Catalytic ceramic candle filters for combined particulate removal and selective catalytic reduction (SCR) of nitrogen oxides
By using a catalyst with a vanadium/titanium ratio controlled between 0.03 and 0.27 on a ceramic candle filter, combining vanadium pentoxide and titanium dioxide, the problem of large vanadium usage is solved, reducing SO2 oxidation and improving the SCR of nitrogen oxides is improved Activity and environmental friendliness.
Patent Information
- Application Number
- CN201980094377.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-26
- Filing Date
- 2019-08-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-08-26
AI Technical Summary
When the existing catalysts remove nitrogen oxides (NOx), vanadium is used in large quantities, resulting in increased oxidation of SO2 and forming undesirable ammonium bisulfate (H2SO4), affecting the efficiency and environment of the catalyst.
A catalyst is used to combine a ceramic candle filter substrate with a vanadium/titanium oxide support coating. The mass ratio of vanadium/titanium is controlled between 0.03 and 0.27. The coating contains vanadium pentoxide and titanium dioxide and is at high temperatures. Activate the catalyst, and deposit the catalyst metal oxide by impregnating the liquid to reduce the use of vanadium.
It effectively reduces the use of vanadium, while reducing the oxidation of SO2, improves the selective catalytic reduction (SCR) activity of nitrogen oxides, avoids unnecessary formation of ammonium bisulfate, and improves the efficiency and environmental friendliness of the catalyst.
Smart Images

Figure CN113613780B_ABST
Abstract
Description
[0001] The present invention relates to a catalyst for the selective catalytic reduction (SCR) of nitrogen oxides by reaction with ammonia. Furthermore, the present invention relates to a method for preparing such a catalyst, which method is based in particular on the use of an impregnation liquid comprising one or more catalyst metal precursor compounds dispersed on nanoparticles of an oxidic metal support. The catalyst can advantageously be applied to a ceramic candle filter.
[0002] Catalysts, especially if applied to ceramic candle filters, can be used to treat process gases by heterogeneous catalysis and are widely used in emission control devices in the glass industry, but are also being studied for treating exhaust gases from other industries. Catalytic ceramic filters for removing dust and particulate matter from process exhaust gases are well known. Catalytic ceramic filters are particularly useful for cleaning process gases or raw gases from industrial processes involving combustion (such as the production of minerals, glass, cement, waste incineration), or from biomass power plants, and optionally process gases or raw gases from coal-fired boilers and engines. Ceramic filters in the shape of filter candles are used in many industries to remove particulate matter from process gases. They constitute one of the most effective types of dust collectors available, and for particles, they can achieve collection efficiencies of more than 99%. The filter can be made of various ceramic materials, including ceramic fibers made of alkali and alkaline earth silicates or aluminum silicates.
[0003] Typical operating temperatures range from 180°C to 400°C, and a single unit may house thousands of filters.
[0004] The present invention provides a novel catalyst applied on such ceramic candle filters.The ceramic candle filter impregnated with the catalyst according to the present invention provides both a filter function for particulate matter and an SCR function.
[0005] One preparation method is to load the catalytically active material in the substrate by applying a support (usually a layer comprising at least one inorganic alkali metal oxide) deposited on the catalyst substrate. Suitable inorganic alkali metal oxides are, for example, TiO2, SiO2, Al2O3, CeO2, ZrO2, La2O3 and mixtures and combinations thereof. Such support materials are well known to the skilled person and can be applied to the present invention without departing from the scope of the claims. After drying and optionally calcining in air under a controlled atmosphere, the support provides a porous high surface area layer bonded to the substrate surface.
[0006] The catalytically active material or its precursor can be deposited on the support before impregnation of the substrate, and finally the thus catalyzed substrate can be activated by calcination at high temperature during production or at the time of installation.
[0007] In the present invention, the substrate is preferably a ceramic candle filter.
[0008] When the SCR catalyst is operated in the removal of nitrogen oxides (NOx), the nitrogen oxides are converted into free nitrogen with a reducing agent (usually ammonia) in the presence of a catalyst supported on or in the pores on the walls of the monolithic substrate by selective catalytic reduction according to reactions I and II:
[0009] 4NO+4NH3+O2→4N2+6H2O I
[0010] NO+NO2+2NH3→2N2+3H2O II
[0011] Catalyst compounds active in the SCR reaction with ammonia are known per se in the art. For example, commonly employed catalysts are vanadium oxides, tungsten oxides, and zeolite materials, usually exchanged with, for example, copper and / or iron, used alone or as mixtures thereof. The most commonly used catalyst for reducing NOx in exhaust gases is vanadium oxide supported on titanium dioxide, optionally promoted with tungsten oxide, molybdenum oxide or antimony oxide.
[0012] WO 2016 / 058713 A1 discloses a method for preparing a catalytic fabric filter, comprising impregnating a fabric filter substrate with an aqueous impregnation liquid comprising an aqueous hydrosol of one or more catalyst metal precursor compounds dispersed on nanoparticles of an oxidized metal support.
[0013] According to the disclosure of WO 2016 / 058713 A1 (see method of Example 1), an NH4VO3 / TiO2 ratio of 0.58 was used, which corresponds to a V / Ti ratio of 0.42.
[0014] WO 2016 / 150464 A1 discloses a catalytic ceramic candle filter and the use of the filter for removing particulate matter in the form of soot, ash, metals and metal compounds, and hydrocarbons and nitrogen oxides present in process exhaust or engine exhaust. The filter contains a combined SCR and oxidation catalyst. The catalytically active substances are vanadium oxide, titanium dioxide and palladium. The vanadium oxide is preferably vanadium pentoxide. Palladium is preferably present in an amount between 20 ppm / filter weight and 1000 ppm / filter weight. The vanadium oxide on titanium dioxide is used as a combined SCR and oxidation catalyst, and Pd is used as an oxidation catalyst.
[0015] However, WO 2016 / 150464 A1 does not mention the total amount of vanadium oxide and titanium dioxide, and there is no information about the suitable range of the vanadium to titanium ratio. The present disclosure includes two examples. Example 1 refers to a ceramic candle filter coated with 1.26 wt. % vanadium and 2.36 wt. % Ti (V:Ti ratio of about 1:2). Example 2 demonstrates the CO oxidation performance of the catalyst of Example 1. There is no information about the dry mass of the carrier coating or the solvents and additives used.
[0016] WO 2016 / 150465 A1 also discloses a catalytic ceramic candle filter and the use of the filter for removing hydrocarbons and nitrogen oxides or particulate matter together with hydrocarbons and nitrogen oxides. The catalytically active substances are also vanadium oxide, titanium dioxide and palladium.
[0017] In WO 2016 / 150464 A1, a combined SCR and oxidation catalyst is arranged at least on the dispersion side and / or in the wall of the filter, and a palladium-containing catalyst is arranged on the permeate side of the filter.
[0018] The combined SCR and oxidation catalyst preferably comprises vanadium oxide and titanium dioxide, and the palladium catalyst may optionally also comprise vanadium oxide and titanium dioxide.
[0019] In contrast, the ceramic candle filter according to WO 2016 / 150465 A1 comprises a combined SCR and oxidation catalyst which is arranged at least on the dispersion side of the filter and / or in the wall of the filter and comprises palladium, vanadium oxide and titanium dioxide.
[0020] Thus, the difference between WO 2016 / 150464 A1 and WO 2016 / 150465 A1 is that the former does not contain palladium in the combined SCR and oxidation catalyst, whereas the latter contains palladium in the combined SCR and oxidation catalyst.
[0021] The terms "dispersion side" and "permeate side" refer to the side of the filter facing the flow of unfiltered exhaust gas and the side of the filter facing the flow of filtered exhaust gas, respectively.
[0022] WO 2017 / 055344 A1 discloses a ceramic dust filter containing a catalyst for exhaust gas cleaning. It contains at least one catalytically active metal and an oxide carrier to form a catalytically active metal oxide carrier. Preferably, the at least one catalytically active metal includes a combined SCR and oxidation catalyst and a catalyst containing a precious metal. The combined SCR and oxidation catalyst preferably contain vanadium oxide, tungsten oxide or molybdenum oxide and titanium dioxide, and the catalyst containing the precious metal is preferably a palladium catalyst. Most preferably, the combined SCR and oxidation catalyst contain vanadium oxide and titanium dioxide. Palladium should be present in an amount between 20ppm / filter weight and 1000ppm / filter weight. However, WO 2017 / 055344 a1 does not mention the preferred V / Ti ratio or the total amount of catalytically active material in the carrier coating or on the filter.
[0023] In R Barthos, A Hegyessy, G Novodárzski, and J Valyon: "Structure and activity of Pd / V2O5 / TiO2 catalysts in Wacker oxidation of ethylene", Appl Catal A 2017, 531, 96-105, the catalytic activity of Pd / V2O5 / TiO2 catalysts with different amounts of Pd, Ti and V was studied. The V2O5 / TiO2 preparations contained 2.2 wt% or 4.6 wt% or 8.6 wt% of vanadium, respectively.
[0024] The deposition of vanadium and vanadium compounds on titanium dioxide is well known in the art. For example, it is described in K Bourikas, I Georgiadou, C Kordulis and A Lycourghiotis: "Mechanism of deposition of vanadium-oxo species on the "anatase / electrolytic solution" interface, J PhysChem B 1997, 101, 8499-8506. In this scientific article, the authors deposited vanadium-oxo species on a single TiOH2 at relatively low and relatively high pH values, respectively. + Or the adsorption reaction on the site where TiOH groups are generated shows the deposition.
[0025] US 2014 / 0271435 A1 discloses a catalytic filter of biosoluble fibers catalyzed with a catalyst comprising vanadium oxide and titanium oxide, wherein the total concentration of alkali metals in the filter is less than 3000 ppm (by weight) and / or the total concentration of alkaline earth metals in the filter is less than 20% (by weight). However, US 2014 / 0271435 A1 does not mention the amount of washcoat to be applied, the amount of vanadium and titanium in the washcoat, and the ratio of vanadium to titanium.
[0026] WO 2018 / 018406 A1 discloses a supported catalyst for removing NOx, an integral selective catalytic reduction (SCR) catalyst, a preparation method thereof, and a method for removing NOx. The supported catalyst comprises a carrier and a catalytically active component supported on the carrier, wherein the catalytically active component comprises vanadium, antimony, and at least one other component selected from the group consisting of silicon, aluminum, and zirconium. Preferably, the content of vanadium is 1% to 10% by weight as calculated by V2O5, the content of antimony is 1% to 20% by weight as calculated by Sb2O3, and the content of at least one other component is 0.5% to 20% by weight as calculated by SiO2, Al2O3, or ZrO2, respectively.
[0027] The inventors of the present invention have now surprisingly found that this ratio can be reduced, i.e. less vanadium can be used, without affecting the DeNOx activity of the catalyst. At the same time, the oxidation of SO2 is reduced, which in turn will lead to less formation of ammonium bisulfate (ABS).
[0028] Therefore, the present invention relates to a catalyst for selective catalytic reduction (SCR) of nitrogen oxides, the catalyst comprising
[0029] Ceramic candle filter substrate and
[0030] a coating comprising an oxidic metal support comprising an oxide of titanium and a catalytic metal oxide comprising an oxide of vanadium, wherein the mass ratio of vanadium to titanium is between 0.03 and 0.27,
[0031] wherein the mass ratio is calculated based on the masses of vanadium metal and titanium metal, and
[0032] wherein the catalyst comprises from 1% to 20% by weight of catalytically active material, and
[0033] • wherein the catalytic metal oxide is adsorbed onto the surface of an oxidic metal support.
[0034] The novel catalyst for the selective catalytic reduction (SCR) of nitrogen oxides according to the invention and the method for preparing the catalyst are explained below, wherein the invention encompasses all embodiments shown below both individually and in combination with one another.
[0035] The substrate is a ceramic candle filter. As mentioned above, ceramic filters in the shape of a filter candle are used in many industries to remove particulate matter from process gases. They constitute one of the most effective types of dust collectors available. The catalyst according to the present invention can be applied to such dust collectors. In one embodiment of the invention, a plurality of catalysts comprising a ceramic candle filter substrate and a coating comprising an oxidized metal support are used in parallel, the oxidized metal support comprising an oxide of titanium and a catalytic metal oxide comprising an oxide of vanadium, wherein the mass ratio of vanadium / titanium is 0.03 to 0.27. These arrangements are known to the skilled person and can be applied without departing from the scope of the claims.
[0036] The catalytic metal oxide containing vanadium oxide of the coating preferably comprises vanadium pentoxide (V2O5). In addition, the coating optionally also comprises oxides of other metals, in particular tungsten oxide and / or molybdenum oxide and / or antimony oxide. Preferred tungsten oxide, molybdenum oxide and antimony oxide are tungsten trioxide (WO3), molybdenum trioxide (MoO3) and antimony pentoxide (Sb2O5), respectively.
[0037] The oxidic metal support containing the titanium oxide of the coating generally comprises titanium dioxide. The titanium dioxide can be selected from anatase, rutile, brookite and mixtures thereof. Preferably, the titanium dioxide comprises at least 95% by weight of anatase, preferably at least 98% by weight of anatase, wherein the residue totaling 100% by weight consists of rutile, brookite or a mixture of rutile and brookite. In addition, the titanium dioxide optionally also comprises an oxide of another metal, in particular an oxide of aluminum, silicon, cerium, zirconium, or a mixture, mixed oxide or compound containing at least one of these oxides.
[0038] Preferably, the oxidized metal support has a primary particle size D 50 The primary particle size is between 1 nm and 1000 nm, preferably between 20 nm and 200 nm, and the primary particle size is measured by a laser diffraction particle size analyzer. The primary particle is the smallest identifiable subdivision in the particle system. The primary particle can also be a subunit of the aggregate.
[0039] According to the present invention, the mass ratio of vanadium / titanium is from 0.03 to 0.27, preferably from 0.7 to 0.27, and most preferably from 0.12 to 0.21. For the avoidance of doubt, the mass ratio is calculated based on the mass of vanadium metal and titanium metal. Preferably, the catalyst of the present invention does not contain platinum group metals, in particular does not contain palladium.
[0040] The catalytic metal oxide is adsorbed or precipitated on the surface, either by deposition through impregnation followed by drying or by pH adjustment (ie, precipitation by changing the pH) onto the surface of the oxidic metal support.
[0041] In another embodiment of the invention, the oxidic metal support comprises not only titanium oxides, in particular titanium dioxide, but also vanadium oxides, in particular vanadium pentoxide, and optionally tungsten oxides and / or molybdenum oxides and / or antimony oxides, in particular tungsten trioxide and / or molybdenum trioxide and / or antimony pentoxide.
[0042] This is particularly the case if a recycled or fresh SCR catalyst comprising vanadium pentoxide (V2O5) and titanium dioxide TiO2 and optionally tungsten trioxide (WO3) and / or molybdenum trioxide (MoO3) and / or antimony pentoxide (Sb2O5) is reused.
[0043] In the case where the oxidic metal support comprises an oxide of vanadium, this oxide of vanadium must be taken into account when calculating the mass ratio of vanadium to titanium as described above.
[0044] The catalyst of the present invention comprises 1 wt% to 20 wt%, preferably 2 wt% to 10 wt% of the coating. As used herein, the term "catalyst" includes the ceramic candle filter substrate and the coating.
[0045] The present invention also relates to a method for preparing a catalyst for selective catalytic reduction (SCR) of nitrogen oxides, the method comprising the following steps:
[0046] a) providing a ceramic candle filter substrate;
[0047] b) providing an aqueous impregnation liquid comprising one or more catalyst metal precursor compounds comprising a vanadium compound dispersed on particles of an oxidic metal support comprising titanium oxide;
[0048] c) impregnating the ceramic candle filter substrate with the impregnation liquid; and
[0049] d) drying and thermally activating the impregnated ceramic candle filter substrate at a temperature of 150° C. to 600° C. to convert the one or more metal precursor compounds into their catalytically active form.
[0050] With regard to step b), the catalyst metal precursor compound comprising a vanadium compound is preferably ammonium metavanadate. In case the catalyst of the invention comprises an oxide of tungsten and / or an oxide of molybdenum, the impregnation liquid preferably comprises ammonium metatungstate and / or ammonium heptamolybdate.
[0051] In some applications of the method according to the present invention, the ceramic candle filter substrate is pre-coated prior to dipping the ceramic candle filter substrate to provide a larger substrate surface area.
[0052] Therefore, in one embodiment of the present invention, the ceramic candle filter substrate is impregnated with an oxidic metal support comprising an oxide of titanium and optionally an oxide of aluminum, cerium, zirconium or a mixture, mixed oxide or compound containing at least one of these oxides before impregnating the ceramic candle filter substrate with the impregnation liquid in step (c).
[0053] The thermal activation of the impregnated ceramic candle filter substrate according to step d) can be performed before installing the impregnated substrate or after installing the impregnated substrate in the SCR unit.Preferably, the thermal activation temperature is between 200°C and 450°C.
[0054] As used herein, the term "thermal activation" means treating one or more catalyst metal precursor compounds at a temperature suitable for converting the one or more catalyst metal precursor compounds into their catalytically active form. The skilled person knows which temperature range is suitable for converting one or more given catalyst metal precursor compounds into their corresponding catalytically active form. The skilled person can apply this knowledge without departing from the scope of the claims.
[0055] In the case where the method of the invention comprises providing in step a) a recycled catalyst which already comprises vanadium pentoxide (V2O5) and titanium dioxide TiO2 and optionally tungsten trioxide (WO3) and / or molybdenum trioxide (MoO3), the amount of said oxide precursors in the aqueous impregnation liquid can be reduced accordingly to obtain the desired amount of the corresponding metal in the final coating A. The skilled person can calculate the corresponding amounts of metal oxides and metal precursors, for example the amount of vanadium pentoxide (V2O5) and the amount of ammonium metavanadate from the recycled catalyst, which are necessary to achieve the desired amount of vanadium in the final impregnation liquid. This applies on the one hand to the use of titanium dioxide, tungsten trioxide, molybdenum trioxide and antimony pentoxide from the recycled catalyst and on the other hand to the use of fresh titanium dioxide, ammonium metatungstate and / or ammonium heptamolybdate and / or antimony oxalate and / or antimony acetate, respectively. Without departing from the scope of the claims, the skilled person can use this knowledge to calculate the amount of recycled catalyst and precursor compounds to be used.
[0056] In the preparation of the aqueous impregnation liquid as disclosed in more detail below, the oxidic metal support is present in the impregnation solution in the form of small particles, a portion of which may be agglomerated to a particle size larger than the preferred size.
[0057] Primary amines have been shown to be useful for preventing agglomeration, or for breaking up agglomerates that have formed. It is therefore preferred to add a dispersant selected from one or more primary amines to the impregnation liquid. The primary amine is preferably soluble in the aqueous impregnation liquid when added in an amount that results in the above disclosed purposes. Primary amines containing less than seven carbon atoms are water-soluble, and therefore preferred primary amines for use in the present invention are monomethylamine, monoethylamine, monopropylamine, monobutylamine or mixtures thereof. Among them, the most preferred dispersant is monoethylamine.
[0058] Good results are obtained when the primary amine dispersant is added to the impregnation liquid in an amount resulting in a pH value of the impregnation liquid above 7, preferably between pH 8.5 and pH 10.
[0059] As is known in the art, an effective catalyst requires a monolayer coverage of the catalytically active material on the oxidic metal support. The formation of an excess of crystalline catalytically active material on the support should be avoided.
[0060] When the so-called equilibrium deposition method is used alone or in combination with a primary amine dispersant, a high degree of dispersion of the catalytically active material is possible after thermal activation at low temperatures. In this method, the electrostatic attraction between oppositely charged metal compounds is utilized to bind one metal compound in finely divided form to the surface of an oppositely charged metal compound.
[0061] TiO2 and V x O y z- In the pH range of 4 to 6, the surface charges are opposite. Therefore, electrostatic attraction causes V x O y z- Deposited onto TiO2.
[0062] V x O y z- The limited solubility of V is circumvented by Le Chatelier's principle. x O y z- Bonded to Ti-OH2 + When the new V x O y z- The ions dissolve. This continuous process takes place at room temperature and requires only stirring and pH adjustment.
[0063] The skilled person knows that various vanadium oxides coexist in aqueous solution. The suffix "x" as given above represents the number of vanadium atoms in the vanadium-oxygen species, "y" represents the number of oxygen atoms, and "z" represents the charge of the vanadium-oxygen species. The nature of each of these coexisting vanadium-oxygen species and the relative amount of each of these species depends on the pH of the aqueous solution and on the voltage potential of each individual vanadium-oxygen species compared to a standard hydrogen electrode.
[0064] In electrochemistry, the Pourbaix diagram (also called potential / pH diagram, E H -PH diagram or pE / pH diagram) plots possible stable (equilibrium) phases of aqueous electrochemical systems. The main ion boundaries are represented by lines. Pourbaix diagrams are known to the skilled person and are disclosed in M Pourbaix: "Atlas of Electrochemical Equilibrium in Aqueous Solutions", National Association of Corrosion Engineers, 1974, ISBN 0-915567-98-9. In addition, Pourbaix diagrams related to vanadium-oxygen species are described in K Post, RG Robins: "Thermodynamic diagram for the vanadium-water system at 298.15K", Electrochim Acta 1976, 21, 401-405, and in BM Weckhuysen, DE Keller: "Chemistry, spectroscopy ad the role of supported vanadium oxides in heterogeneous catalysis", Catal Today 2003, 78, 25-46.
[0065] Therefore, the aqueous impregnation liquid is preferably prepared by the following steps:
[0066] i. adding the one or more catalyst metal precursor compounds and the oxidized metal support to water and continuously adding an acid to the mixture thus obtained so as to maintain the pH of the mixture at a value at which the surface charge of the one or more catalyst precursor metal compounds is negative and the zeta potential of the oxidized metal support is positive;
[0067] ii. adsorbing the one or more catalyst metal precursor compounds onto the surface of the oxidic metal support; and optionally
[0068] iii. adding a dispersant to the mixture thus prepared in an amount to obtain a pH value of above 7 for the slurry thus prepared.
[0069] iv. optionally grinding the mixture.
[0070] Some commercially available oxidic metal supports, such as commercially available TiO2, have an average particle size D50 of about 1 μm, for example between 800 nm and 1200 nm. In this case, the mixture obtained by adding one or more catalyst metal precursor compounds and the oxidic metal support to water is a so-called "slurry". In one embodiment of the present invention, the mixture obtained after step iii) is milled as described in step iv) above.
[0071] As used in the present invention, the term "slurry" refers to a heterogeneous mixture of at least one liquid and solids finely dispersed in the liquid. The at least one liquid is water, but the slurry may additionally contain other liquids such as amines, as described above. The solids of the slurry according to the present invention comprise an oxidized metal support and a catalytic metal oxide. The oxidized metal support and the catalytic metal oxide are suspended or dispersed in at least one liquid. According to common definitions, a "suspension" comprises solid particles with an average particle size D50 of 1 μm to 100 μm, and a "dispersion" comprises solid particles with an average particle size D50 of 1 nm to 1 μm. Therefore, a "slurry" in the sense of the present invention can be a suspension or a dispersion, depending on the average particle size D50, but it always involves a heterogeneous mixture in which the solid particles will settle over time if undisturbed.
[0072] If solids (i.e., oxidized metal support and catalytic metal oxide, respectively) are added to water, then dispersants are added, then the pH value is adjusted to above 7, preferably 8 to 10, then ground as described above, the solid particles become smaller. During grinding, the mixture of water, oxide and dispersant changes from a suspension or dispersion (depending on the initial average particle size D50) to a colloidal system. A colloidal system is a system in which the suspended particles are smaller than those of a dispersion or suspension, and if not disturbed, the particles do not settle over time. The transition from a dispersion to a colloid depends not only on the particle size, but also on the properties of the liquid and the solid, and is mobile to a certain extent. In the present invention, if the average particle size D50 is in the range of 90nm to 110nm, the mixture of water, oxide and dispersant becomes colloidal. The colloidal system behaves like a liquid solution, i.e., like a homogeneous mixture of at least one liquid and at least one solid, wherein if not disturbed, the at least one solid does not settle over time. In the context of the present invention, the colloidal system is referred to as an "impregnation liquid". The impregnation liquid may be used to apply the oxidic metal support and the catalytic metal oxide to the substrate.
[0073] If the average particle size D50 of the oxidic metal support (such as commercially available TiO2) is in the range of 90 nm to 110 nm, the mixture obtained by adding one or more catalyst metal precursor compounds and the oxidic metal support will already be colloidal and therefore a liquid solution as defined above. In this case, it is not necessary to grind the mixture according to step iv).
[0074] Thus, as used above in steps i), ii) and iv), the term "mixture" refers to slurries and colloidal systems as defined above, depending on the average particle size D50 of the oxidic metal support applied in step i).
[0075] Preferably, the pH value in steps (i) and (ii) is maintained between 2.5 and 5.5.
[0076] The acid used in step a) to maintain the pH of the liquid at a negative value for the surface charge of the catalyst precursor metal compound(s) and a positive value for the zeta potential of the oxidized metal support is preferably selected from nitric acid, formic acid, acetic acid, citric acid and mixtures thereof. More preferably, the acid is selected from a mixture of nitric acid and at least one of formic acid, acetic acid and citric acid, and even more preferably, the acid is nitric acid.
[0077] In step (iv), the slurry is ground to adjust the size of the particles comprising the oxidized metal support and the catalytic metal precursor. In one embodiment, the average particle size D after grinding is measured by a laser diffraction particle size analyzer and / or dynamic light scattering. 50 Between 1 nm and 1000 nm, preferably between 40 nm and 300 nm.
[0078] Suitable mills are, for example, bead mills and ball mills. The skilled person knows which mills are suitable for grinding the slurry containing the particles. The skilled person can apply the method without departing from the scope of the claims.
[0079] The catalyst of the invention is suitable for treating exhaust gases from automobiles and stationary sources and for selectively reducing the nitrogen oxides contained in said exhaust gases.
[0080] The invention therefore also relates to a process for treating exhaust gases from automobiles and stationary sources and for the selective reduction of nitrogen oxides contained in said exhaust gases, characterized in that the exhaust gases are passed over a catalyst according to the invention.
[0081] In an embodiment of the invention, the catalyst of the invention is used to treat process gases in emission control devices in the glass industry, biomass power plants, waste-to-energy plants, cement plants, and other types of plants in the chemical industry.
[0082] Example 1
[0083] a) Preparation of the impregnation liquid comprising ammonium vanadate / titanium dioxide
[0084] 1. Mix 160 kg of demineralized water with 70.4 kg of TiO2.
[0085] 2. Add 14.5 kg of ammonium metavanadate (AMV) under continuous stirring. The ratio of NH4VO3 / TiO2 is 0.23.
[0086] 3. The pH was monitored and continued to increase.
[0087] 4. Use concentrated nitric acid to adjust the pH to between 4.0 and 4.5.
[0088] 5. After a few hours, keep the pH of the liquid constant and keep the slurry under constant stirring for at least 5-10 hours. However, it is necessary to adjust the pH every 3 hours.
[0089] The resulting slurry was yellow, and 5.58 kg of ethylamine (68% in water) was added (or until pH was about 9.2-9.5).
[0090] The slurry turned pale yellow and was subsequently ground to a particle size (D50) of 90 nm to 110 nm, at which the slurry acquired liquid properties.
[0091] 6. Dilute the liquid to about 9% dry matter by weight with 575 L of 0.12% ethylamine solution.
[0092] 7. Optionally add rheology modifiers and / or surface tension modifiers to change the liquid properties.
[0093] Suitable rheology modifiers are nonionic or ionic dispersants or thickeners. Dispersants can be selected from polymers and polymer electrolytes having a molecular weight of 2,000 to a maximum of 100,000. Typical functional groups of these dispersants include hydroxyl (-OH), carboxyl (-COOH), sulfonate (-SO3H), sulfate (-OSO3-), ammonium (-NH4+), amino (-NH2), imino (-NH-) and polyoxyethylene (-CH2CH2O-) groups.
[0094] Suitable surfactants may also be nonionic or ionic. Anionic surfactants are, for example, sulfates, sulfonates, carboxylates and phosphates. Cationic surfactants are primary, secondary or tertiary amines (depending on the pH value) and quaternary organic ammonium salts. Nonionic surfactants may be selected from:
[0095] Ethoxylates: Alcohol ethoxylates, Alkylphenol ethoxylates (APE), Fatty acid ethoxylates, Ethoxylated fatty esters and oils, Ethoxylated amines and / or fatty acid amides, End-capped ethoxylates
[0096] Fatty acid esters of polyols: fatty acid esters of glycerol, fatty acid esters of sorbitol, fatty acid esters of sucrose, alkyl polyglucosides
[0097] Amine oxide
[0098] Sulfoxide
[0099] Phosphine oxide
[0100] It is apparent from the above list that some of the substances listed above can be used as both rheology modifiers and surface tension adjusters. This is well known to the skilled person.
[0101] b) Impregnation of the ceramic candle filter substrate with the aqueous impregnation liquid. The V / Ti ratio of the catalyst thus obtained was 0.17.
[0102] Example 2
[0103] The method of Example 1 was repeated except that the catalyst obtained had a V / Ti ratio of 0.12.
[0104] Example 3
[0105] The method of Example 1 was repeated except that the catalyst obtained had a V / Ti ratio of 0.21.
[0106] Example 4
[0107] The method of Example 1 was repeated except that the catalyst obtained had a V / Ti ratio of 0.24.
[0108] Example 5
[0109] The method of Example 1 was repeated except that the catalyst obtained had a V / Ti ratio of 0.27.
[0110] test
[0111] A portion of each aqueous slurry obtained according to Examples 2 to 5 was dried and the powders thus obtained were tested in an ammonia SCR in NO using a gas composition comprising 500 ppm NO, 533 ppm NH3, 10 vol% O2, 4% H2O and the balance N2. The test results are summarized in Table 1 below and are shown in Figure 1 middle.
[0112] Table 1: NOx conversion of Examples 2 to 5 at various temperatures
[0113]
[0114]
[0115] X NO[%] = NOx conversion rate, in percentage
[0116] As from Figure 1 It is evident that the powders corresponding to the catalysts of Examples 2 to 5 according to the invention have very good NO conversion activity at higher temperatures. It is also evident that increasing the Ti / V ratio to values above 0.20 (especially above 0.24) does not lead to higher activity, the activity tends to level out.
[0117] On the other hand, it is common knowledge for those skilled in the art in the field of selective catalytic reduction of nitrogen oxides that the (unwanted) oxidation of SO 2 increases with increasing Ti / V ratio (see, for example, Applied Catalysis b: Environmental 19 (1998) 103-117).
[0118] The invention thus allows to obtain an optimum NO conversion while limiting the undesired SO2 oxidation to a minimum.
[0119] Particle size distribution
[0120] The particles obtained in Examples 2 to 5 were bead milled for 8.75 hours. Thereafter, the particle size (D50) was determined using laser diffraction analysis.
[0121] The results are Figure 2 Shown in.
Claims
1. A catalyst for selective catalytic reduction of nitrogen oxides, the catalyst comprising Ceramic candle filter substrate, and a coating comprising an oxidic metal support comprising an oxide of titanium and a catalytic metal oxide comprising an oxide of vanadium, wherein the mass ratio of vanadium to titanium is between 0.21 and 0.27, wherein the mass ratio is calculated based on the masses of vanadium metal and titanium metal, and wherein the catalyst comprises from 1% to 20% by weight of catalytically active material, and • wherein the catalytic metal oxide is adsorbed onto the surface of the oxidic metal support.
2. The catalyst of claim 1, wherein the catalytic metal oxide of the vanadium-containing oxide of the coating comprises vanadium pentoxide.
3. The catalyst according to claim 2, wherein the catalytic metal oxide containing vanadium oxide of the coating layer further comprises tungsten oxide and / or molybdenum oxide and / or antimony oxide.
4. The catalyst according to any one of claims 1 to 3, wherein the oxidic metal support containing titanium oxide of the coating comprises titanium dioxide.
5. The catalyst according to claim 4, wherein the oxidic metal support containing titanium oxide of the coating layer further comprises at least one oxide selected from the group consisting of aluminum oxide, cerium oxide and zirconium oxide.
6. The catalyst according to any one of claims 1 to 3, wherein the oxidic metal support consists of single or agglomerated titanium dioxide nanoparticles having a primary particle size between 1 nm and 1000 nm.
7. The catalyst according to any one of claims 1 to 3, wherein the catalyst does not contain platinum group metals.
8. A method for preparing a catalyst according to any one of claims 1 to 7, said method The following steps are involved: a) providing a ceramic candle filter substrate; b) providing an aqueous impregnation liquid comprising one or more catalyst metal precursor compounds comprising a vanadium compound dispersed on particles of an oxidic metal support comprising titanium oxide; The impregnation liquid is prepared by the following steps: i. adding the one or more catalyst metal precursor compounds and the oxidized metal support to water and continuously adding an acid to the mixture thus obtained so as to maintain the pH of the mixture at a value at which the surface charge of the one or more catalyst precursor metal compounds is negative and the zeta potential of the oxidized metal support is positive; ii. adsorbing the one or more catalyst metal precursor compounds onto the surface of the oxidic metal support; and optionally iii. adding a dispersant to the mixture thus prepared in an amount such that the washcoat slurry thus prepared has a pH value above 7; iv. optionally grinding the mixture; c) impregnating the ceramic candle filter substrate with the obtained impregnation liquid; as well as d) drying and thermally activating the impregnated ceramic candle filter substrate at a temperature of 150° C. to 600° C. to convert the one or more metal precursor compounds to their catalytically active form.
9. The process according to claim 8, wherein the catalyst metal precursor compound containing a vanadium compound is ammonium metavanadate.
10. A method according to claim 8 or 9, wherein the aqueous impregnation liquid comprises a primary amine which is soluble in the liquid.
11. The method of claim 10, wherein the primary amine is monoethylamine.
12. Process for treating exhaust gases from automobiles and stationary sources and for selectively reducing nitrogen oxides contained in said exhaust gases, wherein the process comprises passing said exhaust gases over a catalyst according to any one of claims 1 to 7.