Method for manufacturing a flow sensor

By using low-pressure chemical vapor deposition and photolithography drying etching processes in the flow sensor, the annular groove structure is formed, and the thermal resistance layer and passivation layer are made on the upper support layer, the strength and thermal insulation performance of the cavity film layer in the sensor are solved. The problem of high mechanical strength and thermal insulation effect are achieved.

CN113654600BActive Publication Date: 2024-11-19LESENT (SUZHOU) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110841185.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-23
Publication Date
2024-11-19
Estimated Expiration
2041-07-23

AI Technical Summary

Technical Problem

In semiconductor processes, it is difficult to achieve a cavity film layer with high support strength in the flow sensor, and the front corrosion process is difficult to achieve deeper depth and strength requirements.

Method used

The animatic groove structure is formed on the substrate through low-pressure chemical vapor deposition and photolithography drying etching process, the third silicon nitride layer is filled, the lateral corrosion stop layer is formed, and the thermoresistance layer and passivation layer are made on the upper support layer. Finally, a double-layer thermal insulation cavity structure is formed through a wet release process.

Benefits of technology

The high mechanical strength and good thermal insulation performance of the sensor are achieved, solving the problems of support layer thickness and strength control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113654600B_ABST
    Figure CN113654600B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for manufacturing a flow sensor, comprising forming a lower cavity structure layer on the front side of a silicon wafer by photolithography, etching and oxidation processes, and then sequentially forming a lower support layer, an upper cavity structure layer and an upper support layer on the lower cavity structure layer, and at the same time forming a lateral corrosion barrier layer by photolithography, etching and filling processes. Then, a thermal resistor layer pattern, a passivation layer pattern and a release hole pattern are made on the upper support layer, and finally, the upper cavity structure layer and the lower cavity structure layer are released by a wet etching process to form an upper and lower double-layer heat-insulating cavity. The flow sensor manufactured by the technical solution described in the present invention has good heat insulation performance and mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of flow sensors, and in particular to a method for manufacturing a flow sensor. Background Art

[0002] In the structure of some temperature-related semiconductor sensors, it is sometimes necessary to place the sensor on a suspended membrane. After packaging, the substrate under the sensor is not in contact with the base of the package, but is suspended and in contact with the air or vacuum, so as to reduce the interference of external environmental temperature.

[0003] For semiconductor processes, it is very difficult to obtain accurate surface support thickness through low-cost backside etching process, which is mainly through precise control of time and closely related to the purity, concentration and temperature of the etching solution used. When processing in semiconductor factories with larger sizes and more batches, the uniformity of devices in the wafer and the repeatability of devices between wafers are more obvious. Although the front side etching process can obtain accurate surface thickness, the depth of its cavity is affected by the capacity and production capacity of the production equipment, and it is difficult to reach a deeper depth. In addition, the most critical problem is that the strength of the suspended film formed by the front side etching process has very high stress control requirements for the entire device layer.

[0004] Therefore, technicians in this field are committed to developing a method for manufacturing a flow sensor, which can well solve the above-mentioned problems. The manufactured sensor has the advantages of precise support layer thickness and the membrane layer is not easy to be damaged (high support strength). Summary of the invention

[0005] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is how to realize a cavity membrane layer with higher supporting strength in a flow sensor.

[0006] To achieve the above object, the present invention provides a method for manufacturing a flow sensor, comprising the following steps:

[0007] Providing a substrate 001;

[0008] Growing a first silicon nitride layer 002 on the substrate 001 by low pressure chemical vapor deposition;

[0009] The first silicon nitride layer 002 and the substrate 001 are successively etched by photolithography and dry etching to form a groove 003 on the substrate 001;

[0010] Growing a first silicon oxide layer 005 in the groove 003 by a silicon local oxidation isolation process;

[0011] removing the first silicon nitride layer 002;

[0012] Depositing a second silicon oxide layer 006, a second silicon nitride layer 007, and a third silicon oxide layer 008 in sequence;

[0013] Forming an annular groove structure by photolithography and dry etching, wherein the depth of the annular groove structure is the total thickness of the second silicon oxide layer 006, the second silicon nitride layer 007 and the third silicon oxide layer 008;

[0014] The annular groove structure is filled with the third silicon nitride layer 010 by low-pressure chemical vapor deposition to form a lateral etching stop layer;

[0015] Forming a pattern 011 containing a metal material on the third silicon nitride layer 010 by a patterning process;

[0016] alloying the pattern by a furnace tube process;

[0017] Depositing a passivation protection layer 012;

[0018] Forming a metal PAD window and a release hole 015 by photolithography and etching;

[0019] The third silicon oxide layer 008 , the first silicon oxide layer 005 and the second silicon oxide layer 006 are removed by a wet release process to form a cavity.

[0020] Furthermore, the annular groove structure surrounds the groove in a vertical direction.

[0021] Furthermore, the cavity is divided into two upper and lower parts by the second silicon nitride layer.

[0022] Furthermore, the second silicon nitride layer is prepared by low pressure chemical vapor deposition.

[0023] Furthermore, the pattern containing the metal material is a single layer or a multi-layer.

[0024] Furthermore, the metal material exhibits a characteristic that resistivity changes with temperature.

[0025] Furthermore, the metal material is Pt.

[0026] Furthermore, the third silicon nitride layer has a thickness of 2000 angstroms and a stress value of 500 MPa.

[0027] Furthermore, when dry etching the release hole, the second silicon nitride layer needs to be etched through.

[0028] Furthermore, the etchant in the wet release process is HF or BOE.

[0029] The method for manufacturing a flow sensor described in the present invention includes forming a lower cavity structure layer on the front side of a silicon wafer by photolithography, etching and oxidation processes, and then sequentially forming a lower support layer, an upper cavity structure layer and an upper support layer on the lower cavity structure layer, and at the same time forming a lateral corrosion barrier layer by photolithography, etching and filling processes. Then, a thermal resistor layer pattern, a passivation layer pattern and a release hole pattern are made on the upper support layer, and finally, the upper cavity structure layer and the lower cavity structure layer are released by a wet etching process to form an upper and lower double-layer thermal insulation cavity. The flow sensor manufactured by the technical solution described in the present invention has good thermal insulation performance and mechanical strength.

[0030] The concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, characteristics and effects of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the planar structure of a temperature resistance sensor structure of a preferred embodiment of the present invention;

[0032] Figure 2 yes Figure 1 The schematic diagram of the cross-sectional structure of the temperature resistance sensor structure shown in the figure along the AA' direction;

[0033] Figure 3-Figure 22 The figure is a schematic cross-sectional structure diagram of a manufacturing process of a temperature resistance sensor according to a preferred embodiment of the present invention. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with specific embodiments and drawings. More details are elaborated in the following description to facilitate a full understanding of the present invention. However, the present invention can obviously be implemented in a variety of other ways different from the description herein. Those skilled in the art can make similar generalizations and deductions based on actual application situations without violating the connotation of the present invention. Therefore, the protection scope of the present invention should not be limited by the contents of this embodiment.

[0035] The invention relates to a temperature resistance sensor, in particular to a device for measuring fluid flow rate by utilizing temperature change. Figure 1 FIG. 1 is a schematic diagram of the planar structure of the temperature resistance sensor structure of this embodiment. Figure 1 In the plan view of the sensor structure shown, a cavity, a heating unit and a temperature measuring unit are included on the substrate. In order to better illustrate the structure of the temperature resistance sensor, a cross-sectional structure schematic diagram of the above sensor structure in the A-A' direction is made, as shown in FIG. Figure 2 As shown. Figure 2 As can be seen in the figure, the heating unit and the temperature measuring unit are formed on a base film with a certain thickness, and the film is suspended above the cavity.

[0036] Those skilled in the art should realize that the above Figure 1 and Figure 2 The distribution diagram of the temperature resistance sensor structure shown is schematic. It should be understood that the positions of the internal units of the temperature resistance sensor structure can be arranged and adjusted as needed, which is within the scope of the protection claimed in the present invention. In addition, the shape and / or size of the heating unit and the temperature measuring unit in the present invention can also be adjusted as needed.

[0037] The manufacturing process of the temperature resistance sensor structure according to the embodiment of the present invention is further described below in conjunction with specific embodiments and drawings.

[0038] Figures 3 to 22 It is a cross-sectional structural diagram of the manufacturing process of a temperature resistance sensor of an embodiment of the present invention. It should be noted that these and other subsequent drawings are only for example, they are not drawn according to the conditions of equal proportion, and should not be used as a limitation on the actual protection scope of the present invention.

[0039] like Figures 3 to 6 As shown, in this embodiment, the substrate 001 takes silicon as an example, but the substrate material that can be used in this embodiment is obviously not limited to this, and those skilled in the art can make corresponding adjustments according to actual needs. First, a first silicon nitride layer 002 is grown on the substrate using an LPCVD process. The role of this silicon nitride layer is to serve as a protective layer for the substrate in the subsequent LOCOS process. Then, the first silicon nitride layer 002 and the substrate 001 are successively etched using a photolithography process and a dry etching process to form a groove 003 (lower cavity structure) in a specified area on the front side of the substrate, wherein the shape and / or depth of the groove can be adjusted according to actual needs. From the top view (not shown), the projection of the groove can be a polygon (including a rectangle), or a circle, and obviously can also be other shapes, which will not be repeated here.

[0040] like Figure 7 As shown, the first silicon oxide layer 005 is grown in the groove 003 using the "Local Oxidation Isolation of Silicon" process (LOCOS). Those skilled in the art should realize that the oxide layer will not grow in the area protected by the first silicon nitride layer 002, and the oxidation reaction only occurs in the groove 003. At the same time, the LOCOS process consumes the silicon at the bottom of the groove 003 while growing the oxide layer. Since LOCOS is the most common process in semiconductor process technology, its specific parameters and formation principle will not be repeated here. After the LOCOS process is completed, the first silicon nitride layer 002 is removed.

[0041] like Figures 8 to 10As shown, the second silicon oxide layer 006, the second silicon nitride layer 007, and the third silicon oxide layer 008 are deposited in sequence. It is explained here that the second silicon nitride layer 007 is a separation layer between the upper and lower parts of the cavity, and its function is to make the device have a stronger structural strength. Compared with a single-layer dielectric as a supporting layer, this embodiment proposes a double-layer isolation dielectric layer (with a cavity) structure, which has higher thermal insulation and structural strength than a single-layer structure. The second silicon nitride layer 007 is the lower auxiliary supporting layer of the double-layer structure. In order to further improve its strength, the second silicon nitride layer 007 is generally prepared by low-pressure chemical vapor deposition (LPCVD). The second silicon oxide layer 006 is used to flatten the surface of the device layer and effectively match the stress of the second silicon nitride layer 007 (silicon nitride is usually tensile stress, and silicon oxide is usually compressive stress). The third silicon oxide layer 008 forms an upper cavity structure, and its thickness determines the depth of the upper half of the thermal insulation wall. Another function of the third silicon oxide layer 008 is to balance the stress of the upper and lower silicon nitride support films. Those skilled in the art should realize that, without considering the complexity of the process and the cost, the purpose described in this embodiment can be achieved by making more supporting layers on the double-layer structure.

[0042] like Figures 11 to 14 As shown, a ring groove structure (such as Figure 1 As shown, the annular groove structure surrounds three cavities, a heating unit and a temperature measuring unit respectively. The depth of the annular groove structure is the total thickness of the second silicon oxide layer 006, the second silicon nitride layer 007, and the third silicon oxide layer 008 by dry etching. Subsequently, the upper main support layer 010 (third silicon nitride layer) of the double-layer structure is deposited by LPCVD, and its typical thickness is 2000 angstroms and the typical stress value is 500Mpa. At the same time, the third silicon nitride layer will fill the annular groove structure to form a lateral corrosion stop layer, and its boundary determines the actual size of the final cavity. Those skilled in the art should recognize that the shape and size of the annular groove structure can be adjusted accordingly according to actual needs. The thickness and stress of the main support layer 010 mentioned above can also be adjusted accordingly according to actual needs. The principle of selection is to match the stress of the multilayer film structure, higher structural strength and slower growth rate (facilitating groove filling).

[0043] like Figures 15 to 17As shown, various graphics 011 containing metal materials are formed on the upper support layer 010 by graphics. The metal-containing material can be a single layer or a multi-layer, and the deposited metal-containing material is characterized in that it can be used as a material for an electric heating device when powered on, and as the temperature changes, the material exhibits the characteristic that the resistivity changes with the temperature. The metal-containing material can be a temperature resistance material such as Pt. It should be clearly pointed out here that the shape, layout, line size, thickness and number of turns of the heating unit and the temperature measuring unit involved in the present invention do not limit the content of the present invention, and can be adjusted according to different needs. After the metal is patterned, the metal is usually alloyed by a 400°C furnace tube process. Then a passivation protective layer 012 is deposited, and a metal PAD window is formed by photolithography and etching processes, and the passivation protective layer can be a single layer or a multi-layer structure.

[0044] like Figures 18 to 22 As shown, when the metal PAD window is formed by photolithography and dry etching processes, a release hole 015 for the cavity structure 003 is formed at the same time. It should be noted here that the lower support layer 007 needs to be etched through when dry etching the release hole. Finally, the third silicon oxide layer 008 in the upper cavity and the first silicon oxide layer 005 and the second silicon oxide layer 006 in the lower cavity are removed by a wet release process (HF or BOE). Finally, a double-layer silicon nitride support structure and a double-layer air cavity insulation structure are formed, while achieving good thermal insulation and mechanical properties. Those skilled in the art should recognize that the shape and / or size and / or number of the release holes can also be adjusted arbitrarily as needed. The release process is not limited to HF or BOE, and the principle of selecting the etching solution is to be able to effectively corrode silicon oxide but not silicon nitride. As Fig. 22 As shown, support point 016 is the support point of the double-layer insulation structure, and its function is to make the double-layer structure stronger, improve the impact resistance, and not easily damaged during the manufacturing process.

[0045] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in the field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in the technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for manufacturing a flow sensor, It is characterized in that The following steps are involved: providing a substrate; growing a first silicon nitride layer on the substrate by low pressure chemical vapor deposition; The first silicon nitride layer and the substrate are successively etched by photolithography and dry etching to form a groove on the substrate; growing a first silicon oxide layer in the groove by a silicon local oxidation isolation process; removing the first silicon nitride layer; sequentially depositing a second silicon oxide layer, a second silicon nitride layer, and a third silicon oxide layer; forming an annular groove structure by photolithography and dry etching, wherein the depth of the annular groove structure is the total thickness of the second silicon oxide layer, the second silicon nitride layer and the third silicon oxide layer; Depositing a third silicon nitride layer by low-pressure chemical vapor deposition, the annular groove structure is filled with the third silicon nitride layer to form a lateral etching stop layer; forming a pattern containing a metal material on the third silicon nitride layer by a patterning process; alloying the pattern by a furnace tube process; Depositing a passivation protective layer; Forming metal PAD windows and release holes by photolithography and etching; The third silicon oxide layer, the first silicon oxide layer and the second silicon oxide layer are removed by a wet release process to form a cavity.

2. The method for manufacturing the flow sensor according to claim 1, It is characterized in that The annular groove structure surrounds the groove in a vertical direction.

3. The method for manufacturing the flow sensor according to claim 1, It is characterized in that The cavity is divided into two upper and lower parts by the second silicon nitride layer.

4. The method for manufacturing a flow sensor according to claim 1, It is characterized in that The second silicon nitride layer is prepared by low pressure chemical vapor deposition.

5. The method for manufacturing the flow sensor according to claim 1, It is characterized in that The pattern containing the metal material is a single layer or a multi-layer.

6. The method for manufacturing the flow sensor according to claim 1, It is characterized in that The metal material exhibits a characteristic that resistivity varies with temperature.

7. The method for manufacturing the flow sensor according to claim 1, It is characterized in that The metal material is Pt.

8. The method for manufacturing the flow sensor according to claim 1, It is characterized in that The third silicon nitride layer has a thickness of 2000 angstroms and a stress value of 500 MPa.

9. The method for manufacturing a flow sensor according to claim 1, It is characterized in that When dry etching the release hole, the second silicon nitride layer needs to be etched through.

10. The method for manufacturing the flow sensor according to claim 1, It is characterized in that The etchant in the wet release process is HF or BOE.