Solid electrolyte, lithium ion battery electrode and lithium ion battery

By replacing part of Li atoms as multivalent atoms in the solid electrolyte of the lithium-ion battery, forming a compound with high conductivity at high temperatures, the problem of low conductivity at high temperatures is solved, and the problem of low conductivity at high temperatures is achieved at 90°C High conductivity and excellent battery performance.

CN113544088BActive Publication Date: 2024-11-26TOYOHASHI UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080018914.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-08
Filing Date
2020-03-06
Publication Date
2024-11-26
Estimated Expiration
2040-03-06

AI Technical Summary

Technical Problem

The current lithium-ion batteries have low conductivity under high temperature conditions, making it difficult to meet the application needs of above 50°C, especially at 90°C, which is not sufficient to ensure excellent battery performance.

Method used

Some Li atoms in Li3PS4, Li6PS5X and Li7P3S11 are replaced by multivalent atoms (such as Ca, Sr, Ba, Zn, Y, Al) to form solid electrolytes with high conductivity at high temperatures, and through different multivalent atom substitution mechanisms Improve the conductivity of lithium ions.

Benefits of technology

The conductivity at 90°C reaches 6×10-3S/cm or above, which is suitable for high-temperature applications above 50°C, significantly improving the battery performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113544088B_ABST
    Figure CN113544088B_ABST
Patent Text Reader

Abstract

The solid electrolyte of the present invention is characterized by comprising at least one of the following compounds (A), (B) and (C). (A) Li 3 PS 4 Compounds in which some of the Li atoms in the (B) Li 6 PS 5 A compound in which some of the Li atoms in X (X is Cl, Br or I) are replaced by polyvalent atoms, (C)Li 7 P 3 S 11 A compound obtained by replacing some of the Li atoms in the compound with polyvalent atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to electrodes such as positive electrodes constituting a lithium ion battery, a solid electrolyte suitable as a forming material for an electrolyte layer or the like, an electrode for a lithium ion battery, and a lithium ion battery. Background Art

[0002] A lithium ion battery is a secondary battery having a structure in which lithium is separated from a positive electrode in the form of ions and moves to a negative electrode and is occluded during charging, and lithium ions are inserted from the negative electrode to the positive electrode and returned during discharging. This lithium ion battery has characteristics such as a large energy density and a long life. Therefore, it has been widely used as a power source for home appliances such as personal computers and cameras, portable electronic devices or communication devices such as mobile phones, and power tools such as power tools. Recently, it has also been applied to large batteries mounted on electric vehicles (EVs), hybrid electric vehicles (HEVs), etc. In such a lithium ion battery, if a solid electrolyte is used instead of an electrolytic solution containing a flammable organic solvent, not only can the safety device be simplified, but also the manufacturing cost, productivity, etc. are excellent. Therefore, research on various materials is being actively carried out. Among them, it is considered that a solid electrolyte containing sulfide has a high conductivity (lithium ion conductivity) and is useful for achieving a high output of the battery.

[0003] As a sulfide solid electrolyte, a solid electrolyte containing lithium element, phosphorus element and sulfur element is known.

[0004] For example, Patent Document 1 discloses a lithium magnesium thiophosphate compound represented by the general formula Li 4- 2x Mg x P2S6 (where 0 < x < 2), and it is described that the conductivity of the compound with x = 2 / 3 is lower than 2.0×10 -6 S / cm.

[0005] Patent Document 2 discloses an all-solid battery system characterized by having an all-solid battery and a heating unit. The all-solid battery includes a positive electrode active material layer containing a positive electrode active material, a negative electrode active material layer containing a negative electrode active material, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer. The heating unit heats the all-solid battery to 40°C or higher, and at least one of the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer contains a sulfide solid electrolyte material substantially free of crosslinked sulfur. And it is described that preferred sulfide solid electrolyte materials are Li2S-P2S5 materials, Li2S-SiS2 materials, Li2S-GeS2 materials or Li2S-Al2S3 materials, and the preferred ionic conductivity at room temperature is 10 -4 S / cm or more.

[0006] Patent document 3 discloses a sulfide solid electrolyte material, characterized in that it has a crystalline phase in which the Li element at the 2a site of the γ-Li3PS4 crystal phase is replaced by an M element (the M element is at least one of a Cu(I) element, a Mg element, and a Ca element) as the main body, and records that the preferred ionic conductivity at 25°C is 1×10 -3 S / cm or more.

[0007] Patent document 4 discloses a sulfide solid electrolyte material, characterized in that it contains Li element, Mg element, P element, S element, and PS4 as an anion structure. 3- The structure is mainly composed of Mg, the ratio of Mg element to the total of Li element and Mg element is in the range of 1.69 to 5.26 mol %, and the preferred ion conductivity at 25°C is described as 1×10 -3 S / cm or more.

[0008] Prior art literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2003-206110

[0010] Patent Document 2: Japanese Patent Application Publication No. 2011-28893

[0011] Patent Document 3: Japanese Patent Application Publication No. 2016-62718

[0012] Patent Document 4: Japanese Patent Application Publication No. 2016-62720 Summary of the invention

[0013] In recent years, the use of lithium-ion batteries has been increasing under conditions of 50°C or above, where the stability of solid electrolytes is beneficial to conductivity, and solid electrolytes constituting lithium-ion batteries that can cope with such uses are required. The present invention aims to provide a solid electrolyte having high conductivity at 90°C, and an electrode for a lithium-ion battery and a lithium-ion battery comprising the solid electrolyte.

[0014] The present invention is as follows.

[0015] [1] A solid electrolyte comprising at least one of the following compounds (A), (B) and (C).

[0016] Compound (A): a compound obtained by replacing some of the Li atoms in Li3PS4 with polyvalent atoms (except Mg);

[0017] Compound (B): a compound obtained by replacing some of the Li atoms in Li6PS5X (X is Cl, Br or I) with polyvalent atoms;

[0018] Compound (C): Li7P3S 11 Compounds obtained by replacing some of the Li atoms in

[0019] [2] The solid electrolyte according to [1] above, wherein the polyvalent atoms are derived from Group 2 elements, Group 3 elements, Group 12 elements, and Group 13 elements of the periodic table.

[0020] [3] According to the solid electrolyte described in [1] or [2] above, the polyvalent atom is at least one selected from Ca, Sr, Ba, Zn, Y and Al.

[0021] [4] The solid electrolyte according to any one of [1] to [3] above, wherein the polyvalent atom in the compound (A) is at least one selected from Ca and Al.

[0022] [5] The solid electrolyte according to any one of [1] to [3] above, wherein the polyvalent atom in the compound (B) is at least one selected from the group consisting of Ca, Sr, Ba, Zn, Y and Al.

[0023] [6] The solid electrolyte according to any one of [1] to [3] above, wherein the polyvalent atom in the compound (C) is at least one selected from Ca, Zn and Al.

[0024] [7] The solid electrolyte according to [4] or [6] above, wherein the compound (A) or compound (C) further contains at least one halogen atom selected from F, Cl, Br and I.

[0025] [8] The solid electrolyte according to any one of [1] to [7], wherein the electrical conductivity at 90°C is 6×10 -3 S / cm or more.

[0026] [9] A lithium ion battery electrode comprising the solid electrolyte according to any one of [1] to [8] above.

[0027]

[10] A lithium ion battery comprising the lithium ion battery electrode according to [9] above.

[0028] The solid electrolyte of the present invention is suitable as a material for forming an electrode constituting a lithium ion battery having a heating unit, for example, and can provide a solid battery having high lithium ion conductivity at a temperature of 50° C. or higher and exhibiting excellent battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic cross-sectional view showing the main parts of the lithium ion battery of the present invention.

[0030] Figure 2 This is a schematic cross-sectional view showing an example of the lithium ion battery of the present invention including a heating unit.

[0031] Figure 3 This is a schematic cross-sectional view showing another example of the lithium ion battery of the present invention including a heating unit.

[0032] Figure 4 These are Raman spectra of the solid compositions obtained in Experimental Examples 1 to 4.

[0033] Figure 5 This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 1 to 4.

[0034] Figure 6 This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 5 to 7.

[0035] Figure 7 These are X-ray diffraction images of the solid compositions obtained in Experimental Examples 8, 9, 11, and 13.

[0036] Figure 8 This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 8 to 13.

[0037] Fig. 9 These are X-ray diffraction images of the solid compositions obtained in Experimental Examples 8 and 14 to 18.

[0038] Fig.10 This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 8 and 14 to 18.

[0039] Fig.11 These are X-ray diffraction images of the solid compositions obtained in Experimental Examples 19 to 23.

[0040] Fig.12 This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 to 23.

[0041] Fig.13 These are X-ray diffraction images of the solid compositions obtained in Experimental Examples 19 and 24.

[0042] Fig.14 This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 and 24.

[0043] Fig.15 These are X-ray diffraction images of the solid compositions obtained in Experimental Examples 19 and 25 to 29.

[0044] Fig.16This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 and 25 to 29.

[0045] Fig.17 This is an X-ray diffraction image of the solid composition obtained in Experimental Examples 19 and 30.

[0046] Fig.18 This is a graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 and 30. DETAILED DESCRIPTION

[0047] The solid electrolyte of the present invention contains at least one of the following compound (A), compound (B) and compound (C).

[0048] (A): Compounds obtained by replacing some Li atoms in Li3PS4 with polyvalent atoms (except Mg);

[0049] (B): A compound obtained by replacing some of the Li atoms in Li6PS5X (X is Cl, Br or I) with polyvalent atoms;

[0050] (C):Li7P3S 11 A compound obtained by replacing some of the Li atoms in the compound with polyvalent atoms.

[0051] Generally, the ion conductivity (σ) of a solid electrolyte material is in accordance with the following equation with respect to temperature (T), and therefore, the Li ion conductivity of the solid electrolyte material increases at a high temperature: Here, E represents the apparent activation energy of conduction, and R represents the gas constant.

[0052] In(σ)=-E / (R·T)+ln(a)

[0053] In the case of using a liquid electrolyte, the decomposition of the electrolyte becomes significant in a high temperature region above 50°C, so it is difficult to use in a high temperature region. In the case of using a solid electrolyte, there is no such stability problem, so it is possible to utilize a high temperature region that is conducive to conductivity. In the case of actually utilizing such a high temperature region, it is difficult to use it because water boils at above 100°C, etc., taking into account the impact on surrounding components. The above-mentioned compounds (A), (B) and (C) having high conductivity at 90°C become very easy to use and advantageous electrolytes when considering their applications.

[0054] Furthermore, the present inventors believe that by exerting a conduction mechanism different from the ion conduction of Li ions in the conventionally known solid electrolytes in the above-mentioned compounds (A), (B) and (C), unprecedented high conductivity is achieved at 90°C. For example, if a monovalent Li ion is replaced by a divalent Ca ion, two monovalent Li ions are separated. The Ca ion enters one of the two ions, and the other one becomes a hole. It is presumed that the conduction via the hopping of the hole works.

[0055] The polyvalent atoms in the compounds (A), (B) and (C) are preferably derived from elements of Group 2, Group 3, Group 12 or Group 13 of the periodic table. That is, the valence of the polyvalent atoms is preferably divalent or trivalent.

[0056] The chemical formulae of the above compounds (A), (B) and (C) can be expressed depending on the valence of the polyvalent atoms contained. The chemical formulae containing divalent and trivalent polyvalent atoms are shown below.

[0057] The above compound (A) is represented by the following general formulae (1) and (2).

[0058] Li 3-2a M 1 a PS4 (1)

[0059] (Where M 1 is a divalent atom other than Mg, 0.001≤a≤0.2)

[0060] Li 3-3b M 2 b PS4 (2)

[0061] (Where M 2 is a trivalent atom, 0.001≤b≤0.15)

[0062] In the above general formula (1), M 1 It is preferably at least one selected from Ca, Sr, Ba, Ra, Zn and Cd, more preferably Ca, Sr, Ba and Zn, and particularly preferably Ca. In addition, a is preferably 0.005≤a≤0.15.

[0063] In the above general formula (2), M 2 It is preferably at least one selected from Sc, Y, Al, Ga and In, more preferably Y and Al, and particularly preferably Al. In addition, b is preferably 0.005≤b≤0.1.

[0064] The compound (A) may further contain at least one halogen atom selected from F, Cl, Br and I in addition to the atoms represented by the general formulae (1) and (2). The constituent ratio of the halogen atom is preferably 0.003 to 0.1 mol per 1 mol of Li atoms. In this case, the molar ratio of P to S may deviate from that specified in the general formulae.

[0065] The above compound (B) is represented by the following general formulae (3) and (4).

[0066] Li 6-2c M 3 c PS5X (3)

[0067] (Where M 3 is a divalent atom, X is Cl, Br or I, 0.001≤c≤0.2)

[0068] Li 6-3d M 4 d PS5X (4)

[0069] (Where M 4 is a trivalent atom, X is Cl, Br or I, 0.001≤d≤0.15)

[0070] In the above general formula (3), M 3 It is preferably at least one selected from Mg, Ca, Sr, Ba, Ra, Zn and Cd, more preferably Mg, Ca, Sr, Ba and Zn, and particularly preferably Ca, Sr, Ba and Zn. In addition, c is preferably 0.005≤c≤0.15.

[0071] In the above general formula (4), M 4 It is preferably at least one selected from Sc, Y, Al, Ga and In, and particularly preferably Y and Al. In addition, d is preferably 0.005≤d≤0.1.

[0072] The above compound (C) is represented by the following general formulae (5) and (6).

[0073] Li 7-2e M 5 e P3S 11 (5)

[0074] (Where M 5 is a divalent atom, 0.001≤e≤0.1)

[0075] Li 7-3f M 6 f P3S 11 (6)

[0076] (Where M 6 is a trivalent atom, 0.001≤f≤0.05)

[0077] In the above general formula (5), M 5 It is preferably at least one selected from Mg, Ca, Sr, Ba, Ra, Zn and Cd, more preferably Mg, Ca, Sr, Ba and Zn, and particularly preferably Ca and Zn. In addition, e is preferably 0.005≤e≤0.05.

[0078] In the above general formula (6), M 6 It is preferably at least one selected from Sc, Y, Al, Ga and In, more preferably Y and Al, and particularly preferably Al. In addition, f is preferably 0.005≤f≤0.03.

[0079] The compound (C) may further contain at least one halogen atom selected from F, Cl, Br and I in addition to the atoms represented by the general formulae (5) and (6). The constituent ratio of the halogen atom is preferably 0.001 to 0.014 mol per 1 mol of Li atoms. In this case, the molar ratio of P to S may deviate from that specified in the general formulae.

[0080] Furthermore, in the above general formulas (1) to (6), anion atoms other than P, S and X may be contained within a range that does not deteriorate the performance, and the ratio of P, S and X may deviate from the above general formula. As a standard for the composition ratio of anion atoms that does not deteriorate the performance, it is 0.1 mol or less relative to 1 mol of Li atoms.

[0081] The above compounds (A), (B) and (C) may be crystalline or amorphous.

[0082] The above compounds (A), (B) and (C) can be produced by contact reaction using compound raw materials containing elements constituting the respective compounds so that the molar ratio of the respective elements becomes a predetermined value.

[0083] Examples of the compound raw materials include Li2S, phosphorus sulfide (P2S5, P4S3, P4S7, etc.), and lithium halide LiX (lithium chloride, lithium bromide, lithium iodide, etc.).

[0084] Examples of the compound raw material containing a polyvalent atom include sulfides, thiophosphoric acid compounds, and halides.

[0085] From the viewpoint of their reactivity, the above-mentioned compound raw materials are preferably in the form of fine particles. The upper limit of the maximum length of the particles is preferably 100 μm, and more preferably 50 μm. However, the lower limit is usually 0.01 μm. Furthermore, when the size of the raw material is large, it is preferably ground with a mortar and pestle so that it falls within the above-mentioned preferred range before use.

[0086] When the contact reaction is used to produce the above-mentioned compound (A), (B) or (C), a ball mill (planetary ball mill, etc.), a vibration mill, a turbo mill, a mechanical fusion, a disc mill, etc. can be used. In addition, the method of using the compound raw materials is not particularly limited, and the total amount of all raw materials can be used to make them contact reaction, and the contact reaction can also be made while changing the type or supply amount of raw materials in stages.

[0087] The atmosphere of the reaction system in the above-mentioned contact reaction is not particularly limited, and may be composed of an inert gas such as nitrogen or argon, dry air, or the like.

[0088] The above-mentioned contact reaction can be carried out in the presence of a solvent. Examples of the solvent include alcohols, carboxylic acids, carboxylic acid esters, ethers, aldehydes, ketones, carbonates, nitriles, amides, nitro groups, phosphates, and halogenated hydrocarbons.

[0089] In the production of the above-mentioned compound (A) or (B), when the contact reaction is carried out in the presence of a solvent, a suspension containing the compound (A) or (B) is usually obtained. Therefore, by removing the solvent thereafter, a solid composition containing the compound (A) or (B) can be obtained.

[0090] As a method for removing the solvent, for example, a method of drying at a temperature lower than 100° C., preferably a method of drying at about 15° C. to 60° C. can be cited. The solvent can be removed under either atmospheric pressure or reduced pressure. The atmosphere when removing the solvent under atmospheric pressure is preferably dry air or an inert gas. The solid composition obtained by removing the solvent may also be further heated.

[0091] In the production of the above-mentioned compound (C), it is preferred to heat-treat the solid composition obtained by removing the solvent from the obtained suspension in the same manner. As a method for removing the solvent from the suspension, for example, a method of drying under reduced pressure at 100° C. to 180° C. can be cited. In the case where the solid composition obtained by removing the solvent is further heat-treated, a method of heat-treating in dry air or an inert gas atmosphere, preferably at 200° C. to 300° C. can be applied.

[0092] In addition, in the manufacture of the above-mentioned compound (A), (B) or (C), as a method for conducting a contact reaction in the presence of the above-mentioned solvent, for example, in the case of a solvent containing a saturated fatty acid ester or a dialkyl carbonate, a ball mill (planetary ball mill, etc.) may not be used, and a method for conducting a contact reaction while vibrating a slurry containing a reaction raw material and a solvent using a stirring blade, a stirring bar, beads, balls, ultrasonic waves, etc. is preferred. In the case of conducting a contact reaction by this method, the solvent can be removed to obtain a solid composition by drying the obtained suspension preferably below 100° C., more preferably at about 15° C. to 60° C. The removal of the solvent can be carried out under either atmospheric pressure or reduced pressure. The atmosphere when removing the solvent under atmospheric pressure is preferably dry air or an inert gas. The solid composition obtained by removing the solvent may also be further heat-treated.

[0093] The solid electrolyte of the present invention may contain other solid electrolytes, conductive additives, binders and other compounds as long as it contains at least one of the above-mentioned compounds (A), (B) and (C). Furthermore, the upper limit of the content of other compounds relative to the whole solid electrolyte is preferably 50% by mass, more preferably 30% by mass.

[0094] In the solid electrolyte of the present invention, the electrical conductivity can be measured by an AC impedance method, and the electrical conductivity at 90°C is higher than that of the case containing the unsubstituted compound. For example, the solid electrolyte containing the above compound (A) or (B) has an electrical conductivity of preferably 6×10 -3 S / cm or more, more preferably 8×10 -3 S / cm or more, more preferably 1×10 -2 S / cm or higher. In addition, the electrical conductivity of the solid electrolyte containing the above compound (C) at 90°C is preferably 4.5×10 -3 S / cm or more, more preferably 6.0×10 -3 S / cm or more, particularly preferably 9.0×10 -3 Therefore, high conductivity can be obtained within a temperature range including preferably 50° C. or higher, more preferably 70° C. or higher.

[0095] The solid electrolyte of the present invention is suitable as a constituent material of an electrode (positive electrode or negative electrode) or an electrolyte layer of a lithium ion battery. Figure 1This is an example of a cross section of a main part of a lithium ion battery, which includes a positive electrode 11, a negative electrode 13, an electrolyte layer 15 disposed between the positive electrode 11 and the negative electrode 13, a positive electrode collector 17 for collecting current from the positive electrode 11, and a negative electrode collector 19 for collecting current from the negative electrode 15. The solid electrolyte of the present invention is suitable as a constituent material of the positive electrode 11, the solid electrolyte layer 15, the negative electrode 13, etc. of a lithium ion battery having such a structure. Among them, it is particularly suitable for forming the positive electrode 11 and the solid electrolyte layer 15.

[0096] The positive electrode 11 and the negative electrode 13 as the lithium ion battery electrodes of the present invention generally contain a positive electrode active material and a negative electrode active material, respectively, and may further contain a binder, a conductive auxiliary agent, other solid electrolytes, and the like.

[0097] Examples of the above-mentioned adhesives include fluorine-containing resins such as polytetrafluoroethylene (PTFE), polyhexafluoropropylene (PHFP), polyvinylidene fluoride (PVdF), and vinylidene fluoride-hexafluoropropylene copolymers; polyolefin resins such as polypropylene and polyethylene; ethylene-propylene-non-conjugated diene rubbers (EPDM, etc.), sulfonated EPDM, and natural butyl rubber (NBR).

[0098] As the conductive auxiliary agent, a material composed of a carbon material, a metal powder, a metal compound, etc. can be used, and a carbon material is preferably used. Examples of the carbon material include plate-like conductive materials such as graphene; linear conductive materials such as carbon nanotubes and carbon fibers; carbon blacks such as Ketjen black, acetylene black, DENKA BLACK (trade name), thermal black, channel black, and granular conductive materials such as graphite.

[0099] Examples of the positive electrode active material contained in the positive electrode 11 include MoO x , WO x , VO x , Li x CoO y (LiCoO2, etc.), Li x MnO y (LiMnO2, LiMn2O4, etc.), Li x NiO y (LiNiO2, etc.), Li x VO y (LiVO2, etc.), Li x Mn y Ni z Co w O(LiNi 1 / 3Co 1 / 3 Mn 1 / 3 O2, etc.), Li x FeP x O y(LiFePO4, etc.), Li x MnP x O y (LiMnPO4, etc.), Li x NiP x O y (LiNiPO4, etc.), Li x CuP x O y (LiCuPO4, etc.) and other oxide (complex oxide) materials; (MoS x , CuS x 、TiS x , WS x )、Li x S y , Li x P y S z Sulfide-based materials; selenide-based materials, etc.

[0100] Examples of the negative electrode active material contained in the negative electrode 13 include carbon materials; metals such as lithium, indium, aluminum, silicon, or alloys containing these; Sn; x O y 、MoO x , WO x , Li x CoO y (LiCoO2, etc.), Li x Mn y Ni z Co w O(LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc.), Li x CuP x O y (LiCuPO4, etc.) and other oxide (complex oxide) materials.

[0101] The electrolyte layer 15 is not particularly limited as long as it contains a solid electrolyte, but is preferably substantially composed of a solid electrolyte. In this case, it may be composed only of the solid electrolyte of the present invention described above, or may be composed of the solid electrolyte of the present invention described above and other solid electrolytes.

[0102] The electrolyte layer 15 is generally in the shape of a sheet.

[0103] The positive electrode current collector 17 or the negative electrode current collector 19 can be made of, for example, stainless steel, gold, platinum, copper, zinc, nickel, tin, aluminum, or an alloy thereof, and can have a plate-like body, a foil-like body, a mesh-like body, or the like.

[0104] As described above, since the electrical conductivity of the solid electrolyte of the present invention is sufficiently high at 90°C, a lithium ion battery having an electrode or electrolyte layer containing the solid electrolyte can exhibit excellent battery performance at a temperature preferably above 50°C, more preferably above 70°C (the upper limit is usually 250°C). A lithium ion battery that can exhibit such an effect preferably has Figure 1 The main part of the unit is heated.

[0105] The lithium ion battery of the present invention comprises the above-mentioned electrode for a lithium ion battery of the present invention, and particularly preferably comprises an electrolyte layer containing the above-mentioned solid electrolyte of the present invention.

[0106] In addition, the lithium ion battery of the present invention has Figure 1 In the case of a unit for heating the main part of the device, the heating unit is not particularly limited, but is preferably a heating element. The structure of the heating element is not particularly limited, but it is preferably heated by a resistor.

[0107] Figure 1 The main part of the battery is usually accommodated inside a storage body (battery case), so the heating element is arranged on the outer peripheral surface side of the main part, the inner surface side of the storage body, inside or outside.

[0108] Figure 2 and Figure 3 This is a schematic diagram illustrating a lithium ion battery of the present invention.

[0109] Figure 2 A lithium ion battery 100 includes: a positive electrode 11 containing solid electrolyte glass and a positive electrode active material, a negative electrode 13 containing solid electrolyte glass and a negative electrode active material, an electrolyte layer 15 disposed between the positive electrode 11 and the negative electrode 13, a positive electrode collector 17 for collecting current from the positive electrode 11, a negative electrode collector 19 for collecting current from the negative electrode 15, a housing 21 for housing them, and a heating element 23 disposed on the outer surface of the housing 21. Figure 2 In the embodiment, the heating element 23 covers the entire outer surface of the storage body 21, but the present invention is not limited thereto and may cover only a part of the outer surface. Figure 2 In the embodiment, the storage body 21 and the heat generating body 23 are in contact with each other, but the present invention is not limited thereto, and a space may be provided between the storage body 21 and the heat generating body 23 .

[0110] also, Figure 3A lithium ion battery 100 includes: a positive electrode 11 containing solid electrolyte glass and a positive electrode active material, a negative electrode 13 containing solid electrolyte glass and a negative electrode active material, an electrolyte layer 15 disposed between the positive electrode 11 and the negative electrode 13, a positive electrode collector 17 for collecting current from the positive electrode 11, a negative electrode collector 19 for collecting current from the negative electrode 15, a heating element 23 disposed on the outer surface of the main part, and a storage body 21 for storing these components. Figure 3 In the embodiment, the heating element 23 covers the entire outer surface of the main part, but the present invention is not limited to this.

[0111] Example

[0112] 1. Manufacturing raw materials

[0113] The raw materials used in the production of the solid electrolyte are as follows.

[0114] 1-1. Lithium sulfide (Li2S) powder

[0115] "Li2S" (trade name) manufactured by Mitsuwa Chemical Industries, Ltd. was used. The purity was 99.9% and the particle size was about 50 μm.

[0116] 1-2. Phosphorus pentasulfide (P2S5) powder

[0117] "P2S5" (trade name) manufactured by Aldrich Co. was used. The purity was 99% and the particle size was 100 μm.

[0118] 1-3. Calcium sulfide (CaS) powder

[0119] "CaS" (trade name) manufactured by Kojundo Chemical Research Institute Co., Ltd. was used. The purity was 99.9% and the particle size was about 50 μm.

[0120] 1-4. Aluminum sulfide (Al2S3) powder

[0121] "Al2S3" (trade name) manufactured by Kojundo Chemical Research Institute Co., Ltd. was used. The purity was 98% and the particle size was about 50 μm.

[0122] 1-5. Magnesium sulfide (MgS) powder

[0123] "MgS" (trade name) manufactured by Kojundo Chemical Research Institute Co., Ltd. was used. The purity was 99.9% and the particle size was several tens of μm.

[0124] 1-6. Strontium chloride (SrCl2) powder

[0125] "SrCl2" (trade name) manufactured by Aldrich was used. The purity was 99.9% and the particle size was several mm.

[0126] 1-7. Barium sulfide (BaS) powder

[0127] "BaS" (trade name) manufactured by Kojundo Chemical Research Institute Co., Ltd. was used. The purity was 99.9% and the particle size was several tens of μm.

[0128] 1-8. Zinc chloride (ZnCl2) powder

[0129] "ZnCl2" (trade name) manufactured by Kojundo Chemical Research Institute Co., Ltd. was used. The purity was 99.9% and the particle size was several mm.

[0130] 1-9. Yttrium chloride (YCl3) powder

[0131] "YCl3" (trade name) manufactured by Kojundo Chemical Research Institute Co., Ltd. was used. The purity was 99.9% and the particle size was several mm.

[0132] 1-10. Calcium thiophosphate (Ca3(PS4)2) powder

[0133] A synthetic product obtained from calcium sulfide (CaS) powder and phosphorus pentasulfide (P2S5) powder was used. The particle size was 20 μm.

[0134] 1-11. Calcium iodide (CaI2) powder

[0135] "CaI2" (trade name) manufactured by Aldrich was used. The purity was 99.9% and the particle size was several mm.

[0136] 1-12. Calcium fluoride (CaF2) powder

[0137] "CaF2" (trade name) manufactured by Aldrich Co. was used. The purity was 99.9% and the particle size was several mm.

[0138] 1-13. Calcium chloride (CaCl2) powder

[0139] "CaCl2" (trade name) manufactured by Aldrich was used. The purity was 99.9% and the particle size was 10 mesh or less.

[0140] 1-14. Lithium chloride (LiCl) powder

[0141] "LiCl" (trade name) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used. The purity was 99.9% and the particle size was several tens of μm.

[0142] 1-15. Acetonitrile

[0143] "Acetonitrile" (trade name) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. was used. The purity was 99.9%.

[0144] 1-16. Calcium iodide (CaI2) powder

[0145] "CaI2" (trade name) manufactured by Aldrich was used. The purity was 99.9% and the particle size was several mm.

[0146] 1-17. Aluminum iodide (AlI3) powder

[0147] "AlI3" (trade name) manufactured by Aldrich Co. was used. The purity was 99.9% and the particle size was several mm.

[0148] 1-18. Zinc iodide (ZnI2) powder

[0149] "ZnI2" (trade name) manufactured by Aldrich Co. was used. The purity was 99.9% and the particle size was several mm.

[0150] 2. Fabrication and evaluation of solid electrolytes

[0151] A solid electrolyte was produced using the above raw materials, and the electrical conductivity was measured by the following method.

[0152] <Measurement method of electrical conductivity>

[0153] The solid electrolyte was made into a disk-shaped test piece (size: radius 5mm×height 0.6mm) using a uniaxial hydraulic press, and placed in a measuring unit (glass container) under an argon atmosphere. A tape heater connected to a thermostat and a heat insulating material were wound around the measuring unit (glass container). The test piece was slowly heated from room temperature using an IMPEDANCE ANALYZER "S1260" (model name) manufactured by SOLATRON, and the conductivity was measured at 50°C, 70°C, 90°C, 110°C or 130°C. Furthermore, the conductivity was measured after the test piece was kept at each temperature for 1 hour. In addition, the conductivity was measured sequentially at each temperature starting from the low temperature side, but the temperature was not raised in stages for measurement, but a method was adopted in which, for example, after measuring at 50°C, the temperature was temporarily returned to 25°C, and then the temperature was raised to 70°C for measurement.

[0154] Experimental Example 1 (Manufacturing of Li3PS4)

[0155] Lithium sulfide (Li2S) powder and phosphorus pentasulfide (P2S5) powder were weighed and mixed so that the molar ratio of Li, P and S was 3:1:4. Then, the mixed powder was put into a planetary ball mill (container: made of zirconia) manufactured by Frisch Co., Ltd. together with zirconia balls with a diameter of 15 mm, and mechanical grinding was performed at a rotation speed of 600 rpm for 20 hours.

[0156] The obtained reaction product (solid composition) was used as a solid electrolyte, and the conductivity was measured. The result was 2.0×10 -3 S / cm.

[0157] Experimental Example 2 (Li 2.94 Mg 0.03 PS4 Manufacturing)

[0158] The same operation as in Experimental Example 1 was performed except that lithium sulfide (Li2S) powder, magnesium sulfide (MgS) powder and phosphorus pentasulfide (P2S5) powder were used in a molar ratio of Li, Mg, P and S of 2.94:0.03:1:4.

[0159] The obtained reaction product (solid composition) was measured by X-ray diffraction, and the result showed that it was amorphous. Therefore, after Raman spectroscopy analysis, in the obtained spectrum, the peak at 420 cm -1 PS4 seen nearby 3- The peak (refer to Figure 4 ).

[0160] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 4.9×10 -3 S / cm.

[0161] Experimental Example 3 (Li 2.94 Ca 0.03 PS4 Manufacturing)

[0162] The same operation as in Experimental Example 1 was performed except that lithium sulfide (Li2S) powder, calcium sulfide (CaS) powder and phosphorus pentasulfide (P2S5) powder were used in a molar ratio of Li, Ca, P and S of 2.94:0.03:1:4.

[0163] The obtained reaction product (solid composition) was measured by X-ray diffraction, and the result showed that it was amorphous. Therefore, Raman spectroscopy was performed, and in the obtained spectrum, the peak at 420 cm -1 PS4 seen nearby 3- The peak (refer to Figure 4 ).

[0164] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 9.1×10 -3 S / cm.

[0165] Experimental Example 4 (Li 2.94 Al 0.02 PS4 Manufacturing)

[0166] The same operation as in Experimental Example 1 was performed except that lithium sulfide (Li2S) powder, aluminum sulfide (Al2S3) powder and phosphorus pentasulfide (P2S5) powder were used in a molar ratio of Li, Al, P and S of 2.94:0.02:1:4.

[0167] The obtained reaction product (solid composition) was measured by X-ray diffraction, and the result showed that it was amorphous. Therefore, Raman spectroscopy was performed, and in the obtained spectrum, the peak at 420 cm -1 PS4 seen nearby 3- The peak (refer to Figure 4 ).

[0168] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 9.9×10 -3 S / cm.

[0169] Figure 5 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 1 to 4.

[0170] Experimental Example 5 (Li 2.94 Ca 0.03 PS4 Manufacturing)

[0171] The same operation as in Experimental Example 3 was performed except that calcium thiophosphate (Ca3(PS4)2) powder was used instead of calcium sulfide (CaS) powder.

[0172] The obtained reaction product (solid composition) was used as a solid electrolyte, and the conductivity was measured. The result was 9.1×10 -3 S / cm.

[0173] Experimental Example 6 (Li 2.94 Ca 0.03 P 0.98 S 3.92 I 0.06 Manufacturing)

[0174] The same operation as in Experimental Example 3 was performed except that calcium iodide (CaI 2 ) powder was used instead of calcium sulfide (CaS) powder.

[0175] The obtained reaction product (solid composition) was used as a solid electrolyte, and the conductivity was measured. The result was 8.9×10 -3 S / cm.

[0176] Experimental Example 7 (Li 2.94 Ca 0.03 P 0.98 S 3.92 F 0.06 Manufacturing)

[0177] The same operation as in Experimental Example 3 was performed except that calcium fluoride (CaF 2 ) powder was used instead of calcium sulfide (CaS) powder.

[0178] The obtained reaction product (solid composition) was used as a solid electrolyte, and the conductivity was measured. The result was 6.2×10 -3 S / cm.

[0179] Figure 6 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 5 to 7.

[0180] Experimental Example 8 (Manufacturing of Li6PS5Cl)

[0181] Lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and lithium chloride (LiCl) powder were weighed and mixed so that the molar ratio of Li, P, S and Cl was 6:1:5:1. Then, the mixed powder was put into a planetary ball mill (container: made of zirconia) manufactured by Frisch Co., Ltd. together with zirconia balls with a diameter of 15 mm, and mechanical grinding was performed for 20 hours at a rotation speed of 600 rpm.

[0182] The obtained reaction product (solid composition) was used as a solid electrolyte, and the conductivity was measured. The result was 4.3×10 -3 S / cm.

[0183] Experimental Example 9 (Li 5.98 Ca 0.01 Production of PS5Cl)

[0184] Lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder, lithium chloride (LiCl) powder and calcium chloride (CaCl2) powder were used in a molar ratio of Li, Ca, P, S and Cl of 5.98:0.01:1:5:1, and the same operation as Experimental Example 8 was performed except that the powder was used.

[0185] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite type crystal structure (refer to Figure 7 ).

[0186] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 6.97×10 -3 S / cm.

[0187] Experimental Example 10 (Li 5.96 Ca 0.02 Production of PS5Cl)

[0188] Lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder, lithium chloride (LiCl) powder and calcium chloride (CaCl2) powder were used in a molar ratio of Li, Ca, P, S and Cl of 5.96:0.02:1:5:1, and the same operation as Experimental Example 9 was performed except that the powder was used.

[0189] The obtained reaction product (solid composition) was used as a solid electrolyte, and the conductivity was measured. The result was 17.2×10 -3 S / cm.

[0190] Experimental Example 11 (Li 5.94 Ca 0.03 Production of PS5Cl)

[0191] Lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder, lithium chloride (LiCl) powder and calcium chloride (CaCl2) powder were used in a molar ratio of Li, Ca, P, S and Cl of 5.94:0.03:1:5:1, and the same operation as Experimental Example 9 was performed except that the powder was used.

[0192] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite-type crystal structure (refer to Figure 7 ).

[0193] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 23.0×10 -3 S / cm.

[0194] Experimental Example 12 (Li 5.9 Ca 0.05 Production of PS5Cl)

[0195] Lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder, lithium chloride (LiCl) powder and calcium chloride (CaCl2) powder were used in a molar ratio of Li, Ca, P, S and Cl of 5.9:0.05:1:5:1, and the same operation as Experimental Example 9 was performed except that the powder was used.

[0196] The obtained reaction product (solid composition) was used as a solid electrolyte, and the conductivity was measured. The result was 18.0×10 -3 S / cm.

[0197] Experimental Example 13 (Li 5.8 Ca 0.1 Production of PS5Cl)

[0198] Lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder, lithium chloride (LiCl) powder and calcium chloride (CaCl2) powder were used in a molar ratio of Li, Ca, P, S and Cl of 5.8:0.1:1:5:1, and the same operation as Experimental Example 9 was performed except that the powder was used.

[0199] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite-type crystal structure (refer to Figure 7 ).

[0200] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 15.9×10 -3 S / cm.

[0201] Figure 8 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 8 to 13.

[0202] Experimental Example 14 (Li 5.94 Ba 0.03 Production of PS5Cl)

[0203] The same operation as in Experimental Example 11 was performed except that lithium sulfide (Li2S) powder, barium sulfide (BaS) powder, phosphorus pentasulfide (P2S5) powder and lithium chloride (LiCl) powder were used in a molar ratio of Li, Ba, P, S and Cl of 5.94:0.03:1:5:1.

[0204] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite-type crystal structure (refer to Fig. 9 ).

[0205] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 18.3×10 -3 S / cm.

[0206] Experimental Example 15 (Li 5.94 Zn 0.03 Production of PS5Cl)

[0207] The same operation as in Experimental Example 11 was performed except that lithium sulfide (Li2S) powder, zinc sulfide (ZnS) powder, phosphorus pentasulfide (P2S5) powder and lithium chloride (LiCl) powder were used in a molar ratio of Li, Zn, P, S and Cl of 5.94:0.03:1:5:1.

[0208] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite-type crystal structure (refer to Fig. 9 ).

[0209] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 24.3×10 -3 S / cm.

[0210] Experimental Example 16 (Li 5.94 Y 0.02 Production of PS5Cl)

[0211] The same operation as in Experimental Example 11 was performed except that lithium sulfide (Li2S) powder, yttrium sulfide (Y2S3) powder, phosphorus pentasulfide (P2S5) powder and lithium chloride (LiCl) powder were used in a molar ratio of Li, Y, P, S and Cl of 5.94:0.02:1:5:1.

[0212] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite-type crystal structure (refer to Fig. 9 ).

[0213] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 33.2×10 -3 S / cm.

[0214] Experimental Example 17 (Li 5.94 Al 0.02 Production of PS5Cl)

[0215] The same operation as in Experimental Example 11 was performed except that lithium sulfide (Li2S) powder, aluminum sulfide (Al2S3) powder, phosphorus pentasulfide (P2S5) powder and lithium chloride (LiCl) powder were used in a molar ratio of Li, Al, P, S and Cl of 5.94:0.02:1:5:1.

[0216] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite-type crystal structure (refer to Fig. 9 ).

[0217] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 18.4×10 -3 S / cm.

[0218] Experimental Example 18 (Li 5.94 Sr 0.03 Production of PS5Cl)

[0219] Lithium sulfide (Li2S) powder, strontium chloride (SrCl2) powder, phosphorus pentasulfide (P2S5) powder and lithium chloride (LiCl) powder were used in a molar ratio of Li, Sr, P, S and Cl of 5.94:0.03:1:5:1, and the same operations as Experimental Example 11 were performed except that the powder was used.

[0220] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the result showed that it had an argyrodite-type crystal structure (refer to Fig. 9 ).

[0221] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 21.4×10 -3 S / cm.

[0222] Fig.10 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 14 to 18.

[0223] Experimental Example 19 (Li7P3S 11 Manufacturing)

[0224] The precursor suspension was synthesized by using lithium sulfide (Li2S) powder and phosphorus pentasulfide (P2S5) powder as raw materials in a molar ratio of Li, P and S of 7:3:11, using acetonitrile (40 ml) as a reaction solvent, stirring at 60°C for 24 hours. The synthesized suspension was dried under reduced pressure at 160°C to remove the solvent to obtain a precursor powder. The obtained precursor powder was heat-treated at 270°C under an argon atmosphere to obtain a reaction product (solid composition).

[0225] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.11 ).

[0226] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 3.0×10 -3 S / cm.

[0227] Experimental Example 20 (Li 6.99 Ca 0.005 P 3.00 S 10.98 I 0.01 Manufacturing)

[0228] With the molar ratio of Li, Ca, P, S and I being 6.99:0.005:3.00:10.98:0.01, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and calcium iodide (CaI2) powder were used as raw materials, and the same operation as Experimental Example 19 was performed except for this.

[0229] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.11 ). No peak derived from CaI2 was observed.

[0230] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 4.0×10 -3 S / cm.

[0231] Experimental Example 21 (Li 6.98 Ca 0.01 P 2.99 S 10.97 I 0.02 Manufacturing)

[0232] With the molar ratio of Li, Ca, P, S and I being 6.98:0.01:2.99:10.97:0.02, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and calcium iodide (CaI2) powder were used as raw materials, and the same operations as those in Experimental Example 19 were performed except for this.

[0233] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.11 ). No peak derived from CaI2 was observed.

[0234] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 5.0×10 -3 S / cm.

[0235] Experimental Example 22 (Li 6.96 Ca 0.02 P 2.98 S 10.94 I 0.04 Manufacturing)

[0236] With the molar ratio of Li, Ca, P, S and I being 6.96:0.02:2.98:10.94:0.04, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and calcium iodide (CaI2) powder were used as raw materials, and the same operation as Experimental Example 19 was performed except for this.

[0237] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.11 ). No peak derived from CaI2 was observed.

[0238] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 14.0×10 -3 S / cm.

[0239] Experimental Example 23 (Li 6.94 Ca 0.03 P 2.97 S 10.90 I 0.06 Manufacturing)

[0240] With the molar ratio of Li, Ca, P, S and I being 6.94:0.03:2.97:10.90:0.06, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and calcium iodide (CaI2) powder were used as raw materials, and the same operations as those in Experimental Example 19 were performed except for this.

[0241] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.11 ). No peak derived from CaI2 was observed.

[0242] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 7.9×10 -3 S / cm.

[0243] Fig.12 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 to 23.

[0244] Experimental Example 24

[0245] For manufacturing Li 6.90 Ca 0.05 P 2.96 S 10.84 I 0.1For the purpose of this experiment, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and calcium iodide (CaI2) powder were used as raw materials in a molar ratio of Li, Ca, P, S and I of 6.90:0.05:2.96:10.84:0.1, and the same operations as those in Experimental Example 19 were performed otherwise.

[0246] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.13 ). Furthermore, a peak derived from CaI2 is seen, indicating that the solid solubility limit has been exceeded.

[0247] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 17.0×10 -3 S / cm.

[0248] In this example, as described above, a peak of CaI2 was observed by X-ray diffraction, but this was because the solid solubility limit of CaI2 was exceeded and the target compound was not obtained. Therefore, it is believed that the obtained solid composition is composed of Li7P3S 11 The solid electrolyte (Li7P3S in Experimental Example 19) is composed of a compound in which some of the Li atoms in the solid electrolyte are replaced by Ca atoms and the residual raw material (CaI2). Moreover, the conductivity of the solid composition is almost unaffected by the residual raw material and is higher than that of the unsubstituted solid electrolyte (Li7P3S in Experimental Example 19). 11 )high.

[0249] Fig.14 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 and 24.

[0250] Experimental Example 25 (Li 6.985 Al 0.005 P 2.99 S 10.98 I 0.015 Manufacturing)

[0251] With the molar ratio of Li, Al, P, S and I being 6.985:0.005:2.99:10.98:0.015, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and aluminum iodide (AlI3) powder were used as raw materials, and the same operations as those in Experimental Example 19 were performed except for this.

[0252] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.15). No peak derived from AlI3 was observed.

[0253] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 11.4×10 -3 S / cm.

[0254] Experimental Example 26 (Li 6.97 Al 0.01 P 2.99 S 10.95 I 0.03 Manufacturing)

[0255] With the molar ratio of Li, Al, P, S and I being 6.97:0.01:2.99:10.95:0.03, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and aluminum iodide (AlI3) powder were used as raw materials, and the same operations as those in Experimental Example 19 were performed except for this.

[0256] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.15 ). No peak derived from AlI3 was observed.

[0257] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 13.4×10 -3 S / cm.

[0258] Experimental Example 27 (Li 6.94 Al 0.02 P 2.97 S 10.90 I 0.06 Manufacturing)

[0259] With the molar ratio of Li, Al, P, S and I being 6.94:0.02:2.97:10.90:0.06, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and aluminum iodide (AlI3) powder were used as raw materials, and the same operations as Experimental Example 19 were performed except for this.

[0260] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.15 ). No peak derived from AlI3 was observed.

[0261] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 6.82×10-3 S / cm.

[0262] Experimental Example 28 (Li 6.925 Al 0.025 P 2.97 S 10.88 I 0.075 Manufacturing)

[0263] With the molar ratio of Li, Al, P, S and I being 6.925:0.025:2.97:10.88:0.075, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and aluminum iodide (AlI3) powder were used as raw materials, and the same operations as those in Experimental Example 19 were performed except for this.

[0264] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.15 ).

[0265] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 10.7×10 -3 S / cm.

[0266] Experimental Example 29

[0267] For manufacturing Li 6.91 Al 0.03 P 2.96 S 10.86 I 0.09 For the purpose of this experiment, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and aluminum iodide (AlI3) powder were used as raw materials in a molar ratio of Li, Al, P, S and I of 6.91:0.03:2.96:10.86:0.09, and the same operations as in Experimental Example 19 were performed otherwise.

[0268] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.15 ). Furthermore, a peak derived from AlI3 is observed, indicating that the solid solubility limit has been exceeded.

[0269] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 15.0×10 -3 S / cm.

[0270] In this example, as described above, the peak of AlI3 was observed by X-ray diffraction, but this was because the solid solubility limit of AlI3 was exceeded and the target compound was not obtained. Therefore, it is believed that the obtained solid composition is composed of Li7P3S 11 The solid electrolyte (Li7P3S in Experimental Example 19) is composed of a compound in which some of the Li atoms in the solid electrolyte are replaced by Al atoms and the residual raw material (AlI3). Moreover, the conductivity of the solid composition is almost unaffected by the residual raw material and is higher than that of the unsubstituted solid electrolyte (Li7P3S in Experimental Example 19). 11 )high.

[0271] Fig.16 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 and 25 to 29.

[0272] Experimental Example 30 (Li 6.98 Zn 0.01 P 2.99 S 10.97 I 0.02 Manufacturing)

[0273] With the molar ratio of Li, Zn, P, S and I being 6.98:0.01:2.99:10.97:0.02, lithium sulfide (Li2S) powder, phosphorus pentasulfide (P2S5) powder and zinc iodide (ZnI2) powder were used as raw materials, and the same operations as those in Experimental Example 19 were performed except for this.

[0274] The obtained reaction product (solid composition) was subjected to X-ray diffraction measurement, and the results showed that it contained a small amount of Li4P2S6 and Li3PS4 crystals, but had Li7P3S 11 The crystal structure (refer to Fig.17 ). No peak derived from ZnI2 was observed.

[0275] In addition, the electrical conductivity of the solid composition was measured as a solid electrolyte and the result was 9.2×10 -3 S / cm.

[0276] Fig.18 A graph showing the temperature dependence of the electrical conductivity of the solid electrolytes obtained in Experimental Examples 19 and 30.

[0277] Industrial Applicability

[0278] The solid electrolyte of the present invention is suitable as a constituent material of lithium-ion batteries in large batteries such as personal computers, cameras and other household appliances, power storage devices, portable electronic devices such as mobile phones or communication equipment, power tools and the like, and electric vehicles (EVs), hybrid electric vehicles (HEVs), etc., that is, a constituent material of electrodes or electrolyte layers for lithium-ion batteries.

[0279] Description of Reference Numerals

[0280] 11: Positive electrode

[0281] 13: Negative electrode

[0282] 5: Electrolyte layer

[0283] 17: Positive electrode collector

[0284] 19: Negative electrode collector

[0285] 21: Storage

[0286] 23: Heat generating element

[0287] 100: Lithium-ion battery

Claims

1. A solid electrolyte, characterized in that: Containing at least one of the following compounds (B1), (B2), (B3) and (B4), Compound (B1): Li 5.94 Ca 0.03 PS5Cl; Compound (B2): Li 5.94 Zn 0.03 PS5Cl; Compound (B3): Li 5.94 Y 0.02 PS5Cl; Compound (B4): Li 5.94 Sr 0.03 PS5Cl.

2. A lithium ion battery electrode, characterized in that: Contains the solid electrolyte according to claim 1.

3. A lithium ion battery, characterized in that: A lithium ion battery electrode according to claim 2.