Rare earth permanent magnet and method for manufacturing the same
By mixing Ce-rich and Ce-poor magnetic powders and sintering them in a magnetic field, combined with heat treatment technology, the problems of high manufacturing cost and low productivity of rare earth permanent magnets are solved, and the efficient preparation and magnetic characteristics of rare earth permanent magnets are achieved.
Patent Information
- Application Number
- CN202011352498.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-11-27
AI Technical Summary
The existing rare earth permanent magnet manufacturing methods are costly and have low productivity, making them difficult to mass produce, and Nd-type rare earth permanent magnets are expensive, and the inherent magnetic characteristics and cost-effectiveness of Ce and La rare earth permanent magnets are not good.
A mixed preparation method of Ce-rich and Ce-leaving magnetic powder is adopted to form rare earth permanent magnets with improved magnetic properties by sintering in a magnetic field and heat treatment, and the chemical composition and microstructure of the alloy are optimized using the diffusion temperature conditions of different rare earth elements.
It reduces the manufacturing cost of rare earth permanent magnets, improves magnetic characteristics, especially coercive forces and residual flux density, and provides a cost-effective solution.
Smart Images

Figure CN113496798B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a rare earth permanent magnet and a method for manufacturing the same, wherein the rare earth permanent magnet has improved magnetic properties due to the inclusion of cerium (Ce)-rich magnetic powder and cerium (Ce)-poor magnetic powder containing substantially no cerium (Ce). Background Art
[0002] Generally, rare earth permanent magnets are magnets with excellent magnetic force, such as R-Fe-B sintered magnets (here, "R" represents a rare earth element, such as Nd, Ce, Y, Dy, Tb, or a rare earth element combination), which can achieve increased output and reduced motor size. Therefore, rare earth permanent magnets have been increasingly used in various fields.
[0003] In particular, as the demand for hybrid vehicles or electric vehicles has recently increased, the demand for rare earth permanent magnets having a magnetic force improved 3 to 5 times compared with ferrite magnets according to the related art has further increased.
[0004] Meanwhile, the magnetic properties of the magnet can be expressed by improving the residual flux density and coercive force. For example, the residual flux density can be determined by the number, density and magnetic orientation of the main phase of the rare earth permanent magnet, and the coercive force indicates the durability of the magnetic force caused by the external magnetic field or heat. The coercive force has a decisive correlation with the microstructure of the rare earth permanent magnet and is determined by the refinement of the grains or the uniform distribution of the grain boundary phase.
[0005] Therefore, various methods for improving the characteristics of permanent magnets have been proposed.
[0006] Recently, for example, a grain boundary diffusion method is mainly used for improving magnetic characteristics such as coercive force by forming a coating containing a rare earth element such as Dy or Tb on the surface of a sintered magnet and then grain boundary diffusing the rare earth element into the sintered magnet.
[0007] Such a grain boundary diffusion method may include forming the coating by vapor deposition or forming the coating by application, depending on the method of forming the coating.
[0008] For example, a method of forming a coating by vapor deposition includes depositing rare earth elements on the surface of a sintered magnet to form a coating, and then performing grain boundary diffusion. In this method, the manufacturing cost increases due to the increase in the cost required for manufacturing equipment and manufacturing processes, and the productivity is poor, which makes mass production difficult.
[0009] In addition, the method of forming a coating by application includes applying rare earth elements to the surface of the sintered magnet in the form of oxides or fluorides, and then performing grain boundary diffusion. This method is relatively simple in process and has excellent productivity; however, since rare earth elements diffuse through substitution reactions, it is difficult for rare earth elements to diffuse into the sintered magnet in large quantities, resulting in a limited increase in coercivity. In particular, fluorides or oxides not only inhibit the grain boundary diffusion of pure rare earth elements, but also remain inside the manufactured permanent magnet, which results in a limited increase in coercivity.
[0010] Meanwhile, as described above, Nd-based rare earth permanent magnets have been mainly used as rare earth permanent magnets manufactured by a single alloy method, but Nd is expensive. Therefore, research has been conducted on rare earth permanent magnets containing Ce and La, the price of which is about 1 / 10 of the price of Nd.
[0011] However, in the case of Ce-based rare earth permanent magnets, the main phase can be easily formed (the ratio of R:Fe:B is 2:14:1), but its inherent magnetic properties are lower than those of Nd-based rare earth permanent magnets. In the case of La-based rare earth permanent magnets, the inherent magnetic properties are better than those of Ce-based rare earth permanent magnets, but as the La content increases, the main phase formation becomes unstable.
[0012] Therefore, when Ce-based rare earth permanent magnets and La-based rare earth permanent magnets are manufactured by a conventional single alloy method in the prior art, the Ce-based rare earth permanent magnets and La-based rare earth permanent magnets are not cost-effective due to low performance and low cost effectiveness.
[0013] The contents described as the related art are provided only to help understanding the background of the present invention and should not be regarded as corresponding to the related art known to those skilled in the art. Summary of the invention
[0014] In a preferred aspect, a rare earth permanent magnet with improved magnetic properties and a method for manufacturing the same are provided, for example, the method uses different magnetic powders (such as Ce-rich magnetic powder and Ce-free magnetic powder) and mixes the Ce-rich magnetic powder and the Ce-free magnetic powder to prepare a magnetic powder containing Ce (Ce can achieve low cost and easily form a main phase).
[0015] In one aspect, a method for manufacturing a rare earth permanent magnet is provided, which may include the following steps: preparing a mixed powder, wherein the mixed powder comprises: i) a first alloy having R1 a R2 b B c M d Fe balwherein R1 is one or two or more of La, Ce and Y; R2 is a rare earth element other than La, Ce and Y; M is a metal element; a+b is about 29 to 34 wt %; a / (a+b) is about 30 to 100 wt %; c is about 0.8 to 1.5 wt %; and d is about 0.1 to 5.0 wt %, the wt % being based on the total weight of the first alloy; and ii) a second alloy having R2 b' B c' M d' Fe bal Represents, wherein R2 is a rare earth element other than La, Ce and Y; M is a metal element; b' is about 29 to 34 wt%; c' is about 0.8 to 1.5 wt%; d' is about 0.1 to 5.0 wt%, and the wt% is based on the total weight of the second alloy; and the prepared mixed powder is sintered in a magnetic field to prepare a sintered body.
[0016] In a preferred aspect, the sintered body may be subjected to a heat treatment, preferably, the heat treatment being based on the diffusion temperature conditions of the R1 component and the R2 component contained in the prepared sintered body. For example, such a post-sintering heat treatment may include different cycles of multiple temperature treatments based on 1) the R1 component of the sintered body and 2) the diffusion conditions of the R2 component of the sintered body. A cooling period (e.g., 0.1 minute, 0.2 minute, 0.5 minute, 1 minute) may be inserted between successive heat treatments of the sintered body, for example, during which a heat source is removed or withdrawn and / or the temperature to which the sintered body is subjected is reduced by 20°C, 30°C, 40°C, 50°C, 100°C, 150°C, 200°C or more. In multiple heating cycles of the sintered body, the temperature of the first heat treatment or the first heat cycle of the sintered body may be different from the temperature of the second heat treatment or the second heat cycle of the sintered body. For example, such a first heat cycle and a second heat cycle may differ by 5°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C or more.
[0017] The term "diffusion" as used herein refers to a process used to make an alloy or a process during the manufacture of an alloy, and during the diffusion process, certain components (e.g., metal elements or atoms) among the different alloy components are transferred, moved or diffused, thereby changing the chemical composition of a portion of the alloy region.
[0018] The term "R1 component" used herein refers to all R1 contained in the sintered body after the sintering process (e.g., all elements selected from one or two or more of La, Ce, and Y), and these elements come from the first alloy (optionally, and / or the second alloy). Similarly, the term "R2 component" refers to all R2 contained in the sintered body after the sintering process (e.g., all elements selected from rare earth elements other than La, Ce, and Y), and these elements come from the first alloy and the second alloy.
[0019] The diffusion temperature of the alloy may be determined by the chemical composition of the alloy (e.g., the content ratio between the R1 component and the R2 component in the alloy composition). For example, the diffusion temperature range of the R1 component is about 550° C. to about 750° C., which is less than the diffusion temperature range of the R2 component (about 750° C. to about 950° C.). In certain embodiments, the range of the diffusion temperature of the alloy may vary relative to the content ratio thereof.
[0020] Preferably, the first alloy may be Ce-rich.
[0021] Preferably, the second alloy may be Ce-poor, or contain no Ce.
[0022] In the first alloy, R1 may include only Ce or may include at least about 70 wt % Ce based on the total weight of R1.
[0023] In the first alloy or the second alloy, M may include one or two or more selected from Co, Ni, Cu, Zn, Al, Ga, Ti, V, Cr, Mn, Zr, Nb, Mo, Hf, Ta, and W.
[0024] The mixed powder can be prepared by the following steps: preparing a first strip and a second strip respectively, the first strip being prepared by melting and then cooling a first alloy, and the second strip being prepared by melting and then cooling a second alloy; preparing a first treated powder and a second treated powder respectively, the first treated powder being prepared by hydrogenating, dehydrogenating and spray-milling the prepared first strip, and the second treated powder being prepared by hydrogenating, dehydrogenating and spray-milling the second strip; and preparing a mixed powder, including, for example, mixing the prepared first treated powder and the second treated powder.
[0025] The mixed powder may include the first treated powder and the second treated powder mixed in a weight ratio of about 50-90: about 50-10.
[0026] Alternatively, the mixed powder may be prepared by the following steps: separately preparing a first strip and a second strip, the first strip being prepared by melting and then cooling a first alloy, and the second strip being prepared by melting and then cooling a second alloy; preparing a mixed strip comprising the first strip and the second strip by mixing; and preparing the mixed powder by subjecting the prepared mixed strip to hydrogenation, dehydrogenation and jet milling treatments.
[0027] The hybrid tape may include the first tape and the second tape in a weight ratio of about 50-90: about 50-10.
[0028] The heat treatment can be performed by the following steps: a primary heat treatment at the diffusion temperature of the R1 component contained in the prepared sintered body; a secondary heat treatment at the diffusion temperature of the R2 component contained in the sintered body subjected to the primary heat treatment; and a tertiary heat treatment so that the atomic lattices of the components constituting the sintered body subjected to the secondary heat treatment are arranged.
[0029] The primary heat treatment may be performed at a temperature range of about 550°C to 750°C, the secondary heat treatment may be performed at a temperature range of about 750°C to 950°C, and the tertiary heat treatment may be performed at a temperature range of about 450°C to 550°C.
[0030] Each of the primary heat treatment step, the secondary heat treatment step, and the tertiary heat treatment step may be performed for about 0.1 hour to 20 hours.
[0031] The heat treatment may be performed by further including the following steps: cooling the sintered body subjected to the primary heat treatment after the primary heat treatment; cooling the sintered body subjected to the secondary heat treatment after the secondary heat treatment; and cooling the sintered body subjected to the tertiary heat treatment after the tertiary heat treatment.
[0032] Each of the primary cooling step, the secondary cooling step, and the tertiary cooling step may be performed at a cooling rate of about 2 to 20° C. / s.
[0033] In one aspect, a method for manufacturing a rare earth permanent magnet is provided, which may include the following steps: preparing a mixed powder, wherein the mixed powder comprises: i) a first alloy having R1 a R2 b B c M d Fe bal wherein R1 is one or two or more of La, Ce and Y; R2 is a rare earth element other than La, Ce and Y; M is a metal element; a+b is about 29 to 34 wt %; a / (a+b) is about 30 to 100 wt %; c is about 0.8 to 1.5 wt %; and d is about 0.1 to 5.0 wt %, the wt % being based on the total weight of the first alloy, and ii) a second alloy having R1 a' R2 b' B c' M d' Fe balRepresents, wherein R1 is one or two or more of La, Ce and Y; R2 is a rare earth element other than La, Ce and Y; M is a metal element; a'+b' is about 29 to 34 wt%; a' / (a'+b') is about 0 to 30% (excluding 0%); c' is 0.8 to 1.5 wt%; d' is about 0.1 to 5.0 wt%, and the wt% is based on the total weight of the second alloy; the prepared mixed powder is pressed into shape and sintered in a magnetic field to prepare a sintered body; and heat treatment is performed based on the diffusion temperature conditions of the R1 component and the R2 component contained in the prepared sintered body.
[0034] Preferably, the first alloy may be Ce-rich.
[0035] Preferably, the second alloy may be Ce-poor, or contain substantially no Ce.
[0036] In the first alloy, R1 may include only Ce or may include at least about 70 wt % Ce based on the total weight of R1.
[0037] In the first alloy or the second alloy, M may include one or two or more elements selected from Co, Ni, Cu, Zn, Al, Ga, Ti, V, Cr, Mn, Zr, Nb, Mo, Hf, Ta, and W.
[0038] The mixed powder can be prepared by the following steps: preparing a first strip and a second strip respectively, the first strip being prepared by melting and then cooling a first alloy, and the second strip being prepared by melting and cooling a second alloy; preparing a first treated powder and a second treated powder respectively, the first treated powder being prepared by subjecting the prepared first strip to hydrogenation, dehydrogenation and spray milling treatments, and the second treated powder being prepared by subjecting the prepared second strip to hydrogenation, dehydrogenation and spray milling treatments; and preparing a mixed powder including the prepared first treated powder and the second treated powder, for example, by mixing.
[0039] The mixed powder may include the first treated powder and the second treated powder mixed in a weight ratio of about 50-90: about 50-10.
[0040] Alternatively, the mixed powder may be prepared by the following steps: separately preparing a first strip and a second strip, the first strip being prepared by melting and then cooling a first alloy, and the second strip being prepared by melting and then cooling a second alloy; preparing a mixed strip comprising the first strip and the second strip by mixing; and preparing the mixed powder by subjecting the prepared mixed strip to hydrogenation, dehydrogenation and jet milling treatments.
[0041] The hybrid tape may include the first tape and the second tape in a weight ratio of about 50-90: about 50-10.
[0042] The heat treatment can be performed by the following steps: a primary heat treatment at the diffusion temperature of the R1 component contained in the prepared sintered body; a secondary heat treatment at the diffusion temperature of the R2 component contained in the sintered body subjected to the primary heat treatment; and a tertiary heat treatment so that the atomic lattices of the components constituting the sintered body subjected to the secondary heat treatment are arranged.
[0043] The primary heat treatment may be performed at a temperature range of about 550°C to 750°C, the secondary heat treatment may be performed at a temperature range of about 750°C to 950°C, and the tertiary heat treatment may be performed at a temperature range of about 450°C to 550°C.
[0044] Each of the primary heat treatment step, the secondary heat treatment step, and the tertiary heat treatment step may be performed for about 0.1 hour to 20 hours.
[0045] The heat treatment may be performed by further including the following steps: cooling the sintered body subjected to the primary heat treatment after the primary heat treatment; cooling the sintered body subjected to the secondary heat treatment after the secondary heat treatment; and cooling the sintered body subjected to the tertiary heat treatment after the tertiary heat treatment.
[0046] Each of the primary cooling step, the secondary cooling step, and the tertiary cooling step may be performed at a cooling rate of about 2 to 20° C. / s.
[0047] On the other hand, a rare earth permanent magnet is provided, which is represented by a R1-R2-BM-Fe type rare earth permanent magnet, R1 is one or two or more of La, Ce and Y, R2 is a rare earth element other than La, Ce and Y, and M is a metal element. The rare earth permanent magnet may include: (R1, R2) 2 BF 14 and a first auxiliary phase and a second auxiliary phase, wherein the first auxiliary phase does not contain Ce or substantially does not contain Ce, the second auxiliary phase contains Ce, and the first auxiliary phase and the second auxiliary phase are formed at the grain boundaries of the main phase.
[0048] Preferably, the first auxiliary phase may be Ce-poor and the second auxiliary phase may be Ce-rich.
[0049] The first auxiliary phase in the Ce-poor state can be R1 e R2 f Fe bal Indicates that e<f,e+f> About 34 wt%, the second auxiliary phase in the Ce-rich state can be R1 e’ R2 f’ Fe bal It means that e'>f', and e'+f'>about 34 weight %.
[0050] The main phase, the first auxiliary phase, and the second auxiliary phase may be formed such that R1 contains only Ce or contains at least about 70 wt % of Ce.
[0051] Other aspects of the invention are disclosed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1A and Figure 1B An exemplary method of manufacturing a rare earth permanent magnet according to an exemplary embodiment of the present invention is shown.
[0053] Figure 2 It is shown that the coercive force varies according to the Ce content in the exemplary first alloy according to the exemplary embodiment of the present invention.
[0054] Figure 3A and Figure 3B The microstructures of samples prepared according to the exemplary embodiment of the present invention according to the variation of Ce content in the exemplary first alloy are shown.
[0055] Figure 4A and Figure 4B Microstructures of samples prepared according to exemplary mixing ratios of an exemplary first alloy and an exemplary second alloy are respectively shown.
[0056] Figure 5A and Figure 5B The microstructures of a sample prepared by a conventional single alloy method in the related art and a sample prepared according to an exemplary method of the present invention are shown. DETAILED DESCRIPTION
[0057] Embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, but can be implemented in various forms. These embodiments are provided only to complete the present invention and enable those skilled in the art to fully understand the scope of the present invention.
[0058] Unless otherwise indicated, all numbers, values and / or expressions relating to quantities of ingredients, reaction conditions, polymer compositions and formulations used herein are to be understood as being modified in all instances by the term "about" since these numbers are approximate in nature and reflect the various measurement uncertainties encountered in obtaining such values.
[0059] In addition, unless otherwise stated or apparent from the context, the term "about" as used herein is understood to be within the normal tolerance range in the art, such as within 2 standard deviations of the average. "About" may be understood to be within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05%, or 0.01% of a specified value. Unless otherwise apparent from the context, all numerical values provided herein are modified by the term "about".
[0060] In this specification, when describing the range of a variable, it will be understood that the variable includes all values including the endpoints of the range. For example, a range of "5 to 10" will be understood to include any sub-ranges, such as 6 to 10, 7 to 10, 6 to 9, 7 to 9, etc., and individual values of 5, 6, 7, 8, 9 and 10, and will also be understood to include any values between the valid integers in the range, such as 5.5, 6.5, 7.5, 5.5 to 8.5, 6.5 to 9, etc. Moreover, for example, a range of "10% to 30%" will be understood to include sub-ranges, such as 10% to 15%, 12% to 18%, 20% to 30%, etc., and all integers, including values of 10%, 11%, 12%, 13%, etc. not exceeding 30%, and will also be understood to include any values between the valid integers in the specified range, such as 10.5%, 15.5%, 25.5%, etc.
[0061] Figure 1A and Figure 1B An exemplary method of manufacturing an exemplary rare earth permanent magnet according to an exemplary embodiment of the present invention is shown.
[0062] As shown in the figure, the manufacturing method of the rare earth permanent magnet may include: a mixed powder preparation step, which prepares a mixed powder comprising a first alloy in a Ce-rich state and a second alloy in a Ce-poor state; a forming step, which presses and sinters the prepared mixed powder in a magnetic field to prepare a sintered body; and a heat treatment step, which performs heat treatment according to the diffusion temperature conditions of the R1 component and the R2 component contained in the prepared sintered body, for example, by grading the heat treatment temperature.
[0063] The first alloy used may be in a Ce-rich state. a R2 b B c M d Fe bal Represents, wherein R1 is one or two or more of La, Ce and Y, R2 is a rare earth element other than La, Ce and Y, M is a metal element, a+b is about 29 to 34 wt.%, a / (a+b) is about 30 to 100%, c is about 0.8 to 1.5 wt.%, d is about 0.1 to 5.0 wt.%, and the wt.% is based on the total weight of the first alloy.
[0064] The first alloy may be formed such that R1 contains only Ce or contains at least about 70 wt % Ce. When R1 contains at least about 70 wt % Ce, Ce may be replaced by La or Y. Preferably, about 25 to 30 wt % of Ce may be replaced by La or Y, accounting for about 25 to 30 wt % of the total weight of Ce.
[0065] For example, the first alloy may be prepared with 12%Ce-19%Nd-1%B-2%M-Bal.%Fe. Preferably, the first alloy may be prepared with 12%Ce-17%Nd-2%Ho-1%B-1%Co-0.15%Cu-0.75%Al-0.35%Nb-0.35%Ga-65.4%Fe by using Ce as R1, Pr-Nd and Ho as R2, Co, Cu, Al, Nb and Ga as M.
[0066] The second alloy may be in a Ce-depleted state, or substantially free of Ce, and the second alloy may be prepared by completely excluding the element corresponding to R1 of the first alloy. b' B c' M d' Fe bal Represented, wherein R2 is a rare earth element other than La, Ce and Y, M is a metal element, b' is about 29 wt % to 34 wt %, c' is about 0.8 wt % to 1.5 wt %, and d' is about 0.1 wt % to 5.0 wt %, the wt % being based on the total weight of the second alloy.
[0067] For example, the second alloy can be prepared with 31% Nd-1% B-2% M-Bal.% Fel. Preferably, the second alloy can be prepared with 30% Nd-1% Ho-1% B-1% Co-0.15% Cu-0.25% Al-0.35% Nb-0.15% Ga-66.1% Fe by excluding R1 and using Pr-Nd and Ho as R2, using Co, Cu, Al, Nb and Ga as M.
[0068] In addition, the second alloy may be in a Ce-poor state, and the second alloy may be prepared by changing the ratio of the first alloy and a' / (a'+b') while including R1 of the first alloy. a' R2 b' B c' M d' Fe balRepresents, wherein R1 is one or two or more of La, Ce and Y, R2 is a rare earth element other than La, Ce and Y, M is a metal element, a'+b' is about 29 to 34 wt.%, a' / (a'+b') is about 0 to 30 wt.% (excluding 0%), c' is about 0.8 to 1.5 wt.%, d' is about 0.1 to 5.0 wt.%, and the wt.% is based on the total weight of the second alloy.
[0069] For example, the second alloy can be prepared with 6%Ce-25%Nd-1%B-2%M-Bal.%Fe. Preferably, the second alloy can be prepared with 6%Ce-22%Nd-3%Ho-1%B-1%Co-0.15%Cu-0.5%Al-0.35%Nb-0.25%Ga-65.75%Fe by using Ce as R1, Pr-Nd and Ho as R2, Co, Cu, Al, Nb and Ga as M.
[0070] In addition, M may appropriately include one or two or more elements selected from Co, Ni, Cu, Zn, Al, Ga, Ti, V, Cr, Mn, Zr, Nb, Mo, Hf, Ta and W.
[0071] For example, the first alloy and the second alloy may be prepared as shown in Table 1-1. In this case, the magnetic properties of the first alloy and the second alloy prepared as shown in Table 1-1 are shown in Table 1-2.
[0072] Table 1-1
[0073]
[0074]
[0075] Table 1-2
[0076]
[0077] The mixed powder preparation step is a step of preparing a mixed powder by using the first alloy and the second alloy. In this case, the mixed powder preparation step can be performed in two ways.
[0078] First, if Figure 1AAs shown, the preparation step of the mixed powder may include: a strip preparation step of preparing a first strip and a second strip respectively, the first strip is prepared by melting and then cooling a first alloy, and the second strip is prepared by melting and then cooling a second alloy; preparing a first treated powder and a second treated powder respectively, the first treated powder is prepared by hydrogenating, dehydrogenating and spray-milling (crushing) the prepared first strip, and the second treated powder is prepared by hydrogenating, dehydrogenating and spray-milling (crushing) the prepared second strip; a mixed powder preparation step, which prepares a mixed powder containing the first treated powder and the second treated powder by mixing, for example.
[0079] For example, in the above-mentioned step of preparing the mixed powder, a first strip and a second strip can be prepared respectively relative to the prepared first alloy and the second alloy, and a first treated powder and a second treated powder can be prepared by hydrogenating, dehydrogenating and spray-milling the first strip and the second strip respectively, and then the first treated powder and the second treated powder are mixed with each other.
[0080] Preferably, the preparation, hydrogenation, dehydrogenation and jet milling treatment of each of the first ribbon and the second ribbon can be carried out by the preparation, hydrogenation, dehydrogenation and jet milling treatment processes applicable to the conventional manufacturing method of rare earth permanent magnets.
[0081] However, preferably, in the mixed powder preparing step, the first treated powder (Ce-rich) and the second treated powder (Ce-poor) may be mixed with each other in a weight ratio of about 50-90:50-10.
[0082] When the mixing amount of the second treated powder (Ce-poor) is smaller than the above-specified range, the coercive force may be reduced compared with the case of the same composition manufactured by a single alloy method.
[0083] On the other hand, when the mixing amount of the second treated powder (Ce-poor) is larger than the above-specified range, the synergistic effect of the coercive force may be insufficient compared with the case of the same composition produced by the single alloy method.
[0084] The reason is that when the mixing amount of the second treated powder (Ce-poor) is greater than about 50 wt %, Nd 2 Fe 17 phase, which is a soft magnetic phase that is detrimental to the hard magnetic properties, and when the mixing amount of the first treated powder (Ce-rich) is greater than about 50 wt %, the soft magnetic phase is not formed.
[0085] In addition, when the mixing amount of the first treated powder (Ce-rich) is greater than about 50 weight %, when the following three heat treatment steps are performed, the Ce-poor (Nd-rich) phase and the Ce-rich phase can be uniformly diffused to the grain boundaries, and therefore, the magnetization reversal suppression effect can be maximized through magnetic isolation, thereby improving the hard magnetic properties.
[0086] Alternatively, when preparing a mixed powder, Figure 1B As shown, the mixed powder preparation step may include: preparing a first strip and a second strip respectively, the first strip being prepared by melting and then cooling a first alloy, and the second strip being prepared by melting and then cooling a second alloy; a mixed strip preparation step, which is, for example, preparing a mixed strip comprising the first strip and the second strip by mixing; and a mixed powder preparation step, which is preparing a mixed powder by subjecting the prepared mixed strip to hydrogenation, dehydrogenation and spray milling treatments.
[0087] Preferably, a first strip and a second strip may be prepared respectively with respect to the prepared first alloy and the second alloy, a mixed strip may be prepared by mixing the prepared first strip and the second strip with each other, and a mixed powder may be prepared by subjecting the prepared mixed strip to hydrogenation, dehydrogenation and jet milling treatments.
[0088] The preparation, hydrogenation, dehydrogenation and jet milling of the mixed strip can be carried out by the preparation, hydrogenation, dehydrogenation and jet milling processes applicable to the conventional manufacturing method of rare earth permanent magnets.
[0089] In the mixed tape preparing step, the first tape and the second tape may be mixed with each other in a weight ratio of about 50-90: about 50-10.
[0090] As described above, the step of mixing the first ribbon material and the second ribbon material with each other may be performed in any of the steps of the mixed powder preparing step.
[0091] Meanwhile, the forming step is a step of press-forming and sintering the prepared mixed powder in a magnetic field to prepare a sintered body, and the forming step is performed by a press-forming step and a sintering step applicable to a conventional manufacturing method of a rare earth permanent magnet.
[0092] In addition, the heat treatment step is performed by classifying the heat treatment temperature based on the diffusion temperature conditions of the R1 component and the R2 component contained in the prepared sintered body, for example.
[0093] For example, the heat treatment step may include: a primary heat treatment step, which performs a primary heat treatment at a diffusion temperature of the R1 component contained in the prepared sintered body; a secondary heat treatment step, which performs a secondary heat treatment at a diffusion temperature of the R2 component contained in the sintered body that has been subjected to the primary heat treatment; and a tertiary heat treatment step, which performs a tertiary heat treatment so that the atomic lattices of the components constituting the sintered body that has been subjected to the secondary heat treatment are arranged.
[0094] The primary heat treatment step may be performed at a temperature range of about 550°C to 750°C, the secondary heat treatment step may be performed at a temperature range of 750°C to about 950°C, and the tertiary heat treatment step may be performed at a temperature range of about 450°C to 550°C.
[0095] The reason why the heat treatment is carried out in three steps in the present embodiment is that by uniformly diffusing the R1 component and the R2 component and arranging the atomic lattices, a first auxiliary phase in a Ce-poor state and a second auxiliary phase in a Ce-rich state can be formed at the grain boundaries of the main phase, and the coercive force and the residual magnetic flux density can be improved by the first auxiliary phase and the second auxiliary phase formed as above.
[0096] In addition, each of the primary heat treatment step, the secondary heat treatment step, and the tertiary heat treatment step may preferably be performed for about 0.1 hour to 20 hours.
[0097] A primary cooling step for cooling the sintered body after the primary heat treatment step may be performed after the primary heat treatment step, a secondary cooling step for cooling the sintered body after the secondary heat treatment step may be performed after the secondary heat treatment step, and a tertiary cooling step for cooling the sintered body after the tertiary heat treatment step may be performed after the tertiary heat treatment step.
[0098] Each of the primary cooling step, the secondary cooling step, and the tertiary cooling step may be performed at a cooling rate of about 2 to 20° C. / s to cool the sintered body to room temperature, and then a subsequent step may be performed.
[0099] The rare earth permanent magnet manufactured by the above manufacturing method is represented as an R1-R2-BM-Fe type rare earth permanent magnet, R1 is one or two or more of La, Ce and Y, R2 is a rare earth element other than La, Ce and Y, and M is a metal element.
[0100] Specifically, the rare earth permanent magnet may include: (R1, R2) 2 BF 14 A main phase containing rare earth elements represented by the present invention; and a first auxiliary phase in a Ce-poor state or substantially containing no Ce and a second auxiliary phase in a Ce-rich state, wherein the first auxiliary phase and the second auxiliary phase are formed at grain boundaries of the main phase.
[0101] In this case, the first auxiliary phase in the Ce-poor (Nd-rich) state is composed of R1 e R2 f Fe bal It represents that R1 is one or two or more of La, Ce and Y, R2 is a rare earth element other than La, Ce and Y, e<f, and e+f>34 wt%.
[0102] In addition, the second auxiliary phase in the Ce-rich state is composed of R1 e’ R2 f’ Fe bal It represents that R1 is one or two or more of La, Ce and Y, R2 is a rare earth element other than La, Ce and Y, e'>f', and e'+f'>34 wt %.
[0103] In addition, the main phase, the first auxiliary phase, and the second auxiliary phase may be formed such that R1 may include only Ce or may include at least about 70 wt % of Ce.
[0104] Example
[0105] The rare earth permanent magnet manufactured as described above will be described with reference to Examples and Comparative Examples.
[0106] First, according to an embodiment of the present invention, a rare earth permanent magnet is manufactured by using a first alloy in a Ce-rich state and a second alloy in a Ce-poor state, but each sample is prepared by changing the Ce content in the first alloy. The coercive force of each sample is measured, and the results are shown in Table 2.
[0107] In addition, the microstructures of the sample (A) in which the Ce content in the first alloy was 20 wt % and the sample (B) in which the Ce content in the first alloy was 80 wt % were observed, and the results are shown in Figure 3A and Figure 3B .
[0108] Figure 2 is a graph showing the change in coercive force according to the change in the Ce content in the first alloy, and, Figure 3A and Figure 3B is a photograph showing the microstructure of samples prepared according to the change of Ce content in the first alloy. In this case, Figure 3A It is shown Figure 2 A microstructure photograph of sample A, and Figure 3B It is shown Figure 2 Photo 2 of the microstructure of sample B. In addition, Figure 3A and Figure 3B The analysis results of the components of the phase formed in are shown in Table 2.
[0109] Table 2
[0110]
[0111]
[0112] Conventional NdFeB magnets in the prior art consist of a main phase and a grain boundary phase. In this case, the main phase consists of Nd 2 Fe 14 B is formed, and the grain boundary phase is formed as a Ce-poor phase.
[0113] On the other hand, the NdCeFeB magnet as a result of the present invention is also composed of a main phase and a grain boundary phase. In this case, the main phase is composed of (Nd, Ce) 2 Fe 14 B is formed, and the grain boundary phase includes an Nd-rich (Ce-poor) phase and a Ce-rich phase. Here, this does not mean that Ce does not exist in the Nd-rich (Ce-poor) phase or that Nd does not exist in the Ce-rich phase. It can be determined that the amount of Nd distributed in the Ce-poor phase is greater than Ce, or the amount of Ce distributed in the Ce-rich phase is greater than Nd. Preferably, #2 and #5 are classified as Nd-rich (Ce-poor) phases (Ce is significantly less than Nd), and #6 is classified as Ce-rich phase (Nd is significantly less than Ce).
[0114] like Figure 2 As shown, the coercive force increases when the Ce content in the first alloy in the Ce-rich state is 50 wt % or more.
[0115] In addition, Figure 3A In the case of sample A (worst case) shown, the (Nd, Ce)-rich phase is mainly localized near the triple grain boundary, and (Nd, Ce) as a soft magnetic phase is observed. 2 Fe 17 From the above reasons, it can be determined that the coercive force is reduced.
[0116] On the other hand, in Figure 3B In the case of sample B (best case) shown, it can be confirmed that a network between a plurality of grains is formed by the distribution of the (Nd, Ce)-rich phase, and the (Nd, Ce)-rich phase is relatively uniformly distributed along the grains.
[0117] In addition, it can be confirmed that there is a shading difference between the (Nd, Ce)-rich phases, and the EDX analysis results show that the Ce content in the phase forming the network is relatively greater than the Nd content. It can be determined that the reason is that Ce is transformed into a liquid phase at a lower temperature than Nd in the sintering step, and the wetting of Ce is more smoothly performed compared to Nd. Therefore, it can be seen that a distribution difference occurs between the (Nd, Ce)-rich phases due to the mixing ratio of the Ce-poor powder and the Ce-rich powder.
[0118] The distributed (Nd,Ce)-rich phase magnetically isolates Re 2 Fe14 The B phase increases the magnetic exchange energy. This is because the 2:14:1 phase as the main phase has an isolation effect that exhibits a magnetization reversal suppression effect.
[0119] According to the results of the above analysis, it can be concluded that when the mixing ratio of the first alloy in a Ce-rich state is 50 wt % or more (particularly 75 wt % to 85 wt %), the coercive force increasing effect is the best.
[0120] Next, magnetic characteristics and microstructure depending on the mixing ratio of the first alloy in a Ce-rich state and the second alloy in a Ce-poor state containing no Ce were studied.
[0121] In this case, the mixing ratio of the first alloy to the second alloy was changed as shown in Table 3-1, and the measured values of the residual magnetic flux density and the coercive force depending on the change are shown in Table 3-2.
[0122] Meanwhile, in order to compare the samples in which the first alloy and the second alloy according to the embodiment of the present invention were mixed with each other and the samples formed by the single alloy method, the residual magnetic flux density and the coercive force of each sample having the same composition but prepared by the single alloy method were measured. The results are shown in Table 3-2.
[0123] In addition, the microstructure photos of samples 1-3 and 1-7 in Table 3-1 are shown in Figure 4A and Figure 4B .
[0124] Table 3-1
[0125]
[0126] Table 3-2
[0127]
[0128]
[0129] As shown in Table 3-2, it can be confirmed that when the mixing ratio of the first alloy in a Ce-rich state is 50 wt % or more, the coercive force increases compared with the single alloy method.
[0130] On the other hand, it was confirmed that when the mixing ratio of the first alloy in a Ce-rich state was less than 50 wt %, the coercive force was reduced compared with the single alloy method.
[0131] In addition, if Figure 4A As shown in FIG. 1 , it can be confirmed that Nd 2 as a soft magnetic phase is formed in the sample in which the mixing ratio of the first alloy in the Ce-rich state is 20 wt %. 2 Fe 17 phase (indicated by arrows). On the other hand, Figure 4BAs shown, it can be confirmed that the soft magnetic phase is not formed in the sample in which the mixing ratio of the first alloy in the Ce-rich state is 80 wt %.
[0132] Next, the magnetic characteristics and microstructures of the samples manufactured by the single alloy method according to the related art and the samples according to the present invention were studied.
[0133] In this case, Table 4 shows the condition of each sample and the measured values of the residual magnetic flux density and the coercive force.
[0134] In addition, the microstructure photos of samples 1-7 and sample 2-1 in Table 4 are shown in Figure 5A and Figure 5B .
[0135] Figure 5A and Figure 5B are photographs showing the microstructures of a sample prepared according to a single alloy method according to the related art and a sample prepared according to an embodiment of the present invention.
[0136] Table 4
[0137]
[0138] As shown in Table 4 and Figure 5A and Figure 5B As shown, it can be confirmed that the residual magnetic flux density and coercive force of the sample prepared according to the present invention are excellent compared with the single alloy method according to the related art.
[0139] Subsequently, tests were conducted to confirm the effect of performing the heat treatment in three steps.
[0140] In this case, the heat treatment steps were changed as shown in Table 5-1, and the measured values of the residual magnetic flux density and the coercive force depending on the changes are shown in Table 5-2.
[0141] Table 5-1
[0142]
[0143] Table 5-2
[0144]
[0145] As shown in Table 5-2, it can be confirmed that in Samples 3-1 and 3-2 which were not subjected to the primary heat treatment, the coercive force was hardly improved or the coercive force was even reduced.
[0146] In addition, it was confirmed that in Sample 3-3 in which the primary heat treatment temperature was lower than the range suggested by the present invention, there was almost no improvement in the coercive force.
[0147] On the other hand, it was confirmed that in Samples 3-4 to 3-6 in which the primary heat treatment temperature fell within the range suggested by the present invention, the coercive force increased.
[0148] Next, magnetic characteristics and microstructure depending on the mixing ratio of the first alloy in a Ce-rich state and the second alloy in a Ce-poor state having a relatively small Ce content were studied.
[0149] In this case, the mixing ratio of the first alloy to the second alloy was changed as shown in Table 6-1, and the measured values of the residual magnetic flux density and the coercive force depending on the change are shown in Table 6-2.
[0150] Meanwhile, in order to compare the samples in which the first alloy and the second alloy according to the embodiment of the present invention are mixed with each other and the samples formed by the single alloy method, the residual magnetic flux density and the coercive force of each sample having the same composition but prepared by the single alloy method are measured. The results are shown in Table 6-2.
[0151] Table 6-1
[0152]
[0153] Table 6-2
[0154]
[0155]
[0156] As shown in Table 6-2, it can be confirmed that when the mixing ratio of the first alloy in a Ce-rich state is 50 wt % or more, the coercive force increases compared with the single alloy method.
[0157] On the other hand, it was confirmed that when the mixing ratio of the first alloy in a Ce-rich state was less than 50 wt %, the coercive force was reduced compared with the single alloy method.
[0158] Next, the magnetic characteristics and microstructures of the samples manufactured by the single alloy method according to the related art and the samples according to the present invention were studied.
[0159] In this case, Table 7 shows the condition of each sample and the measured values of the residual magnetic flux density and the coercive force.
[0160] Table 7
[0161]
[0162] As shown in Table 7, it can be confirmed that the residual magnetic flux density and the coercive force of the sample prepared according to the present invention are excellent compared with the single alloy method according to the related art.
[0163] Subsequently, tests were conducted to confirm the effect of performing the heat treatment in three steps.
[0164] In this case, the heat treatment steps were changed as shown in Table 8-1, and the measured values of the residual magnetic flux density and the coercive force depending on the changes are shown in Table 8-2.
[0165] Table 8-1
[0166]
[0167]
[0168] Table 8-2
[0169]
[0170] As shown in Table 8-2, it can be confirmed that in Samples 6-1 and 6-2 which were not subjected to the primary heat treatment, the coercive force was hardly improved or the coercive force was even reduced.
[0171] In addition, it was confirmed that in Sample 6-3 in which the primary heat treatment temperature was lower than the range suggested by the present invention, there was almost no improvement in the coercive force.
[0172] On the other hand, it was confirmed that in Samples 6-4 to 6-6 in which the primary heat treatment temperature fell within the range suggested by the present invention, the coercive force increased.
[0173] According to various exemplary embodiments of the present invention, a permanent magnet can be manufactured by using Ce, which is cost-competitive compared to Nd, by classifying a magnetic powder containing Ce into a magnetic powder in a Ce-rich state and a magnetic powder in a Ce-poor state to obtain different powders and mixing them, so that the manufacturing cost of the permanent magnet can be reduced and the magnetic properties of the permanent magnet can be improved.
[0174] Although the present invention has been described with reference to the accompanying drawings and the preferred embodiments described above, the present invention is not limited thereto but is defined by the claims. Therefore, those skilled in the art will appreciate that various modifications and changes may be made without departing from the technical spirit of the claims.
Claims
1. A method for manufacturing a rare earth permanent magnet, the method include: Prepare a mixed powder, the mixed powder comprising: i) a first alloy having R1 a R2 b B c M d Fe bal wherein R1 comprises only Ce, or Ce and one or two of La and Y, wherein Ce is at least 70 wt %; R2 is a rare earth element other than La, Ce and Y; M is a metal element; a+b is 29 to 34 wt %; a / (a+b) is 30 to 100 wt %; c is 0.8 to 1.5 wt %; and d is 0.1 to 5.0 wt %, the wt % being based on the total weight of the first alloy; and ii) a second alloy having R2 as the base metal. b' B c' M d' Fe bal wherein R2 is a rare earth element other than La, Ce and Y; M is a metal element; b' is 29 to 34 wt%; c' is 0.8 to 1.5 wt%; d' is 0.1 to 5.0 wt%, the wt% being based on the total weight of the second alloy; the first alloy is mixed in a ratio of 50 wt% or more, sintering the prepared mixed powder in a magnetic field to prepare a sintered body, The sintered body is heat-treated based on the diffusion temperature conditions of the R1 component and the R2 component contained in the prepared sintered body, The heat treatment is carried out by the steps comprising: Performing a heat treatment at a diffusion temperature of the R1 component contained in the prepared sintered body; Performing a secondary heat treatment at a diffusion temperature of the R2 component contained in the sintered body subjected to the primary heat treatment; The third heat treatment is performed so that the atomic lattices of the components constituting the second heat-treated sintered body are arranged, The primary heat treatment is carried out at a temperature range of 550°C to 750°C. The secondary heat treatment is carried out in the temperature range of 750°C to 950°C. The three heat treatments are performed at a temperature range of 450°C to 550°C.
2. The method for manufacturing a rare earth permanent magnet according to claim 1, in, In the first alloy or the second alloy, M includes one or two or more elements selected from Co, Ni, Cu, Zn, Al, Ga, Ti, V, Cr, Mn, Zr, Nb, Mo, Hf, Ta and W.
3. The method for manufacturing a rare earth permanent magnet according to claim 1, in, The mixed powder is prepared by the following steps: preparing a first strip and a second strip, respectively, the first strip being prepared by melting and then cooling a first alloy, and the second strip being prepared by melting and then cooling a second alloy; preparing a first treated powder and a second treated powder respectively, wherein the first treated powder is prepared by subjecting the prepared first strip to hydrogenation, dehydrogenation and jet milling, and the second treated powder is prepared by subjecting the prepared second strip to hydrogenation, dehydrogenation and jet milling; A mixed powder including the prepared first treated powder and the second treated powder is prepared.
4. The method for manufacturing a rare earth permanent magnet according to claim 3, in, The mixed powder includes a first processed powder and a second processed powder mixed in a weight ratio of 50-90:50-10.
5. The method for manufacturing a rare earth permanent magnet according to claim 1, in, The mixed powder is prepared by the following steps: preparing a first strip and a second strip, respectively, the first strip being prepared by melting and then cooling a first alloy, and the second strip being prepared by melting and then cooling a second alloy; preparing a hybrid tape comprising a first tape and a second tape; The mixed powder is prepared by subjecting the prepared mixed strip to hydrogenation, dehydrogenation and jet milling treatments.
6. The method for manufacturing a rare earth permanent magnet according to claim 5, in, The mixed tape includes a first tape and a second tape mixed in a weight ratio of 50-90:50-10.
7. The method for manufacturing a rare earth permanent magnet according to claim 1, in, Each of the primary heat treatment, the secondary heat treatment, and the tertiary heat treatment is performed for 0.1 hour to 20 hours.
8. The method for manufacturing a rare earth permanent magnet according to claim 1, in, The heat treatment is carried out by further comprising the following steps: After the primary heat treatment, cooling the sintered body subjected to the primary heat treatment; After the secondary heat treatment, cooling the secondary heat treated sintered body; After the three heat treatments, the three-times heat-treated sintered body is cooled.
9. The method for manufacturing a rare earth permanent magnet according to claim 8, in, Each of the primary cooling, the secondary cooling, and the tertiary cooling is performed at a cooling rate of 2 to 20° C. / s.
10. A method for manufacturing a rare earth permanent magnet, the method include: Prepare a mixed powder, the mixed powder comprising: i) a first alloy having R1 a R2 b B c M d Fe bal wherein R1 comprises only Ce, or Ce and one or two of La and Y, wherein Ce is at least 70 wt %; R2 is a rare earth element other than La, Ce and Y; M is a metal element; a+b is 29 to 34 wt %; a / (a+b) is 30 to 100 wt %; c is 0.8 to 1.5 wt %; and d is 0.1 to 5.0 wt %, the wt % being based on the total weight of the first alloy; and ii) a second alloy having R1 a’ R2 b’ B c’ M d’ Fe bal wherein R1 is one or two or more of La, Ce and Y; R2 is a rare earth element other than La, Ce and Y; M is a metal element; a'+b' is 29 to 34 wt%; a' / (a'+b') is 0 to 30 wt% and 0% is excluded; c' is 0.8 to 1.5 wt%; d' is 0.1 to 5.0 wt%, the wt% being based on the total weight of the second alloy, wherein the second alloy does not substantially contain Ce; the first alloy is mixed in a ratio of 50 wt% or more, sintering the prepared mixed powder in a magnetic field to prepare a sintered body; Heat treatment is performed based on the diffusion temperature conditions of the R1 component and the R2 component contained in the prepared sintered body, The heat treatment comprises: Performing a heat treatment at a diffusion temperature of the R1 component contained in the prepared sintered body; Performing a secondary heat treatment at a diffusion temperature of the R2 component contained in the sintered body subjected to the primary heat treatment; The third heat treatment is performed so that the atomic lattices of the components constituting the second heat-treated sintered body are arranged, The primary heat treatment is carried out at a temperature range of 550°C to 750°C. The secondary heat treatment is carried out in the temperature range of 750°C to 950°C. The three heat treatments are performed at a temperature range of 450°C to 550°C.
11. The method for manufacturing a rare earth permanent magnet according to claim 10, in, Each of the primary heat treatment, the secondary heat treatment, and the tertiary heat treatment is performed for 0.1 hour to 20 hours.
12. A rare earth permanent magnet, which is represented by R1-R2-BM-Fe type rare earth permanent magnet, R1 contains only Ce, or contains Ce and one or two of La and Y, wherein Ce is at least 70% by weight, R2 is a rare earth element other than La, Ce and Y, and M is a metal element, and the rare earth permanent magnet comprises: From (R1, R2) 2 BF 14 the main aspect represented; and a first auxiliary phase and a second auxiliary phase, wherein the first auxiliary phase and the second auxiliary phase are formed at the grain boundaries of the main phase, The first auxiliary phase in the Ce-poor state is R1 e R2 f Fe bal Indicates that e<f,e+f> 34% by weight The second auxiliary phase is R1 e’ R2 f’ Fe bal It means that e'>f', and e'+f'>34 wt%. 13 . The rare earth permanent magnet according to claim 12 , wherein the main phase and the second auxiliary phase are formed such that R1 contains only Ce or contains at least 70 wt % of Ce.
Citation Information
Patent Citations
Preparation method of R-T-B permanent magnet
CN105469973A
Rare Earth Permanent Magnet And Method For Manufacturing Thereof
CN105788839A