerization temperature of 110° C. for 1.5 h, and then the mixture was heated to 120° C. for polymerization for 2.5 h; the mixture was heated to 130° C. for polymerization at a stirring rate of 200 rpm for 1.5 h, and finally the mixture was heated to 155° C. for polymerization for 2 h, and the reaction product was subjected to vacuum flash evaporation to remove unreacted monomers and solvent to obtain HIPS resin P2.

[0142] After the HIPS resin was dried, its structure and performance were measured. The results are shown in Table 4.

[0143] Examples 9-12

[0144] This example is used to illustrate the HIPS resin and its preparation method of the present invention.

[0145] The method described in Example 7 is different in that low cis polybutadiene rubbers C3-C6 are used instead of low cis polybutadiene rubber C1, so that the reaction products are subjected to vacuum flash evaporation to remove unreacted monomers and solvents to obtain HIPS resins P3-P6 respectively.

[0146] After the HIPS resin was dried, its structure and performance were measured. The results are shown in Table 4.

[0147] Comparative Example 6

[0148] The method described in Example 7 is different in that the low cis polybutadiene rubbers described in DC1-DC5 are used instead of low cis polybutadiene rubber C1, so that the reaction products are subjected to vacuum flash evaporation and unreacted monomers and solvents are removed to obtain HIPS resins DP1-DP5 respectively.

[0149] Comparative Examples 7-8

[0150] The method described in Example 7 is different in that the low cis polybutadiene rubber described in DC6-DC7 is used instead of low cis polybutadiene rubber C1, so that the reaction products are subjected to vacuum flash evaporation and unreacted monomers and solvents are removed to obtain HIPS resins DP6-DP7 respectively.

[0151] Comparative Examples 9-10

[0152] The method of Example 7 is used, except that Asahi Chemical Products 720A and 730A (from which the solvent has been removed) are used instead of low-cis polybutadiene rubber C1 to obtain HIPS resins DP8-DP9 respectively.

[0153] After the HIPS resin was dried, its structure and performance were measured. The results are shown in Table 4.

[0154] Table 4

[0155]

[0156] It can be seen from Table 4 that by using the low-cis polybutadiene containing the present invention as a toughening agent, a HIPS resin with more balanced impact resistance and glossiness can be obtained. The HIPS resin obtained by the present invention has better comprehensive performance than the HIPS resin obtained by using the popular toughening agent on the market.

[0157] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A low-cis polybutadiene rubber, characterized in that: The content of 1,2-polymerized structural units in the low-cis polybutadiene rubber is 8-20% by weight; the number average molecular weight is 70,000-90,000 g / mol; the molecular weight distribution coefficient is 2.25-2.65; the Mooney viscosity ML at 100° C. 1+4 is 40-60; the viscosity of a 5 wt% styrene solution at 25°C is 40-66cp, and the gel content of the low cis polybutadiene rubber is below 200ppm; the chromaticity of a 5 wt% styrene solution of the low cis polybutadiene rubber is below -2.

2. The low-cis polybutadiene rubber according to claim 1, wherein The content of 1,2-polymerized structural units in the low-cis polybutadiene rubber is 9-18% by weight.

3. The low-cis polybutadiene rubber according to claim 1, wherein The content of 1,2-polymerized structural units in the low-cis polybutadiene rubber is 10-16% by weight.

4. The low-cis polybutadiene rubber according to claim 1, wherein The number average molecular weight is 73,000-88,000 g / mol.

5. The low-cis polybutadiene rubber according to claim 1, wherein The number average molecular weight is 75,000-85,000 g / mol.

6. The low-cis polybutadiene rubber according to claim 1, wherein The molecular weight distribution coefficient is 2.28-2.

55.

7. The low-cis polybutadiene rubber according to claim 1, wherein The molecular weight distribution coefficient is 2.3-2.

55.

8. The low-cis polybutadiene rubber according to claim 1, wherein Mooney viscosity ML at 100°C 1+4 Is 40-58.

9. The low-cis polybutadiene rubber according to claim 1, wherein The Mooney viscosity ML1+4 at 100°C is 45-55.

10. The low-cis polybutadiene rubber according to claim 1, wherein The viscosity of a 5 wt% styrene solution at 25°C is 42-66 cp.

11. The low-cis polybutadiene rubber according to claim 1, wherein The viscosity of a 5 wt% styrene solution at 25°C is 44-58 cp.

12. A method for preparing the low-cis polybutadiene rubber according to any one of claims 1 to 11, wherein: The method includes: (1) in an inert solvent, in the presence of an organic lithium initiator, a gel inhibitor and a structure regulator, 1,3-butadiene and a branched monomer are continuously introduced into a reactor from the bottom of the reactor to perform an anionic solution polymerization reaction until the conversion rate of 1,3-butadiene reaches more than 99%; (2) contacting the mixture obtained in step (1) with a terminator to terminate the reaction, The gel inhibitor is one or more of tetramethylethylenediamine / 1,2-butadiene, C4 residue and 1,2-butadiene.

13. The preparation method according to claim 12, wherein: The organic lithium initiator is a compound represented by the formula RLi, wherein R is selected from a C1-C20 alkyl group, a C6-C20 cycloalkyl group or a C6-C20 aryl group.

14. The preparation method according to claim 12, wherein: The organic lithium initiator is one or more of methyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, isobutyl lithium, tert-butyl lithium, cyclohexyl lithium, 4-cyclohexylbutyl lithium, phenyl lithium, triphenylmethyl lithium and 2-naphthyl lithium.

15. The preparation method according to claim 12, wherein: The organic lithium initiator is n-butyl lithium and / or sec-butyl lithium.

16. The preparation method according to claim 12, wherein: The molar ratio of the organic lithium initiator to 1,3-butadiene is 750-1300:

1.

17. The preparation method according to claim 12, wherein: The molar ratio of the organic lithium initiator to 1,3-butadiene is 850-1200:

1.

18. The preparation method according to claim 12, wherein: The molar ratio of the organic lithium initiator to 1,3-butadiene is 900-1100:

1.

19. The preparation method according to claim 12, wherein: The inert solvent is C5-C8 cycloalkane and / or C5-C9 alkane.

20. The preparation method according to claim 12, wherein: The inert solvent is one or more of cyclohexane, methylcyclopentane, methylcyclohexane, methylpentane, n-hexane, n-heptane and isooctane.

21. The method according to claim 12, wherein: The conditions for the anionic solution polymerization reaction include: temperature of 0-120° C.; time of 30-90 min; and gauge pressure of 0.1-2 MPa.

22. The method according to claim 12, wherein: The conditions for the anionic solution polymerization reaction include: temperature of 40-115° C.; time of 40-80 min; and gauge pressure of 0.5-1 MPa.

23. The method according to claim 12, wherein: The conditions for the anionic solution polymerization reaction include: a temperature of 50-110°C.

24. The preparation method according to any one of claims 12 to 23, wherein: The structure regulator is potassium alkoxide.

25. The preparation method according to any one of claims 12 to 23, wherein: The structure regulator is potassium tert-pentyl oxide and / or potassium 2-hexanol.

26. The preparation method according to any one of claims 12 to 23, wherein: The molar ratio of the structure regulator to the initiator is 0.05-0.5:

1.

27. The preparation method according to any one of claims 12 to 23, wherein: The molar ratio of the structure regulator to the initiator is 0.1-0.2:

1.

28. The preparation method according to any one of claims 12 to 23, wherein: The weight ratio of the gel inhibitor to 1,3-butadiene is 1-10:10000.

29. The preparation method according to any one of claims 12 to 23, wherein: The weight ratio of the gel inhibitor to 1,3-butadiene is 5-8:10000.

30. The preparation method according to any one of claims 12 to 23, wherein: The branching monomer is a C10-C16 aromatic vinyl monomer.

31. The preparation method according to any one of claims 12 to 23, wherein: The branching monomer is one or more of divinylbenzene, dipropylenebenzene and diallylbenzene.

32. The preparation method according to any one of claims 12 to 23, wherein: The molar ratio of the branched monomer to the organic lithium initiator is 0.4-1:

1.

33. The preparation method according to any one of claims 12 to 23, wherein: The molar ratio of the branched monomer to the organic lithium initiator is 0.4-0.8:

1.

34. The method according to any one of claims 12 to 23, wherein: The terminator is one or more of C1-C4 alcohol, organic acid and carbon dioxide.

35. The method according to any one of claims 12 to 23, wherein: The terminator is one or more of isopropyl alcohol, stearic acid, citric acid and carbon dioxide.

36. The method according to any one of claims 12 to 23, wherein: The terminator is carbon dioxide.

37. The method according to any one of claims 12 to 23, wherein: The method comprises the step of removing the solvent from the mixed solution obtained in step (2).

38. A method for preparing a HIPS resin, the method comprising: (1) providing a low-cis polybutadiene rubber solution, wherein the low-cis polybutadiene rubber solution contains the low-cis polybutadiene rubber obtained by the method according to any one of claims 12 to 37; (2) In the presence of a free radical initiator, polymerizing styrene and a toughening agent; wherein the toughening agent contains the low-cis polybutadiene rubber solution obtained in step (1).

39. The preparation method according to claim 38, wherein The solvent in the low-cis polybutadiene rubber solution is a benzene solvent, and the benzene solvent is one or more of unsubstituted or C1-C4 alkyl-substituted benzene.

40. The preparation method according to claim 38, wherein Based on the total weight of styrene, benzene solvent and toughening agent, the amount of the benzene solvent is 6-18% by weight.

41. The preparation method according to claim 38, wherein The weight ratio of styrene to toughening agent is 550-2500:100 on a dry weight basis.

42. The preparation method according to claim 38, wherein The weight ratio of styrene to toughening agent is 600-2000:100 on a dry weight basis.

43. The preparation method according to claim 38, wherein The weight ratio of styrene to toughening agent is 900-1900:100 on a dry weight basis.

44. The preparation method according to claim 38 or 39, wherein: The free radical initiator is one or more of diacyl peroxide, peroxydicarbonate, peroxycarboxylate, alkyl peroxide and azobisnitrile compounds.

45. The preparation method according to claim 38 or 39, wherein: The free radical initiator is one or more of tert-butyl peroxy-2-ethylhexyl tert-butyl carbonate, dibenzoyl peroxide, di-o-methylbenzoyl peroxide, tert-butyl perbenzoate, diisopropylbenzene peroxide, azobisisobutyronitrile and azobisisoheptylnitrile.

46. ​​The preparation method according to claim 38 or 39, wherein: The free radical initiator is one or more of dibenzoyl peroxide, di-o-methylbenzoyl peroxide, tert-butyl perbenzoate, diisopropylbenzene peroxide, azobisisobutyronitrile and azobisisoheptylnitrile.

47. The preparation method according to claim 38 or 39, wherein: The weight ratio of styrene to the free radical initiator is 2500-12000:

1.

48. The preparation method according to claim 38 or 39, wherein The weight ratio of styrene to the free radical initiator is 3000-9500:

1.

49. The preparation method according to claim 38 or 39, wherein: The weight ratio of styrene to the free radical initiator is 4000-9000:

1.

50. The preparation method according to claim 38 or 39, wherein: The weight ratio of styrene to the free radical initiator is 5000-8500:

1.

51. The preparation method according to claim 38 or 39, wherein: The polymerization reaction conditions include: temperature of 100-150°C and time of 7-9h; Alternatively, the polymerization reaction conditions include: first reacting at 100-110° C. for 1-3 h, then reacting at 115-125° C. for 1-3 h, then reacting at 130-140° C. for 1-3 h, and finally reacting at 145-155° C. for 1-3 h.

52. The preparation method according to claim 38 or 39, wherein: The polymerization reaction conditions include: first reacting at 105-110° C. for 1.5-2.5 h, then reacting at 120-125° C. for 1.5-2.5 h, then reacting at 130-135° C. for 1.5-2.5 h, and finally reacting at 150-155° C. for 1.5-2.5 h.

53. HIPS resin obtained by the preparation method described in any one of claims 38 to 52.

54. The HIPS resin according to claim 53, wherein The content of the structural unit of styrene in the HIPS resin is 85-95% by weight; the number average molecular weight of the HIPS resin is 60,000-150,000.

55. The HIPS resin according to claim 53, wherein The content of the structural unit of styrene in the HIPS resin is 90-95% by weight; the number average molecular weight of the HIPS resin is 80,000-120,000.

56. The HIPS resin according to claim 53, whereinThe surface glossiness of the HIPS resin at 60° is above 70, and the Izod notched impact strength measured according to the GB / T 1843 method is 10 kJ / m 2 above.

Citation Information

Patent Citations

  • Low cis-polybutadiene rubber and preparing method and application thereof

    CN106589247A

  • Low cis-polybutadiene rubber and preparation method thereof, and high-impact polystyrene (HIPS) resin and preparation method thereof

    CN109251263A

  • Rubber modified and impact preventing polystyrene resin compsns.

    CN1519269A