Solid-state batteries
By designing the shape of the electrode layer in a solid battery as a tapered shape with the side surface in contact with the external terminals, the side reaction problems caused by moisture intrusion are solved, and the long-term reliability and structural stability of the battery are improved.
Patent Information
- Application Number
- CN202080022443.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Solid batteries are prone to undesirable side reactions when moisture invades, resulting in deterioration of battery characteristics.
A solid battery laminate is designed, in which the shape of the electrode layer becomes tapered on the side surface in contact with the external terminal, which increases the interval distance during moisture invasion and reduces the occurrence of side reactions.
It effectively prevents the deterioration of solid battery performance and improves the long-term reliability and structural stability of the battery.
Smart Images

Figure CN113597688B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a solid battery. Background Art
[0002] Secondary batteries that can be repeatedly charged and discharged have been used in various applications. For example, secondary batteries are used as power sources for electronic devices such as smartphones and laptop computers.
[0003] In a secondary battery, ion movement contributes to charging and discharging, and a liquid electrolyte is generally used as a medium for ion movement. That is, a so-called electrolyte is used in a secondary battery. However, in such a secondary battery, safety is generally required in terms of preventing leakage of the electrolyte. In addition, organic solvents and the like used in the electrolyte are flammable substances, and therefore safety is also required in this regard.
[0004] Therefore, research is being conducted on solid batteries using solid electrolytes instead of electrolyte solutions.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2016-207540 Summary of the invention
[0008] Technical problem to be solved by the invention
[0009] Solid-state batteries need to reliably take necessary measures in advance against moisture in the air. This is because if moisture enters the interior of a solid-state battery, side reactions other than battery reactions may occur in the components of the solid-state battery (for example, the electrode layer), causing degradation of the battery characteristics.
[0010] The inventors of the present application have recognized that there are still problems to be overcome in the currently proposed solid-state batteries, and have discovered the necessity of taking corresponding countermeasures. Specifically, the inventors of the present application have discovered the following problems.
[0011] A solid battery has a solid battery stack composed of a positive electrode layer, a negative electrode layer, and a solid electrolyte layer therebetween (see Patent Document 1). Figure 8 (A) and Figure 8 As shown in (B), in the solid battery stack 500', the positive electrode layer 10A, the solid electrolyte layer 20, and the negative electrode layer 10B are stacked in sequence. In the solid battery stack 500', a positive terminal 30A and a negative terminal 30B as external terminals are provided in a manner connected to two opposing side surfaces (i.e., the positive electrode side end face 500'A and the negative electrode side end face 500'B). Among them, in the existing solid battery, the positive electrode layer and the negative electrode layer usually adopt a shape that is roughly rectangular in a plan view.
[0012] In such a solid battery, water may sometimes intrude into the solid battery stack from the boundary between the solid battery stack and the external terminal (particularly the corner of the solid battery stack). In the solid battery stack, if the distance between such a water intrusion site and the electrode layer is insufficient, the intruded water easily reaches the electrode layer, causing an unexpected side reaction in the electrode layer, which may cause the degradation of the battery characteristics.
[0013] The present invention has been made in view of this problem. That is, the main object of the present invention is to provide a solid battery that can reduce the occurrence of undesired side reactions even when moisture intrudes into the interior of a solid battery stack, thereby more appropriately preventing degradation of battery performance.
[0014] Means for solving technical problems
[0015] The inventors of the present application have attempted to solve the above-mentioned problems by approaching the problem from a new direction instead of simply extending the existing technology. As a result, they have completed the invention of a solid-state battery that achieves the above-mentioned main purpose.
[0016] The present invention provides a solid battery having:
[0017] A solid battery stack having at least one battery constituent unit along a stacking direction, wherein the battery constituent unit has a positive electrode layer, a negative electrode layer, and a solid electrolyte layer sandwiched between the positive electrode layer and the negative electrode layer; and
[0018] The external terminals of the positive terminal and the negative terminal are respectively provided on the side surfaces of the solid battery stack.
[0019] In a plan view of the solid battery, at least one of the positive electrode layer and the negative electrode layer has a tapered shape whose size decreases toward a side surface of the side surface where the electrode layer contacts the external terminal.
[0020] Effects of the Invention
[0021] The solid battery of the present invention can reduce the occurrence of undesired side reactions even when moisture intrudes into the interior of the solid battery stack, thereby more appropriately preventing degradation of battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a plan view schematically showing one embodiment of the solid battery of the present invention.
[0023] Figure 2 This is a plan view schematically showing an embodiment in which the electrode layer in the solid battery of the present invention is formed into a tapered shape.
[0024] Figure 3This is a plan view schematically showing another embodiment in which the electrode layer in the solid battery of the present invention is tapered.
[0025] Figure 4 This is a plan view schematically showing another embodiment in which the electrode layer in the solid battery of the present invention is tapered.
[0026] Figure 5 This is a plan view schematically showing one embodiment of the solid battery of the present invention.
[0027] Figure 6 This is a cross-sectional view schematically showing one embodiment of the solid battery of the present invention.
[0028] Figure 7 It is a schematic diagram (cross-sectional view (left figure) and plan view (right figure)) for explaining a method for manufacturing a solid battery according to one embodiment of the present invention.
[0029] Figure 8 It is a schematic diagram (cross-sectional view and plan view) of an existing solid battery. DETAILED DESCRIPTION
[0030] The "solid battery" of the present invention will be described in detail below. Although the description will be made with reference to the drawings as needed, the contents of the drawings are only schematically and exemplarily shown for understanding the present invention, and the appearance and dimensional ratios may be different from the actual objects.
[0031] The "solid battery" described in the present invention refers to a battery whose constituent elements are composed of solids in a broad sense, and refers to an all-solid battery whose constituent elements (especially preferably all constituent elements) are composed of solids in a narrow sense. In a preferred embodiment, the solid battery in the present invention is a stacked solid battery, which is configured to form layers stacked on each other to form a battery constituent unit, and preferably, the above layers are composed of sintered bodies. It should be pointed out that "solid batteries" include not only so-called "secondary batteries" that can be repeatedly charged and discharged, but also "primary batteries" that can only be discharged. In a preferred embodiment of the present invention, the "solid battery" is a secondary battery. "Secondary battery" is not overly rigid in its name, for example, it can also include power storage devices, etc.
[0032] The "plan view" described in this specification is based on the form when the object is observed from the upper side or the lower side along the thickness direction, wherein the thickness direction is based on the stacking direction of the layers constituting the solid battery. In addition, the "cross-sectional view" described in this specification is based on the form when observed from a direction substantially perpendicular to the thickness direction (in simple terms, the form after being cut by a plane parallel to the thickness direction), wherein the thickness direction is based on the stacking direction of the layers constituting the solid battery.
[0033] [Basic structure of solid-state batteries]
[0034] The solid battery has a solid battery stack, and the solid battery stack includes at least one battery constituent unit along the stacking direction, and the battery constituent unit is composed of a positive electrode layer, a negative electrode layer, and a solid electrolyte layer interposed therebetween.
[0035] When each layer constituting a solid battery is formed by firing, the positive electrode layer, negative electrode layer, and solid electrolyte layer form a sintered layer. Preferably, the positive electrode layer, negative electrode layer, and solid electrolyte are fired integrally with each other, so that the battery constituent unit forms an integral sintered body.
[0036] The positive electrode layer is an electrode layer comprising at least a positive electrode active material. The positive electrode layer may further comprise a solid electrolyte and / or a positive electrode current collecting layer. In a preferred embodiment, the positive electrode layer is composed of a sintered body comprising at least a positive electrode active material, solid electrolyte particles and a positive electrode current collecting layer. On the other hand, the negative electrode layer is an electrode layer comprising at least a negative electrode active material. The negative electrode layer may further comprise a solid electrolyte and / or a negative electrode current collecting layer. In a preferred embodiment, the negative electrode layer is composed of a sintered body comprising at least a negative electrode active material, solid electrolyte particles and a negative electrode current collecting layer.
[0037] The positive electrode active material and the negative electrode active material are substances that participate in electron transport in a solid battery. Charge and discharge are performed by moving (conducting) ions between the positive electrode layer and the negative electrode layer via a solid electrolyte, and transferring electrons between the positive electrode layer and the negative electrode layer via an external circuit. The positive electrode layer and the negative electrode layer are particularly preferably layers of lithium ions or sodium ions that can be absorbed and released. That is, it is preferably a fully solid secondary battery in which lithium ions move between the positive electrode layer and the negative electrode layer via a solid electrolyte to charge and discharge the battery.
[0038] (Positive electrode active material)
[0039] The positive electrode active material contained in the positive electrode layer is, for example, a lithium-containing compound. The type of lithium compound is not particularly limited, and examples thereof include lithium transition metal composite oxides and lithium transition metal phosphate compounds. Lithium transition metal composite oxides are a general term for oxides containing lithium and one or more transition metal elements as constituent elements, and lithium transition metal phosphate compounds are a general term for phosphate compounds containing lithium and one or more transition metal elements as constituent elements. The type of transition metal element is not particularly limited, and examples thereof include cobalt (Co), nickel (Ni), manganese (Mn), and iron (Fe).
[0040] Lithium transition metal composite oxides are, for example, Li x M1O2 and Li y Compounds represented by M2O4, etc. Lithium transition metal phosphate compounds are, for example, Li zCompounds represented by M3PO4, etc. Among them, M1, M2, and M3 are each one or more transition metal elements. The values of x, y, and z are each arbitrary.
[0041] Specifically, the lithium transition metal composite oxides are, for example, LiCoO2, LiNiO2, LiVO2, LiCrO2, LiMn2O4, etc. In addition, the lithium transition metal phosphate compounds are, for example, LiFePO4, LiCoPO4, etc.
[0042] In addition, in the case where the positive electrode layer is a layer capable of occluding and releasing sodium ions, as the positive electrode active material, at least one selected from the group consisting of sodium-containing phosphate compounds having a NASICON (sodium superionic conductor) type structure, sodium-containing phosphate compounds having an olivine type structure, sodium-containing layered oxides, and sodium-containing oxides having a spinel type structure can be cited.
[0043] (Negative electrode active material)
[0044] As the negative electrode active material contained in the negative electrode layer, for example, carbon materials, metal materials, lithium alloys, and lithium-containing compounds, etc.
[0045] Specifically, the carbon materials are, for example, graphite, graphitizable carbon, non-graphitizable carbon, mesocarbon microbeads (MCMB), highly oriented pyrolytic graphite (HOPG), etc.
[0046] The metal materials are a general term for materials containing any one or more of metal elements and metalloid elements that can form an alloy with lithium as constituent elements. The metal materials can be a single substance, an alloy, or a compound. The purity of the single substance described here is not necessarily limited to 100%, so the single substance can also contain trace impurities.
[0047] The metal elements and metalloid group elements are, for example, silicon (Si), tin (Sn), aluminum (Al), indium (In), magnesium (Mg), boron (B), gallium (Ga), germanium (Ge), lead (Pb), bismuth (Bi), cadmium (Cd), titanium (Ti), chromium (Cr), iron (Fe), niobium (Nb), molybdenum (Mo), silver (Ag), zinc (Zn), hafnium (Hf), zirconium (Zr), yttrium (Y), palladium (Pd), and platinum (Pt), etc.
[0048] Specifically, the metal materials are, for example, Si, Sn, SiB4, TiSi2, SiC, Si3N4, SiO v (0 < v ≤ 2), LiSiO, SnO w (0 < w ≤ 2), SnSiO3, LiSnO, and Mg2Sn, etc.
[0049] The lithium-containing compound is, for example, a lithium transition metal composite oxide. The definition of the lithium transition metal composite oxide is as described above. Specifically, the lithium transition metal composite oxide is, for example, Li3V2(PO4)3, Li3Fe2(PO4)3, LiTi2(PO4)3, LiCuPO4, Li4Ti5O 12 wait.
[0050] In addition, when the negative electrode layer is a layer that can absorb and release sodium ions, the negative electrode active material that can absorb and release sodium ions can be at least one selected from the group consisting of sodium-containing phosphate compounds with a NASICON type structure, sodium-containing phosphate compounds with an olivine type structure, and sodium-containing oxides with a spinel type structure.
[0051] It should be noted that the positive electrode layer and / or the negative electrode layer may contain a conductive additive. The conductive additive contained in the positive electrode layer and / or the negative electrode layer may be, for example, a carbon material and a metal material. Specifically, carbon materials may be, for example, graphite and carbon nanotubes. Metal materials may be, for example, copper (Cu), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), indium (In), gold (Au), platinum (Pt), silver (Ag) and palladium (Pd), or an alloy of two or more thereof.
[0052] In addition, the positive electrode layer and / or the negative electrode layer may further include a binder. The binder may be, for example, any one or more of synthetic rubber and polymer materials. Specifically, the synthetic rubber may be, for example, styrene butadiene rubber, fluorine rubber, and ethylene propylene rubber. The polymer material may be, for example, at least one selected from the group consisting of polyvinylidene fluoride, polyimide, and acrylic resin.
[0053] In addition, the positive electrode layer and / or the negative electrode layer may further contain a sintering aid. Examples of the sintering aid include at least one selected from the group consisting of lithium oxide, sodium oxide, potassium oxide, boron oxide, silicon oxide, bismuth oxide, and phosphorus oxide.
[0054] The thickness of the positive electrode layer and the negative electrode layer is not particularly limited, and can be, for example, independently 2 μm to 100 μm, and particularly 5 μm to 50 μm.
[0055] (Solid Electrolyte)
[0056] The solid electrolyte forms a battery unit in a solid battery and forms a layer between the positive electrode layer and the negative electrode layer that can conduct lithium ions or sodium ions. It should be noted that the solid electrolyte is at least provided between the positive electrode layer and the negative electrode layer. That is, the solid electrolyte can also exist around the positive electrode layer and / or the negative electrode layer in a manner extending from between the positive electrode layer and the negative electrode layer. As a specific solid electrolyte, for example, any one or more of a crystalline solid electrolyte and a glass ceramic solid electrolyte are included.
[0057] Crystalline solid electrolytes are crystalline electrolytes. Specifically, crystalline solid electrolytes include inorganic materials and polymer materials, and the inorganic materials include sulfides and oxides. Sulfides include Li2S-P2S5, Li2S-SiS2-Li3PO4, Li7P3S 11 , Li 3.25 Ge 0.25 P 0.75 S and Li 10 GeP2S 12 The oxide is, for example, Li x M y (PO4)3 (1≤x≤2, 1≤y≤2, M is at least one selected from the group consisting of Ti, Ge, Al, Ga and Zr), Li7La3Zr2O 12 , Li 6.75 Ln3Z 1.75 Nb 0.25 O 12 、Li6BaLa2Ta2O 12 , Li 1+x Al x Ti 2-x (PO4)3, La 2 / 3-x Li 3x TiO3、Li 1.2 Al 0.2 Ti 1.8 (PO4)3, La 0.55 Li 0.35 TiO3 and Li7La3Zr2O 12 Etc. The polymer material is, for example, polyethylene oxide (PEO) and the like.
[0058] Glass ceramic solid electrolyte is an electrolyte in a state of mixed existence of amorphous and crystalline. The glass ceramic solid electrolyte is, for example, an oxide containing lithium (Li), silicon (Si) and silicon (B) as constituent elements, and more specifically, contains lithium oxide (Li2O), silicon oxide (SiO2) and boron oxide (B2O3). The ratio of the content of lithium oxide to the total content of lithium oxide, silicon oxide and boron oxide is not particularly limited, for example, it is 40 mol% or more and 73 mol% or less. The ratio of the content of silicon oxide to the total content of lithium oxide, silicon oxide and boron oxide is not particularly limited, for example, it is 8 mol% or more and 40 mol% or less. The ratio of the content of boron oxide to the total content of lithium oxide, silicon oxide and boron oxide is not particularly limited, for example, it is 10 mol% or more and 50 mol% or less. In order to determine the respective contents of lithium oxide, silicon oxide and boron oxide, for example, inductively coupled plasma emission spectrometry (ICP-AES) is used to analyze the glass ceramic solid electrolyte.
[0059] It should be noted that, in the case where the solid electrolyte forms a layer that can conduct sodium ions, examples of the solid electrolyte include sodium-containing phosphate compounds having a NASICON structure, oxides having a perovskite structure, and oxides having a garnet-type or garnet-like structure. Examples of sodium-containing phosphate compounds having a NASICON structure include Na x M y (PO4)3 (1≤x≤2, 1≤y≤2, M is at least one selected from the group consisting of Ti, Ge, Al, Ga and Zr).
[0060] The solid electrolyte layer may further contain a binder and / or a sintering aid. The binder and / or sintering aid contained in the solid electrolyte layer may be selected from the same materials as the binder and / or sintering aid that may be contained in the positive electrode layer and / or the negative electrode layer.
[0061] The thickness of the solid electrolyte layer is not particularly limited, and may be, for example, 1 μm or more and 15 μm or less, and particularly 1 μm or more and 5 μm or less.
[0062] (Positive electrode current collecting layer / Negative electrode current collecting layer)
[0063] As the positive current collecting material constituting the positive current collecting layer and the negative current collecting material constituting the negative current collecting layer, it is preferred to use a material with high electrical conductivity, for example, it is preferred to use at least one selected from the group consisting of carbon materials, silver, palladium, gold, platinum, aluminum, copper and nickel. The positive current collecting layer and the negative current collecting layer each have an electrical connection portion for electrical connection to the outside, and are configured to be electrically connected to the terminal. The positive current collecting layer and the negative current collecting layer can each have the form of a foil, but from the viewpoint of improving electronic conductivity and reducing manufacturing costs by integral sintering, it is preferred to have an integral sintered form. It should be noted that in the case where the positive current collecting layer and the negative current collecting layer have the form of a sintered body, for example, they can be composed of a sintered body containing a conductive aid, a binder and / or a sintering aid. The conductive aid contained in the positive current collecting layer and the negative current collecting layer can, for example, be selected from the same material as the conductive aid that can be contained in the positive layer and / or the negative layer. The binder and / or sintering aid contained in the positive electrode current collecting layer and the negative electrode current collecting layer can be selected from the same materials as the binder and / or sintering aid that can be contained in the positive electrode layer and / or the negative electrode layer, for example.
[0064] The thickness of the positive electrode current collecting layer and the negative electrode current collecting layer is not particularly limited, and can be, for example, independently 1 μm to 10 μm, and particularly 1 μm to 5 μm.
[0065] (Insulation layer)
[0066] The insulating layer refers to a layer composed of a material that cannot pass electricity, that is, a non-conductive material, in a broad sense, and refers to a layer composed of an insulating material in a narrow sense. Without being particularly limited, the insulating layer can be composed of, for example, a glass material, a ceramic material, etc. As the insulating layer, for example, a glass material can be selected. Without being particularly limited, the glass material can be listed as at least one selected from the group consisting of soda-lime glass, potassium glass, borate glass, borosilicate glass, barium borosilicate glass, sub-borate glass, barium borosilicate glass, bismuth borosilicate glass, bismuth zinc borate glass, bismuth silicate glass, phosphate glass, aluminum phosphate glass, and sub-phosphate glass. In addition, without being particularly limited, the ceramic material can be listed as at least one selected from the group consisting of aluminum oxide (Al2O3), boron nitride (BN), silicon dioxide (SiO2), silicon nitride (Si3N4), zirconium oxide (ZrO2), aluminum nitride (AlN), silicon carbide (SiC) and barium titanate (BaTiO3).
[0067] (Protective layer)
[0068] The protective layer can usually be formed on the outermost side of the solid battery for electrical, physical and / or chemical protection. As the material constituting the protective layer, it is preferred that the material has excellent insulation, durability and / or moisture resistance and is safe for the environment. For example, glass, ceramics, thermosetting resins and / or light-curing resins are preferably used.
[0069] (external terminal)
[0070] Solid batteries are usually provided with external terminals. In particular, positive and negative terminals are provided in pairs on the sides of the solid battery. More specifically, a terminal on the positive electrode side connected to the positive electrode layer and a terminal on the negative electrode side connected to the negative electrode layer are provided in pairs. Such terminals are preferably made of materials with high electrical conductivity. The material of the terminal is not particularly limited, and at least one selected from the group consisting of silver, gold, platinum, aluminum, copper, tin and nickel can be cited.
[0071] [Characteristics of the solid state battery of the present invention]
[0072] The solid battery of the present invention comprises a solid battery stack, the solid battery stack comprises at least one battery constituent unit along the stacking direction, the battery constituent unit comprises a positive electrode layer, a negative electrode layer, and a solid electrolyte layer sandwiched between the positive electrode layer and the negative electrode layer. The solid battery of the present invention has external terminals of a positive electrode terminal and a negative electrode terminal respectively arranged on the side surfaces of the solid battery stack. The solid battery of the present invention has characteristics in the shape of the electrode layers (i.e., the positive electrode layer and the negative electrode layer).
[0073] More specifically, in a plan view of the solid battery, at least one of the electrode layers of the positive electrode layer and the negative electrode layer is formed into a tapered shape with a size decreasing toward the side of the electrode layer in contact with the external terminal. In other words, compared with the existing solid battery (see Figure 8 (A) and Figure 8 Compared with (B)), at least one of the electrode layers has a shape in which a corner portion of the side of the electrode layer in contact with the external terminal is missing.
[0074] exist Figure 1 In the illustrated example, in a plan view of a solid battery stack 500', a positive electrode layer 10A, a solid electrolyte layer 20, and a negative electrode layer 10B are sequentially provided. In the solid battery stack 500', a positive terminal 30A and a negative terminal 30B are provided in contact with two opposing side surfaces (i.e., a positive electrode side end surface 500'A and a negative electrode side end surface 500'B).
[0075] The positive electrode layer 10A and the negative electrode layer 10B are provided in a manner of being joined to each terminal at the positive electrode side end face 500'A and the negative electrode side end face 500'B. The positive electrode layer 10A is composed of a positive electrode tapered portion 11A and a positive electrode non-tapered portion 12A, the size of the positive electrode tapered portion 11A decreases toward the positive electrode side end face 500'A, and the positive electrode non-tapered portion 12A forms the portion other than the positive electrode tapered portion 11A, i.e., the main surface of the positive electrode layer. In addition, the negative electrode layer 10B is composed of a negative electrode tapered portion 11B and a negative electrode non-tapered portion 12B, the size of the negative electrode tapered portion 11B decreases toward the negative electrode side end face 500'B, and the negative electrode non-tapered portion 12B forms the portion other than the negative electrode tapered portion 11B, i.e., the main surface of the negative electrode layer. For example, the ratio (L1 / L2) of the tapered portion length (L1) to the non-tapered portion length (L2) in a plan view is greater than or equal to 0.01 and less than or equal to 1.0. Here, the positive electrode tapered portion 11A and the negative electrode tapered portion 11B are electrically connected to the positive electrode terminal 30A and the negative electrode terminal 30B, respectively. The non-tapered portion as the main surface of each electrode layer may be substantially rectangular in plan view.
[0076] According to the above configuration, by forming at least one of the electrode layers into a tapered shape whose size decreases toward the side in contact with the external terminal, the distance between the corner of the solid battery stack, where moisture in the air is particularly easy to penetrate, and the electrode layer can be increased compared to when the planar shape of the electrode layer is a roughly rectangular shape. In other words, compared to when the planar shape of the electrode layer is a roughly rectangular shape, the contact area between the electrode layer and the external terminal can be relatively reduced.
[0077] In addition, there are battery constituent materials such as solid electrolytes, insulating materials, and current collecting materials between the tapered portion of the electrode layer and the external terminal, and water molecules have movement resistance to these battery constituent materials, so the actual movement distance can be further increased. Thus, even if moisture invades the interior of the solid battery stack, the generation of undesired side reactions on the electrode layer can be reduced. Therefore, the degradation of the battery performance of the solid battery can be more appropriately prevented, thereby improving the long-term reliability of the solid battery.
[0078] The "taper whose dimensions decrease toward the side where the electrode layer contacts the external terminal" mentioned in this specification refers to a shape in which, in a plan view of the same electrode layer, the width dimension of at least the portion in contact with the external terminal is smaller than the width dimension of the other portions. In other words, it refers to a shape in which the corner of the side of the electrode layer in contact with the external terminal in a plan view is missing. Here, the "shape in which the corner is missing" refers to a shape in which, in a plan view of the same electrode layer, the shape of the corner (for example, a roughly right-angled shape) on the side that does not contact the external electrode is cut off.
[0079] As a specific taper, the width dimension may be formed into a curved shape in a plan view of the solid battery so as to become thinner toward the side surface in contact with the external terminal (see Figure 2 (A)), or it can also form a straight line (see Figure 2 (B)), the same tapered portion may be mixed with curved and straight shapes. From the perspective of increasing the distance between the external terminal and the electrode layer, the tapered portion is preferably formed in a curved shape in a plan view of the solid battery.
[0080] In a plan view of the solid battery, the cone can be formed approximately symmetrically in the width direction (see Figure 2 (A)), it may also be formed only at any end in the width direction (see Figure 3 (A)). From the perspective of being able to further increase the spacing between the external terminal and the electrode layer and also being able to improve the structural stability of the solid battery, the taper is preferably formed substantially symmetrically in the width direction of the solid battery in a plan view.
[0081] When the cone is formed into a curve, it can be formed into a random curve or a regular curve. The regular curve can be, for example, an arc shape that bends inward (i.e., a concave arc shape) (see Figure 2 (A)), it can also be an arc shape that bends outward (i.e., a convex arc shape) (see Figure 3 (B)). The “arc shape” may be an arc on a perfect circle or an arc on an ellipse.
[0082] In one embodiment, the cone forms an arc shape that bends inward. By adopting such a structure, the spacing distance of the corner of the solid battery stack with the electrode layer can be further increased. In addition, in the electrode layer near the external terminal, the electron conduction of the solid battery in a plan view can be made more uniform, and the reaction in the electrode layer can be more effectively uniform. In the above embodiment, the curvature radius R of the arc shape that bends inward is preferably greater than 25 μm and less than 10000 μm (see Figure 2 By setting the radius of curvature of the arc shape that bends inwardly to be within the above range, the electron flow of the electrode layer can be made more uniform, and the electrode layer and the corner of the solid battery stack can be more effectively isolated.
[0083] When the taper is formed into a straight line, the width dimension may be formed into a straight line so as to gradually taper toward the side surface in contact with the external terminal (see Figure 2 (B)), it can also be formed into a straight line in a step-wise tapering manner (see Figure 3 (C)).
[0084] In one embodiment, the cone is formed into a straight line. By adopting such a structure, the stress that can be generated in the electrode layer during the manufacture or use of the solid battery can be improved in terms of structural stability. In the above embodiment, the cone angle α of the cone is greater than 40 degrees and less than 80 degrees, and more preferably greater than 40 degrees and less than 65 degrees (see Figure 2 By setting the taper angle of the taper within the above range, the structural stability of the electrode layer can be further improved, and the electrode layer and the corner of the solid battery stack can be more effectively isolated.
[0085] In one embodiment, in a plan view of the electrode layer, the ratio of the width dimension W1 of the contact portion of the external terminal to the width dimension W2 of the portion other than the tapered portion (i.e., the non-tapered portion) is 0.3 or more and 0.9 or less (see Figure 2 (A)). If the aspect ratio is greater than 0.3, the electron flow of the electrode layer in the width direction can be made more uniform, and the structural stability of the electrode layer can be further improved. In addition, if the aspect ratio is less than 0.9, the electrode layer and the corner of the solid battery stack can be more effectively isolated. Preferably, the aspect ratio is greater than 0.5 and less than 0.8.
[0086] In one embodiment, in the electrode layer, the contour between the portion forming the taper (ie, the taper portion) and the non-tapered portion as the main surface portion of the electrode layer has a rounded corner (see Figure 4 (A)). In other words, the shape of the corner portion of the tapered portion forms a convex arc shape that bends outward. By adopting such a structure, the electron conduction on the electrode layer can be made more uniform, so that the reaction in the electrode layer can be more effectively uniform. In the above embodiment, the radius of curvature of the contour is preferably greater than 25 μm and less than 10,000 μm. By making the radius of curvature within the above range, the required amount of electrode active material can be maintained and the electron flow on the electrode layer can be made more uniform. Similarly, the contour of the junction between the electrode layer and the external terminal may also have rounded corners (see Figure 4 (B)).
[0087] In one embodiment, in a cross-sectional view of a solid battery, at least a portion of the tapered portion of an electrode layer (i.e., a positive electrode layer or a negative electrode layer) forms a non-opposing portion, and the non-opposing portion is not directly opposed to a heteropolar layer (i.e., a negative electrode layer relative to the positive electrode layer, or a positive electrode layer relative to the negative electrode layer) adjacent to the electrode layer in the stacking direction. Figure 1In the illustrated example, the positive electrode layer 10A is composed of a positive electrode tapered portion 11A and a positive electrode non-tapered portion 12A, and the negative electrode layer 10B is composed of a negative electrode tapered portion 11B and a negative electrode non-tapered portion 12B. Among them, a part of the positive electrode tapered portion 11A forms a non-opposing portion that is not directly opposed to the negative electrode layer 10B adjacent to the stacking direction, and the negative electrode tapered portion 11B forms a non-opposing portion that is not directly opposed to the positive electrode layer 10A adjacent to the stacking direction. In other words, the positive electrode tapered portion 11A has at least a portion where there is no negative electrode layer 10B directly opposed in the stacking direction, and the negative electrode tapered portion 11B does not have a positive electrode layer 10A directly opposed in the stacking direction.
[0088] By adopting the above-mentioned structure, the long distance between the opposing electrode layers can be reduced. As a result, the distance between the opposing electrode layers of the same electrode layer becomes more uniform, and the balance of the charge and discharge reaction in the electrode layer becomes good. Therefore, the charge and discharge efficiency of the solid battery can be improved, and the cycle characteristics and input and output characteristics can be improved.
[0089] The taper may be formed in either the positive electrode layer or the negative electrode layer, or in both the positive electrode layer and the negative electrode layer. From the perspective of further improving structural stability and operability, it is preferred that the taper be formed in both the positive electrode layer and the negative electrode layer (see Figure 1 ).
[0090] A solid electrolyte, an insulating material, a current collecting material, or the same material as the external terminal may be provided between the tapered portion of the electrode layer and the external terminal. In one embodiment, the same material as the external terminal is provided between the tapered portion of the electrode layer and the external terminal. In other words, the same material as the external terminal is provided between the tapered contour of the electrode layer and the inner contour of the external terminal. By adopting such a structure, the bonding between the electrode layer and the external terminal can be improved, thereby further preventing the intrusion of moisture. Figure 5 In the illustrated example, in a plan view of the solid battery 500 , an external terminal 30 ′ is provided between the positive electrode tapered portion 11A and the positive electrode terminal 30A, and an external terminal 30 ′ is provided between the negative electrode tapered portion 11B and the negative electrode terminal 30B.
[0091] In one embodiment, at least one electrode layer is composed of an electrode active material layer and a current collecting layer. By adopting such a composition, it is possible to impart higher conductivity to the electrode layer. Thus, the cycle characteristics and input-output characteristics of the solid battery can be improved. In the case where the electrode layer is composed of an electrode active material layer and a current collecting layer, only the electrode active material layer can be formed into a cone, or both the electrode active material layer and the current collecting layer can be formed into a cone.
[0092] In a preferred embodiment, the solid battery may further include a protective layer. Figure 6As shown, the protective layer 40 may be provided on the outer sides of the solid battery stack 500 ′, the positive electrode terminal 30A, and the negative electrode terminal 30B so as to be integrated with them.
[0093] The structure of the solid battery of this specification can be observed from an image obtained by cutting a cross section in the cross-sectional direction by an ion milling device (model IM4000PLUS manufactured by Hitachi High-Tech Co., Ltd.) and using a scanning electron microscope (SEM) (model SU-8040 manufactured by Hitachi High-Tech Co., Ltd.). In addition, the curvature radius R, cone angle and the above-mentioned dimension ratio of the cone described in this specification can refer to the value calculated based on the size measured from the image obtained by the above method.
[0094] The solid battery of the present invention is a stacked solid battery in which the layers constituting the battery constituent unit are stacked, and can be manufactured by a printing method such as a screen printing method, a raw sheet method using raw sheets, or a composite method of these. Therefore, each layer constituting the battery constituent unit is composed of a sintered body. Preferably, the positive electrode layer, the negative electrode layer, and the solid electrolyte layer are sintered integrally with each other. That is, it can be considered that the solid battery stack forms a fired integrated body. In such a fired integrated body, at least one layer of the electrode layer forms a cone whose size becomes smaller toward the side in contact with the external terminal.
[0095] [Method for manufacturing solid state battery]
[0096] As described above, the solid battery of the present invention can be manufactured by a printing method such as screen printing, a green sheet method using a green sheet, or a composite method thereof. Hereinafter, for the purpose of understanding the present invention, the case of using the printing method will be described in detail, but the present invention is not limited to this method.
[0097] (Solid battery stack precursor formation step)
[0098] In this process, multiple slurries such as positive electrode layer slurry, negative electrode layer slurry, solid electrolyte layer slurry, current collector layer slurry, electrode separator slurry and protective layer slurry are used as ink. That is, the slurry is applied by printing to form a slurry of a predetermined structure on a support substrate.
[0099] During printing, a solid battery stack precursor corresponding to the structure of a predetermined solid battery can be formed on a substrate by sequentially stacking printed layers with a predetermined thickness and pattern shape. The type of pattern forming method is not particularly limited as long as it is a method that can form a predetermined pattern, and for example, it can be any one or more of screen printing and gravure printing.
[0100] The slurry can be prepared by wet mixing the specified constituent materials of each layer and the organic carrier. The specified constituent materials of each layer are appropriately selected from the group consisting of positive electrode active material, negative electrode active material, conductive additive, solid electrolyte material, current collecting layer material, insulating material, adhesive and sintering aid. The organic carrier is formed by dissolving the organic material in a solvent. The slurry for the positive electrode layer, for example, contains positive electrode active material, conductive additive, solid electrolyte material, adhesive, sintering aid, organic material and solvent. The slurry for the negative electrode layer, for example, contains negative electrode active material, conductive additive, solid electrolyte material, adhesive, sintering aid, organic material and solvent. The slurry for the solid electrolyte layer, for example, contains solid electrolyte material, adhesive, sintering aid, organic material and solvent. The slurry for the positive current collecting layer and the slurry for the negative current collecting layer contain conductive additive, adhesive, sintering aid, organic material and solvent. The slurry for the protective layer, for example, contains insulating material, adhesive, organic material and solvent. The slurry for the insulating layer, for example, contains insulating material, adhesive, organic material and solvent.
[0101] The organic material contained in the slurry is not particularly limited, and at least one polymer material selected from the group consisting of polyvinyl acetal resin, cellulose resin, polyacrylic resin, polyurethane resin, polyvinyl acetate resin, and polyvinyl alcohol resin can be used. The type of solvent is not particularly limited, and for example, it can be any one or two or more organic solvents such as butyl acetate, N-methyl-pyrrolidone, toluene, terpineol, and N-methyl-pyrrolidone.
[0102] Wet mixing can use a medium, specifically, a ball mill method or a viscosity mill method, etc. On the other hand, a wet mixing method without using a medium can also be used, and a sand mixing method, a high pressure homogenization method, a kneading dispersion method, etc. can be used.
[0103] The support substrate is not particularly limited as long as it can support each slurry layer, and is, for example, a release film with a release treatment applied to one side. Specifically, a substrate composed of a polymer material such as polyethylene terephthalate can be used. When each slurry layer is maintained on the substrate and supplied to the firing process, the substrate can use an article that exhibits heat resistance to the firing temperature.
[0104] During printing, by sequentially stacking the printed layers according to a predetermined thickness and pattern shape, an unfired laminate corresponding to the structure of a predetermined solid battery can be formed on the substrate. When each printed layer is formed, a drying process is performed. During the drying process, the solvent evaporates from the unfired laminate. After the unfired laminate is formed, the unfired laminate can be peeled off from the substrate and supplied to the firing process, or the unfired laminate can be held on a supporting substrate and supplied to the firing process.
[0105] (Firing process)
[0106] In the firing step, the solid battery stack precursor is fired. The firing is performed by removing the organic material in a nitrogen atmosphere or in the air containing oxygen at, for example, 500°C, and then heating in a nitrogen atmosphere or in the air at, for example, 550°C to 5000°C, but this is only an example. The solid battery stack precursor may also be fired while being pressurized in the stacking direction (sometimes in the stacking direction and in a direction perpendicular to the stacking direction).
[0107] By performing such firing, a solid battery stack is formed, and finally a desired solid battery is obtained.
[0108] (About the production of the characteristic part of the present invention)
[0109] Regarding the taper of the electrode layer of the solid battery of the present invention, as long as the size of the electrode layer decreases toward the side in contact with the external terminal in the plan view of the solid battery, it can be formed by any method. As an example, the electrode layer precursor of the unfired laminate is pre-patterned by screen printing, etc., in a manner in which its size decreases toward the side in contact with the external terminal (for example, it becomes thinner to form an arc or a straight line). If such an electrode layer precursor is fired, a solid battery having a desired battery constituent unit can be obtained, and the battery constituent unit is formed by an electrode layer having a through opening.
[0110] The following is based on Figure 7 The exemplary embodiments shown in (A) to (F) will specifically describe the method for manufacturing a solid battery.
[0111] [Solid battery stack formation step]
[0112] First, a protective solid electrolyte, a solvent, and a protective binder selected as needed are mixed to prepare a protective paste. Alternatively, a protective solid electrolyte, a solvent, an insulating material, and a protective binder selected as needed are mixed to prepare a protective paste. Next, Figure 7 As shown in FIG. 2 (A), a protective slurry is applied on one side of a substrate (not shown) to form a protective layer 40 .
[0113] Next, a solid electrolyte, a solvent, and an electrolyte binder selected as needed are mixed to prepare a slurry for a solid electrolyte layer. Figure 7 As shown in (B) , a slurry for a solid electrolyte layer is applied on one surface of the protective layer 40 , thereby forming a slurry-like solid electrolyte layer 20 .
[0114] Next, the negative electrode active material, the solvent, and the negative electrode active material binder selected as needed are mixed to prepare a negative electrode slurry. Figure 7As shown in (C), the negative electrode slurry is applied to the surface of the solid electrolyte layer 20 using a pattern forming method, thereby forming a slurry-like negative electrode layer 10B. At this time, the size of the negative electrode slurry decreases toward one side of the outer edge of the solid electrolyte layer 20 (for example, it becomes thinner as shown in FIG. Figure 7 The negative electrode layer 10B is formed in an arc shape as shown in (C). The negative electrode layer 10B is formed to extend along the above-mentioned one side within the outer edge of the solid electrolyte layer 20, but not along the other three sides of the outer edge of the solid electrolyte layer 20.
[0115] Then, if Figure 7 As shown in (D), the solid electrolyte layer slurry is applied to fill the space between the negative electrode layer 10B and the outer edge of the solid electrolyte layer 20. The solid electrolyte layer slurry is further applied to one side thereof, thereby forming the solid electrolyte layer 20 in a slurry state.
[0116] Next, the positive electrode active material, the solvent, and the positive electrode active material binder selected as needed are mixed to prepare a positive electrode slurry. Figure 7 As shown in (E), a positive electrode slurry is applied to the surface of the solid electrolyte layer 20 using a pattern forming method, thereby forming a slurry-like positive electrode layer 10A. At this time, on the outer edge of the solid electrolyte layer 20, its size becomes smaller toward the side opposite to the side extending from the negative electrode layer 10B (for example, it becomes thinner as shown in FIG. Figure 7 The slurry positive electrode layer 10A is formed in the form of an arc shape (as exemplified in (E)). The slurry positive electrode layer 10A is formed to extend along the above-mentioned one side within the outer edge of the solid electrolyte layer 20, but not along the other three sides of the outer edge of the solid electrolyte layer 20.
[0117] Then, if Figure 7 As shown in (F), the solid electrolyte layer slurry is applied to fill the space between the positive electrode layer 10A and the outer edge of the solid electrolyte layer 20. The solid electrolyte layer slurry is further applied to one surface thereof, thereby forming the slurry-like solid electrolyte layer 20.
[0118] Next, the protective layer 40 is formed on the solid electrolyte layer 20 by the same process as the process for forming the protective layer 40. In this way, a solid battery stack precursor is formed.
[0119] Finally, the solid battery stack precursor is heated. In this case, the heating temperature is set so that a series of layers constituting the solid battery stack precursor are sintered. Other conditions such as the heating time can be set arbitrarily.
[0120] The series of layers constituting the solid battery stack precursor are sintered by the heating treatment, and thus the series of layers are thermally pressed together, thereby forming the solid battery stack 500 ′.
[0121] [Positive and negative terminal formation process]
[0122] For example, a positive terminal is bonded to the solid laminate using a conductive adhesive, and a negative terminal is bonded to the solid laminate using a conductive adhesive. Thus, the positive terminal and the negative terminal are respectively attached to the solid laminate, thereby completing a solid battery.
[0123] The embodiments of the present invention have been described above, but these are only typical examples, so the present invention is not limited thereto, and it is easy for a person skilled in the art to understand that various solutions can be conceived without changing the gist of the present invention.
[0124] For example, although in the above description, for example Figure 1 The solid battery exemplified in the above is mainly described, but the present invention is not limited thereto. In the present invention, any solid battery can be applied as long as it has a positive electrode layer, a negative electrode layer, and a solid electrolyte layer, and at least one of the electrode layers forms a tapered shape with a size decreasing toward the side of the electrode layer in contact with the external terminal in the plan view of the solid battery.
[0125] Industrial Applicability
[0126] The solid battery of the present invention can be used in various fields where it is envisioned that electricity storage is required. The solid battery of the present invention can be used in electrical / information / communication fields (e.g., mobile devices such as mobile phones, smart phones, laptops and digital cameras, activity meters, ARM computers, electronic paper, etc.) using mobile devices, household / small industrial uses (e.g., power tools, golf carts, home / care / industrial robots), large industrial uses (e.g., forklifts, elevators, port cranes), transportation system fields (e.g., hybrid vehicles, electric vehicles, buses, trams, electric power-assisted bicycles, electric motorcycles, etc.), power system uses (e.g., various power generation, load regulators, smart grids, general household setting type storage systems, etc.), medical uses (medical equipment fields such as earphones and hearing aids), medical uses (fields such as taking management systems), and IoT fields, space / deep sea uses (e.g., fields such as space probes and submersible survey ships), etc., but these are only examples.
[0127] Explanation of symbols
[0128] 10 Electrode layer
[0129] 10A positive electrode layer
[0130] 11A Positive cone
[0131] 12A Positive non-tapered part
[0132] 10B Negative layer
[0133] 11B Negative electrode cone
[0134] 12B Negative non-tapered part
[0135] 20 Solid electrolyte layer
[0136] 30 external terminals
[0137] 30A positive terminal
[0138] 30B Negative terminal
[0139] 30' External Terminal Blocks
[0140] 40 protective layer
[0141] 500' solid battery stack
[0142] 500'A positive side end face
[0143] 500'B Negative side end face
[0144] 500 solid batteries.
Claims
1. A solid battery having: A solid battery stack having at least one battery constituent unit along a stacking direction, wherein the battery constituent unit comprises: a positive electrode layer; a negative electrode layer; and a solid electrolyte layer sandwiched between the positive electrode layer and the negative electrode layer, and The external terminals of the positive terminal and the negative terminal are respectively provided on the side surfaces of the solid battery stack. In a plan view of the solid battery, the electrode layer of the positive electrode layer and the electrode layer of the negative electrode layer form a tapered shape whose size becomes smaller toward a side of the side where the electrode layer contacts the external terminal. The electrode layer is composed of a tapered portion and a non-tapered portion, and a ratio L1 / L2 of a length L1 of the tapered portion to a length L2 of the non-tapered portion in a plan view is greater than or equal to 0.01 and less than or equal to 1.0, In a plan view, the distance between the corners of the solid battery stack and the electrode layer is relatively increased compared to a case where the electrode layer has a substantially rectangular shape.
2. The solid battery according to claim 1, wherein: In a plan view, compared with a case where the electrode layer has a substantially rectangular shape, contact portions of the electrode layer with the external terminal are relatively reduced.
3. The solid battery according to claim 1 or 2, wherein: The taper is formed in a curved shape.
4. The solid battery according to claim 3, wherein: The taper is formed in an arc shape that curves inward.
5. The solid battery according to claim 4, wherein: The radius of curvature of the inwardly curved arc-shaped taper is greater than or equal to 25 μm and less than or equal to 10000 μm.
6. The solid battery according to claim 1 or 2, wherein: In the electrode layer, a contour between a portion forming the tapered shape and a non-tapered portion serving as a main surface portion of the electrode layer is rounded.
7. The solid battery according to claim 1 or 2, wherein: The same material as that of the external terminal is provided between the portion forming the tapered shape and the external terminal.
8. The solid battery according to claim 1 or 2, wherein: In the cross-sectional view of the solid battery, at least a portion of the portion of the electrode layer forming the tapered shape is formed as a non-opposing portion that does not directly oppose a different-polarity layer adjacent to the stacking direction.
9. The solid battery according to claim 1 or 2, wherein: The positive electrode layer and the negative electrode layer are layers capable of occluding and releasing lithium ions.
Citation Information
Patent Citations
Method of manufacturing highly multilayered all solid lithium ion secondary battery
JP2016207540A
Sheet electrode and battery using it
JP1998270014A
Electrical double-layer capacitor
JP2009188115A
Method of Manufacturing Electrode Plate Using Electrode Sheet Including Notching Part
KR1020170055722A